Polybutylene terephthalate thermoforming method

By adding a low melting point thermoplastic polymer to the polybutylene terephthalate molding composition, the problems of necking and stress growth during the thermoforming process are solved, and the uniformity and elongation performance of the material thickness are improved.

CN113692343BActive Publication Date: 2024-11-08BASF SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080027731.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-04-11
Filing Date
2020-04-08
Publication Date
2024-11-08
Estimated Expiration
2040-04-08

AI Technical Summary

Technical Problem

The polybutylene terephthalate molding composition has problems of necking and stress growth during the thermoforming process, resulting in uneven material thickness, affecting the mechanical properties and appearance of the finished product.

Method used

The thermoplastic polymer with a melting point below 220°C was added to the polybutylene terephthalate molding composition to reduce necking and stress growth and uniformize the elongation performance.

Benefits of technology

By adding a low melting point thermoplastic polymer, the necking and stress growth of the polybutylene terephthalate molding composition during the thermoforming process is significantly reduced, and the elongation uniformity and thermoforming properties of the material are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113692343B_ABST
    Figure CN113692343B_ABST
Patent Text Reader

Abstract

The invention relates to the use of a thermoplastic polymer having a melting point below 220° C. as an additive in a polybutylene terephthalate molding composition for reducing the necking of a sheet or film of the polybutylene terephthalate molding composition during elongation, preferably wherein the polybutylene terephthalate molding composition comprises a) 50 to 95% by weight of polybutylene terephthalate as component A, b) 5 to 50% by weight of a thermoplastic polymer having a melting point below 220° C. as component B, c) 0 to 45% by weight of a filler as component C, d) 0 to 20% by weight of other additives as component D, wherein the total amount of components A to D is 100% by weight.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for thermoforming polybutylene terephthalate, the use of specific additives therein, thermoformed moldings and molding compositions. Background Art

[0002] Thermoforming is a manufacturing process in which a plastic sheet is heated to a soft forming temperature, formed into a specific shape in a mold, cooled to a solid state, and then trimmed to produce a usable product. The sheet (or "film" when thinner gauges and certain material types are involved) is heated in an oven to a high enough temperature to allow it to be stretched and cooled to its final shape in or on a mold. A simplified version of this is vacuum forming.

[0003] In its simplest form, a small benchtop or laboratory machine can be used to heat a small cut section of plastic sheet and stretch it over a mold using a vacuum. This method is often used for samples and prototype parts. In complex and high-volume applications, very large production machines are used to heat and form the plastic sheet and trim the molded parts from the plastic sheet in a continuous, high-speed process, and can produce thousands of finished parts per hour, depending on the size of the machine and mold and the size of the part being molded.

[0004] Thermoforming is different from injection molding, blow molding, rotational molding and other forms of processing plastics. Thin-gauge thermoforming is mainly used to make disposable cups, containers, lids, trays, blisters, clamshells and other products for the food, medical and general retail industries. Thick-gauge thermoforming includes a variety of parts such as car doors and dashboards, multi-purpose lathes and plastic trays.

[0005] In the most common method of high-volume, continuous thermoforming of thin-gauge products, a plastic sheet is fed from a roll or from an extruder into a set of indexing chains containing pins or spikes that pierce the sheet and convey it through an oven to be heated to the forming temperature. The heated sheet is then indexed to the forming station where a mating mold and pressure box close over the sheet and a vacuum is then applied to remove trapped air and pull the material into or onto the mold along with pressurized air to form the plastic into the fine shape of the mold. In the case of taller, deeper molded parts, a plunger assist is often used in addition to the vacuum to provide the desired material distribution and thickness in the finished part. After a short molding cycle, as the molding tool opens, a reverse stream of air pressure, often called an air jet, is initiated from the vacuum side of the mold to break the vacuum and help the molded part disengage from or out of the mold. A stripper plate may also be used on the mold as it opens to eject finer parts or parts with negative draft, undercut areas. The sheet containing the formed parts is then indexed to a trimming station on the same machine where parts are die cut from the remaining web of sheet material, or to a separate trimmer where the formed parts are trimmed. The remaining web of sheet material after trimming the formed parts is typically wound onto a take-up reel or fed into an in-line granulator for recycling.

[0006] Thermoplastic molding compositions based on polybutylene terephthalate are known, for example, from US 2016 / 0122530 A1 and US 2008 / 0281018 A1. Summary of the invention

[0007] The object of the present invention is to provide a polybutylene terephthalate molding composition with improved thermoforming properties. Advantageously, the sheet or film of the polybutylene terephthalate molding composition should have reduced necking when stretched, reduced stress growth when strain is applied to the sheet or film and / or homogenized elongation properties when strain is applied to the sheet or film.

[0008] According to the present invention, these objects are achieved by using a thermoplastic polymer having a melting point below 220° C. as an additive in a polybutylene terephthalate molding composition to reduce the necking of a sheet or film of the polybutylene terephthalate molding composition during elongation.

[0009] Furthermore, the object is achieved by using thermoplastic polymers with a melting point below 220° C. as additives in polybutylene terephthalate molding compositions to reduce the stress growth when strain is applied to sheets or films of polybutylene terephthalate molding compositions, for example during thermoforming and / or hot film extrusion.

[0010] Furthermore, the object is achieved by using a thermoplastic polymer having a melting point below 220° C. as an additive in the polybutylene terephthalate molding composition to homogenize the elongation properties of a sheet or film of the polybutylene terephthalate molding composition when stress is applied to the sheet or film of the polybutylene terephthalate molding composition.

[0011] This advantage is most evident in thermoforming processes and / or hot film extrusion, which typically precedes a thermoforming step.

