Lithium borate compound, additive for lithium secondary battery, non-aqueous electrolyte for lithium secondary battery, lithium secondary battery precursor, and method for producing lithium secondary battery

By using a nonaqueous electrolyte containing lithium borate compound and a cyclic carbonate in a lithium secondary battery, the problem of high resistance of lithium secondary battery is solved, the stability and performance of the battery are improved, and the battery resistance is reduced and the battery resistance is reduced. Improved stability.

CN113557238BActive Publication Date: 2024-11-01MITSUI CHEMICALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080020059.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-14
Filing Date
2020-03-12
Publication Date
2024-11-01
Estimated Expiration
2040-03-12

AI Technical Summary

Technical Problem

The existing lithium secondary batteries have a high battery resistance after storage and charging and discharging cycles, which affects the stability and performance of the battery.

Method used

The lithium secondary battery nonaqueous electrolyte containing lithium borate compound is used. By adding lithium borate compound and cyclic carbonate with unsaturated bonds to the electrolyte, the internal resistance of the battery is reduced, and the stability of the battery is improved by maturation treatment.

Benefits of technology

It effectively reduces the battery resistance after storage and charging and discharging cycle of lithium secondary batteries, improves the stability and performance of the battery, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113557238B_ABST
    Figure CN113557238B_ABST
Patent Text Reader

Abstract

The present invention provides a lithium borate compound represented by the following formula (I). 1 , R 2 and R 3 Each independently represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. 10 It represents a fluorine atom, a hydrocarbonoxy group having 1 to 10 carbon atoms, a hydrocarbon group having 1 to 10 carbon atoms, or a fluorinated hydrocarbon group having 1 to 10 carbon atoms. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a novel lithium borate compound, an additive for a lithium secondary battery, a non-aqueous electrolyte for a lithium secondary battery, a lithium secondary battery precursor, and a method for producing a lithium secondary battery. Background Art

[0002] Lithium borate compounds are used, for example, in the field of electrochemistry.

[0003] For example, an electrolyte for a lithium ion battery containing lithium bis(oxalate)borate as an electrolyte is known (for example, see Patent Document 1). In addition, for example, an electrolyte for a lithium ion battery containing lithium difluoro(oxalate)borate as an electrolyte is also known (for example, see Patent Document 2).

[0004] Patent Document 1: Japanese Patent No. 3730855

[0005] Patent Document 2: Japanese Patent No. 3722685 Summary of the invention

[0006] Problems to be solved by the invention

[0007] An object of one embodiment of the present disclosure is to provide a novel lithium borate compound and an additive for a lithium secondary battery containing the lithium borate compound.

[0008] In addition, another aspect of the present disclosure is to provide a non-aqueous electrolyte for a lithium secondary battery that can reduce the battery resistance after storage and after charge and discharge cycles, a lithium secondary battery precursor containing the above-mentioned non-aqueous electrolyte for a lithium secondary battery, and a method for manufacturing a lithium secondary battery using the above-mentioned lithium secondary battery precursor.

[0009] Means for solving problems

[0010] The above-mentioned means for solving the problems include the following aspects.

[0011] <1> A lithium borate compound represented by the following formula (I).

[0012] [Chemical formula 1]

[0013]

[0014] [In formula (I), R 1 , R 2 and R 3 Each independently represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. 10 represents a fluorine atom, a hydrocarbyloxy group having 1 to 10 carbon atoms, a hydrocarbon group having 1 to 10 carbon atoms, or a fluorinated hydrocarbon group having 1 to 10 carbon atoms.]

[0015] <2> The lithium borate compound as described in <1>, wherein the R 10 It is a fluorine atom, an alkoxy group having 1 to 3 carbon atoms, an alkyl group having 1 to 3 carbon atoms, or a perfluoroalkyl group having 1 to 3 carbon atoms.

[0016] <3> The lithium borate compound as described in <1> or <2>, wherein the R 10 It is trifluoromethyl.

[0017] <4> The lithium borate compound according to any one of <1> to <3>, wherein R 1 , the above R 2 And the above R 3 Each is independently methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, vinyl, allyl, ethynyl, phenyl, or 4-fluorophenyl.

[0018] <5> The lithium borate compound according to any one of <1> to <4>, which is a lithium borate compound represented by the following formula (II), the following formula (III), the following formula (IV), or the following formula (V).

[0019] [Chemical formula 2]

[0020]

[0021] <6> An additive for a lithium secondary battery, comprising the lithium borate compound according to any one of <1> to <5>.

[0022] <7> A non-aqueous electrolyte for a lithium secondary battery, comprising: an electrolyte that is a lithium salt containing fluorine; a non-aqueous solvent; and the lithium borate compound according to any one of <1> to <5>.

[0023] <8> The non-aqueous electrolyte for lithium secondary batteries according to <7>, wherein the content of the lithium borate compound is 0.1% by mass to 5.0% by mass based on the total amount of the non-aqueous electrolyte for lithium secondary batteries.

[0024] <9> The nonaqueous electrolyte for lithium secondary batteries according to <7> or <8>, further comprising a cyclic carbonate having an unsaturated bond.

[0025] <10> The non-aqueous electrolyte for a lithium secondary battery according to <9>, wherein the cyclic carbonate having an unsaturated bond is vinylene carbonate.

[0026] <11> The non-aqueous electrolyte for a lithium secondary battery according to <10>, wherein a ratio of the content mass of the vinylene carbonate to the content mass of the lithium borate compound is in the range of 0.1 to 10.

[0027] <12> A lithium secondary battery precursor comprising:

[0028] a housing; and

[0029] The positive electrode, negative electrode, separator, and electrolyte contained in the shell,

[0030] The positive electrode is a positive electrode that can absorb and release lithium ions.

[0031] The negative electrode is a negative electrode that can absorb and release lithium ions.

[0032] The electrolyte solution is the non-aqueous electrolyte solution for a lithium secondary battery according to any one of <7> to <11>.

[0033] <13> A method for manufacturing a lithium secondary battery, comprising the following steps:

[0034] A step of preparing the lithium secondary battery precursor described in <12>; and,

[0035] a step of obtaining a lithium secondary battery by subjecting the lithium secondary battery precursor to an aging treatment,

[0036] The aging treatment includes charging and discharging the lithium secondary battery precursor in an environment of 20° C. to 60° C.

[0037] Effects of the Invention

[0038] According to one embodiment of the present disclosure, a novel lithium borate compound and an additive for a lithium secondary battery including the lithium borate compound are provided.

[0039] In addition, according to another embodiment of the present disclosure, there are provided a non-aqueous electrolyte for a lithium secondary battery that can reduce the battery resistance after storage and after charge and discharge cycles, a lithium secondary battery precursor containing the non-aqueous electrolyte for a lithium secondary battery, and a method for manufacturing a lithium secondary battery using the lithium secondary battery precursor. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] [ Figure 1 ] is a schematic three-dimensional diagram showing an example of a lithium secondary battery of the present disclosure, that is, an example of a laminated battery.

[0041] [ Figure 2 ] to accommodate Figure 1 Schematic cross-sectional view of a laminated electrode body in the thickness direction of the laminated battery shown.

[0042] [ Figure 3 ] is a schematic cross-sectional view showing another example of the lithium secondary battery of the present disclosure, namely, an example of a button-type battery. DETAILED DESCRIPTION

[0043] In the present specification, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit.

[0044] In the present specification, when the amount of each component in the composition contains a plurality of substances belonging to each component, unless otherwise specified, it means the total amount of the plurality of substances present in the composition.

[0045] In the present specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process can be achieved.

[0046] 〔Lithium borate compounds〕

[0047] The lithium borate compound of the present disclosure is a novel lithium borate compound represented by the following formula (I). Hereinafter, the lithium borate compound represented by formula (I) is also referred to as a "lithium borate compound".

[0048] [Chemical formula 3]

[0049]

[0050] In formula (I), R 1 , R 2 and R 3 Each independently represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent.

[0051] The hydrocarbon group having 1 to 20 carbon atoms means a group having 1 to 20 carbon atoms in a skeleton formed only of a hydrocarbon group having no substituent.

[0052] In formula (I), R 1 , R 2 and R 3 Each is independently a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, and preferably R 1 , R 2 and R 3 Two or more of them are hydrocarbon groups having 1 to 20 carbon atoms which may have the same substituent, and R 1 , R 2 and R 3 These three groups are all hydrocarbon groups having 1 to 20 carbon atoms and may have the same substituent.

[0053] As R 1 ~R 3 Examples of the hydrocarbon group having 1 to 20 carbon atoms which may have a substituent include an aryl group having 6 to 20 carbon atoms which may have a substituent and an aliphatic group having 1 to 20 carbon atoms which may have a substituent.

[0054] Examples of the aryl group having 6 to 20 carbon atoms which may have a substituent include: phenyl; groups obtained by removing one hydrogen atom from an alkylbenzene (e.g., benzyl, tolyl, xylyl, mesityl, etc.); naphthyl; groups obtained by removing one hydrogen atom from an alkyl substituted naphthalene; and the like.

[0055] Among the above, as the aryl group having 6 to 20 carbon atoms which may have a substituent, a phenyl group, a 4-methylphenyl group or a 4-fluorophenyl group is preferred, and a phenyl group or a 4-fluorophenyl group is more preferred.

[0056] Among the aryl groups having 6 to 20 carbon atoms which may have a substituent, examples of the substituent that the aryl group may have (hereinafter also referred to as "the substituent that may be contained in formula (I)") include a halogen atom, an unsubstituted alkyl group, a halogenated alkyl group, an unsubstituted alkoxy group, a halogenated alkoxy group, an unsubstituted alkenyl group, a halogenated alkenyl group, an unsubstituted alkynyl group, and a halogenated alkynyl group. Among the above, the substituent that may be contained in formula (I) is preferably a halogen atom.

[0057] As the halogen atom which may be a substituent in formula (I), a fluorine atom, a chlorine atom, a bromine atom or an iodine atom is preferred, a fluorine atom, a chlorine atom or a bromine atom is more preferred, a fluorine atom or a chlorine atom is further preferred, and a fluorine atom is particularly preferred.

[0058] Preferred embodiments of the halogen atom contained in the structures of the haloalkyl, haloalkoxy, haloalkenyl, and haloalkynyl groups which may be substituents in formula (I) are the same as the preferred embodiments of the halogen atom as a substituent which may be contained in formula (I).

[0059] The unsubstituted alkyl group which may be a substituent in formula (I) is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and still more preferably an alkyl group having 1 to 3 carbon atoms.

