Memory cell, memory device and method for forming the same
By using the interface between dielectric materials and oxide semiconductor layer in semiconductor memory devices to control hydrogen concentration and hydrogen diffusion, combined with ferroelectric materials, the volatile and stability problems of semiconductor memory devices are solved, and the storage performance and data retention capabilities are improved. .
Patent Information
- Application Number
- CN202110241841.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-11
- Filing Date
- 2021-03-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-03-04
AI Technical Summary
After the power outage, existing semiconductor memory devices volatilely store information, resulting in data loss, and hydrogen diffusion leads to device stability problems, affecting memory performance.
Thin film transistor memory unit is used, including the interface between the dielectric material and the oxide semiconductor layer. The hydrogen concentration of the dielectric material does not exceed 3 at%. By controlling the flow rate of the hydrogen precursor and the ratio of the hydrogen-free precursor, hydrogen diffusion is reduced, and combined with ferroelectric materials. Memory film for improved stability.
It improves the stability and data retention capabilities of the memory device, reduces hydrogen diffusion, and enhances the storage performance and reliability of the device.
Smart Images

Figure CN113540114B_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present application relate to memory cells, memory devices, and methods of forming the same. Background Art
[0002] Semiconductor memory is used in integrated circuits for electronic applications including radios, televisions, cell phones, and personal computing devices, as examples. Semiconductor memory includes two main categories. One is volatile memory; the other is nonvolatile memory. Volatile memory includes random access memory (RAM), which can be further divided into two subcategories, static random access memory (SRAM) and dynamic random access memory (DRAM). Both SRAM and DRAM are volatile because they lose the information they store when power is removed.
[0003] On the other hand, non-volatile memories can retain the data stored on them. One type of non-volatile semiconductor memory is ferroelectric random access memory (FeRAM or FRAM). The advantages of FeRAM include fast read / write speeds and a compact size. Summary of the invention
[0004] An embodiment of the present application provides a memory cell, comprising: a thin film transistor located above a semiconductor substrate, the thin film transistor comprising: a memory film contacting a word line; and an oxide semiconductor (OS) layer contacting a source line and a bit line, wherein the memory film is arranged between the OS layer and the word line; and a dielectric material separating the source line and the bit line, wherein the dielectric material forms an interface with the OS layer; wherein the dielectric material comprises hydrogen, and wherein the hydrogen concentration at the interface between the dielectric material and the OS layer does not exceed 3 atomic percent (at%).
[0005] The embodiment of the present application also provides a device, comprising: a semiconductor substrate; a first memory cell located above the semiconductor substrate, the first memory cell comprising a first thin film transistor, wherein the first thin film transistor comprises: a gate electrode comprising a portion of a first word line; a first portion of a ferroelectric material, the first portion of the ferroelectric material being located on a sidewall of the first word line; and a first channel region located on a sidewall of the ferroelectric material, the first channel region comprising hydrogen, and the hydrogen concentration of the first channel region is between 10 20 atoms per cubic centimeter to 10 22atoms per cubic centimeter; a source line, wherein a first portion of the source line provides a first source / drain electrode for the first thin film transistor; a bit line, wherein a first portion of the bit line provides a second source / drain electrode for the first thin film transistor; a first dielectric material separating the source line and the bit line, wherein the first dielectric material physically contacts the first channel region; and a second memory cell located above the first memory cell.
[0006] An embodiment of the present application also provides a method, comprising: patterning a first trench extending through a first conductive line; depositing a memory film along a bottom surface and side walls of the first trench; depositing an oxide semiconductor (OS) layer above the memory film, the OS layer extending along a bottom surface and side walls of the first trench; depositing a first dielectric material above the OS layer and contacting the OS layer, wherein depositing the first dielectric material comprises simultaneously applying a first hydrogen-containing precursor at a first flow rate and a second hydrogen-free precursor at a second flow rate, and wherein a ratio of the second flow rate of the second hydrogen-free precursor to the first flow rate of the first hydrogen-containing precursor is at least 60; and depositing a second dielectric material above the first dielectric material to fill a remaining portion of the first trench.
[0007] Embodiments of the present application provide a memory array isolation structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] When read in conjunction with the accompanying drawings, various aspects of the present invention can be best understood from the following detailed description. It should be noted that, in accordance with standard practice in the industry, the various components are not drawn to scale. In fact, for clarity of discussion, the size of the various components may be arbitrarily increased or reduced.
[0009] Figure 1A , Figure 1B and 1C A perspective view, a circuit diagram, and a top view of a memory array according to some embodiments are shown.
[0010] Figure 2 , Figure 3A , Figure 3B , Figure 4 , Figure 5 , Figure 6 , Figure 7 , Figure 8 , Fig. 9 , Fig.10 , Fig.11 , Fig. 12A , Fig. 12B , Fig.13 , Fig.14 , Fig.15 , Fig.16 , Fig.17A , Fig. 17B , Fig.18A , Fig.18B , Fig.19A , Fig.19B , Fig. 20 , Fig.21 , Fig.22A , Fig. 22B , Fig.23A , Fig. 23B , Fig.23C , Fig.24A , Fig. 24B , Fig.24C , Fig.25A , Fig.25B , Fig.25C , Fig.26A , Fig.26B , Fig.26C , Fig.27A , Fig.27B , Fig.27C , Fig.28A , Fig.28B , Fig.28C and Fig.28D Various diagrams illustrating fabrication of a memory array according to some embodiments are shown.
[0011] Fig.29 , Fig.30 and Fig.31 Various diagrams of memory arrays are shown in accordance with some embodiments.
[0012] Fig.32A and Fig.32B Features of a device according to some embodiments are shown.
[0013] Fig.33A , Fig.33B , Fig.33C and Fig.33D Embodiments of memory arrays in accordance with some embodiments are shown. DETAILED DESCRIPTION
[0014] The following disclosure provides many different embodiments or examples for implementing different components of the present invention. Specific examples of components and arrangements are described below to simplify the present invention. Of course, these are merely examples and are not intended to limit the present invention. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly in contact with each other, and may also include an embodiment in which an additional component may be formed between the first component and the second component so that the first component and the second component may not be in direct contact. In addition, the present invention may repeat reference numbers and / or letters in various examples. This repetition is for the purpose of simplicity and clarity and does not itself indicate the relationship between the various embodiments and / or structures discussed.
[0015] Further, for ease of description, spatially relative terms such as "below," "beneath," "lower," "above," "upper," etc. may be used herein to easily describe the relationship of one element or component to another element or component as shown in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein should likewise be interpreted accordingly.
[0016] Various embodiments provide a 3D memory array having a plurality of vertically stacked memory cells. Each memory cell includes a thin film transistor (TFT) having a word line region as a gate electrode, a bit line region as a first source / drain electrode, and a source line region as a second source / drain electrode. Each TFT also includes an insulating memory film (e.g., as a gate dielectric) and an oxide semiconductor (OS) channel region.
[0017] Figure 1A , Figure 1B and Figure 1C An example of a memory array according to some embodiments is shown. Figure 1A An example of a portion of a memory array 200 is shown in three views; Figure 1B A simplified circuit diagram of a memory array 200 is shown; Figure 1C A top view of a memory array 200 according to some embodiments is shown. The memory array 200 includes a plurality of memory cells 202 that may be arranged in a grid of rows and columns. The memory cells 202 may be further stacked vertically to provide a three-dimensional memory array, thereby increasing device density. The memory array 200 may be disposed in the back end of line (BEOL) of a semiconductor die. For example, the memory array may be disposed in an interconnect layer of a semiconductor die, such as above one or more active devices (e.g., transistors) formed on a semiconductor substrate.
[0018] In some embodiments, the memory array 200 is a flash memory array, such as a NOR flash memory array, etc. Each memory cell 202 may include a thin film transistor (TFT) 204 having an insulating memory film 90 as a gate dielectric. In some embodiments, the gate of each TFT 204 is electrically coupled to a corresponding word line (e.g., conductor 72), the first source / drain region of each TFT 204 is electrically coupled to a corresponding bit line (e.g., conductor 106), and the second source / drain region of each TFT 204 is electrically coupled to a corresponding source line (e.g., conductor 108), which electrically couples the second source / drain region to ground. The memory cells 202 in the same horizontal row of the memory array 200 may share a common word line, while the memory cells 202 in the same vertical column of the memory array 200 may share a common source line and a common bit line.
[0019] The memory array 200 includes a plurality of vertically stacked conductive lines 72 (eg, word lines), and a dielectric layer 52 is disposed between adjacent conductive lines 72. The conductive lines 72 are parallel to the underlying substrate (eg, at Figure 1A and Figure 1B The conductor 72 may have a stepped configuration such that the lower conductor 72 is longer than the upper conductor 72 and extends laterally beyond the end point of the upper conductor 72. For example, Figure 1A , multiple stacked layers of conductors 72 are shown, with the topmost conductor 72 being the shortest and the bottommost conductor 72 being the longest. The respective lengths of the conductors 72 may increase in a direction toward the underlying substrate. In this manner, portions of each conductor 72 may be accessed from above the memory array 200, and conductive contacts may be fabricated to the exposed portions of each conductor 72.