[0012] The material thickness during thermoforming is balanced by using thermoplastic polymers with a melting point below 220° C. as additives in the polybutylene terephthalate molding composition.

[0013] The term "melting point" is mainly used for semi-crystalline polymers, while for amorphous polymers, the glass transition temperature Tg replaces the melting point. Therefore, the term "melting point" as used herein defines or refers to the melting point of a semi-crystalline polymer, and the Tg of an amorphous polymer.

[0014] Preferably, all of the above effects are achieved by the use of the present invention.

[0015] The object is furthermore achieved by a process for producing a molding comprising or preferably consisting of a polybutylene terephthalate molding composition, wherein the polybutylene terephthalate molding composition comprises:

[0016] a) 50 to 95% by weight of polybutylene terephthalate as component A,

[0017] b) 5 to 50% by weight of a thermoplastic polymer having a melting point below 220° C. as component B,

[0018] c) 0 to 45% by weight of fillers as component C,

[0019] d) 0 to 20% by weight of other additives as component D,

[0020] The total amount of components A to D is 100 wt %,

[0021] By heating a sheet or film comprising or preferably made of a polybutylene terephthalate molding composition to a soft molding temperature, thermoforming the heated sheet or film into a desired shape in a mold, cooling the molded article to solidify it and optionally trimming the molded article.

[0022] The object is furthermore achieved by a corresponding polybutylene terephthalate moulding composition which can be used, for example, for thermoforming or injection moulding, and thermoformed or injection moulded mouldings are obtainable by the above-described process. DETAILED DESCRIPTION

[0023] Polybutylene terephthalate (PBT) is a thermoplastic engineering polymer used, for example, as an insulator in the electrical and electronics industry. It is a thermoplastic and semi-crystalline polymer or polyester with a melting point of 222 to 225°C, typically 223°C.

[0024] According to the present invention, it was found that by adding a thermoplastic polymer having a melting point lower than that of polybutylene terephthalate, the sliding curve represented by the stress / strain diagram can be smoothed and the initial "bump" observed during 0 to 30% strain can be avoided. This "bump" is an increase in stress, which generally decreases again after 20% to 30% strain until a lower plateau is reached. This "bump" can be compared to the activation energy in a catalytic process and can be described as the necking experienced by the stretch rod when the strain is applied. This "necking" can be seen as a reduction in cross-sectional area in the area of ​​the stretch rod that experiences more elongation than other parts of it. This "necking" usually occurs when a heated polymer sheet or film is stretched in the longitudinal direction between hot and cold rollers. The "necking" causes the cross-sectional area of ​​the stretch rod to be non-uniform when the strain is applied. In the thermoforming process, this leads to a reduction in the material thickness in the high strain area. However, it is desirable to have a uniform material thickness as much as possible throughout the thermoformed body to avoid thin areas of material, which can lead to mechanical weaknesses and non-uniform appearance, such as for colored or colored molded parts.

[0025] By adding a low melting point thermoplastic polymer to PBT, necking during elongation can be reduced, which can also be described as reducing the stress growth when strain is applied to the sheet or film, or homogenizing the elongation properties of the sheet or film.

[0026] Typically, "necking" is more pronounced at lower thermoforming temperatures. In other words, by adding low-melting thermopolymers to PBT, the temperature window in which thermoforming can be performed can be widened.

[0027] Figure 1 Shows PBT( Typical stress-strain diagram of B6550LN). The tensile test was performed according to ISO527-2:2012 at a speed of 50 mm / min as described in the experimental section.

[0028] In all figures, the stress as a function of strain is monitored for different temperatures (increasing from the top curve to the bottom curve). From these sliding curves a theoretical hot forming temperature window of 210 to 220° C. can be determined.

[0029] By including the low melting point thermoplastic polymer of the present invention, the theoretical thermoforming window can be significantly broadened, such as Figure 2, which shows similar tensile test results, where the PBT contains 20% by weight of a polyester based on aliphatic and aromatic dicarboxylic acids and aliphatic dihydroxy compounds ( B6550 LN, which has 20 wt.% F Blend C1200, both purchased from BASF SE).

[0030] According to the present invention, all thermoplastic polymers having a lower melting point (or Tg in the case of amorphous polymers) than PBT can be used. However, it is preferred that the thermoplastic polymer can be easily dispersed in the PBT matrix and remain dispersed in the PBT matrix during the thermoforming process without showing large-scale phase separation. Therefore, thermoplastic polymers with chemical properties similar to PBT are preferred.

[0031] Preferred thermoplastic polymers are selected from semiaromatic polyesters, preferably polyesters based on aliphatic and aromatic dicarboxylic acids and aliphatic dihydroxy compounds; thermoplastic elastomers; copolymers of acrylates, styrene and acrylonitrile; polylactic acid; polypropylene; polyethylene and mixtures thereof.

[0032] On the other hand, polyketones and polyamides are not preferred.

[0033] The amount of the thermoplastic polymer is preferably 5 to 40% by weight, more preferably 10 to 30% by weight, most preferably 15 to 25% by weight, based on 100% by weight of the total amount of the polybutylene terephthalate molding composition.

[0034] In the context of the present invention, the term "polybutylene terephthalate molding composition" should be described as the final molding composition for thermoforming a sheet or film. Therefore, the polybutylene terephthalate molding composition comprises all the ingredients of the final molding composition. In addition, in these polybutylene terephthalate molding compositions, PBT is the matrix polymer that forms the continuous matrix of the molding composition. In this matrix, other ingredients are included, preferably in the final dispersed form. Therefore, the amount of PBT in the polybutylene terephthalate molding composition is at least 50% by weight, more preferably at least 60% by weight, and most preferably at least 65% by weight, based on the total amount of 100% by weight of the polybutylene terephthalate molding composition.