[0060] As the unsubstituted alkoxy group which may be a substituent in formula (I), an alkoxy group having 1 to 12 carbon atoms is preferred, an alkoxy group having 1 to 6 carbon atoms is more preferred, and an alkoxy group having 1 to 3 carbon atoms is further preferred.

[0061] The unsubstituted alkenyl group which may be a substituent in formula (I) is preferably an alkenyl group having 2 to 12 carbon atoms, more preferably an alkenyl group having 2 to 6 carbon atoms, and still more preferably an alkenyl group having 2 to 3 carbon atoms.

[0062] The unsubstituted alkynyl group which may be a substituent in formula (I) is preferably an alkynyl group having 2 to 12 carbon atoms, more preferably an alkynyl group having 2 to 6 carbon atoms, and still more preferably an alkynyl group having 2 to 3 carbon atoms.

[0063] The preferred range of the number of carbon atoms in each of the haloalkyl, haloalkoxy, haloalkenyl, and haloalkynyl groups which may be substituents in formula (I) is the same as the preferred range of the number of carbon atoms in the unsubstituted alkyl, unsubstituted alkoxy, unsubstituted alkenyl, and unsubstituted alkynyl groups which may be substituents in formula (I).

[0064] The aliphatic group having 1 to 20 carbon atoms which may have a substituent may be a saturated aliphatic group (ie, an alkyl group) or an unsaturated aliphatic group (ie, an alkenyl group or an alkynyl group).

[0065] The aliphatic group having 1 to 20 carbon atoms which may have a substituent may be linear, branched or cyclic.

[0066] The aliphatic group having 1 to 20 carbon atoms which may have a substituent is preferably an aliphatic group having 1 to 16 carbon atoms, and more preferably an aliphatic group having 1 to 12 carbon atoms.

[0067] Examples of the aliphatic group having 1 to 12 carbon atoms include:

[0068] A straight-chain or branched saturated aliphatic group (i.e., alkyl) such as methyl, ethyl, n-propyl, isopropyl, 1-ethylpropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, 2-methylbutyl, 3,3-dimethylbutyl, n-pentyl, isopentyl, neopentyl, 1-methylpentyl, n-hexyl, isohexyl, sec-hexyl, tert-hexyl, n-heptyl, isoheptyl, sec-heptyl, tert-heptyl, n-octyl, isooctyl, sec-octyl, tert-octyl, nonyl, decyl, undecyl, and dodecyl;

[0069] Straight-chain or branched unsaturated aliphatic groups (i.e., alkenyl or alkynyl) such as vinyl, 1-propenyl, allyl (2-propenyl), isopropenyl, 1-butenyl, 2-butenyl, 3-butenyl, pentenyl, hexenyl, 2-methyl-2-propenyl, 1-methyl-2-propenyl, 2-methyl-1-propenyl, hexenyl, ethynyl, 1-propynyl, 2-propynyl (same meaning as propargyl), 1-butynyl, 2-butynyl, 3-butynyl, 1-pentynyl, 2-pentynyl, 3-pentynyl, 4-pentynyl, 5-hexynyl, 1-methyl-2-propynyl, 2-methyl-3-butynyl, 2-methyl-3-pentynyl, 1-methyl-2-butynyl, 1,1-dimethyl-2-propynyl, 1,1-dimethyl-2-butynyl, and 1-hexynyl;

[0070] Cyclic aliphatic groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, 1-cyclopentenyl, 1-cyclohexenyl, etc.; and the like.

[0071] Among the above, as R 1 ~R3 The aliphatic group having 1 to 12 carbon atoms represented by alkyl is preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-hexyl group, an n-octyl group, a vinyl group, an allyl group, or an ethynyl group, and more preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a vinyl group, an allyl group, or an ethynyl group.

[0072] In the aliphatic group having 1 to 20 carbon atoms which may be contained in formula (I) and may have a substituent, the substituent which the aliphatic group may have is the same as the preferred embodiment of the substituent which the aryl group may have.

[0073] R in formula (I) 1 , R 2 and R 3 Each is independently preferably methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, vinyl, allyl, ethynyl, phenyl, or 4-fluorophenyl.

[0074] In formula (I), R 10 It represents a fluorine atom, a hydrocarbyloxy group having 1 to 10 carbon atoms, a hydrocarbon group having 1 to 10 carbon atoms, or a fluorinated hydrocarbon group having 1 to 10 carbon atoms.

[0075] R 10 The hydrocarbyloxy group having 1 to 10 carbon atoms may be a linear hydrocarbyloxy group or a hydrocarbyloxy group having a branched chain and / or a ring structure.

[0076] As R 10 The number of carbon atoms in the hydrocarbonoxy group having 1 to 10 carbon atoms represented by is preferably 1 to 6, more preferably 1 to 3, further preferably 1 or 2, and particularly preferably 1.

[0077] R 10 The hydrocarbon group having 1 to 10 carbon atoms represented by may be a linear hydrocarbon group or a hydrocarbon group having a branched chain and / or a ring structure.

[0078] As R 10 The hydrocarbon group having 1 to 10 carbon atoms represented by is preferably an alkyl group or an aryl group, and more preferably an alkyl group.

[0079] As R 10 The number of carbon atoms in the hydrocarbon group having 1 to 10 represented by is preferably 1 to 6, more preferably 1 to 3, further preferably 1 or 2, and particularly preferably 1.

[0080] R 10 The fluorinated hydrocarbon group having 1 to 10 carbon atoms represented by may be a linear fluorinated hydrocarbon group or a fluorinated hydrocarbon group having a branched chain and / or a ring structure.

[0081] As R 10The fluorinated hydrocarbon group having 1 to 10 carbon atoms represented by is preferably a fluorinated alkyl group or a fluorinated aryl group, more preferably a fluorinated alkyl group, further preferably a perfluoroalkyl group, and particularly preferably a trifluoromethyl group (-CF3).

[0082] Among the above, R 10 Preferred are fluorine atoms, alkoxy groups having 1 to 3 carbon atoms, alkyl groups having 1 to 3 carbon atoms, and perfluoroalkyl groups having 1 to 3 carbon atoms, and more preferred are trifluoromethyl groups (—CF 3 ).

[0083] Preferred specific examples of the lithium borate compound represented by formula (I) include lithium borate compounds represented by the following formula (II), the following formula (III), the following formula (IV) and the following formula (V). However, the lithium borate compound represented by formula (I) is not limited to these specific examples.

[0084] [Chemical formula 4]

[0085]

[0086] [An example of a method for producing a lithium borate compound (production method X)]

[0087] An example of a method for producing a lithium borate compound of the present disclosure (Production Method X) is shown below. However, the method for producing a lithium borate compound of the present disclosure is not limited to Production Method X.

[0088] Preparation method X includes the following steps: a first reaction step, in which (trifluoromethyl)trimethylsilane, potassium halide and borate compound are reacted in a solvent to obtain a potassium borate compound as a reaction intermediate; and a second reaction step, in which the potassium borate compound and lithium halide are reacted in a solvent to obtain the lithium borate compound of the present disclosure.

[0089] Examples of the potassium halide in the first reaction step include potassium fluoride, potassium chloride, potassium bromide, and potassium iodide, and among these, potassium fluoride and potassium chloride are more preferred. The potassium halide may be used alone or in combination of two or more.

[0090] As the borate compound in the first reaction step, trimethyl borate, triethyl borate, tri-n-propyl borate, triisopropyl borate, tri-n-butyl borate, triisobutyl borate, tri-sec-butyl borate, tri-tert-butyl borate, trihexyl borate, tricyclohexyl borate, trioctyl borate, triphenyl borate, etc. can be cited, preferably trimethyl borate, triethyl borate, tri-n-propyl borate, triisopropyl borate, tri-n-butyl borate, tricyclohexyl borate, triphenyl borate, etc., among which trimethyl borate, triethyl borate, triisopropyl borate, or tri-n-butyl borate is more preferred. The borate compound can be used alone or in combination of two or more.

[0091] Examples of the lithium halide in the second reaction step include lithium fluoride, lithium chloride, lithium bromide, and lithium iodide, and lithium fluoride or lithium chloride is more preferred. The lithium halide may be used alone or in combination of two or more.

[0092] As the solvent in the first reaction step and the second reaction step, for example, acetone, ethyl acetate, acetonitrile, tetrahydrofuran, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, pentane, hexane, heptane, octane, nonane, decane, toluene, xylene (i.e., o-xylene, m-xylene, or p-xylene), ethylbenzene, butylbenzene, pentylbenzene, hexylbenzene, heptylbenzene, propylbenzene, isopropylbenzene (also known as cumene), cyclohexylbenzene, tetralin, mesitylene, methylcyclopentane, cyclohexane, methylcyclohexane, cycloheptane, cyclooctane, cyclononane and other non-aqueous solvents can be mentioned. The solvent can be used alone or in combination of two or more.

[0093] The first reaction step and the second reaction step may be performed under normal pressure or under reduced pressure.

[0094] The first reaction step and the second reaction step may be performed in either an air atmosphere or an inert atmosphere.

[0095] For example, from the viewpoint of preventing the mixing of components (such as water) that inhibit the formation of potassium borate compounds and lithium borate compounds, the first reaction step and the second reaction step are preferably carried out under an inert atmosphere (for example, an inert gas atmosphere such as nitrogen or argon).

[0096] The reaction temperature in the first reaction step is preferably 0°C to 120°C, more preferably 10°C to 100°C, and even more preferably 20°C to 80°C.

[0097] From the viewpoint of efficiently producing the potassium borate compound, the reaction time in the first reaction step is preferably 30 minutes to 48 hours, more preferably 1 hour to 30 hours.

[0098] The reaction temperature in the second reaction step is preferably 10°C to 150°C, more preferably 20°C to 120°C, and even more preferably 40°C to 100°C.

[0099] When the reaction temperature in the second reaction step is 10° C. or higher, the formation of the lithium borate compound is easily promoted. On the other hand, when the reaction temperature in the second reaction step is 150° C. or lower, the decomposition of the generated lithium borate compound is suppressed, and the formation rate is easily increased.

[0100] From the viewpoint of efficiently producing the lithium borate compound, the reaction time in the second reaction step is preferably 30 minutes to 12 hours, and more preferably 30 minutes to 8 hours.

[0101] The second reaction step may be a method of directly mixing the reaction solution obtained after the first reaction step with the lithium halide, or a method of mixing the solid obtained by distilling off the product such as halogenated trimethylsilane and the solvent from the reaction solution obtained after the first reaction step with the lithium halide.

[0102] There is no particular limitation on the method for taking out the lithium borate compound after the second reaction step.