[0020] The memory array 200 also includes a plurality of conductors 106 (e.g., bit lines) and conductors 108 (e.g., source lines). Conductors 106 and 108 may each extend in a direction perpendicular to conductor 72. Dielectric material 98 is disposed between adjacent conductors 106 and 108 and isolates adjacent conductors 106 and 108. In some embodiments, at least a portion of dielectric material 98 is a low hydrogen material formed using a hydrogen-containing precursor introduced at a reduced flow rate. For example, at least a portion of dielectric material 98 (e.g., dielectric material 98A) that physically contacts oxide semiconductor (OS) layer 92 (described below) may have a relatively low hydrogen concentration, such as less than 3 atomic percent (at%). Low hydrogen concentration (e.g., within the above range) may reduce hydrogen diffusion into OS layer 92, thereby reducing defects and improving device stability. For example, by reducing hydrogen diffusion with dielectric material 98 of an embodiment, the threshold voltage (Vth) curve of TFT 204 may be offset in the positive bias direction, enhancing the stability of TFT 204. A relatively low hydrogen concentration in dielectric material 98 can be achieved by, for example, reducing the flow rate of a hydrogen-containing precursor used to deposit dielectric material 98. For example, in embodiments where dielectric material 98 includes silicon oxide, silicon nitride, etc., material 98 can be deposited by a process having a relatively low SiH4 precursor flow rate to suppress H o or H + diffused into dielectric material 98 and OS layer 92 .
[0021] The paired conductive lines 106 and 108 and the intersecting conductive lines 72 define the boundaries of each memory cell 202, and the dielectric material 102 is disposed between and isolates adjacent pairs of conductive lines 106 and 108. In some embodiments, conductive line 108 is electrically coupled to ground. Figure 1AA particular arrangement of conductors 106 relative to conductors 108 is shown, and it should be understood that in other embodiments, the arrangement of conductors 106 and 108 may be reversed.
[0022] As described above, memory array 200 may also include oxide semiconductor (OS) layer 92. OS layer 92 may provide a channel region of memory cell 202 for TFT 204. For example, when an appropriate voltage (e.g., higher than a corresponding threshold voltage (Vth) of corresponding TFT 204) is applied through corresponding conductive line 72, the region of OS layer 92 intersecting conductive line 72 may allow current to flow from conductive line 106 to conductive line 108 (e.g., in the direction indicated by arrow 206). OS layer 92 may have a relatively low hydrogen concentration, such as, as measured by time-of-flight secondary ion mass spectrometry (ToF-SIMS) analysis, at about 10 20 to about 10 22 As a result, the stability of the TFT 204 can be improved compared to a TFT having an OS layer with a higher hydrogen concentration.
[0023] The memory film 90 is disposed between the conductive line 72 and the OS layer 92, and the memory film 90 may provide a gate dielectric for the TFT 204. In some embodiments, the memory film 90 includes a ferroelectric material such as hafnium oxide, hafnium zirconium oxide, silicon-doped hafnium oxide, etc. Accordingly, the memory array 200 may also be referred to as a ferroelectric random access memory (FERAM) array. Alternatively, the memory film 90 may include a plurality of SiO2-doped ferroelectric random access memory layers. x SiN between layers (e.g., ONO structure) x Multilayer structures of layers, different ferroelectric materials, different types of storage layers (e.g., capable of storing bits), etc.
[0024] In an embodiment where the memory film 90 includes a ferroelectric material, the memory film 90 can be polarized in one of two different directions, and the polarization direction can be changed by applying an appropriate voltage difference across the memory film 90 and generating an appropriate electric field. The polarization can be relatively local (e.g., generally contained within each boundary of the memory cell 202), and a continuous region of the memory film 90 can extend across multiple memory cells 202. Depending on the polarization direction of a particular region of the memory film 90, the threshold voltage of the corresponding TFT 204 changes, and a digital value (e.g., 0 or 1) can be stored. For example, when a region of the memory film 90 has a first electrical polarization direction, the corresponding TFT 204 can have a relatively low threshold voltage, and when a region of the memory film 90 has a second electrical polarization direction, the corresponding TFT 204 can have a relatively high threshold voltage. The difference between the two threshold voltages can be referred to as a threshold voltage shift. A larger threshold voltage shift makes it easier to read the digital value stored in the corresponding memory cell 202 (e.g., less error prone).
[0025] In such an embodiment, in order to perform a write operation on the memory cell 202, a write voltage may be applied to the entire portion of the memory film 90 corresponding to the memory cell 202. The write voltage may be applied, for example, by applying an appropriate voltage to the corresponding conductive line 72 (e.g., word line) and the corresponding conductive line 106 / 108 (e.g., bit line / source line). By applying the write voltage to the entire portion of the memory film 90, the polarization direction of the region of the memory film 90 may be changed. As a result, the corresponding threshold voltage of the corresponding TFT 204 may also be switched from a low threshold voltage to a high threshold voltage, or vice versa, and a digital value may be stored in the memory cell 202. Because the conductive line 72 intersects with the conductive lines 106 and 108, a separate memory cell 202 may be selected for a write operation.
[0026] In such an embodiment, to perform a read operation on the memory cell 202, a read voltage (a voltage between the low threshold voltage and the high threshold voltage) is applied to the corresponding conductive line 72 (e.g., a word line). Depending on the polarization direction of the corresponding region of the memory film 90, the TFT 204 of the memory cell 202 may be turned on or off. As a result, the conductive line 106 may be discharged or not discharged through the conductive line 108 (e.g., a source line electrically coupled to ground), and the digital value stored in the memory cell 202 may be determined. Because the conductive line 72 intersects the conductive lines 106 and 108, an individual memory cell 202 may be selected for a read operation.
[0027] Figure 1AReference cross sections of memory array 200 used in subsequent figures are further illustrated. Cross section BB′ is along the longitudinal axis of conductive line 72 and in a direction, for example, parallel to the current flow direction of TFT 204. Cross section CC′ is perpendicular to cross section BB′ and perpendicular to the longitudinal axis of conductive line 72. Cross section CC′ extends through conductive line 106. Cross section D-D′ is parallel to cross section CC′ and extends through dielectric material 102. For clarity, subsequent figures refer to these reference cross sections.
[0028] exist Figure 2 In the invention, a substrate 50 is provided. The substrate 50 may be a semiconductor substrate such as a bulk semiconductor, a semiconductor on insulator (SOI) substrate, which may be doped (e.g., with a p-type or n-type dopant) or undoped. The substrate 50 may be a wafer such as a silicon wafer. Typically, an SOI substrate is a semiconductor material layer formed on an insulator layer. The insulator layer may be, for example, a buried oxide (BOX) layer, a silicon oxide layer, etc. An insulating layer is provided on a substrate of a typical silicon or glass substrate. Other substrates such as multilayer substrates or gradient substrates may also be used. In some embodiments, the semiconductor material of the substrate 50 may include silicon, germanium, a compound semiconductor including silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide and / or indium antimonide, an alloy semiconductor including silicon germanium, gallium arsenide phosphide, aluminum indium arsenide, aluminum gallium arsenide, gallium indium arsenide, gallium indium phosphide and / or gallium indium arsenide phosphide, or a combination thereof.
[0029] Figure 2 Further shown is a circuit that may be formed above the substrate 50. The circuit includes an active device (e.g., a transistor) at the top surface of the substrate 50. The transistor may include a gate dielectric layer 202 located above the top surface of the substrate 50 and a gate electrode 204 located above the gate dielectric layer 202. Source / drain regions 206 are disposed in the substrate 50 on opposite sides of the gate dielectric layer 202 and the gate electrode 204. Gate spacers 208 are formed along the sidewalls of the gate dielectric layer 202 and separate the source / drain regions 206 from the gate electrode 204 by an appropriate lateral distance. In some embodiments, the transistor may be a planar field effect transistor (FET), a fin field effect transistor (finFET), a nano field effect transistor (nanoFET), etc.