[0035] Further constituents of the molding compositions may be mineral fillers and other additives.

[0036] Preferably, the polybutylene terephthalate molding composition comprises:

[0037] a) 50 to 95% by weight of polybutylene terephthalate as component A,

[0038] b) 5 to 50% by weight of a thermoplastic polymer having a melting point below 220° C. as component B,

[0039] c) 0 to 45% by weight of fillers as component C,

[0040] d) 0 to 20% by weight of other additives as component D,

[0041] Components A to D together make up 100% by weight.

[0042] If a (mineral) filler is present, it is preferably present in an amount of 5 to 45 wt %. The upper limit of component A is then reduced to 90 wt %, so that the sum of the wt % does not exceed 100 wt %. If a (mineral) filler is present, its amount is more preferably 7 to 15 wt %, most preferably 8 to 12 wt %, for example about 10 wt %, and the upper limit of component A is reduced accordingly.

[0043] Component B is used in an amount of preferably 10 to 30% by weight, more preferably 15 to 25% by weight.

[0044] The amount of other additives is 0 to 20 wt %, more preferably 0 to 10 wt %, most preferably 0 to 5 wt %.

[0045] Therefore, the amount of component A is preferably 50 to 83 wt%, most preferably 50 to 77 wt%.

[0046] If further additives are present, their minimum amount is preferably 0.1% by weight, more preferably 0.3% by weight. In this case, the upper limit of component A is reduced by 0.1% by weight or preferably 0.3% by weight, so that the sum of components A to D is 100% by weight.

[0047] By adding (mineral) fillers, an accurate reproduction of surface details can be achieved.

[0048] Preferred PBTs have viscosity values ​​of 120 to 200, preferably 130 to 190, measured in accordance with ISO 1628 effective in 2019 at 25° C. in a 0.5% by weight solution in a phenol / o-dichlorobenzene mixture (weight ratio 1:1).

[0049] The PBT preferably has a terminal carboxyl content of up to 100 meq / kg polyester, preferably up to 40 meq / kg polyester, in particular up to 30 meq / kg polyester. For example, polyesters of this type can be produced by the process of DE-A 44 01 055. The terminal carboxyl content is usually determined by titration (e.g. potentiometry).

[0050] Particularly preferred PBT is produced using a Ti catalyst. Their residual Ti content after the polymerization process is preferably less than 250 ppm, more preferably less than 200 ppm, in particular less than 150 ppm.

[0051] The melting point of the thermoplastic polymer additive B is below 220° C., preferably below 200° C., more preferably below 180° C., most preferably below 160° C., especially below 130° C., for example below 120° C. According to the present invention, the melting point range that can be considered is 40 to 219° C., preferably 50 to 199° C., more preferably 60 to 179° C., especially 80 to 129° C., more particularly 90 to 119° C., for example 100 to 119° C. The melting point can be determined by differential scanning calorimetry (DSC) at a heating rate of 20° C. / min according to ISO 11357-1 / -3, which came into force in 2019.

[0052] Component B may be a polyester, such as an aliphatic polyester, an aromatic polyester or a semi-aromatic polyester. Semi-aromatic polyesters may contain aliphatic dicarboxylic acid units and / or aliphatic dihydroxy compound units and contain at least one aromatic dicarboxylic acid unit and an aromatic dihydroxy compound unit. Aliphatic polyesters do not contain aromatic units. Aromatic polyesters do not contain aliphatic units.

[0053] Preferably, any polyester based on aliphatic and aromatic dicarboxylic acids and aliphatic dihydroxy compounds (referred to as semiaromatic polyesters) can be used as component B to prepare the preferred biodegradable polyester mixtures of the present invention. The molar ratio of aliphatic and aromatic dicarboxylic acids can be 0.5:10 to 10:0.5, preferably 1:10 to 10:1, more preferably 3:7 to 10:1. Of course, mixtures of two or more of these polyesters are also suitable as component B.

[0054] According to the invention, the term "semiaromatic polyester" is also intended to include polyester derivatives, such as polyetheresters, polyesteramides or polyetheresteramides. Suitable semiaromatic polyesters are linear, non-chain-extended polyesters (WO 92 / 09654). Preference is given to chain-extended and / or branched semiaromatic polyesters. The latter are disclosed in the specifications WO 96 / 15173-15176, WO 21689-21692, WO 25446, WO 25448, WO 98 / 12242 mentioned at the outset, which are hereby incorporated into the present description by reference. It is also possible to use mixtures of different semiaromatic polyesters. In particular, the term semiaromatic polyester is intended to mean products such as (BASF Aktiengesellschaft) and Bio (Novamont).