[0103] For example, in the case where only the target component (ie, the lithium borate compound itself) is obtained in a solid form, the solid can be taken out as the lithium borate compound without any special treatment.

[0104] When a slurry in which the lithium borate compound is dispersed in a solvent is obtained by the second reaction step, the solvent can be separated from the slurry into solid and liquid by filtration or the like, and the obtained filtrate can be dried to remove the lithium borate compound.

[0105] When a solution in which a lithium borate compound is dissolved in a solvent is obtained by the second reaction step, the lithium borate compound can be taken out by distilling off the solvent from the solution by heating and concentration.

[0106] In addition, when a solution in which a lithium borate compound is dissolved in a solvent is obtained by the second reaction step, the lithium borate compound can also be precipitated by adding a solvent that does not dissolve the lithium borate compound to the solution, and then the lithium borate compound precipitated from the solution is separated from the solvent by solid-liquid separation, and the obtained solid is dried to thereby remove the lithium borate compound.

[0107] As methods for drying the taken-out lithium borate compound, the following methods can be applied: a static drying method using a tray dryer; a fluid drying method using a conical dryer; a drying method using a heating plate, an oven or the like; a method using a dryer such as a dryer to supply warm air or hot air; and the like.

[0108] The pressure at the time of drying the taken-out lithium borate compound may be either normal pressure or reduced pressure.

[0109] The temperature when the taken-out lithium borate compound is dried is preferably 20°C to 150°C, more preferably 50°C to 140°C, and further preferably 80°C to 130°C.

[0110] When the temperature is 20° C. or higher, the drying efficiency is excellent. When the temperature is 150° C. or lower, the decomposition of the generated lithium borate compound is suppressed, and the lithium borate compound can be easily and stably taken out.

[0111] The taken out lithium borate compound may be used directly, or may be used after being dispersed or dissolved in a solvent, or may be used after being mixed with other solid substances.

[0112] The lithium borate compound of the present disclosure can be advantageously used as an additive for lithium batteries (preferably an additive for lithium secondary batteries, more preferably an additive for non-aqueous electrolytes for lithium secondary batteries), a reaction reagent, a synthesis reaction catalyst, an electrolyte for various electrochemical devices, a dopant, an additive for lubricating oils, and the like.

[0113] 〔Additives for lithium secondary batteries〕

[0114] The secondary battery additive of the present disclosure includes the lithium borate compound of the present disclosure. The secondary battery additive of the present disclosure is particularly suitable as an additive for a non-aqueous electrolyte of a lithium secondary battery.

[0115] [Non-aqueous electrolyte for lithium secondary batteries]

[0116] A nonaqueous electrolyte for a lithium secondary battery according to one embodiment of the present disclosure (hereinafter also simply referred to as “the nonaqueous electrolyte of the present embodiment”) contains an electrolyte as a lithium salt containing fluorine, a nonaqueous solvent, and the lithium borate compound of the present disclosure.

[0117] According to the nonaqueous electrolyte solution of this embodiment, the battery resistance after storage and after charge and discharge cycles can be reduced.

[0118] The non-aqueous electrolyte solution of the present embodiment (hereinafter, also simply referred to as “non-aqueous electrolyte solution”) contains a lithium borate compound.

[0119] The non-aqueous electrolyte of the present disclosure can reduce the battery resistance after storage and after charge and discharge cycles by containing a lithium borate compound.

[0120] The reasons for obtaining the above effects are presumed to be as follows. However, the non-aqueous electrolyte solution of the present embodiment is not limited to the following reasons.

[0121] It is believed that when a lithium secondary battery is manufactured using the non-aqueous electrolyte of the present embodiment, in its manufacturing process (for example, the aging process described later), a reaction product of a lithium borate compound and LiF generated from an electrolyte is generated near the surface of the negative electrode of the lithium secondary battery, and then a component of a decomposition product as a reaction product is generated. It is believed that this component moves near the positive electrode surface and the negative electrode surface during the manufacturing process, adheres to the positive electrode surface and the negative electrode surface, and forms a positive electrode film and a negative electrode film. It is believed that the stability of the battery after storage and charge and discharge cycles is improved (for example, the dissolution of metal elements in the positive electrode active material can be suppressed), and as a result, the battery resistance after storage and charge and discharge cycles is reduced.

[0122] Based on the above reasons, it is considered that the nonaqueous electrolyte solution according to the present embodiment can reduce the battery resistance after storage and after charge and discharge cycles.

[0123] It is considered that the above-mentioned components adhere to the positive electrode surface and the negative electrode surface (that is, the formation of the positive electrode film and the negative electrode film) after the lithium secondary battery is manufactured and also during the storage period when the lithium secondary battery is stored.

[0124] Therefore, when the lithium secondary battery is stored, it is considered that the battery resistance of the lithium secondary battery decreases with respect to the storage period of the lithium secondary battery.

[0125] The non-aqueous electrolyte of the present disclosure may contain only one type of the above-mentioned lithium borate compound, or may contain two or more types.

[0126] The non-aqueous electrolyte of the present disclosure may contain the lithium borate compound as a battery additive, or may contain the lithium borate compound as a supply source of an electrolyte.

[0127] The content of the lithium borate compound in the non-aqueous electrolyte of the present disclosure is not particularly limited, but is preferably 0.1% by mass to 5.0% by mass relative to the total amount of the non-aqueous electrolyte.

[0128] When the content of the lithium borate compound is 0.1% by mass or more relative to the total amount of the nonaqueous electrolyte, the effect brought by the nonaqueous electrolyte of the present disclosure can be more effectively obtained. The content of the lithium borate compound relative to the total amount of the nonaqueous electrolyte is more preferably 0.2% by mass or more, further preferably 0.3% by mass or more, and further preferably 0.5% by mass or more.

[0129] When the content of the lithium borate compound is 5.0 mass % or less based on the total amount of the non-aqueous electrolyte, the chemical stability of the non-aqueous electrolyte is further improved.

[0130] The content of the lithium borate compound relative to the total amount of the non-aqueous electrolyte is more preferably 3.0% by mass or less, further preferably 2.0% by mass or less, and further preferably 1.0% by mass or less.

[0131] When the non-aqueous electrolyte of the present disclosure contains the above-mentioned lithium borate compound as a supply source of the electrolyte, the concentration of the electrolyte is preferably 0.1 mol / L to 3 mol / L, more preferably 0.5 mol / L to 2 mol / L.

[0132] It should be noted that, in fact, when analyzing the non-aqueous electrolyte collected by disassembling the battery, the amount of the above-mentioned lithium borate compound may sometimes decrease relative to the amount added to the non-aqueous electrolyte. Therefore, even if only a small amount of the above-mentioned lithium borate compound can be detected in the non-aqueous electrolyte taken out of the battery, it is also included in the scope of the non-aqueous electrolyte of the present disclosure.

[0133] Even if the lithium borate compound cannot be detected from the non-aqueous electrolyte, detection of a compound derived from the decomposition product of the lithium borate compound in the non-aqueous electrolyte or in the electrode film is considered to be included in the scope of the non-aqueous electrolyte of the present disclosure.

[0134] These treatments are also applied to compounds other than the above-mentioned lithium borate compound that may be contained in the non-aqueous electrolyte.

[0135] <Electrolytes>

[0136] The nonaqueous electrolyte solution of the present embodiment contains at least one electrolyte which is a lithium salt containing fluorine (hereinafter also referred to as “fluorine-containing lithium salt”).

[0137] Examples of the lithium salt containing fluorine include:

[0138] Inorganic acid anion salts such as lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), and lithium hexafluorotantalate (LiTaF6);

[0139] Organic acid anion salts such as lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(fluorosulfonyl)imide (Li(FSO2)2N), lithium bis(trifluoromethanesulfonyl)imide (Li(CF3SO2)2N), and lithium bis(pentafluoroethanesulfonyl)imide (Li(C2F5SO2)2N);

[0140] etc.

[0141] As the lithium salt containing fluorine, LiPF6 is particularly preferred.

[0142] The non-aqueous electrolyte solution of the present embodiment may contain an electrolyte which is a lithium salt not containing fluorine.

[0143] Examples of fluorine-free lithium salts include lithium perchlorate (LiClO4), lithium tetrachloroaluminate (LiAlCl4), lithium decachlorodecaborate (Li2B 10 Cl 10 )wait.

[0144] The proportion of the fluorine-containing lithium salt in the entire electrolyte contained in the nonaqueous electrolyte solution of the present embodiment is preferably 50 to 100 mass %, more preferably 60 to 100 mass %, and even more preferably 80 to 100 mass %.

[0145] The proportion of LiPF6 in the entire electrolyte contained in the non-aqueous electrolyte of this embodiment is preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and further preferably 80% by mass to 100% by mass.

[0146] The concentration of the electrolyte in the nonaqueous electrolyte solution of the present embodiment is preferably 0.1 mol / L to 3 mol / L, and more preferably 0.5 mol / L to 2 mol / L.

[0147] The concentration of LiPF6 in the non-aqueous electrolyte of the present embodiment is preferably 0.1 mol / L to 3 mol / L, and more preferably 0.5 mol / L to 2 mol / L.

[0148] <Non-aqueous solvent>

[0149] The nonaqueous electrolyte solution of the present embodiment contains at least one nonaqueous solvent.

[0150] Examples of the nonaqueous solvent include cyclic carbonates, fluorinated cyclic carbonates, chain carbonates, fluorinated chain carbonates, aliphatic carboxylates, fluorinated aliphatic carboxylates, γ-lactones, fluorinated γ-lactones, cyclic ethers, fluorinated cyclic ethers, chain ethers, fluorinated chain ethers, nitriles, amides, lactams, nitromethane, nitroethane, sulfolane, trimethyl phosphate, dimethyl sulfoxide, dimethyl sulfoxide phosphoric acid, and the like.

[0151] Examples of the cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC).

[0152] Examples of the fluorine-containing cyclic carbonates include fluoroethylene carbonate (FEC) and the like.

[0153] Examples of the chain carbonates include dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and dipropyl carbonate (DPC).

[0154] Examples of the aliphatic carboxylic acid esters include methyl formate, methyl acetate, methyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylbutyrate, ethyl formate, ethyl acetate, ethyl propionate, ethyl butyrate, ethyl isobutyrate, and ethyl trimethylbutyrate.

[0155] Examples of the γ-lactones include γ-butyrolactone and γ-valerolactone.

[0156] Examples of the cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, and 1,4-dioxane.

[0157] Examples of the chain ethers include 1,2-ethoxyethane (DEE), ethoxymethoxyethane (EME), diethyl ether, 1,2-dimethoxyethane, and 1,2-dibutoxyethane.