[0030] The first ILD 210 surrounds and isolates the source / drain regions 206, the gate dielectric layer 202, and the gate electrode 204, and the second ILD 212 is located above the first ILD 210. The source / drain contacts 214 extend through the second ILD 212 and the first ILD 210 and are electrically coupled to the source / drain regions 206, and the gate contact 216 extends through the second ILD 212 and is electrically coupled to the gate electrode 204. An interconnect structure 220 including one or more stacked dielectric layers 224 and conductive features 222 formed in the one or more dielectric layers 224 is located above the second ILD 212, the source / drain contacts 214, and the gate contact 216. Although Figure 2 Two stacked dielectric layers 224 are shown, it should be understood that the interconnect structure 200 may include any number of dielectric layers 224 having conductive features 222 disposed therein. The interconnect structure 220 may be electrically connected to the gate contact 216 and the source / drain contacts 214 to form a functional circuit. In some embodiments, the functional circuit formed by the interconnect structure 220 may include a logic circuit, a memory circuit, a sense amplifier, a controller, an input / output circuit, an image sensor circuit, etc. or a combination thereof. Although Figure 2 While transistors formed over substrate 50 are discussed, other active devices (eg, diodes, etc.) and / or passive devices (eg, capacitors, resistors, etc.) may be formed as part of functional circuits.
[0031] exist Figure 3A and Figure 3B in Figure 2 The multilayer stack 58 is formed above the structure. For the purpose of simplicity and clarity, the substrate 50, transistors, ILDs, and interconnect structure 120 may be omitted from subsequent figures. Although the multilayer stack 58 is shown as contacting the dielectric layer 224 of the interconnect structure 220, any number of intermediate layers may be disposed between the substrate 50 and the multilayer stack 58. For example, one or more additional interconnect layers including conductive features disposed in an insulating layer (e.g., a low-k dielectric layer) may be disposed between the substrate 50 and the multilayer stack 58. In some embodiments, the conductive features may be patterned to provide for active devices on the substrate 50 and / or the memory array 200 (see Figure 1A and Figure 1B )’s power, ground, and / or signal lines.
[0032] Multilayer stack 58 includes alternating layers of conductive lines 72A-D (collectively, conductive layers 54) and dielectric layers 52A-C (collectively, dielectric layers 52). Conductive layers 54 may be patterned in a subsequent step to define conductive lines 72 (e.g., word lines). Conductive layers 54 may include conductive materials such as copper, titanium, titanium nitride, tantalum, tantalum nitride, tungsten, ruthenium, aluminum, combinations thereof, and the like, and dielectric layers 52 may include insulating materials such as silicon oxide, silicon nitride, silicon oxynitride, combinations thereof, and the like. Conductive layers 54 and dielectric layers 52 may each be formed using, for example, chemical vapor deposition (CVD), atomic layer deposition (ALD), physical vapor deposition (PVD), plasma enhanced CVD (PECVD), and the like. Although Figure 3A and Figure 3B A particular number of conductive layers 54 and dielectric layers 52 are shown, and other embodiments may include different numbers of conductive layers 54 and dielectric layers 52 .
[0033] Figures 4 to 12B is a diagram of an intermediate stage in the fabrication of a staircase structure of a memory array 200 according to some embodiments. Figures 4 to 11 and Fig. 12B It is shown along the reference cross section BB' shown in FIG. 1 . Fig. 12A Shown in a 3D view.
[0034] exist Figure 4 In the embodiment of the present invention, a photoresist 56 is formed over a multilayer stack 58. As described above, the multilayer stack 58 may include alternating layers of conductive layers 54 (labeled 54A, 54B, 54C, and 54D) and dielectric layers 52 (labeled 52A, 52B, and 52C). The photoresist 56 may be formed by using a spin coating technique.
[0035] exist Figure 5 In the embodiment of the present invention, photoresist 56 is patterned to expose multilayer stack 58 in region 60 while masking the remainder of multilayer stack 58. For example, the topmost layer of multilayer stack 58 (e.g., conductive layer 54D) may be exposed in region 60. Photoresist 56 may be patterned using acceptable photolithography techniques.
[0036] exist Figure 6In the embodiment of the present invention, the exposed portion of the multilayer stack 58 in the region 60 is etched using the photoresist 56 as a mask. The etching can be any acceptable etching process, such as by wet etching or dry etching, reactive ion etching (RIE), neutral beam etching (NBE), etc. or a combination thereof. The etching can be anisotropic. The etching can remove the conductive layer 54D and the portion of the dielectric layer 52C in the region 60 and define the opening 61. Because the conductive layer 54D and the dielectric layer 52C have different material compositions, the etchant used to remove the exposed portions of these layers can be different. In some embodiments, while etching the conductive layer 54D, the dielectric layer 52C acts as an etch stop layer, and while etching the dielectric layer 52C, the conductive layer 54C acts as an etch stop layer. As a result, portions of the conductive layer 54D and the dielectric layer 52C can be selectively removed without removing the remaining layers of the multilayer stack 58, and the opening 61 can extend to a desired depth. Optionally, after the opening 61 reaches the desired depth, a timed etching process can be used to stop etching the opening 61. In the resulting structure, conductive layer 54C is exposed in region 60 .
[0037] exist Figure 7 In the embodiment of the present invention, photoresist 56 is trimmed to expose additional portions of multilayer stack 58. The photoresist may be trimmed using acceptable photolithography techniques. As a result of the trimming, the width of photoresist 56 is reduced, and portions of multilayer stack 58 in regions 60 and 62 may be exposed. For example, the top surface of conductive layer 54C may be exposed in region 60, and the top surface of conductive layer 54D may be exposed in region 62.
[0038] exist Figure 854D, dielectric layer 52C, portions of conductive layer 54C and dielectric layer 52B in regions 60 and 62 are removed by an acceptable etching process using photoresist 56 as a mask. Etching can be any acceptable etching process, such as by wet etching or dry etching, reactive ion etching (RIE), neutral beam etching (NBE), etc. or a combination thereof. Etching can be anisotropic. Etching can extend opening 61 further into multilayer stack 58. Because conductive layer 54D / 54C and dielectric layer 52C / 52B have different material compositions, the etchants used to remove exposed portions of these layers can be different. In some embodiments, dielectric layer 52C acts as an etch stop layer while etching conductive layer 54D, and conductive layer 54C acts as an etch stop layer while etching dielectric layer 52C; dielectric layer 52B acts as an etch stop layer while etching conductive layer 54C; and conductive layer 54B acts as an etch stop layer while etching dielectric layer 52B. As a result, portions of conductive layer 54D / 54C and dielectric layer 52C / 52B can be selectively removed without removing the remaining layers of multilayer stack 58, and opening 61 can extend to a desired depth. Further, during the etching process, the unetched portions of conductive layer 54 and dielectric layer 52 act as a mask for the underlying layers, and as a result, the previous pattern of conductive layer 54D and dielectric layer 52C can be transferred to the underlying conductive layer 54C and dielectric layer 52B. In the resulting structure, conductive layer 54B is exposed in region 60, and conductive layer 54C is exposed in region 62.
[0039] exist Fig. 9 5. In the embodiment of the present invention, photoresist 56 is trimmed to expose additional portions of multilayer stack 58. The photoresist may be trimmed using acceptable photolithography techniques. As a result of the trimming, the width of photoresist 56 is reduced, and portions of multilayer stack 58 may be exposed in regions 60, 62, and 64. For example, the top surface of conductive layer 54B may be exposed in region 60; the top surface of conductive layer 54C may be exposed in region 62; and the top surface of conductive layer 54D may be exposed in region 64.
[0040] exist Fig.10In the embodiment of the present invention, portions of the conductive layers 54D, 54C, and 54B in regions 60, 62, and 64 are removed by an acceptable etching process using the photoresist 56 as a mask. The etching may be any acceptable etching process, such as by wet etching or dry etching, reactive ion etching (RIE), neutral beam etching (NBE), etc., or a combination thereof. The etching may be anisotropic. The etching may extend the opening 61 further into the multilayer stack 58. In some embodiments, while etching the conductive layer 54D, the dielectric layer 52C serves as an etch stop layer; while etching the conductive layer 54C, the dielectric layer 52B serves as an etch stop layer; and while etching the conductive layer 54B, the dielectric layer 52A serves as an etch stop layer. As a result, portions of the conductive layers 54D, 54C, and 54B may be selectively removed without removing the remaining layers of the multilayer stack 58, and the opening 61 may be extended to a desired depth. Further, during the etching process, each dielectric layer 52 serves as a mask for the layers below, and as a result, the dielectric layers 52C / 52B (see Fig. 9 ) is transferred to the underlying conductive layer 54C / 54B. In the resulting structure, dielectric layer 52A is exposed in region 60; dielectric layer 52B is exposed in region 62; and dielectric layer 52C is exposed in region 64.
[0041] exist Fig.11 , the photoresist 56 can be removed, such as by an acceptable ashing or wet stripping process. Thus, a stair structure 68 is formed. The stair structure includes a stack of alternating conductive layers 54 and dielectric layers 52. The lower conductive layer 54 is wider and extends laterally beyond the upper conductive layer 54, and the width of each conductive layer 54 increases in a direction toward the substrate 50. For example, conductive layer 54A can be longer than conductive layer 54B; conductive layer 54B can be longer than conductive layer 54C; and conductive layer 54C can be longer than conductive layer 54D. As a result, in subsequent process steps, conductive contacts to each conductive layer 54 can be made from above the stair structure 68.