[0055] Particularly preferred semiaromatic polyesters for component B are polyesters which comprise the following essential components:

[0056] BA) an acid component consisting of:

[0057] a1) 30 to 99 mol % of at least one aliphatic or at least one cycloaliphatic dicarboxylic acid, or an ester-forming derivative thereof, in particular an ester or anhydride thereof, or a mixture thereof,

[0058] a2) 1 to 70 mol % of at least one aromatic dicarboxylic acid or an ester-forming derivative thereof, in particular an ester or anhydride thereof, or a mixture thereof, and

[0059] a3) 0 to 5 mol% of a compound containing a sulfonate group, BB) a diol component selected from at least one C2-C 12 Alkanediol and at least one C5-C 10 ring

[0060] Alkanediols, or mixtures thereof,

[0061] and, if necessary, one or more components selected from the following: BC) components selected from the following:

[0062] c1) at least one dihydroxy compound containing an ether function and having the formula I

[0063] HO-[(CH2) n -O m -H (I)

[0064] wherein n is 2, 3 or 4 and m is an integer from 2 to 250,

[0065] c2) at least one hydroxycarboxylic acid of the formula IIa or IIb

[0066]

[0067] wherein p is an integer from 1 to 1500 and r is an integer from 1 to 4, and G is a group selected from the following: phenylene; -(CH2) q —, wherein q is an integer from 1 to 5; —C(R)H— and —C(R)HCH2, wherein R is methyl or ethyl,

[0068] c3) at least one amino-C2-C 12 Alkanol, or at least one amino-C5-C 10 Cycloalkanol, or a mixture thereof,

[0069] c4) at least one diamino-C1-C8 alkane,

[0070] c5) at least one 2,2'-dioxazoline of formula III

[0071]

[0072] Where R 1 is a single bond, (CH2) Z - alkylene, wherein z is 2, 3 or 4, or phenylene

[0073] c6) at least one aminocarboxylic acid selected from naturally occurring amino acids, polyamides obtainable by polycondensation of dicarboxylic acids having 4 to 6 carbon atoms with diamines having 4 to 10 carbon atoms, compounds of the formula IVa and IVb

[0074]

[0075] wherein s is an integer from 1 to 1500 and t is an integer from 1 to 4, and T is a group selected from the following: phenylene; -(CH2) u —, where u is an integer from 1 to 12; —C(R 2 )H— and—C(R 2 )HCH2—, where R 2 is methyl or ethyl,

[0076] and a polyoxazoline having a repeating unit V

[0077]

[0078] Where R 3 is hydrogen, C1-C6-alkyl, C5-C8-cycloalkyl, phenyl which may be unsubstituted or substituted by up to 3 C1-C4-alkyl substituents, or tetrahydrofuranyl,

[0079] or a mixture consisting of C1 to C6,

[0080] as well as

[0081] BD) is selected from the following components:

[0082] d1) at least one compound having at least three groups capable of forming esters,

[0083] d2) at least one isocyanate,

[0084] d3) at least one divinyl ether,

[0085] Or a mixture consisting of d1) to d3).

[0086] In a preferred embodiment, the acid component BA of the semiaromatic polyester comprises 30 to 70 mol %, in particular 40 to 60 mol %, of a1 and 30 to 70 mol %, in particular 40 to 60 mol %, of a2.

[0087] The fatty acids and corresponding derivatives a1 that can be used are generally those with 2 to 10 carbon atoms, preferably 4 to 6 carbon atoms. They can be straight-chain or branched. The alicyclic dicarboxylic acids that can be used for the purposes of the present invention are generally those with 7 to 10 carbon atoms, in particular those with 8 carbon atoms. However, in principle, dicarboxylic acids with a greater number of carbon atoms, for example with up to 36 carbon atoms, can also be used.

[0088] Examples which may be mentioned are: malonic acid, succinic acid, glutaric acid, 2-methylglutaric acid, 3-methylglutaric acid, adipic acid, pimelic acid, azelaic acid, sebacic acid, fumaric acid, 2,2-dimethylglutaric acid, suberic acid, 1,3-cyclopentanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, diglycolic acid, itaconic acid, maleic acid and 2,5-norbornanedicarboxylic acid and its fatty acid dimers.

[0089] It is also possible to use ester derivatives of the above-mentioned aliphatic or alicyclic dicarboxylic acids, in particular di-C1-C6-alkyl esters, such as dimethyl ester, diethyl ester, di-n-propyl ester, diisopropyl ester, di-n-butyl ester, diisobutyl ester, di-tert-butyl ester, di-n-pentyl ester, diisopentyl ester or di-n-hexyl ester. It is also possible to use anhydrides of the dicarboxylic acids.

[0090] The dicarboxylic acids or ester-forming derivatives thereof may be used here alone or in the form of a mixture of two or more thereof.

[0091] Succinic acid, adipic acid, azelaic acid, sebacic acid, tridecanedioic acid, or their respective ester derivatives, or mixtures thereof are preferably used. Succinic acid, adipic acid or sebacic acid, or their respective ester derivatives, or mixtures thereof are particularly preferably used. Adipic acid or its ester derivatives, such as its alkyl esters or mixtures thereof are particularly preferably used. When preparing polymer mixtures with "hard" or "brittle" components (such as polyhydroxybutyrate or in particular polylactide), sebacic acid or mixtures of sebacic acid and adipic acid are preferably used as aliphatic dicarboxylic acids. When preparing polymer mixtures with "soft" or "hard" components (such as polyhydroxybutyrate valerate copolymers), succinic acid or mixtures of succinic acid and adipic acid are preferably used as aliphatic dicarboxylic acids.

[0092] Succinic acid, azelaic acid, sebacic acid and tridecanedioic acid have the additional advantage of being available in the form of renewable raw materials.

[0093] Aromatic dicarboxylic acids a2 that may be mentioned are generally those having 8 to 12 carbon atoms and preferably those having 8 carbon atoms. For example, phthalic acid, terephthalic acid, isophthalic acid, 2,6-naphthoic acid and 1,5-naphthoic acid, and their ester derivatives may be mentioned. Di-C1-C6-alkyl esters may be mentioned here in particular, such as dimethyl ester, diethyl ester, di-n-propyl ester, diisopropyl ester, di-n-butyl ester, diisobutyl ester, di-tert-butyl ester, di-n-pentyl ester, diisopentyl ester or di-n-hexyl ester. The anhydrides of dicarboxylic acids a2 are also suitable ester derivatives.