[0158] Examples of the nitriles include acetonitrile, glutaronitrile, adiponitrile, methoxyacetonitrile, and 3-methoxypropionitrile.

[0159] Examples of the amides include N,N-dimethylformamide and the like.

[0160] Examples of the lactams include N-methylpyrrolidone, N-methyloxazolidinone, and N,N′-dimethylimidazolidinone.

[0161] The nonaqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, and fluorine-containing chain carbonates.

[0162] In this case, the total proportion of cyclic carbonates, fluorinated cyclic carbonates, chain carbonates, and fluorinated chain carbonates in the nonaqueous solvent is preferably 50% to 100% by mass, more preferably 60% to 100% by mass, and further preferably 80% to 100% by mass.

[0163] In addition, the nonaqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates and chain carbonates.

[0164] In this case, the total proportion of the cyclic carbonates and the chain carbonates in the nonaqueous solvent is preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and further preferably 80% by mass to 100% by mass.

[0165] The ratio of the nonaqueous solvent in the nonaqueous electrolyte solution of the present embodiment is preferably 60% by mass or more, and more preferably 70% by mass or more.

[0166] The upper limit of the proportion of the non-aqueous solvent in the non-aqueous electrolyte of this embodiment is also affected by the content of other components (lithium borate compound, electrolyte, etc.), but the upper limit is, for example, 99% by mass, preferably 97% by mass, and more preferably 90% by mass.

[0167] The intrinsic viscosity of the nonaqueous solvent is preferably 10.0 mPa·s or less at 25° C. from the viewpoint of further improving the dissociation property of the electrolyte and the mobility of the ions.

[0168] <Cyclic carbonate having an unsaturated bond>

[0169] From the viewpoint of further improving the chemical stability of the nonaqueous electrolyte, the nonaqueous electrolyte of the present embodiment preferably contains at least one type of cyclic carbonate having an unsaturated bond.

[0170] Generally, when a non-aqueous electrolyte contains a cyclic carbonate having an unsaturated bond, the internal resistance of the battery tends to increase.

[0171] However, since the nonaqueous electrolyte solution of the present embodiment contains a lithium borate compound, the internal resistance of the battery can be reduced even when the nonaqueous electrolyte solution further contains a cyclic carbonate having an unsaturated bond.

[0172] When the non-aqueous electrolyte solution of the present embodiment contains a cyclic carbonate having an unsaturated bond, there is an advantage that the improvement range of the internal resistance reduction due to the addition of the lithium borate compound is wide.

[0173] Examples of the cyclic carbonate having an unsaturated bond include vinylene carbonate compounds, vinyl ethylene carbonate compounds, and methylene vinyl carbonate compounds.

[0174] Examples of the vinylene carbonate-based compounds include vinylene carbonate (another name: 1,3-dioxol-2-one), methyl vinylene carbonate (another name: 4-methyl-1,3-dioxol-2-one), ethyl vinylene carbonate (another name: 4-ethyl-1,3-dioxol-2-one), 4,5-dimethyl-1,3-dioxol-2-one, 4,5-diethyl-1,3-dioxol-2-one, 4-fluoro-1,3-dioxol-2-one, and 4-trifluoromethyl-1,3-dioxol-2-one.

[0175] Examples of the vinyl ethylene carbonate-based compounds include vinyl ethylene carbonate (also known as 4-vinyl-1,3-dioxolane-2-one), 4-methyl-4-vinyl-1,3-dioxolane-2-one, 4-ethyl-4-vinyl-1,3-dioxolane-2-one, 4-n-propyl-4-vinyl-1,3-dioxolane-2-one, 5-methyl-4-vinyl-1,3-dioxolane-2-one, 4,4-divinyl-1,3-dioxolane-2-one, and 4,5-divinyl-1,3-dioxolane-2-one.

[0176] Examples of the methylene carbonate-based compound include 4-methylene-1,3-dioxolane-2-one, 4,4-dimethyl-5-methylene-1,3-dioxolane-2-one, and 4,4-diethyl-5-methylene-1,3-dioxolane-2-one.

[0177] As the cyclic carbonate having an unsaturated bond, vinylene carbonate is particularly preferred.

[0178] In the case where the nonaqueous electrolyte of the present embodiment contains a cyclic carbonate with an unsaturated bond, the content of the cyclic carbonate with an unsaturated bond is preferably 0.1% by mass to 5.0% by mass, more preferably 0.2% by mass to 3.0% by mass, further preferably 0.2% by mass to 2.0% by mass, and further preferably 0.3% by mass to 1.0% by mass, relative to the total amount of the nonaqueous electrolyte.

[0179] When the non-aqueous electrolyte of the present embodiment contains vinylene carbonate, the content of vinylene carbonate is preferably 0.1 mass % to 5.0 mass %, more preferably 0.2 mass % to 3.0 mass %, further preferably 0.2 mass % to 2.0 mass %, further preferably 0.3 mass % to 1.0 mass %, relative to the total amount of the non-aqueous electrolyte.

[0180] When the non-aqueous electrolyte of the present embodiment contains vinylene carbonate, the ratio of the mass content of vinylene carbonate to the mass content of the lithium borate compound (hereinafter also referred to as "mass content ratio [vinylene carbonate / lithium borate compound]") is preferably greater than 0.05, more preferably greater than 0.1, and further preferably greater than 0.3.

[0181] When the content mass ratio [vinylene carbonate / lithium borate compound] is 0.05 or more, an increase in the internal resistance of the lithium secondary battery after storage can be further suppressed.

[0182] The upper limit of the content mass ratio [vinylene carbonate / lithium borate compound] is not particularly limited, but is preferably 10 or less, more preferably 5 or less, and further preferably 3 or less from the viewpoint of more effectively obtaining the effect of vinylene carbonate.

[0183] <Other ingredients>

[0184] The nonaqueous electrolyte solution of the present embodiment may contain at least one component other than the above components.

[0185] Examples of other components include known additives that may be contained in a non-aqueous electrolyte (hereinafter also referred to as “known additives”), such as sultone (ie, cyclic sulfonic acid ester), acid anhydride, oxalic acid compound, cyclic sulfate ester compound, and the like.

[0186] When the nonaqueous electrolyte solution of the present embodiment contains a known additive, the content of the known additive is preferably 0.1% by mass to 3% by mass, and more preferably 0.5% by mass to 3% by mass, based on the total amount of the nonaqueous electrolyte solution.

[0187] Examples of sultones include propane sultone and propene sultone, and specific examples include 1,3-propane sultone, 1,4-butane sultone, 1,3-propene sultone, 1-methyl-1,3-propene sultone, 2-methyl-1,3-propene sultone, and 3-methyl-1,3-propene sultone. These may be used alone or in combination of two or more.

[0188] As the sultone, propene sultone is preferred.

[0189] Examples of the acid anhydride include:

[0190] Carboxylic anhydrides such as succinic anhydride, glutaric anhydride, maleic anhydride, etc.

[0191] Disulfonic anhydrides such as ethanedisulfonic anhydride and propanedisulfonic anhydride;

[0192] Anhydrides of carboxylic acids and sulfonic acids such as sulfobenzoic anhydride, sulfopropionic anhydride, and sulfobutyric anhydride;

[0193] etc.

[0194] These may be used alone or in combination of two or more.

[0195] As the acid anhydride, sulfobenzoic anhydride is preferred.

[0196] Examples of the oxalic acid compound include lithium difluorobis(oxalate)phosphate, lithium tetrafluoro(oxalate)phosphate, lithium tri(oxalate)phosphate, lithium difluoro(oxalate)borate, and lithium bis(oxalate)borate.

[0197] Examples of the cyclic sulfate ester compound include:

[0198] Catechol sulfate, 1,2-cyclohexyl sulfate, 2,2-dioxo-1,3,2-dioxathiolane, 4-methyl-2,2-dioxo-1,3,2-dioxathiolane, 4-ethyl-2,2-dioxo-1,3,2-dioxathiolane, 4-propyl-2,2-dioxo-1,3,2-dioxathiolane, 4-butyl-2,2-dioxo-1,3,2-dioxathiolane, 4-pentyl-2,2-dioxo-1,3,2-dioxathiolane, 4-hexyl-2,2-dioxo-1,3,2-dioxathiolane,

[0199] 4-Methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, 4-ethylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, bis((2,2-dioxo-1,3,2-dioxathiolan-4-yl)methyl) sulfate, 4,4'-bis(2,2-dioxo-1,3,2-dioxathiolane);

[0200] etc.

[0201] In addition, other additives include:

[0202] Sulfur compounds such as vinyl sulfite, propylene sulfite, vinyl sulfate, propylene sulfate, butylene sulfate, hexenyl sulfate, vinylene sulfate, 3-cyclobutene sulfone, divinyl sulfone, dimethyl sulfate, diethyl sulfate; vinyl boric acid compounds such as dimethyl vinyl borate, diethyl vinyl borate, dipropyl vinyl borate, dibutyl vinyl borate;

[0203] Amides such as dimethylformamide;

[0204] Chain carbamates such as N,N-dimethylcarbamate;

[0205] Cyclic amides such as N-methylpyrrolidone;

[0206] Cyclic ureas such as N,N-dimethylimidazolidinone;

[0207] Boric acid esters such as trimethyl borate, triethyl borate, tributyl borate, trioctyl borate, tris(trimethylsilyl) borate;

[0208] Phosphates such as lithium difluorophosphate, lithium monofluorophosphate, trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, tris(trimethylsilyl) phosphate, and triphenyl phosphate;

[0209] Ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, polyethylene glycol dimethyl ether and other ethylene glycol derivatives;

[0210] Aromatic hydrocarbons such as biphenyl, fluorobiphenyl, o-terphenyl, toluene, ethylbenzene, fluorobenzene, cyclohexylbenzene, 2-fluoroanisole, 4-fluoroanisole, etc.

[0211] Carboxylic anhydrides having a carbon-carbon unsaturated bond, such as maleic anhydride and norbornene dicarboxylic anhydride;

[0212] etc.

[0213] The intrinsic viscosity of the non-aqueous electrolyte solution of the present embodiment is preferably 10.0 mPa·s or less at 25° C. from the viewpoint of further improving the dissociation property of the electrolyte and the mobility of ions.

[0214] <Method for producing non-aqueous electrolyte>

[0215] The method for producing the nonaqueous electrolyte solution of the present embodiment is not particularly limited, and the nonaqueous electrolyte solution of the present embodiment may be produced by mixing the components.