[0042] In FIG. 12 , an intermetallic dielectric (IMD) 70 is deposited over the multilayer stack 58. The IMD 70 may be formed of a dielectric material and may be deposited by any suitable method such as CVD, plasma enhanced CVD (PECVD), or FCVD. The dielectric material may include phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), undoped silicate glass (USG), etc. Other insulating materials formed by any acceptable process may be used. The IMD 70 extends along the sidewalls of the conductive layer 54 and the sidewalls of the dielectric layer 52. Further, the IMD 70 may contact the top surface of each dielectric layer 52.
[0043] 12 , a removal process is then applied to IMD 70 to remove excess dielectric material located above multilayer stack 58. In some embodiments, a planarization process such as chemical mechanical polishing (CMP), an etch-back process, a combination thereof, etc. may be utilized. The planarization process exposes multilayer stack 58 such that after the planarization process is completed, the top surfaces of IMD 70 and multilayer stack 58 are level.
[0044] Figures 13 to 17B is a diagram of an intermediate stage in the fabrication of a memory array 200 according to some embodiments. Figures 13 to 17B In the embodiment, a multilayer stack 58 is formed, and trenches are formed in the multilayer stack 58, thereby defining conductive lines 72. The conductive lines 72 may correspond to word lines in the memory array 200, and the conductive lines 72 may further provide gate electrodes for the resulting TFTs of the memory array 200. Fig.17A Shown in a 3D view. Figures 13 to 16 and Fig. 17B is along Figure 1A The reference section CC' shown in FIG.
[0045] exist Fig.13 In the embodiment of the present invention, a hard mask 80 and a photoresist 82 are deposited over the multilayer stack 58. The hard mask layer 80 may include, for example, silicon nitride, silicon oxynitride, etc., which may be deposited by CVD, PVD, ALD, PECVD, etc. For example, the photoresist 82 may be formed by using a spin coating technique.
[0046] exist Fig.14 In the embodiment of the present invention, the photoresist 82 is patterned to form grooves 86. The photoresist can be patterned using an acceptable photolithography technique. For example, the photoresist 82 is exposed to light for patterning. After the exposure process, depending on whether a negative resist or a positive resist is used, the photoresist 82 is developed to remove the exposed or unexposed portions of the photoresist, thereby defining a pattern that forms the grooves 86.
[0047] exist Fig.15 In the embodiment of the present invention, the pattern of the photoresist 82 is transferred to the hard mask 80 using an acceptable etching process, such as by wet etching or dry etching, reactive ion etching (RIE), neutral beam etching (NBE), etc. or a combination thereof. The etching can be anisotropic. Thus, a trench 86 extending through the hard mask 80 is formed. For example, the photoresist 82 can be removed by an ashing process.
[0048] exist Fig.16In the embodiment of the present invention, the pattern of the hard mask 80 is transferred to the multilayer stack 58 using one or more acceptable etching processes, such as by wet etching or dry etching, reactive ion etching (RIE), neutral beam etching (NBE), etc. or a combination thereof. The etching can be anisotropic. Therefore, the trench 86 extends through the multilayer stack 58, and the conductive lines 72 (e.g., word lines) are formed by the conductive layer 54. By etching the trench 86 through the conductive layer 54, adjacent conductive lines 72 can be spaced apart from each other. Subsequently, in Fig.17A and Fig. 17B The hard mask 80 may then be removed by an acceptable process such as a wet etching process, a dry etching process, a planarization process, a combination thereof, etc. Due to the stepped shape of the multilayer stack 58 (see, e.g., FIG. 12 ), the conductive lines 72 may have varying lengths that increase in a direction toward the substrate 50. For example, the conductive line 72A may be longer than the conductive line 72B; the conductive line 72B may be longer than the conductive line 72C; and the conductive line 72C may be longer than the conductive line 72D.
[0049] FIG. 18A to FIG. 23C The formation and patterning of the TFT 204 (see FIG. Figure 1A ) channel region. Fig.18A , Fig.19A and Fig.23A is shown in a three-dimensional view. Fig.18B , Fig.19B , Fig. 20 , Fig.21 , Fig.22A , Fig. 22B and Fig. 23B Provided along the Figure 1A Cross-sectional view along line CC'. Fig.23C A corresponding top view of the TFT structure is shown.
[0050] exist Fig.18A and Fig.18B 8, a memory film 90 is conformally deposited in the trench 86. The memory film 90 may have a material capable of storing a bit, such as a material that can be switched between two different polarization directions by applying an appropriate voltage difference across the memory film 90. For example, the polarization of the memory film 90 may change due to an electric field generated by the applied voltage difference.
[0051] For example, the memory film 90 may be a high-k dielectric material, such as a hafnium-based (Hf) dielectric material, etc. In some embodiments, the memory film 90 includes a ferroelectric material such as hafnium oxide, hafnium zirconium oxide, silicon-doped hafnium oxide, etc. In other embodiments, the memory 90 may be a multilayer structure (e.g., an ONO structure) including a SiNx layer disposed between two SiOx layers. In other embodiments, the memory film 90 may include different ferroelectric materials or different types of memory materials. The memory film 90 may be deposited by CVD, PVD, ALD, PECVD, etc. to extend along the sidewalls and bottom surface of the trench 86. After the memory film 90 is deposited, an annealing step (e.g., in a temperature range of about 300° C. to 600° C.) may be performed to achieve a desired crystalline phase, improve film quality, and reduce film-related defects / impurities for the memory film 90. In some embodiments, the annealing step may be further below 400° C. to meet the BEOL thermal budget and reduce defects that may result from the high temperature annealing process that cause other components.
[0052] exist Fig.19A and Fig.19B In the embodiment, the OS layer 92 is conformally deposited in the trench 86 above the memory film 90. The OS layer 92 includes a suitable material for providing a TFT (eg, TFT 204, see Figure 1A ) of the channel region. In some embodiments, the OS layer 92 includes an indium-containing material, such as In x Ga y Zn z MO, where M can be Ti, Al, Ag, Si, Sn, etc. X, Y, and Z can each be any value between 0 and 1. In other embodiments, different semiconductor materials can be used for the OS layer 92. The OS layer 92 can be deposited by CVD, PVD, ALD, PECVD, etc. The OS layer 92 can extend along the sidewalls and bottom surface of the trench 86 above the FE layer 90. After depositing the OS layer 92, an annealing step (e.g., in a temperature range of about 300°C to about 450°C or in a range of about 300°C to about 400°C) can be performed in an oxygen-related environment to activate the charge carriers of the OS layer 92.
[0053] exist Fig. 20In the embodiment, dielectric material 98A is deposited on the sidewalls and bottom surface of trench 86 and is located above OS layer 92. Dielectric material 98A may include, for example, silicon oxide, silicon nitride, silicon oxynitride, etc., which may be deposited by CVD, PVD, ALD, PECVD, etc. In some embodiments, depositing dielectric material 98A may include reducing the flow rate of a hydrogen-containing precursor, so that dielectric material 98A having a relatively low hydrogen concentration is formed. For example, in an embodiment where dielectric material 98A is a silicon-containing insulating material (e.g., silicon oxide, silicon nitride, silicon oxynitride, etc.), a first hydrogen-containing precursor (e.g., silane (SiH4), tetraethyl silicate (TEOS), etc.) and a second hydrogen-free precursor may be applied simultaneously during the deposition process. Because the first hydrogen-containing precursor is used. When dielectric material 98A includes silicon oxide, the second hydrogen-free precursor may be, for example, N2O, and when dielectric material 98A includes silicon nitride, the second hydrogen-free precursor may be, for example, NH3. Using the flow rate of the first hydrogen-containing precursor, hydrogen ions (e.g., H + ) and / or hydrogen species (H o ) can diffuse into the OS layer 92 through the dielectric material 98A, resulting in instability of the resulting transistor. Accordingly, various embodiments improve the stability of the transistor by reducing the flow rate of the first hydrogen-containing precursor. For example, the ratio of the flow rate of the second hydrogen-free precursor to the flow rate of the first hydrogen-containing precursor can be at least 60. It has been observed that by keeping the precursor flow rate within the above ratio, the hydrogen diffused into the OS layer 92 can be reduced to a desired level and the device stability can be improved.