[0094] In principle, however, it is also possible to use aromatic dicarboxylic acids a2 having a higher number of carbon atoms, for example up to 20 carbon atoms.

[0095] The aromatic dicarboxylic acids or their ester-forming derivatives a2 can be used alone or as a mixture of two or more thereof. It is particularly preferred to use terephthalic acid or its ester-forming derivatives, such as dimethyl terephthalate.

[0096] The compound containing a sulfonate group used is usually an alkali metal salt or alkaline earth metal salt of a sulfonate-containing dicarboxylic acid or an ester-forming derivative thereof, preferably an alkali metal salt of 5-sulfoisophthalic acid or a mixture thereof, particularly preferably a sodium salt.

[0097] In a preferred embodiment, the acid component BA comprises 40 to 60 mol% of a1, 40 to 60 mol% of a2 and 0 to 2 mol% of a3. In another preferred embodiment, the acid component A comprises 40 to 59.9 mol% of a1, 40 to 59.9 mol% of a2 and 0.1 to 1 mol% of a3, in particular 40 to 59.8 mol% of a1, 40 to 59.8 mol% of a2 and 0.2 to 0.5 mol% of a3.

[0098] The diol BB is generally chosen from branched or straight-chain alkanediols having from 2 to 12 carbon atoms, preferably from 4 to 6 carbon atoms, or from cycloalkanediols having from 5 to 10 carbon atoms.

[0099] Examples of suitable alkanediols are ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,4-butanediol, 1,5-pentanediol, 2,4-dimethyl-2-ethyl-1,3-hexanediol, 2,2-dimethyl-1,3-propylene glycol, 2-ethyl-2-butyl-1,3-propylene glycol, 2-ethyl-2-isobutyl-1,3-propylene glycol and 2,2,4-trimethyl-1,6-hexanediol, in particular ethylene glycol, 1,3-propylene glycol, 1,4-butanediol or 2,2-dimethyl-1,3-propylene glycol (neopentyl glycol); cyclopentanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol or 2,2,4,4-tetramethyl-1,3-cyclobutanediol. Particular preference is given to 1,4-butanediol, in particular in combination with 1,3-propanediol and adipic acid as component a1), in particular in combination with sebacic acid as component a1). 1,3-Propanediol and 1,4-butanediol have the additional advantage of being available in the form of renewable raw materials. Mixtures of different alkanediols can also be used.

[0100] Depending on whether an excess of acid groups or OH end groups is desired, component BA or component BB can be used in excess. In a preferred embodiment, components BA and BB can be used in a molar ratio of 0.4:1 to 1.5:1, preferably 0.6:1 to 1.1:1.

[0101] Besides components BA and BB, the polyesters on which the polyester mixtures according to the invention are based may comprise further components.

[0102] Preferred dihydroxy compounds c1 are diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol and polytetrahydrofuran (poly-THF), particularly preferably diethylene glycol, triethylene glycol and polyethylene glycol, and mixtures thereof may also be used, such as possible compounds with different variables n (see formula I), for example polyethylene glycol comprising propylene units (n=3), obtainable, for example, by polymerization using polymerization processes known per se, first with ethylene oxide and then with propylene oxide, and particularly preferably polymers based on polyethylene glycol with different variables n, in which units formed from ethylene oxide predominate. The molar mass (M) of the polyethylene glycol is n ) is generally 250 to 8000 g / mol, preferably 600 to 3000 g / mol.

[0103] In a preferred embodiment for preparing semiaromatic polyesters, for example, 15 to 98 mol %, preferably 60 to 99.5 mol %, of diols BB and 0.2 to 85 mol %, preferably 0.5 to 30 mol %, of dihydroxy compounds c1, based on the molar amounts of BB and c1, can be used.

[0104] In a preferred embodiment, the hydroxycarboxylic acid c2) used is glycolic acid, D-lactic acid, L-lactic acid or D,L-lactic acid, 6-hydroxycaproic acid, their cyclic derivatives, such as glycolide (1,4-dioxane-2,5-dione), D-dilactide or L-dilactide (3,6-dimethyl-1,4-dioxane-2,5-dione), p-hydroxybenzoic acid, or their oligomers and polymers, such as 3-polyhydroxybutyric acid, polyhydroxyvaleric acid, polylactide (for example, which can be obtained as Nature (Cargill)), or a mixture of 3-polyhydroxybutyric acid and polyhydroxyvaleric acid (the latter can be obtained as Available from Zeneca) and is used to prepare semiaromatic polyesters, with low molecular weight and cyclic derivatives thereof being particularly preferred.

[0105] Examples of amounts of hydroxycarboxylic acids which can be used are from 0.01 to 50% by weight, preferably from 0.1 to 40% by weight, based on the amount of BA and BB.

[0106] For the purposes of the present invention, amino-C2-C 12 Alkyl alcohol or amino-C5-C 10 Cycloalkanols (component c3) also include 4-aminomethylcyclohexanemethanol, preferably amino-C2-C6-alkanols, such as 2-aminoethanol, 3-aminopropanol, 4-aminobutanol, 5-aminopentanol or 6-aminohexanol, or amino-C5-C6-cycloalkanols, such as aminocyclopentanol and aminocyclohexanol, or mixtures thereof.

[0107] The diamino-C1-C8-alkanes (component c4) used are preferably diamino-C4-C6-alkanes, for example 1,4-diaminobutane, 1,5-diaminopentane or 1,6-diaminohexane (hexamethylenediamine, “HMD”).