[0216] As a method for producing the non-aqueous electrolyte solution of the present embodiment, for example, there can be mentioned a production method including the following steps:

[0217] a step of dissolving an electrolyte in a non-aqueous solvent to obtain a solution; and

[0218] A step of adding a lithium borate compound (and other additives as necessary) to the obtained solution and mixing the mixture to obtain a non-aqueous electrolyte solution.

[0219] In the manufacturing method involved in this example, the conductivity of the obtained non-aqueous electrolyte is preferably reduced relative to the conductivity of the solution (before adding the lithium borate compound). According to the non-aqueous electrolyte obtained by the manufacturing method of this mode, the effect of the aforementioned non-aqueous electrolyte (i.e., the effect of reducing the internal resistance of the battery) can be more effectively exerted.

[0220] 〔Lithium secondary battery precursor〕

[0221] A lithium secondary battery precursor according to one embodiment of the present disclosure (hereinafter also referred to as “battery precursor according to the present embodiment”) comprises:

[0222] a housing; and

[0223] The positive electrode, negative electrode, separator, and electrolyte contained in the shell,

[0224] The positive electrode is a positive electrode that can absorb and release lithium ions.

[0225] The negative electrode is a negative electrode that can absorb and release lithium ions.

[0226] The electrolyte solution is the nonaqueous electrolyte solution of the present embodiment described above.

[0227] Here, the lithium secondary battery precursor refers to a lithium secondary battery before charging and discharging.

[0228] The lithium secondary battery of this embodiment described below is manufactured by housing a positive electrode, a negative electrode, a separator, and a nonaqueous electrolyte in a case to manufacture a lithium secondary battery precursor, and subjecting the obtained lithium secondary battery precursor to charging and discharging (preferably including an aging treatment of charging and discharging).

[0229] The battery precursor of the present embodiment includes the nonaqueous electrolyte solution of the present embodiment.

[0230] Therefore, the battery precursor of the present embodiment can achieve the same effects as those achieved by the non-aqueous electrolyte solution of the present embodiment.

[0231] <Housing>

[0232] The case in the battery precursor of the present embodiment is not particularly limited, and examples thereof include cases for known lithium secondary batteries.

[0233] Examples of the case include a case made of a laminate film and a case formed of a battery case and a battery case cover.

[0234] <Positive electrode>

[0235] The positive electrode in the battery precursor of the present embodiment is a positive electrode that can store and release lithium ions.

[0236] The positive electrode in the battery precursor of this embodiment preferably contains at least one positive electrode active material that can occlude and release lithium ions.

[0237] The positive electrode in the battery precursor of the present embodiment more preferably includes: a positive electrode current collector; and a positive electrode mixed material layer containing a positive electrode active material and a binder.

[0238] The positive electrode mixed material layer is provided on at least a portion of the surface of the positive electrode current collector.

[0239] (Positive electrode active material)

[0240] The positive electrode active material is not particularly limited as long as it is a material that can absorb and release lithium ions, and may be a positive electrode active material commonly used in lithium secondary batteries.

[0241] Examples of the positive electrode active material include:

[0242] Oxides with lithium (Li) and nickel (Ni) as constituent metal elements;

[0243] An oxide containing at least one of Li, Ni, and a metal element other than Li and Ni (e.g., a transition metal element, a typical metal element, etc.) as a constituent metal element;

[0244] etc.

[0245] The oxide preferably contains a metal element other than Li and Ni at a ratio equivalent to or less than that of Ni in terms of atomic number.

[0246] The metal element other than Li and Ni may be, for example, at least one selected from the group consisting of Co, Mn, Al, Cr, Fe, V, Mg, Ca, Na, Ti, Zr, Nb, Mo, W, Cu, Zn, Ga, In, Sn, La and Ce. These positive electrode active materials may be used alone or in combination.

[0247] The positive electrode active material preferably includes a lithium-containing composite oxide (hereinafter also referred to as “NCM”) represented by the following general formula (C1).

[0248] The lithium-containing composite oxide (C1) has advantages such as high energy density per unit volume and excellent thermal stability.

[0249] LiNi a Co b Mn c O2…General formula (C1)

[0250] [In the general formula (C1), a, b and c are each independently greater than 0 and less than 1, and the total of a, b and c is 0.99 to 1.00.]

[0251] As a specific example of NCM, LiNi 0.33 Co 0.33 Mn 0.33 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2, etc.

[0252] The positive electrode active material may include a lithium-containing composite oxide (hereinafter, also referred to as “NCA”) represented by the following general formula (C2).

[0253] Li t Ni 1-x-y Co x Al y O2…General formula (C2)

[0254] (In general formula (C2), t is 0.95 to 1.15, x is 0 to 0.3, y is 0.1 to 0.2, and the total of x and y is less than 0.5.)

[0255] As a specific example of NCA, LiNi 0.8 Co 0.15 Al 0.05 O2, etc.

[0256] In the case where the positive electrode in the battery precursor of the present embodiment comprises a positive electrode collector, and a positive electrode composite layer containing a positive electrode active material and a binder, the content of the positive electrode active material in the positive electrode composite layer is, for example, 10 mass % or more, preferably 30 mass % or more, further preferably 50 mass % or more, and particularly preferably 70 mass % or more, relative to the total amount of the positive electrode composite layer.

[0257] The content of the positive electrode active material in the positive electrode mixed material layer is, for example, 99.9 mass % or less, or preferably 99 mass % or less.

[0258] (Adhesive)

[0259] Examples of the binder that may be contained in the positive electrode material layer include polyvinyl acetate, polymethyl methacrylate, nitrocellulose, fluororesin, and rubber particles.

[0260] Examples of the fluororesin include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), and vinylidene fluoride-hexafluoropropylene copolymer.

[0261] Examples of the rubber particles include styrene-butadiene rubber particles and acrylonitrile rubber particles.

[0262] Among these, fluororesins are preferred from the viewpoint of improving the oxidation resistance of the positive electrode mixed material layer.

[0263] The binder may be used alone or in combination of two or more as necessary.

[0264] From the viewpoint of achieving both the physical properties of the positive electrode composite layer (eg, electrolyte permeability, peel strength, etc.) and battery performance, the content of the binder in the positive electrode composite layer is preferably 0.1 to 4 mass % relative to the positive electrode composite layer.

[0265] When the content of the binder is 0.1 mass % or more, the adhesiveness between the positive electrode mixed material layer and the positive electrode current collector and the binding properties between the positive electrode active materials are further improved.

[0266] When the content of the binder is 4% by mass or less, the amount of the positive electrode active material in the positive electrode mixed material layer can be increased, so the battery capacity is further improved.

[0267] (Conductive additive)

[0268] When the positive electrode in the battery precursor of the present embodiment includes a positive electrode current collector and a positive electrode mixed material layer, the positive electrode mixed material layer preferably contains a conductive auxiliary agent.

[0269] As the conductive auxiliary agent, a known conductive auxiliary agent can be used.

[0270] As the conductive auxiliary agent, a known conductive auxiliary agent can be used.

[0271] Known conductive additives are not particularly limited as long as they are carbon materials having conductivity, and graphite, carbon black, conductive carbon fibers (carbon nanotubes, carbon nanofibers, carbon fibers), fullerenes, etc. may be used alone or in combination of two or more.

[0272] Examples of commercially available carbon black include TOKABLACK #4300, #4400, #4500, #5500, etc. (manufactured by Tokai Carbon Co., Ltd., furnace black), Printex L, etc. (manufactured by Degussa, furnace black), Raven 7000, 5750, 5250, 5000ULTRAIII, 5000ULTRA, etc., Conductex SC ULTRA, Conductex 975ULTRA, etc., PUER BLACK 100, 115, 205, etc. (manufactured by Columbia, furnace black), #2350, #2400B, #2600B, #30050B, #3030B, #3230B, #3350B, #3400B, #5400B, etc. (manufactured by Mitsubishi Chemical Corporation, furnace black), MONARCH 1400, 1300, 900, Vulcan XC-72R, Black Pearls 2000, LITX-50, LITX-200, etc. (produced by Cabot, furnace black), Ensaco 250G, Ensaco 260G, Ensaco 350G, Super-P (produced by TIMCAL), Ketjenblack EC-300J, EC-600JD (produced by Akzo), Denka Black, Denka Black HS-100, FX-35 (produced by Denki Kagaku Kogyo Co., Ltd., acetylene black), etc.

[0273] Examples of graphite include artificial graphite, natural graphite (for example, flaky graphite, massive graphite, earthy graphite, etc.), and the like, but are not limited to these.

[0274] (Other ingredients)

[0275] When the positive electrode in the battery precursor of the present embodiment includes a positive electrode current collector and a positive electrode mixed material layer, the positive electrode mixed material layer may contain other components in addition to the above-mentioned components.

[0276] Examples of other components include a thickener, a surfactant, a dispersant, a wetting agent, and a defoaming agent.

[0277] (Positive electrode collector)

[0278] As the positive electrode current collector, various substances can be used, for example, metals or alloys can be used.

[0279] More specifically, the positive electrode current collector includes aluminum, nickel, SUS, etc. Among them, aluminum is preferred from the viewpoint of the balance between high and low conductivity and cost. Here, "aluminum" refers to pure aluminum or an aluminum alloy.

[0280] As the positive electrode current collector, aluminum foil is particularly preferred.

[0281] The aluminum foil is not particularly limited, and examples thereof include A1085 material and A3003 material.

[0282] (Method for forming positive electrode composite layer)

[0283] The positive electrode mixed material layer can be formed, for example, by applying a positive electrode mixed material slurry containing a positive electrode active material and a binder onto the surface of a positive electrode current collector and drying the slurry.

[0284] As the solvent contained in the positive electrode material slurry, an organic solvent such as N-methyl-2-pyrrolidone (NMP) is preferable.

[0285] When the positive electrode mixture slurry is applied to the positive electrode current collector and then dried, the application method and the drying method are not particularly limited.

[0286] Examples of the coating method include slot-die coating, slide coating, curtain coating, and gravure coating.

[0287] Examples of the drying method include drying with warm air, hot air, or low-humidity air; vacuum drying; and drying with infrared (eg, far-infrared) irradiation.

[0288] The drying time and the drying temperature are not particularly limited, but the drying time is, for example, 1 minute to 30 minutes, and the drying temperature is, for example, 40°C to 80°C.

[0289] The method for producing the positive electrode mixture layer preferably includes the steps of applying the positive electrode mixture slurry on the positive electrode current collector and drying it, and then reducing the porosity of the positive electrode active material layer by a press process using a die press, a roll press, or the like.

[0290] <Negative electrode>

[0291] The negative electrode in the battery precursor of the present embodiment is a negative electrode that can store and release lithium ions.