[0054] In some embodiments, after the dielectric material 98A is deposited, the hydrogen concentration of the OS layer 92 may be about 10 20 Atoms per cubic centimeter about 10 22 atoms per cubic centimeter. Fig.32A A graph 300 of hydrogen concentration (e.g., curve 302) in the OS layer 92 and the dielectric material 98A according to some embodiments is shown. In the graph 300, the x-axis represents the sputtering time corresponding to the detection time (e.g., distance) during the ToF-SIMs analysis. By maintaining the hydrogen concentration of the OS layer 92 within this range, the threshold voltage characteristic curve of the resulting transistor 204 can be shifted in the positive bias direction, enhancing the stability of the transistor. For example, Fig.32BA graph 304 depicting a threshold voltage characteristic curve 306 of a first transistor and a threshold voltage characteristic curve 308 of a second transistor is shown. The first transistor (e.g., corresponding to curve 306) has a channel region (e.g., OS layer) having a hydrogen concentration exceeding the above range, and the second transistor (e.g., corresponding to curve 308) has a channel region having a hydrogen concentration within the above range. Arrow 310 indicates a positive bias direction offset of the threshold voltage characteristic curve 308 compared to the threshold voltage characteristic curve 306.
[0055] As a result of the example deposition process, the hydrogen concentration in dielectric material 98A may be relatively low. For example, when dielectric material 98A includes silicon oxide (e.g., SiO x ), the hydrogen concentration of dielectric material 98A may be greater than 0 and less than 5 at%. As another example, when dielectric material 98A includes silicon nitride (eg, SiN x ), the total hydrogen concentration of dielectric material 98A can be greater than 0 and less than 10 at%. The total hydrogen concentration at interface 96 between OS layer 92 and dielectric material 98A can be less than about 3 at%. Maintaining the hydrogen concentration of dielectric material 98A within these ranges can achieve advantages such as reduced diffusion into OS layer 92 and improved transistor stability.
[0056] exist Fig.21 In the embodiment, for example, a combination of photolithography and etching is used to remove the bottom of the dielectric material 98A in the trench 86. The etching can be any acceptable etching process, such as by wet etching or dry etching, reactive ion etching (RIE), neutral beam etching (NBE), etc. or a combination thereof. The etching can be anisotropic.
[0057] Then, as Fig.21 As shown, dielectric material 98A may be used as an etching mask to etch through the bottom of OS layer 92 in trench 86. Etching may be any acceptable etching process, such as by wet etching or dry etching, reactive ion etching (RIE), neutral beam etching (NBE), etc. or a combination thereof. Etching may be anisotropic. Etching OS layer 92 may expose portions of memory film 90 located on the bottom surface of trench 86. Thus, portions of OS layer 92 located on opposite sidewalls of trench 86 may be spaced apart from each other, which improves the memory array 200 (see Figure 1A ) between memory cells 202.
[0058] exist Fig.22A and Fig. 22B In the embodiment, additional dielectric material 98B or dielectric material 98C may be deposited to fill the remaining portion of trench 86. Fig.22AIn some embodiments, dielectric material 98B can have the same material composition and be formed using a process similar to dielectric material 98A. For example, dielectric material 98B can be formed using a deposition process of a hydrogen-containing precursor having a relatively low flow rate. In some embodiments, dielectric material 98B can be formed using a deposition process in which the ratio of the flow rate of a hydrogen-free precursor (e.g., N2O) to the flow rate of a hydrogen-containing precursor (e.g., SiH4) is at least 60. In some embodiments, the respective ratios of the flow rate of the hydrogen-free precursor to the flow rate of the hydrogen-containing precursor used to deposit dielectric material 98B and to deposit dielectric material 98A can be the same. As a result, the hydrogen concentration of dielectric material 98B is relatively low. For example, when dielectric material 98B includes silicon oxide (e.g., SiO x ), the total hydrogen concentration of dielectric material 98B may be greater than 0 and less than 5 at%. As another example, when dielectric material 98B includes silicon nitride (eg, SiN x ), the total hydrogen concentration of the dielectric material 98B can be greater than 0 and less than 10 at %.
[0059] Fig. 22B An alternative embodiment of a memory array 200' is shown in which a dielectric material 98C is deposited to fill the remaining portion of the trench 86 instead of the dielectric material 98B. The dielectric material 98C may have a different material composition than the dielectric material 98A and may be formed using a different process than the dielectric material 98A. The dielectric material 98C may include, for example, silicon oxide, silicon nitride, silicon oxynitride, etc., which may be deposited by CVD, PVD, ALD, PECVD, etc. However, depositing the dielectric material 98C may include increasing the inflow of a hydrogen-containing precursor compared to the dielectric material 98A. As a result, the formed dielectric material 98C has a relatively high hydrogen concentration. For example, in an embodiment where the dielectric material 98C is a silicon-containing insulating material (e.g., silicon oxide, silicon nitride, silicon oxynitride, etc.), a third hydrogen-containing precursor (e.g., SiH4, TEOS, etc.) and a fourth hydrogen-free precursor may be simultaneously flowed during the deposition process. When dielectric material 98C comprises silicon oxide, the fourth hydrogen-free precursor may be, for example, N2O, and when dielectric material 98C comprises silicon nitride, the fourth hydrogen-free precursor may be, for example, NH3. For example, the ratio of the flow rate of the second hydrogen-free precursor to the flow rate of the first hydrogen-containing precursor may be greater than 60, such as up to 70. It has been observed that maintaining the precursor flow rates at the above ratios, the hydrogen concentration of dielectric material 98C may be greater than the hydrogen concentration of dielectric material 98A. For example, when dielectric material 98C comprises silicon oxide (e.g., SiO x ), the total hydrogen concentration of the dielectric material 98C may be about 1×10 21 Atom / cm 3 Up to 1×10 22 Atom / cm 3 As another example, when the dielectric material 98C includes silicon nitride (e.g., SiNx ), the total hydrogen concentration of the dielectric material 98C may be greater than 1×10 22 Atom / cm 3 Because relatively low hydrogen concentration dielectric material 98A separates relatively high hydrogen concentration dielectric material 98C and OS layer 92 , the high hydrogen concentration in dielectric material 98C may not significantly degrade the device performance of the resulting transistor, and the benefits described above may still be achieved.
[0060] For ease of explanation, the following figures show Fig.22A Further processing of the embodiment of the present invention (for example, wherein the dielectric material 98B and the dielectric material 98A have the same material composition). The dielectric material 98B and the dielectric material 98A may be collectively referred to as the dielectric material 98 hereinafter. It should be understood that the dielectric material 98 may be Fig. 22B Embodiments where dielectric material 98C and dielectric material 98A have different material compositions (eg, wherein dielectric material 98C and dielectric material 98A have different material compositions) apply similar processing. FIG. 33A to FIG. 33C Shown according to Fig. 22B The memory array 200' of the embodiment.
[0061] exist FIG. 23A to FIG. 23C In the embodiment of the present invention, a removal process is then applied to dielectric material 98, OS layer 92, and memory film 90 to remove excess material located above multilayer stack 58. In some embodiments, a planarization process such as chemical mechanical polishing (CMP), an etch-back process, a combination thereof, etc. may be utilized. The planarization process exposes multilayer stack 58 so that the top surface of multilayer stack 58 is level after the planarization process is completed. Fig.23C Shows Fig.23A A corresponding top view of the structure shown in FIG.
[0062] FIG. 24A to FIG. 27C An intermediate step in fabricating conductive lines 106 and 108 (e.g., source lines and bit lines) in memory array 200 is shown. Conductive lines 106 and 108 may extend in a direction perpendicular to conductive line 72, thereby allowing individual cells of memory array 200 to be selected for read and write operations. FIG. 24A to FIG. 27C In the figure, the figure ending with "A" shows a 3D view. The figure ending with "B" shows a top view, and the figure ending with "C" shows the Figure 1A Corresponding cross-sectional view parallel to line CC'.
[0063] exist Fig.24A , Fig. 24B and Fig.24C In the embodiment of the present invention, trenches 100 are patterned to pass through OS layer 92 and dielectric material 98 (including dielectric material 98A and dielectric material 98B). Fig.24C Shows Fig. 24B2 is a cross-sectional view of the line CC' in FIG. For example, the patterning of the groove 100 may be performed by a combination of photolithography and etching. The groove 100 may be disposed between opposite side walls of the memory film 90, and the groove 100 may be disposed between the memory array 200 (see FIG. Figure 1A ) are physically separated from adjacent stacks of memory cells.
[0064] exist Fig.25A , Fig.25B and Fig.25C In the process, a dielectric material 102 is deposited in the trench 100 and fills the trench 100 . Fig.25C Shows Fig.25B . The dielectric layer 102 may include, for example, silicon oxide, silicon nitride, silicon oxynitride, etc., which may be deposited by CVD, PVD, ALD, PECVD, etc. The dielectric layer 102 may extend along the sidewalls and bottom surface of the trench 86 located above the OS layer 92. After deposition, a planarization process (e.g., CMP, etch back, etc.) may be performed to remove excess portions of the dielectric material 102. In the resulting structure, the top surfaces of the multilayer stack 58, the memory film 90, the OS layer 92, and the dielectric material 102 may be substantially horizontal (e.g., within process variations). In some embodiments, the materials of the dielectric materials 98 and 102 may be selected so that they may be selectively etched relative to each other. For example, in some embodiments, the dielectric material 98 is an oxide and the dielectric material 102 is a nitride. In some embodiments, the dielectric material 98 is a nitride and the dielectric material 102 is an oxide. Other materials are also possible.