[0108] In a preferred embodiment for preparing semiaromatic polyesters, 0.5 to 99.5 mol %, preferably 0.5 to 50 mol %, of c3, based on the molar amount of BB, and 0 to 50 mol %, preferably 0 to 35 mol %, of c4, based on the molar amount of BB, can be used.

[0109] 2,2'-Bisoxazolines c5 of the formula III can generally be obtained by the process of Angew. Chem. Int. Edit., Vol. 11 (1972), pp. 287 to 288. Particularly preferred bisoxazolines are those in which R 1 is a single bond, (CH2) z-alkylene where z=2, 3 or 4, for example methylene, ethane-1,2-diyl, propane-1,3-diyl or propane-1,2-diyl, or phenylene. Particularly preferred bisoxazolines which may be mentioned are 2,2′-bis(2-oxazoline), bis(2-oxazolinyl)methane, 1,2-bis(2-oxazolinyl)ethane, 1,3-bis(2-oxazolinyl)propane and 1,4-bis(2-oxazolinyl)butane, in particular 1,4-bis(2-oxazolinyl)benzene, 1,2-bis(2-oxazolinyl)benzene or 1,3-bis(2-oxazolinyl)benzene.

[0110] For example, in the preparation of semiaromatic polyesters, 70 to 98 mol % of BB, up to 30 mol % of c3 and 0.5 to 30 mol % of c4 and 0.5 to 30 mol % of c5 can be used, in each case based on the total molar amount of components BB, c3, c4 and c5. In a further preferred embodiment, 0.1 to 5 wt. %, preferably 0.2 to 4 wt. %, of c5, based on the total weight of BA and BB, can be used.

[0111] The component c6 used may be a naturally occurring aminocarboxylic acid. They include valine, leucine, isoleucine, threonine, methionine, phenylalanine, tryptophan, lysine, alanine, arginine, aspartic acid, cysteine, glutamic acid, glycine, histidine, proline, serine, tyrosine, asparagine and glutamine.

[0112] Preferred aminocarboxylic acids of formula IVa and IVb are those wherein s is an integer from 1 to 1000, t is an integer from 1 to 4, preferably 1 or 2, and t is selected from phenylene and —(CH 2 ) u —, where u is 1, 5, or 12.

[0113] c6 may also be a polyoxazoline of the formula V. However, c6 may also be a mixture of different aminocarboxylic acids and / or polyoxazolines.

[0114] In a preferred embodiment, c6 is used in an amount of 0.01 to 50% by weight, preferably 0.1 to 40% by weight, based on the total amount of components BA and BB.

[0115] If desired, further components which can be used for the preparation of the semiaromatic polyesters are compounds d1 which comprise at least three groups which are capable of forming esters.

[0116] Compound d1 preferably contains three to ten functional groups capable of forming ester bonds. Particularly preferred compounds d1 have three to six such functional groups in the molecule, in particular three to six hydroxyl and / or carboxyl groups. Examples which should be mentioned are: tartaric acid, citric acid, maleic acid; trimethylolpropane, trimethylolethane; pentaerythritol; polyether triols; glycerol; trimesic acid; trimellitic acid, trimellitic anhydride; pyromellitic acid, pyromellitic anhydride and hydroxyisophthalic acid.

[0117] The compound d1 is generally used in an amount of 0.01 to 15 mol %, preferably 0.05 to 10 mol %, particularly preferably 0.1 to 4 mol %, based on component BA.

[0118] The component d2 used is an isocyanate or a mixture of different isocyanates. For example, aromatic or aliphatic diisocyanates can be used. However, higher-functional isocyanates can also be used.

[0119] For the purposes of the present invention, the aromatic diisocyanate d2 is especially toluene 2,4-diisocyanate, toluene 2,6-diisocyanate, diphenyltoluene 2,2′-diisocyanate, diphenyltoluene 2,4′-diisocyanate, diphenylmethane 4,4-diisocyanate, naphthylene 1,5-diisocyanate or xylene diisocyanate.

[0120] Among them, diphenylmethane 2,2'-diisocyanate, diphenylmethane 2,4'-diisocyanate and diphenylmethane 4,4'-diisocyanate are particularly preferred as d2. The latter diisocyanates are usually used as a mixture.

[0121] A tricyclic isocyanate d2 which can also be used is tris(4-isocyanatophenyl)methane. For example, polycyclic aromatic diisocyanates are produced during the preparation of monocyclic or bicyclic diisocyanates.

[0122] Component d2 may also comprise minor amounts, for example up to 5% by weight, based on the total weight of component d2, of uretdione groups, for example for blocking isocyanate groups.

[0123] For the purposes of the present invention, aliphatic diisocyanates d2 are primarily linear or branched alkylene diisocyanates or cycloalkylene diisocyanates having 2 to 20 carbon atoms, preferably 3 to 12 carbon atoms, such as hexamethylene 1,6-diisocyanate, isophorone diisocyanate or methylenebis(4-isocyanatocyclohexane). Hexamethylene 1,6-diisocyanate and isophorone diisocyanate are particularly preferred aliphatic diisocyanates d2.

[0124] Preferred isocyanurates are those derived from C2-C 20 , preferably C3-C 12The alkylene diisocyanates are preferably aliphatic isocyanurates of cycloalkylene diisocyanates or alkylene diisocyanates, such as isophorone diisocyanate or methylenebis(4-isocyanatocyclohexane). The alkylene diisocyanates here may be linear or branched. Particularly preferred are isocyanurates based on n-hexamethylene diisocyanate, such as cyclic trimers, pentamers or higher oligomers of n-hexamethylene diisocyanate.

[0125] Component d2 is generally used in an amount of 0.01 to 5 mol %, preferably 0.05 to 4 mol %, particularly preferably 0.1 to 4 mol %, based on the total molar amount of BA and BB.