[0292] The negative electrode in the battery precursor of this embodiment preferably contains at least one negative electrode active material that can occlude and release lithium ions.

[0293] The negative electrode in the battery precursor of the present embodiment more preferably includes: a negative electrode current collector; and a negative electrode mixed material layer containing a negative electrode active material and a binder.

[0294] The negative electrode mixed material layer is provided on at least a portion of the surface of the negative electrode current collector.

[0295] (Negative electrode active material)

[0296] The negative electrode active material can be any material that can absorb and release lithium ions without any particular limitation. For example, at least one material selected from the group consisting of metallic lithium, lithium-containing alloys, metals or alloys that can be alloyed with lithium, oxides that can be doped / dedoped with lithium ions, transition metal nitrides that can be doped / dedoped with lithium ions, and carbon materials that can be doped / dedoped with lithium ions can be used (they can be used alone or as a mixture of two or more of them).

[0297] Among these, carbon materials that can be doped and dedoped with lithium ions are preferred.

[0298] Examples of the carbon material include carbon black, activated carbon, graphite materials (for example, artificial graphite, natural graphite, etc.), and amorphous carbon materials.

[0299] The carbon material may be in any of the following forms: fiber, spherical, potato, or flake.

[0300] The particle size of the carbon material is not particularly limited, and is, for example, 5 μm to 50 μm, and preferably 20 μm to 30 μm.

[0301] Specific examples of the amorphous carbon material include hard carbon, coke, mesocarbon microbeads (MCMB) sintered at 1500° C. or lower, and mesophase pitch carbon fibers (MCF).

[0302] Examples of the graphite material include natural graphite and artificial graphite.

[0303] As artificial graphite, graphitized MCMB, graphitized MCF, etc. can be used.

[0304] In addition, as the graphite material, a graphite material containing boron or the like may be used.

[0305] In addition, as the graphite material, a graphite material coated with a metal such as gold, platinum, silver, copper, or tin, a graphite material coated with amorphous carbon, or a graphite material obtained by mixing amorphous carbon and graphite can also be used.

[0306] These carbon materials may be used alone or in combination of two or more.

[0307] (Conductive additive)

[0308] When the negative electrode in the battery precursor of the present embodiment includes a negative electrode current collector and a negative electrode mixed material layer, the negative electrode mixed material layer preferably contains a conductive auxiliary agent.

[0309] As the conductive auxiliary agent, a known conductive auxiliary agent can be used.

[0310] Specific examples of the conductive auxiliary agent that can be included in the negative electrode mixed material layer are the same as the specific examples of the conductive auxiliary agent that can be included in the above-mentioned positive electrode mixed material layer.

[0311] (Other ingredients)

[0312] When the negative electrode in the battery precursor of the present embodiment includes a negative electrode current collector and a negative electrode mixed material layer, the negative electrode mixed material layer may contain other components in addition to the above-mentioned components.

[0313] Examples of other components include a thickener, a surfactant, a dispersant, a wetting agent, and a defoaming agent.

[0314] (Method for forming negative electrode composite layer)

[0315] The negative electrode mixed material layer can be formed, for example, by applying a negative electrode mixed material slurry containing a negative electrode active material and a binder onto the surface of a negative electrode current collector and drying the slurry.

[0316] As the solvent contained in the negative electrode composite slurry, water is preferably used, and a liquid medium compatible with water may be used as necessary, for example, in order to improve coating properties on a current collector.

[0317] Examples of the water-compatible liquid medium include alcohols, glycols, cellosolves, amino alcohols, amines, ketones, carboxylic acid amides, phosphoric acid amides, sulfoxides, carboxylates, phosphoric acid esters, ethers, nitriles, and the like, and any of them can be used within the range of compatibility with water.

[0318] A preferred embodiment of the method for forming the negative electrode mixed material layer is the same as the preferred embodiment of the method for forming the positive electrode mixed material layer described above.

[0319] <Diaphragm>

[0320] Examples of the separator in the battery precursor of this embodiment include porous flat plates made of resins such as polyethylene (PE), polypropylene (PP), polyester, cellulose, and polyamide. In addition, examples of the separator include nonwoven fabrics made of the above resins.

[0321] Preferred examples include porous resin sheets having a single-layer or multi-layer structure mainly composed of one or more polyolefin resins.

[0322] The thickness of the separator may be, for example, 5 μm to 30 μm.

[0323] The separator is preferably disposed between the positive electrode and the negative electrode.

[0324] <Electrolyte>

[0325] The electrolyte solution in the battery precursor of the present embodiment is the nonaqueous electrolyte solution of the present embodiment described above.

[0326] Preferred aspects of the nonaqueous electrolyte solution of this embodiment are as described above.

[0327] <Method for producing battery precursor>

[0328] The method for producing the battery precursor of the present embodiment is not particularly limited.

[0329] An example of a method for producing the battery precursor of the present embodiment includes a step of housing a positive electrode, a negative electrode, a separator, and an electrolyte solution in a case.

[0330] The above example preferably includes:

[0331] The process of housing the positive electrode, the negative electrode, and the separator in a casing; and

[0332] The process of injecting electrolyte into the case containing the positive electrode, negative electrode and separator.

[0333] <Battery Structure>

[0334] The lithium secondary battery of the present disclosure can adopt various known shapes, such as cylindrical, button, square, laminated, film, and other arbitrary shapes. However, regardless of the shape, the basic structure of the battery is the same, and the design can be changed according to the purpose.

[0335] As an example of the lithium secondary battery of the present disclosure, a laminated type battery can be mentioned.

[0336] Figure 1 1 is a schematic perspective view showing an example of a lithium secondary battery of the present disclosure, that is, an example of a laminated type battery. Figure 2 To accommodate Figure 1 Schematic cross-sectional view of a laminated electrode body in the thickness direction of the laminated battery shown.

[0337] Figure 1 The laminated battery shown in the figure has a non-aqueous electrolyte ( Figure 1 not shown) and a stacked electrode body ( Figure 1 The laminated outer casing 1 is a laminated outer casing 1 having a sealed periphery (not shown) and an interior thereof. As the laminated outer casing 1, for example, an aluminum laminated outer casing can be used.

[0338] For the stacked electrode assembly contained in the laminated outer casing 1, Figure 2As shown, there is a stacked body composed of positive electrode plates 5 and negative electrode plates 6 alternately stacked with separators 7 interposed therebetween, and a separator 8 surrounding the stacked body. The positive electrode plates 5, negative electrode plates 6, separators 7, and separators 8 are impregnated with the nonaqueous electrolyte of the present disclosure.

[0339] The plurality of positive electrode plates 5 in the stacked electrode assembly are all electrically connected to the positive electrode terminal 2 via the positive electrode tab (not shown), and a portion of the positive electrode terminal 2 protrudes outward from the peripheral end of the laminated outer casing 1 ( Figure 1 )) The portion of the laminated outer casing 1 where the positive electrode terminal 2 protrudes is sealed by an insulating sealing material 4 .

[0340] Similarly, the plurality of negative electrode plates 6 in the stacked electrode assembly are electrically connected to the negative electrode terminal 3 via the negative electrode tab (not shown), and a portion of the negative electrode terminal 3 protrudes outward from the peripheral end of the laminated outer casing 1 ( Figure 1 The portion of the laminated outer casing 1 where the negative electrode terminal 3 protrudes is sealed by an insulating sealing material 4 .

[0341] It should be noted that, for the laminated battery involved in the above example, the number of positive plates 5 is 5, the number of negative plates 6 is 6, and the positive plates 5 and the negative plates 6 are stacked with the outermost layers on both sides being the negative plates 6 via the separator 7. However, the number of positive plates, the number of negative plates, and the arrangement in the laminated battery are of course not limited to this example, and various changes can be made.

[0342] As another example of the lithium secondary battery of the present disclosure, a button-type battery can also be mentioned.

[0343] Figure 3 This is a schematic perspective view showing another example of the lithium secondary battery of the present disclosure, that is, an example of a button-type battery.

[0344] Figure 3 In the button-type battery shown, a disc-shaped negative electrode 12, a separator 15 injected with a non-aqueous electrolyte, a disc-shaped positive electrode 11, and separators 17 and 18 made of stainless steel or aluminum as required are stacked in sequence and housed between a positive electrode case 13 (hereinafter also referred to as a "battery case") and a sealing plate 14 (hereinafter also referred to as a "battery case cover"). The positive electrode case 13 and the sealing plate 14 are sealed by caulking with a gasket 16 interposed therebetween.

[0345] In this example, as the nonaqueous electrolyte solution injected into the separator 15 , the nonaqueous electrolyte solution of the present disclosure is used.

[0346] The lithium secondary battery of the present disclosure may be a lithium secondary battery obtained by charging and discharging a lithium secondary battery (lithium secondary battery before charging and discharging) including a negative electrode, a positive electrode, and the above-mentioned nonaqueous electrolyte of the present disclosure.

[0347] That is, the lithium secondary battery of the present disclosure can be a lithium secondary battery (a lithium secondary battery that has been charged and discharged) manufactured in the following manner: first, a lithium secondary battery before charge and discharge is manufactured, which includes a negative electrode, a positive electrode, and the non-aqueous electrolyte of the present disclosure, and then, the lithium secondary battery before charge and discharge is charged and discharged more than once.

[0348] [Method for producing lithium secondary battery]

[0349] A method for manufacturing a lithium secondary battery according to an embodiment of the present disclosure (hereinafter also referred to as “a method for manufacturing a battery according to the present embodiment”) includes the following steps:

[0350] a step of preparing a battery precursor of the present embodiment (hereinafter also referred to as a "preparation step"); and,

[0351] A step of obtaining a lithium secondary battery by subjecting a battery precursor to an aging treatment (hereinafter also referred to as a "aging step"),

[0352] The aging treatment includes the steps of charging and discharging the battery precursor in an environment of 20°C to 60°C.

[0353] The aging process in the aging process preferably includes the following stages:

[0354] An initial holding stage of maintaining the battery precursor in an environment of 20°C to 60°C;

[0355] An initial charging stage in which the battery precursor after the initial holding stage is charged in an environment of 20° C. to 60° C.;

[0356] A second holding stage of holding the battery precursor after the initial charging stage in an environment of 20° C. to 60° C.; and

[0357] The battery precursor after the second maintenance stage is subjected to a charge and discharge stage of a combination of charge and discharge one or more times in an environment of 20° C. to 60° C.

[0358] According to the above preferred embodiment, the battery resistance of the lithium secondary battery after storage and cycling can be effectively reduced.