[0065] exist Fig.26A , Fig.26B and Fig.26C In FIG. 1 , patterned trenches 104 are used for conductive lines 106 and 108 . Fig.26C Shows Fig.26B 1. A cross-sectional view of line CC' in FIG. The trench 104 is patterned by patterning dielectric material 98 (including dielectric material 98A and dielectric material 98C) using, for example, a combination of photolithography and etching.
[0066] For example, a photoresist 118 may be deposited over the multilayer stack 58, the dielectric material 98, the dielectric material 102, the OS layer 92, and the memory film 90. The photoresist 118 may be formed by using, for example, a spin coating technique. The photoresist 118 is patterned to define openings 120. Each opening 120 may overlap a corresponding region of the dielectric material 102, and each opening 120 may further partially expose two spaced-apart regions of the dielectric material 98. For example, each opening 120 may expose a region of the dielectric material 102; partially expose a first region of the dielectric material 98; and partially expose a second region of the dielectric material 98, which is spaced apart from the first region of the dielectric material 98 by a region of the dielectric material 102. In this manner, each opening 120 may define a pattern of the conductive wire 106 and adjacent conductive wires 108 spaced apart by the dielectric material 102. The photoresist may be patterned using an acceptable photolithography technique. For example, the photoresist 120 is exposed to light for patterning. After the exposure process, the photoresist 118 may be developed to remove exposed or unexposed portions of the photoresist, depending on whether a negative resist or a positive resist is used, thereby defining the pattern of the formed openings 120 .
[0067] Subsequently, the portion of dielectric material 98 exposed by opening 122 may be removed by, for example, etching. The etching may be any acceptable etching process, such as by wet etching or dry etching, reactive ion etching (RIE), neutral beam etching (NBE), etc. or a combination thereof. The etching may be anisotropic. The etching process may use an etchant that etches dielectric material 98 without significantly etching dielectric material 102. As a result, even though opening 122 exposes dielectric material 102, dielectric material 102 may not be significantly removed. The pattern of trench 104 may correspond to conductive lines 106 and 108 (see Fig.27A , Fig.27B and Fig.27C ). For example, portions of dielectric material 98 between each pair of trenches 104 may remain, and dielectric material 102 may be disposed between adjacent pairs of trenches 104. After patterning the trenches 104, the photoresist 118 may be removed by, for example, ashing.
[0068] exist Fig.27A , Fig.27B and Fig.27C In the embodiment of the present invention, trench 104 is filled with a conductive material to form conductive lines 106 and 108 . Fig.27C Shows Fig.27B. Wires 106 and 108 may each include a conductive material, such as copper, titanium, titanium nitride, tantalum, tantalum nitride, tungsten, ruthenium, aluminum, combinations thereof, and the like, which may each be formed using, for example, CVD, ALD, PVD, PECVD, and the like. After depositing wires 106 and 108, planarization (e.g., CMP, etch back, etc.) may be performed to remove excess portions of the conductive material, thereby forming wires 106 and 108. In the resulting structure, the top surfaces of the multilayer stack 58, memory film 90, OS layer 92, wire 106, and wire 108 may be substantially horizontal (e.g., within process variations). Wire 106 may correspond to a bit line in a memory array, and wire 108 may correspond to a source line in memory array 200. Although Fig.27C A cross-sectional view showing only conductor 106 is shown, and a cross-sectional view of conductor 108 may be similar.
[0069] Thus, stacked TFTs 204 may be formed in the memory array 200. Each TFT 204 includes a gate electrode (e.g., a portion of a corresponding conductive line 72), a gate dielectric (e.g., a portion of a corresponding memory film 90), a channel region (e.g., a portion of a corresponding OS layer 92), and source and drain electrodes (e.g., portions of corresponding conductive lines 106 and 108). The dielectric material 102 isolates adjacent TFTs 204 in the same column and at the same vertical level. The TFTs 204 may be arranged in an array of vertically stacked rows and columns.
[0070] exist Fig.28A , Fig.28B , Fig.28C and Fig.28D In the embodiment of the present invention, contacts 110 are made to wire 72 , wire 106 , and wire 108 . Fig.28A shows a perspective view of a memory array 200; Fig.28B shows a top view of memory array 200; and Fig.28C Shown along Fig.28A A cross-sectional view of the device and underlying substrate along line 28C'-28C'. Fig.28D Shown along Figure 1A' is a cross-sectional view of the device along line BB' of . In some embodiments, the stepped shape of the wire 72 can provide a surface located on each wire 72 for the conductive contact 110 to fall on it. Forming the contact 110 can include patterning the IMD 70 and the opening in the dielectric layer 52 using a combination of, for example, photolithography and etching to expose a portion of the conductive layer 54. A liner (not shown) such as a diffusion barrier layer, an adhesion layer, etc. and a conductive material are formed in the opening. The liner can include titanium, titanium nitride, tantalum, tantalum nitride, etc. The conductive material can be copper, copper alloy, silver, gold, tungsten, cobalt, aluminum, nickel, etc. A planarization process such as CMP can be performed to remove excess material from the surface of the IMD 70. The remaining liner and conductive material form the contact 110 in the opening.
[0071] Also like Fig.28A As shown in the perspective view of FIG. 1 , conductive contacts 112 and 114 may be made to conductors 106 and 108, respectively. Conductive contacts 110, 112, and 114 may be electrically connected to conductors 116A, 116B, and 116C, respectively, which connect the memory array to underlying / overhead circuitry (e.g., control circuitry) and / or signal, power, and ground lines in the semiconductor die. For example, conductive vias 118 may extend through IMD 70 to electrically connect conductor 116C to underlying circuitry of interconnect structure 220 and active devices located on substrate 50, such as Fig.28C Other conductive vias may be formed through IMD 70 to electrically connect conductors 116A and 116B to the underlying circuitry of interconnect structure 220. In alternative embodiments, wiring and / or power lines to and from the memory array may be provided by an interconnect structure formed above memory array 200 in addition to or in lieu of interconnect structure 220. Thus, memory array 200 may be completed.
[0072] although Figures 2 to 28B The embodiments of the present invention show a specific pattern for the conductors 106 and 108, and other configurations are also possible. For example, in these embodiments, the conductors 106 and 108 have a staggered pattern. In some embodiments, the conductors 106 and 108 in the same row of the array are all aligned with each other. Fig.29 shows a top view, and Fig.30 Shown along Fig.29 Cross-sectional view along line CC′. Fig.31 Shown along Fig.29 A cross-sectional view of line DD′. Fig.29 , Fig.30 and Fig.31 In the present invention, similar reference numerals denote Figures 2 to 28B Similar components are formed by similar processes.
[0073] Fig.33A , Fig.33B , Fig.33C and Fig.33D It shows that according to the above Fig. 22B An alternative embodiment of a memory array 200' is described and shown. Fig.33A shows a perspective view of a memory array 200; Fig.33B shows a top view of a memory array 200; Fig.33C Shown along Fig.33A A cross-sectional view of the substrate and device below line 30C'-30C'; and Fig.33D Shown along Figure 1A 2 is a cross-sectional view of a device taken along line BB' of FIG. 2. Memory array 200' can be similar to memory array 200, wherein like reference numerals represent like elements formed using like processes. However, dielectric material 98B is replaced with dielectric material 98C, and dielectric material 98C has a different material composition than dielectric material 98A. For example, as described above, dielectric material 98C can have a higher hydrogen concentration than dielectric material 98A. This can be achieved, for example, by increasing the flow rate of the hydrogen-containing precursor while depositing dielectric material 98C as compared to depositing dielectric material 98A.
[0074] Various embodiments provide a 3D memory array with vertically stacked memory cells. Each memory cell includes a TFT having a memory film, a gate dielectric material, and an oxide semiconductor channel region. The TFT includes a source / drain electrode that is also a source line and a bit line in the memory array. The dielectric material is disposed between adjacent source / drain electrodes and isolates adjacent source / drain electrodes. In some embodiments, at least a portion of the dielectric material is a low hydrogen material formed using a hydrogen-containing precursor introduced at a reduced flow rate. For example, at least a portion of the dielectric material (e.g., a layer) that physically contacts the channel region of the TFT may have a relatively low hydrogen concentration, such as less than 3at%. The low hydrogen concentration (e.g., within the above range) may reduce hydrogen diffusion into the channel region, thereby reducing defects and improving stability. A relatively low hydrogen concentration may be achieved in the dielectric material by, for example, reducing the flow rate of the hydrogen-containing precursor used to deposit the dielectric material.