[0126] Divinyl ethers d3 which can be used are generally any customary and commercially available divinyl ethers. Preference is given to using 1,4-butanediol divinyl ether, 1,6-hexanediol divinyl ether or 1,4-cyclohexanedimethanol divinyl ether or mixtures thereof.

[0127] The divinyl ether is preferably used in an amount of 0.01 to 5% by weight, in particular 0.2 to 4% by weight, based on the total weight of BA and BB.

[0128] Examples of preferred semiaromatic polyesters are based on the following components:

[0129] BA, BB, d1

[0130] BA, BB, d2

[0131] BA, BB, d1, d2

[0132] BA, BB, d3

[0133] BA, BB, c1

[0134] BA, BB, c1, d3

[0135] BA, BB, c3, c4

[0136] BA, BB, c3, c4, c5

[0137] BA, BB, d1, c3, c5

[0138] BA, BB, c3, d3

[0139] BA, BB, c3, d1

[0140] BA, BB, c1, c3, d3

[0141] BA, BB, c2.

[0142] Among them, semiaromatic polyesters based on BA, BB and d1, or BA, BB and d2, or BA, BB, d1 and d2 are particularly preferred. In another preferred embodiment, the semiaromatic polyester is based on BA, BB, c3, M and c5 or BA, BB, d1, c3 and c5.

[0143] A suitable polyester is poly(butylene adipate terephthalate) (PBAT), available from BASF SE as Obtained under the brand name F Blend C1200.

[0144] Preferred PBATs may comprise adipate and terephthalate units in a molar ratio of 0.5:10 to 10:0.5, preferably 1:10 to 10:1.

[0145] Suitable thermoplastic elastomers are described, for example, in WK Witsiepe, Segmented Polyester Thermoplastic Elastomers, published in Polymerization Reactions and New Polymers, Chapter 4, 1973, pages 39 to 60. An example of a thermoplastic elastomer is TPEE, which can be obtained as 4056 was obtained from DuPont.

[0146] Copolymers of acrylates, styrene and acrylonitrile are called ASA polymers. They are produced by INEOSStyrolution 358N. ABS (acrylonitrile butadiene styrene copolymer) can also be used.

[0147] Polylactic acid (PLA) can be obtained from NatureWorks ( PLA 4044).

[0148] Polyketone (reference example) can be used, for example, PK-VM was obtained from AKRO Plastic.

[0149] Different grades of polyethylene can be used, such as HDPE (from LyondellBasell 4261AG) or LDPE (from LyondellBasell 2420F).

[0150] Fillers (component C) can be selected from granular or fibrous inorganic materials (mineral fillers), such as basalt, kaolin, wollastonite. Granular materials are preferred over fibers. Possible fibers include glass fibers, carbon fibers, aramid fibers, carbon nanotubes. Granular fillers include talc, carbon black, aluminum oxide, titanium dioxide, silicon dioxide and mixed oxides thereof. Preferably, talc is used.

[0151] Other additives (component D) can be selected from a variety of additives. Particular additives are stabilizers, nucleating agents, lubricants and anti-adhesives, such as stearates (especially calcium stearate), waxes, such as beeswax or beeswax esters; plasticizers, such as citrates (especially acetyl tributyl citrate), glycerides, such as glycerol triacetate, or ethylene glycol derivatives; surfactants, such as polysorbates, palmitates, laurates; antistatic agents, antifogging agents or dyes. See also US 2003 / 195296 for a list of more additives.

[0152] According to one embodiment of the present invention, the polybutylene terephthalate molding composition does not contain epoxy-containing olefin resins such as ethylene / glycidyl methacrylate and ethylene / methyl acrylate / glycidyl methacrylate copolymers, polyethylene such as LDPE polycarbonate, thermoplastic polyester elastomers (TPEE) (such as poly(butylene glycol), ethylene / butyl acrylate / glycidyl methacrylate copolymers or copolyetherester elastomer soft phases) 4056).

[0153] Preferred additives are copolymers containing epoxy groups and based on styrene, acrylates and / or methacrylates, bisphenol A epoxides, or fatty acid esters containing epoxy groups or fatty acid amides of natural oils, or mixtures thereof, each based on 100% by weight of the total amount of compounds A to D. The amount of the additive is preferably 0.1 to 2% by weight, more preferably 0.15 to 1% by weight, most preferably 0.2 to 0.4% by weight, based on 100% by weight of the total amount of components A to D. The upper limit of component A is reduced accordingly.

[0154] Most preferably, component D comprises styrene-acrylic acid-glycidyl methacrylate copolymer, which is available from BASF SE ( ADR 4400), melting point: 115°C.

[0155] The method for preparing a molded article made of the above-mentioned polybutylene terephthalate molding composition comprises heating a sheet or foil made of the polybutylene terephthalate molding composition to a soft molding temperature, thermoforming the heated sheet into a desired shape in a mold, cooling the molded article to solidify it, and optionally trimming the molded article.

[0156] The thickness of sheets is typically 0.2 to 10 mm, while the thickness of foils is typically 15 to 150 μm.

[0157] The soft forming temperature can be determined by routine experiments.Preferably, the thermoforming window should be in the range of 120 to 225°C, more preferably 150 to 221°C, especially 170 to 220°C.