[0359] Preferred embodiments of the nonaqueous electrolyte solution in the lithium secondary battery of the present embodiment are the same as those of the nonaqueous electrolyte solution of the present embodiment, except that the nonaqueous electrolyte solution is not limited to contain the lithium borate compound of the present disclosure.

[0360] The nonaqueous electrolyte in the battery of this embodiment may contain a lithium borate compound.

[0361] For example, when the battery of this embodiment is manufactured by the method for manufacturing a battery of this embodiment, the lithium borate compound may be completely consumed by the aging treatment, or a part of the lithium borate compound may remain.

[0362] The additives for lithium secondary batteries of the present disclosure, the non-aqueous electrolyte for lithium secondary batteries of the present disclosure, the lithium secondary battery precursor of the present disclosure, the method for manufacturing lithium secondary batteries of the present disclosure, and the lithium secondary batteries of the present disclosure described above can be applied to the following purposes, for example: electronic devices such as mobile phones and laptop computers; electric vehicles; hybrid vehicles; power sources for power storage; etc.

[0363] The lithium secondary battery additive of the present disclosure, the nonaqueous electrolyte for lithium secondary batteries of the present disclosure, the lithium secondary battery precursor of the present disclosure, the method for producing a lithium secondary battery of the present disclosure, and the lithium secondary battery of the present disclosure can be particularly preferably used in hybrid vehicles or electric vehicles.

[0364] Example

[0365] Hereinafter, examples of the present disclosure will be described, but the present disclosure is not limited to the following examples.

[0366] [Example 1] Synthesis of lithium borate compound represented by formula (II)

[0367] (1) First reaction step

[0368] Prepare a 100mL flask equipped with a stirring device, a thermometer, a gas introduction line, an exhaust line, and a drop-feeding tube. After purging the above 100mL flask with dry nitrogen, add 2.91g (0.05mol) of potassium fluoride, 5.20g (0.05mol) of trimethyl borate, and 50g of tetrahydrofuran and stir and mix to obtain a slurry. While stirring the slurry, add 7.11g (0.05mol) of (trifluoromethyl)trimethylsilane dropwise from the drop-feeding tube and continue stirring at room temperature (25°C) for 24 hours. The reaction solution after the above reaction changes from the slurry before the start of the reaction to a uniform solution. The solution is filtered to remove dust, and the obtained filtrate is dried at 60°C and 10kPa or less to obtain 9.86g of a solid product.

[0369] A portion of the obtained solid was dissolved in heavy water solvent and then subjected to 1 H-NMR analysis, 11 B-NMR analysis, and 19 F-NMR analysis: The chemical shifts (ppm) of the spectra obtained by each NMR analysis are shown below.

[0370] 1 H-NMR: 3.2 ppm(s).

[0371] 11 B-NMR: -2.2 ppm (m).

[0372] 19 F-NMR: -74.7 ppm (m).

[0373] From the NMR spectrum pattern, it was confirmed that the obtained product was potassium trimethoxy(trifluoromethyl)borate, which is a reaction intermediate shown in the following reaction pathway.

[0374] (2) Second Reaction Step

[0375] 8.48 g (0.04 mol) of the above reaction intermediate and 50 g of methanol were added to the original reaction flask, and then 1.70 g (0.04 mol) of lithium chloride was added thereto and stirred to obtain a uniform solution. Then, the solution was heated to 65°C and stirred for 1 hour under reflux of the solvent. The reaction solution obtained by this step changed from a uniform solution to a slurry with solid salt precipitated. The slurry was filtered to remove the solid, and the obtained filtrate was dried at 60°C and 10 kPa or less to obtain 6.51 g of the product as a white crystalline solid.

[0376] A portion of the obtained solid was dissolved in heavy water solvent and then subjected to 1 H-NMR analysis, 7 Li-NMR analysis, 11 B-NMR analysis, and 19 F-NMR analysis: The chemical shifts (ppm) of the spectra obtained by each NMR analysis are shown below.

[0377] 1 H-NMR: 3.2 ppm(s).

[0378] 7 Li-NMR: 2.9 ppm(s).

[0379] 11 B-NMR: -2.0 ppm (m).

[0380] 19 F-NMR: -74.7 ppm (m).

[0381] As shown above, it was confirmed that the product obtained by the synthesis of Example 1 was the lithium borate compound of the present disclosure shown in the following reaction pathway, that is, the lithium borate compound represented by formula (II) (hereinafter also referred to as "lithium borate compound (II)").

[0382] [Chemical formula 5]

[0383]

[0384] [Example 2] Synthesis of lithium borate compound represented by formula (III)

[0385] Synthesis was carried out in the same manner as in Example 1 except that the second reaction step in Example 1 was changed to the method shown below.

[0386] 8.48 g (0.04 mol) of the above reaction intermediate and 60 g of ethanol were added to the original reaction flask, and then 1.70 g (0.04 mol) of lithium chloride was added thereto and stirred to obtain a uniform solution. Then, the solution was heated to 80°C and stirred for 1 hour under reflux of the solvent. The reaction solution obtained by this step changed from a uniform solution to a slurry with solid salt precipitated. The slurry was filtered to remove the solid, and the obtained filtrate was dried at 60°C and 10 kPa or less to obtain 6.83 g of the product as a white crystalline solid.

[0387] A portion of the obtained solid was dissolved in heavy water solvent and then subjected to 1 H-NMR analysis, 7 Li-NMR analysis, 11 B-NMR analysis, and 19 F-NMR analysis: The chemical shifts (ppm) of the spectra obtained by each NMR analysis are shown below.

[0388] 1 H-NMR: 1.0ppm(t), 3.4ppm(q).

[0389] 7 Li-NMR: 2.9 ppm(s).

[0390] 11 B-NMR: -2.2 ppm (m).

[0391] 19 F-NMR: -74.7 ppm (m).

[0392] As shown above, it was confirmed that the product obtained by the synthesis of Example 2 was the lithium borate compound of the present disclosure shown in the following reaction pathway, that is, the lithium borate compound represented by formula (III) (hereinafter also referred to as "lithium borate compound (III)").

[0393] [Chemical formula 6]

[0394]

[0395] [Example 3] Synthesis of lithium borate compound represented by formula (IV)

[0396] Synthesis was carried out in the same manner as in Example 1 except that the second reaction step in Example 1 was changed to the method shown below.

[0397] 8.48 g (0.04 mol) of the above reaction intermediate and 80 g of isopropanol were added to the original reaction flask, and then 1.70 g (0.04 mol) of lithium chloride was added thereto and stirred to obtain a uniform solution. Then, the solution was heated to 85°C and stirred for 1 hour under reflux of the solvent. The reaction solution obtained by this step changed from a uniform solution to a slurry with solid salt precipitated. The slurry was filtered to remove the solid, and the obtained filtrate was dried at 60°C and 10 kPa or less to obtain 7.04 g of the product as a white crystalline solid.

[0398] A portion of the obtained solid was dissolved in heavy water solvent and then subjected to 1 H-NMR analysis, 7 Li-NMR analysis, 11 B-NMR analysis, and 19 F-NMR analysis: The chemical shifts (ppm) of the spectra obtained by each NMR analysis are shown below.

[0399] 1 H-NMR: 1.0ppm(d), 3.8ppm(m).

[0400] 7 Li-NMR: 2.9 ppm(s).

[0401] 11 B-NMR: -2.0 ppm (m).

[0402] 19 F-NMR: -74.7 ppm (m).

[0403] As shown above, it was confirmed that the product obtained by the synthesis of Example 3 was the lithium borate compound of the present disclosure shown in the following reaction pathway, that is, the lithium borate compound represented by formula (IV) (hereinafter also referred to as "lithium borate compound (IV)").

[0404] [Chemical formula 7]

[0405]

[0406] [Example 4] Synthesis of lithium borate compound represented by formula (V)

[0407] The synthesis was carried out in the same manner as in Example 1 except that the second reaction step in Example 1 was changed to the synthesis method shown below.

[0408] The above reaction intermediate 6.36g (0.03mol) and n-butanol 80g are added to the original reaction flask, and then lithium chloride 1.23g (0.03mol) is added thereto and stirred to obtain a uniform solution. Then, the solution is heated to 85°C and stirred at this temperature for 1 hour. The reaction solution obtained by this step changes from a uniform solution to a slurry with solid salt precipitated. The slurry is filtered to remove solids, and the obtained filtrate is dried at 80°C and 10kPa or less to obtain 8.36g of a product as a white crystalline solid.

[0409] A portion of the obtained solid was dissolved in heavy water solvent and then subjected to 1 H-NMR analysis, 7 Li-NMR analysis, 11 B-NMR analysis, and 19 F-NMR analysis: The chemical shifts (ppm) of the spectra obtained by each NMR analysis are shown below.

[0410] 1 H-NMR: 0.7ppm(t), 1.2ppm(m), 1.4ppm(m), 3.4ppm(t).

[0411] 7 Li-NMR: 2.9 ppm(s).

[0412] 11 B-NMR: -2.0 ppm (m).

[0413] 19 F-NMR: -74.7 ppm (m).

[0414] As shown above, it was confirmed that the product obtained by the synthesis of Example 4 was the lithium borate compound of the present disclosure shown in the following reaction pathway, that is, the lithium borate compound represented by formula (V) (hereinafter also referred to as "lithium borate compound (V)").

[0415] [Chemical formula 8]

[0416]

[0417] [Example 101]

[0418] Follow the steps below to create a Figure 3 A button-type lithium secondary battery (hereinafter also referred to as a "button-type battery") having the structure shown.

[0419] <Production of negative electrode>

[0420] Amorphous coated natural graphite (97 parts by mass), carboxymethyl cellulose (1 part by mass), and SBR latex (2 parts by mass) were kneaded in an aqueous solvent to prepare a negative electrode mixture slurry in a paste form.

[0421] Next, the negative electrode mixture slurry was applied to a negative electrode collector made of a strip of copper foil with a thickness of 10 μm and dried, and then compressed with a roller press to obtain a sheet-shaped negative electrode composed of the negative electrode collector and the negative electrode active material layer. The coating density of the negative electrode active material layer at this time was 10 mg / cm 2 , filling density is 1.5g / ml.

[0422] <Production of positive electrode>

[0423] Using N-methylpyrrolidone as solvent, LiNi 0.5 Mn 0.3 Co 0.2 O2 (90 parts by mass), acetylene black (5 parts by mass) and polyvinylidene fluoride (5 parts by mass) were kneaded to prepare a paste-like positive electrode mixture slurry.