[0075] In some embodiments, a memory cell includes a thin film transistor located above a semiconductor substrate. The thin film transistor includes a memory film contacting a word line; and an oxide semiconductor (OS) layer contacting a source line and a bit line, wherein the memory film is disposed between the OS layer and the word line; and a dielectric material separating the source line and the bit line. The dielectric material forms an interface with the OS layer. The dielectric material includes hydrogen, and the hydrogen concentration at the interface between the dielectric material and the OS layer does not exceed 3 atomic percent (at%). Optionally, in some embodiments, the dielectric material includes: a first dielectric material contacting the OS layer, the first dielectric material extending continuously from the source line to the bit line; and a second dielectric material located on the side of the first dielectric material opposite to the OS layer, the second dielectric material extending continuously from the source line to the bit line, the second dielectric material having a hydrogen concentration greater than that of the first dielectric material. Optionally, in some embodiments, the dielectric material includes silicon oxide, and the total hydrogen concentration of the dielectric material is greater than 0at% and less than 5at%. Optionally, in some embodiments, the dielectric material includes silicon nitride, and the total hydrogen concentration of the dielectric material is greater than 0at% and less than 10at%. Optionally, in some embodiments, the OS layer includes hydrogen. Optionally, in some embodiments, the hydrogen concentration of the OS layer is between 10 20 atoms per cubic centimeter to 10 22 In some embodiments, the longitudinal axis of the word line extends parallel to the main surface of the semiconductor substrate, the longitudinal axis of the source line extends perpendicular to the main surface of the semiconductor substrate, and the longitudinal axis of the bit line extends perpendicular to the main surface of the semiconductor substrate.
[0076] In some embodiments, a device includes: a semiconductor substrate; a first memory cell located above the semiconductor substrate, the first memory cell including a first thin film transistor, wherein the first thin film transistor includes: a gate electrode including a portion of a first word line; a first portion of a ferroelectric material, the first portion of the ferroelectric material being located on a sidewall of the first word line; and a first channel region located on the sidewall of the ferroelectric material, the first channel region including hydrogen, and the hydrogen concentration of the first channel region is between 10 20 atoms per cubic centimeter to 10 22atoms per cubic centimeter; a source line, wherein a first portion of the source line provides a first source / drain electrode for a first thin film transistor; a bit line, wherein a first portion of the bit line provides a second source / drain electrode for the first thin film transistor; a first dielectric material separating the source line and the bit line, wherein the first dielectric material physically contacts the first channel region; and a second memory cell located above the first memory cell. Optionally, in some embodiments, the second memory cell includes a second thin film transistor, wherein a second portion of the source line provides a first source / drain electrode for the second thin film transistor, and wherein a second portion of the bit line provides a second source / drain electrode for the second thin film transistor. Optionally, in some embodiments, the device further includes a second word line located above the first word line, wherein a gate electrode of the second thin film transistor includes a portion of the second word line, and wherein the first word line is longer than the second word line. Optionally, in some embodiments, the hydrogen concentration at the interface between the first dielectric material and the first channel region is less than 3 atomic percent. Optionally, in some embodiments, the device further comprises a second dielectric material separating the source line and the bit line, the second dielectric material being separated from the first channel region by the first dielectric material, and the first dielectric material having a different material composition than the second dielectric material. Optionally, in some embodiments, the second dielectric material has a hydrogen concentration greater than the hydrogen concentration of the first dielectric material.
[0077] In some embodiments, a method includes patterning a first trench extending through a first conductive line; depositing a memory film along a bottom surface and sidewalls of the first trench; depositing an oxide semiconductor (OS) layer over the memory film, the OS layer extending along a bottom surface and sidewalls of the first trench; depositing a first dielectric material over the OS layer and contacting the OS layer, wherein depositing the first dielectric material includes simultaneously applying a first flow rate of a first hydrogen-containing precursor and a second flow rate of a second hydrogen-free precursor, and wherein a ratio of the second flow rate of the second hydrogen-free precursor to the first flow rate of the first hydrogen-containing precursor is at least 60; and depositing a second dielectric material over the first dielectric material to fill a remaining portion of the first trench. Optionally, in some embodiments, depositing the second dielectric material includes simultaneously applying a third hydrogen-containing precursor at a third flow rate and a fourth hydrogen-free precursor at a fourth flow rate, and wherein a ratio of the fourth flow rate of the fourth hydrogen-free precursor to the third flow rate of the third hydrogen-containing precursor is the same as a ratio of the second flow rate of the second hydrogen-free precursor to the first flow rate of the first hydrogen-containing precursor. Optionally, in some embodiments, depositing the second dielectric material includes simultaneously applying a third hydrogen-containing precursor at a third flow rate and a fourth hydrogen-free precursor at a fourth flow rate, and wherein the third flow rate of the third hydrogen-containing precursor is greater than the first flow rate of the first hydrogen-containing precursor. Optionally, in some embodiments, the method further includes patterning a third trench in the first dielectric material and the second dielectric material; patterning a fourth trench in the first dielectric material and the second dielectric material; and filling the third trench and the fourth trench with a conductive material to define a source line and a bit line. Optionally, in some embodiments, the first hydrogen-containing precursor is silane (SiH4) and the second hydrogen-free precursor is N2O. Optionally, in some embodiments, after depositing the first dielectric material, the hydrogen concentration at the interface between the first dielectric material and the OS layer is 3at% or less. Optionally, in some embodiments, depositing the first dielectric material includes diffusing hydrogen into the OS layer.
[0078] An embodiment of the present application provides a memory cell, comprising: a thin film transistor located above a semiconductor substrate, the thin film transistor comprising: a memory film contacting a word line; and an oxide semiconductor (OS) layer contacting a source line and a bit line, wherein the memory film is arranged between the OS layer and the word line; and a dielectric material separating the source line and the bit line, wherein the dielectric material forms an interface with the OS layer; wherein the dielectric material comprises hydrogen, and wherein the hydrogen concentration at the interface between the dielectric material and the OS layer does not exceed 3 atomic percent (at%).
[0079] In some embodiments, the dielectric material includes: a first dielectric material contacting the OS layer, the first dielectric material extending continuously from the source line to the bit line; and a second dielectric material located on a side of the first dielectric material opposite to the OS layer, the second dielectric material extending continuously from the source line to the bit line, the hydrogen concentration of the second dielectric material being greater than the hydrogen concentration of the first dielectric material.
[0080] In some embodiments, the dielectric material includes silicon oxide, and the total hydrogen concentration of the dielectric material is greater than 0 at% and less than 5 at%. In some embodiments, the dielectric material includes silicon nitride, and the total hydrogen concentration of the dielectric material is greater than 0 at% and less than 10 at%. In some embodiments, the OS layer includes hydrogen. In some embodiments, the hydrogen concentration of the OS layer is greater than 10 at%. 20 atoms per cubic centimeter to 10 22 In some embodiments, the longitudinal axis of the word line extends parallel to the main surface of the semiconductor substrate, the longitudinal axis of the source line extends perpendicular to the main surface of the semiconductor substrate, and the longitudinal axis of the bit line extends perpendicular to the main surface of the semiconductor substrate.
[0081] The embodiment of the present application also provides a device, comprising: a semiconductor substrate; a first memory cell located above the semiconductor substrate, the first memory cell comprising a first thin film transistor, wherein the first thin film transistor comprises: a gate electrode comprising a portion of a first word line; a first portion of a ferroelectric material, the first portion of the ferroelectric material being located on a sidewall of the first word line; and a first channel region located on a sidewall of the ferroelectric material, the first channel region comprising hydrogen, and the hydrogen concentration of the first channel region is between 10 20 atoms per cubic centimeter to 10 22 atoms per cubic centimeter; a source line, wherein a first portion of the source line provides a first source / drain electrode for the first thin film transistor; a bit line, wherein a first portion of the bit line provides a second source / drain electrode for the first thin film transistor; a first dielectric material separating the source line and the bit line, wherein the first dielectric material physically contacts the first channel region; and a second memory cell located above the first memory cell.
[0082] In some embodiments, the second memory cell includes a second thin film transistor, wherein the second portion of the source line provides a first source / drain electrode for the second thin film transistor, and wherein the second portion of the bit line provides a second source / drain electrode for the second thin film transistor. In some embodiments, it also includes: a second word line located above the first word line, wherein the gate electrode of the second thin film transistor includes a portion of the second word line, and wherein the first word line is longer than the second word line. In some embodiments, the hydrogen concentration at the interface between the first dielectric material and the first channel region is less than 3 atomic percent. In some embodiments, it also includes: a second dielectric material that separates the source line and the bit line, the second dielectric material is separated from the first channel region by the first dielectric material, and the first dielectric material has a different material composition than the second dielectric material. In some embodiments, the hydrogen concentration of the second dielectric material is greater than the hydrogen concentration of the first dielectric material.
[0083] An embodiment of the present application also provides a method, comprising: patterning a first trench extending through a first conductive line; depositing a memory film along a bottom surface and side walls of the first trench; depositing an oxide semiconductor (OS) layer above the memory film, the OS layer extending along a bottom surface and side walls of the first trench; depositing a first dielectric material above the OS layer and contacting the OS layer, wherein depositing the first dielectric material comprises simultaneously applying a first hydrogen-containing precursor at a first flow rate and a second hydrogen-free precursor at a second flow rate, and wherein a ratio of the second flow rate of the second hydrogen-free precursor to the first flow rate of the first hydrogen-containing precursor is at least 60; and depositing a second dielectric material above the first dielectric material to fill a remaining portion of the first trench.
[0084] In some embodiments, depositing the second dielectric material comprises simultaneously applying a third hydrogen-containing precursor at a third flow rate and a fourth hydrogen-free precursor at a fourth flow rate, and wherein the ratio of the fourth flow rate of the fourth hydrogen-free precursor to the third flow rate of the third hydrogen-containing precursor and the ratio of the second flow rate of the second hydrogen-free precursor to the first flow rate of the first hydrogen-containing precursor are the same. In some embodiments, depositing the second dielectric material comprises simultaneously applying a third hydrogen-containing precursor at a third flow rate and a fourth hydrogen-free precursor at a fourth flow rate, and wherein the third flow rate of the third hydrogen-containing precursor is greater than the first flow rate of the first hydrogen-containing precursor. In some embodiments, further comprising: patterning a third trench in the first dielectric material and the second dielectric material; patterning a fourth trench in the first dielectric material and the second dielectric material; and filling the third trench and the fourth trench with a conductive material to define a source line and a bit line. In some embodiments, the first hydrogen-containing precursor is silane (SiH4), and the second hydrogen-free precursor is N2O. In some embodiments, after depositing the first dielectric material, a hydrogen concentration at an interface between the first dielectric material and the OS layer is 3 at % or less. In some embodiments, depositing the first dielectric material includes diffusing hydrogen into the OS layer.
[0085] The features of several embodiments are summarized above so that those skilled in the art can better understand the various aspects of the present invention. Those skilled in the art should understand that they can easily use the present invention as a basis to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those skilled in the art should also appreciate that such equivalent constructions do not deviate from the spirit and scope of the present invention, and that they can make various changes, substitutions and modifications herein without deviating from the spirit and scope of the present invention.
Claims
1. A memory cell, comprising: A thin film transistor is located above a semiconductor substrate, and the thin film transistor comprises: a memory film contacting the word line; and an oxide semiconductor layer contacting a source line and a bit line, wherein the memory film is provided between the oxide semiconductor layer and the word line; and a dielectric material separating the source line from the bit line, wherein the dielectric material forms an interface with the oxide semiconductor layer; wherein the dielectric material comprises hydrogen, and wherein a concentration of hydrogen at the interface between the dielectric material and the oxide semiconductor layer does not exceed 3 atomic percent, Wherein, the dielectric material comprises: a first dielectric material contacting the oxide semiconductor layer, the first dielectric material continuously extending from the source line to the bit line; and A second dielectric material is located on a side of the first dielectric material opposite to the oxide semiconductor layer, the second dielectric material continuously extending from the source line to the bit line, and the second dielectric material has a hydrogen concentration greater than that of the first dielectric material.
2. The memory cell according to claim 1, wherein: A hydrogen concentration at the interface between the first dielectric material and the oxide semiconductor layer is less than 3 atomic percent.
3. The memory cell according to claim 1, wherein: The dielectric material includes silicon oxide, and a total hydrogen concentration of the dielectric material is greater than 0 atomic percent and less than 5 atomic percent.
4. The memory cell according to claim 1, wherein: The dielectric material includes silicon nitride, and a total hydrogen concentration of the dielectric material is greater than 0 atomic percent and less than 10 atomic percent.
5. The memory cell according to claim 1, wherein: The oxide semiconductor layer includes hydrogen.
6. The memory cell according to claim 1, wherein: The hydrogen concentration of the oxide semiconductor layer is 10 20 atoms per cubic centimeter to 10 22 atoms per cubic centimeter.
7. The memory cell according to claim 1, wherein the longitudinal axis of the word line extends parallel to the main surface of the semiconductor substrate, the longitudinal axis of the source line extends perpendicular to the main surface of the semiconductor substrate, and the longitudinal axis of the bit line extends perpendicular to the main surface of the semiconductor substrate.
8. A storage device comprising: Semiconductor substrate; A first memory unit is located above the semiconductor substrate, wherein the first memory unit includes a first thin film transistor, wherein the first thin film transistor includes: a gate electrode including a portion of the first word line; a first portion of a ferroelectric material, the first portion of the ferroelectric material being located on a sidewall of the first word line; and A first channel region is located on the sidewall of the ferroelectric material, the first channel region includes hydrogen, and the hydrogen concentration of the first channel region is 10 20 atoms per cubic centimeter to 10 22 atoms per cubic centimeter; a source line, wherein a first portion of the source line provides a first source / drain electrode for the first thin film transistor; a bit line, wherein a first portion of the bit line provides a second source / drain electrode for the first thin film transistor; a first dielectric material separating the source line and the bit line, wherein the first dielectric material physically contacts the first channel region; a second dielectric material separating the source line and the bit line, the second dielectric material being separated from the first channel region by the first dielectric material, and the first dielectric material having a material composition different from that of the second dielectric material; and The second memory unit is located above the first memory unit.
9. The memory device according to claim 8, wherein: The second memory cell includes a second thin film transistor, wherein the second portion of the source line provides a first source / drain electrode for the second thin film transistor, and wherein the second portion of the bit line provides a second source / drain electrode for the second thin film transistor.
10. The memory device according to claim 9, further comprising: A second word line is located above the first word line, wherein the gate electrode of the second thin film transistor includes a portion of the second word line, and wherein the first word line is longer than the second word line.
11. The memory device according to claim 8, wherein: A hydrogen concentration at an interface between the first dielectric material and the first channel region is less than 3 atomic percent.
12. The memory device according to claim 8, wherein: The first dielectric material includes silicon oxide or silicon nitride.
13. The memory device according to claim 8, wherein: The second dielectric material has a hydrogen concentration greater than a hydrogen concentration of the first dielectric material.
14. A method of forming a memory device, comprising: patterning a first trench extending through the first conductive line; depositing a memory film along a bottom surface and sidewalls of the first trench; depositing an oxide semiconductor layer over the memory film, the oxide semiconductor layer extending along a bottom surface and sidewalls of the first trench; depositing a first dielectric material over and contacting the oxide semiconductor layer, wherein depositing the first dielectric material comprises simultaneously applying a first flow rate of a first hydrogen-containing precursor and a second flow rate of a second hydrogen-free precursor, and wherein a ratio of the second flow rate of the second hydrogen-free precursor to the first flow rate of the first hydrogen-containing precursor is at least 60; and A second dielectric material is deposited over the first dielectric material to fill a remaining portion of the first trench.
15. The method for forming a memory device according to claim 14, wherein: Depositing the second dielectric material comprises simultaneously applying a third flow rate of a third hydrogen-containing precursor and a fourth flow rate of a fourth hydrogen-free precursor, and wherein a ratio of the fourth flow rate of the fourth hydrogen-free precursor to the third flow rate of the third hydrogen-containing precursor is the same as a ratio of the second flow rate of the second hydrogen-free precursor to the first flow rate of the first hydrogen-containing precursor.
16. The method for forming a memory device according to claim 14, wherein: Depositing the second dielectric material includes simultaneously applying a third flow rate of a third hydrogen-containing precursor and a fourth flow rate of a fourth hydrogen-free precursor, and wherein the third flow rate of the third hydrogen-containing precursor is greater than the first flow rate of the first hydrogen-containing precursor.
17. The method for forming a memory device according to claim 14, further comprising: patterning third trenches in the first dielectric material and the second dielectric material; patterning fourth trenches in the first dielectric material and the second dielectric material; as well as The third trench and the fourth trench are filled with a conductive material to define a source line and a bit line.
18. The method according to claim 14, wherein: The first hydrogen-containing precursor is silane (SiH4), and the second hydrogen-free precursor is N2O.
19. The method for forming a memory device according to claim 14, wherein: After depositing the first dielectric material, a hydrogen concentration at an interface between the first dielectric material and the oxide semiconductor layer is 3 atomic percent or less.
20. The method for forming a memory device according to claim 14, wherein: Depositing the first dielectric material includes diffusing hydrogen into the oxide semiconductor layer.
Citation Information
Patent Citations
Stability enhancement in metal-oxide-semiconductor thin-film transistors
CN102265405A
Thin film transistor and display device
CN104584200A
Thin film trnasistor having hydrogen blocking layer and display device comprising same
CN109768082A
Thin film transistor and method for manufacturing same
US20150084042A1
Three dimensional ferroelectric memory
US20200075631A1