[0424] Next, the positive electrode mixture slurry was applied to a positive electrode current collector of a 20 μm thick strip of aluminum foil and dried, and then compressed using a roller press to obtain a sheet-shaped positive electrode consisting of a positive electrode current collector and a positive electrode active material layer. The coating density of the positive electrode active material layer at this time was 16 mg / cm 2 , filling density is 2.5g / ml.

[0425] <Preparation of non-aqueous electrolyte>

[0426] As a non-aqueous solvent, ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) were mixed at a ratio of 30:35:35 (volume ratio) to obtain a mixed solvent.

[0427] LiPF 6 as an electrolyte was dissolved in the obtained mixed solvent so that the electrolyte concentration in the finally prepared non-aqueous electrolyte solution became 1.2 mol / L.

[0428] To the obtained solution, a lithium borate compound (II) was added in an amount shown in Table 1 and dissolved to obtain a non-aqueous electrolyte solution.

[0429] <Production of button-type batteries>

[0430] Separately, the negative electrode was punched into a disc with a diameter of 14 mm, and the positive electrode was punched into a disc with a diameter of 13 mm, respectively, to obtain a button-shaped negative electrode and a button-shaped positive electrode. In addition, a microporous polyethylene film with a thickness of 20 μm was punched into a disc with a diameter of 17 mm to obtain a separator.

[0431] The obtained button-shaped negative electrode, separator, and button-shaped positive electrode were sequentially stacked in a stainless steel battery case (2032 size), and then 20 μL of the above-mentioned nonaqueous electrolyte was injected into the battery case to impregnate the separator, positive electrode, and negative electrode.

[0432] Next, an aluminum plate (1.2 mm thick, 16 mm in diameter) and a spring were placed on the positive electrode, and the battery case lid was caulked via a polypropylene gasket to seal the battery.

[0433] Through the above method, a 20 mm diameter and 3.2 mm height Figure 3 A button-type battery (ie, a button-type lithium secondary battery) having the structure shown.

[0434] [Examples 102 to 104, Comparative Example 101]

[0435] A lithium secondary battery was prepared in the same manner as in Example 101 except that the type of additive contained in the nonaqueous electrolyte was changed as shown in Table 1, and the following evaluation was performed in the same manner as in Example 101. The results are shown in Table 1.

[0436] The following evaluations were performed on the obtained button-type batteries.

[0437] Table 1 shows the evaluation results.

[0438] <Evaluation of DC resistance of batteries after storage>

[0439] For each of the batteries of Examples 101 to 104 and Comparative Example 101, direct current resistance was evaluated as evaluation of the internal resistance of the battery.

[0440] The details are shown below.

[0441] (Initial resistance (25℃))

[0442] The button-type battery was charged and discharged three times at a constant voltage of 4.2V, and then charged to a constant voltage of 3.6V. Then, the charged button-type battery was cooled to 25°C in a thermostatic chamber, and discharged at a constant current of 0.2mA at 25°C. The potential drop at 10 seconds from the start of discharge was measured, and the DC resistance [Ω] of the button-type battery was measured, and the obtained value was taken as the initial resistance [Ω] (25°C). The initial resistance value [Ω] (25°C) was also measured in the same manner for the button-type battery of Comparative Example 101 described later.

[0443] Based on the above results, the "initial resistance (25°C) (relative value; %)" was calculated using the following formula as the initial resistance value (relative value; %) in Example 101 when the initial resistance value [Ω] (25°C) in Comparative Example 101 was set to 100%. The results are shown in Table 1.

[0444] Initial resistance (25℃) (relative value; %)

[0445] =(initial resistance value [Ω] (25°C) in Example 101 / initial resistance value [Ω] (25°C) in Comparative Example 101) × 100

[0446] (Resistance after 6 days of storage)

[0447] The button-type battery was charged and discharged repeatedly three times at a constant voltage of 4.2 V, then charged to 4.2 V and stored at 60° C. for 6 days. The DC resistance of the battery after 6 days of storage was calculated using the same method as the initial resistance, and the obtained DC resistance value was used as the DC resistance of the battery after 6 days of storage.

[0448] The DC resistance value of the battery after storage for 6 days was determined as a relative value when the initial DC resistance value of the battery in Comparative Example 101 was set to 100.

[0449] In Table 1, the initial DC resistance in Comparative Example 101 is set to 100, and the relative values ​​of the DC resistance after 6 days of storage are shown (ie, relative values ​​when the initial DC resistance in Comparative Example 101 is set to 100).

[0450] [Table 1]

[0451]

[0452] As can be seen from Table 1, in the Examples in which the lithium borate compound of the present disclosure is contained in the non-aqueous solvent, the battery resistance after storage is lower than that of the Comparative Examples.

[0453] [Examples 111 to 114]

[0454] A lithium secondary battery was prepared in the same manner as in Example 101 except that the type and content of the additive contained in the nonaqueous electrolyte were changed as shown in Table 2.

[0455] The button-type batteries obtained as shown in Table 2 were subjected to the following evaluations.

[0456] Table 2 shows the evaluation results.

[0457] <Evaluation of DC resistance of battery after cycling>

[0458] For each battery obtained in each example, a DC resistance was evaluated as an evaluation of the internal resistance of the battery after cycles. The details are shown below.

[0459] The following operations were performed at a temperature of 55°C.

[0460] The battery was charged at a charging rate of 0.2C to a SOC of 80%, and then discharged at a discharging rate of 1C to a SOC of 20%, with this being considered as one cycle. The cycles were repeated for 0, 100, and 200 cycles.

[0461] The DC resistance (Ω) of the battery obtained after each cycle was measured by the method shown below. The relative value was determined when the DC resistance value of the battery in Comparative Example 101 after 0 cycles (ie, initial value) was set to 100. The results are shown in Table 2.

[0462] (Initial resistance (-20℃))

[0463] The button-type battery was repeatedly charged and discharged three times at a constant voltage of 4.2V, then charged to a constant voltage of 3.6V, then the charged button-type battery was cooled to -20°C in a thermostatic chamber, and discharged at a constant current of 0.2mA at -20°C, and the potential drop at 10 seconds from the start of discharge was measured, thereby measuring the DC resistance [Ω] of the button-type battery, and the obtained value was used as the resistance after 0 cycles (also referred to as "initial resistance [Ω] (-20°C)".). The initial resistance [Ω] (-20°C) was also measured in the same manner for the button-type battery of Comparative Example 101 described later.

[0464] Based on the above results, the "initial resistance (-20°C) (relative value; %)" was calculated using the following formula as the initial resistance value (relative value; %) in Example 101 when the initial resistance [Ω] (-20°C) in Comparative Example 101 was set to 100%. The results are shown in Table 2.

[0465] Initial resistance (-20℃) (relative value; %)

[0466] =(initial resistance value [Ω] (-20°C) in Example 101 / initial resistance value [Ω] (-20°C) in Comparative Example 101) × 100

[0467] [Table 2]

[0468]

[0469] As can be seen from Table 2, in the examples containing the lithium borate compound of the present disclosure in the non-aqueous solvent, the battery resistance after cycling is lower than that of the comparative example.

[0470] [Examples 121 to 124, Comparative Example 121]

[0471] A lithium secondary battery was produced in the same manner as in Example 101 except that the type and content of the lithium borate compound contained in the non-aqueous electrolyte were as shown in Table 3 and the content of vinylene carbonate contained in the non-aqueous electrolyte was as shown in Table 3 to prepare the non-aqueous electrolyte.

[0472] The battery resistance after the cycles was evaluated for the button-type batteries shown in Table 3 using the same method as the method for measuring the DC resistance (Ω) of the batteries obtained after each cycle described above. The results are shown in Table 3.

[0473] [Table 3]

[0474]

[0475] As can be seen from Table 3, in the examples in which the non-aqueous solvent contains vinylene carbonate and the lithium borate compound of the present disclosure, the battery resistance after cycling is lower than that of the comparative example.

[0476] The entire disclosure of Japanese Patent Application No. 2019-046971 filed on March 14, 2019 is incorporated into this specification by reference.

[0477] All documents, patent applications, and technical standards described in this specification are incorporated into this specification by reference to the same extent as if each document, patent application, and technical standard was specifically and individually described.

Claims

1. A lithium borate compound represented by the following formula (I), In formula (I), R 1 , R 2 and R 3 R each independently represents methyl, ethyl, n-propyl, isopropyl, 1-ethylpropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, 2-methylbutyl, 3,3-dimethylbutyl, n-pentyl, isopentyl, neopentyl, 1-methylpentyl, n-hexyl, isohexyl, sec-hexyl, or tert-hexyl; 10 represents trifluoromethyl.

2. The lithium borate compound according to claim 1, in, The R 1 , the R 2 And the R 3 Each is independently methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, or tert-butyl.

3. The lithium borate compound according to claim 1 or 2, which is a lithium borate compound represented by the following formula (II), the following formula (III), the following formula (IV), or the following formula (V), 4 . An additive for a lithium secondary battery, comprising the lithium borate compound according to claim 1 .

5. A non-aqueous electrolyte for a lithium secondary battery, comprising: As an electrolyte for lithium salts containing fluorine; non-aqueous solvent; and The lithium borate compound according to any one of claims 1 to 3.

6. The non-aqueous electrolyte for lithium secondary battery according to claim 5, in, The content of the lithium borate compound is 0.1 mass % to 5.0 mass % based on the total amount of the non-aqueous electrolyte for lithium secondary batteries. 7 . The non-aqueous electrolyte for lithium secondary batteries according to claim 5 , further comprising a cyclic carbonate having an unsaturated bond.

8. The non-aqueous electrolyte for lithium secondary battery according to claim 7, in, The cyclic carbonate having an unsaturated bond is vinylene carbonate.

9. The non-aqueous electrolyte for lithium secondary battery according to claim 8, in, The ratio of the content mass of the vinylene carbonate to the content mass of the lithium borate compound is in the range of 0.1 to 10.

10. A lithium secondary battery precursor comprising: a housing; and, The positive electrode, the negative electrode, the separator, and the electrolyte are contained in the shell. The positive electrode is a positive electrode that can absorb and release lithium ions. The negative electrode is a negative electrode that can absorb and release lithium ions. The electrolyte solution is the non-aqueous electrolyte solution for a lithium secondary battery according to any one of claims 5 to 9.

11. A method for manufacturing a lithium secondary battery, comprising the following steps: A step of preparing the lithium secondary battery precursor according to claim 10; and a step of obtaining a lithium secondary battery by subjecting the lithium secondary battery precursor to an aging treatment, The aging treatment includes the steps of charging and discharging the lithium secondary battery precursor in an environment of 20° C. to 60° C.