[0158] Thermoforming methods can be as follows:

[0159] There are two general types of thermoforming methods. Sheets less than 1.5 mm (0.060 in) thick are typically fed to the thermoformer from a roll or sheet extruder. Thin-gauge roll-fed or in-line extrusion thermoforming applications are dominated by rigid or semi-rigid disposable packaging. Sheets thicker than 3 mm (0.120 in) are typically fed to the forming machine by hand or automatic feeding methods and already cut to final size. Heavy or thick-gauge cut sheet thermoforming applications are primarily used as permanent structural components. Medium gauge refers to sheets with a thickness of 1.5 mm to 3 mm.

[0160] Heavy gauge molding uses the same basic method as continuous thin gauge sheet molding, typically by draping a heated plastic sheet over a mold. Many heavy gauge molding applications use only vacuum during the molding process, although some use two mating molding tool halves and include air pressure to assist in molding. Aircraft windshields and machine gun turret windows can be used. Heavy gauge parts are used as decorative surfaces on permanent structures, such as kiosks, automobiles, trucks, medical devices, material handling equipment, spas and shower enclosures, and electrical and electronic equipment. Unlike most thin gauge thermoformed parts, heavy gauge parts are often hand machined after molding to trim to final shape or perform additional drilling, cutting, or finishing, depending on the product. Heavy gauge products are generally of a "permanent" end-use nature, while thin gauge parts are typically designed to be disposable or recyclable, primarily used to package or contain food or products.

[0161] Microprocessor and computer control on thermoforming machinery allows for improved process control and repeatability of identical job setups from one production run, with the ability to save oven heater and process timing settings between jobs. The ability to place formed sheets into in-line trimming stations for more precise trimming positioning is improved due to the common use of electric servomotors for chain indexing compared to pneumatic cylinders, racks and pinions, and clutches. Electric servomotors are also used on more complex forming machines to drive the machine platens in which the forming and trimming tools are mounted, rather than pneumatic cylinders, allowing for more precise control of the speed and timing of closing and opening the tools. Quartz and radiant plate oven heaters generally provide more precise and thorough heating of the sheet than cal-rod type heaters and better allow the oven to be zoned into zones with adjustable heat.

[0162] Modern thermoforming machines use multiple sensors to record production operation data in real time, including air pressure, temperature, tool strain gauges and other technical parameters. Whenever the preset production parameters are compromised during operation, the system will issue multiple warnings and alarms, thereby reducing machine downtime, shortening startup time and reducing startup scrap.

[0163] A major part of the thermoforming process is the tooling, which is specific to each part to be produced. Thin-gauge thermoforming as described above is almost always performed on an in-line machine and typically requires the tooling, plug assist, press box and all mounting plates as well as trimming tools and stacker components. Thick or heavy-gauge thermoforming also requires tooling specific to each part, but since part sizes can be very large, the tooling can be either cast aluminum or composite or machined aluminum in thin gauges. Typically, thick-gauge parts must be trimmed on a CNC router or hand trimmed using a saw or hand router.

[0164] The invention also relates to a thermoformed moulding obtainable by the process described above.

[0165] The invention also relates to a polybutylene terephthalate molding composition as defined above.

[0166] According to one embodiment, the molding composition comprises less than 10% by weight, based on the polybutylene terephthalate molding composition, of a biodegradable homo- or copolyester selected from the group consisting of polylactides, polycaprolactones, polyhydroxyalkanoates and polyesters composed of aliphatic dicarboxylic acids and aliphatic diols.

[0167] According to one embodiment of the invention, the polybutylene terephthalate molding composition contains no polymers containing repeating units comprising acrylic acid and / or styrene other than the styrene-acrylic acid-glycidyl methacrylate copolymer.

[0168] Thermoformed moldings may result from a variety of possible applications as outlined in the introduction above.

[0169] The present invention is described in more detail in the following examples.

[0170] Example

[0171] Differential scanning calorimetry (DSC) was carried out at 20 K / min in accordance with ISO 11357-1. The glass transition temperature was determined in accordance with ISO 11357-2 and the melting point in accordance with ISO 11357-3, respectively.

[0172] Material

[0173] Poly(butylene terephthalate) (PBT): BASF SE B6550, melting point: 223°C;

[0174] Poly(butylene adipate terephthalate) (PBAT): BASF SE F Blend C1200, melting point: 110 to 115°C;

[0175] Thermoplastic Elastomer (TPEE): DuPont 4056, melting point: 152°C;

[0176] Acrylate, Styrene Acrylonitrile (ASA): NEOS Styrolution 358N, melting point: 111°C;

[0177] Poly(lactic acid) (PLA): NatureWorks PLA 4044, melting point: 153°C;

[0178] Poly(ketone)(PK): AKRO Plastic PK-VM, melting point: 220°C;

[0179] Poly(ethylene) (HDPE): LyondellBasell 4261AG, melting point: 131°C;

[0180] Poly(ethylene) (LDPE): LyondellBasell 2420F, melting point: 111℃;

[0181] Polyamide-6.6: BASF SE A 24E, melting point: 263°C.

[0182] Preparation of Example V1

[0183] B6550 was extruded in a twin screw extruder (ZE40AUTXi) at a melt temperature of 275°C. 4056. After extrusion, the strands were cooled with water and cut into pellets. The samples were dried at 100°C for four hours. The samples were injection molded using an Arburg 470 at 260°C with a molding time of 5 to 10 seconds. This process produced a tensile rod with a thickness of 4.0 mm ( Figure 3 specific content in ).

[0184] Examples V2 to V6 and C1 were prepared using the same method.

[0185] Figure 3 The dimensions of the tensile rod are shown in mm.

[0186] test

[0187] The tensile test was performed according to ISO 527-2:2012 at 50 mm / min at different temperatures ranging from 23°C to 230°C.

[0188] Table 1. Compositions of Examples V1 to V6 and Comparative Examples C1 to C3, all in wt %

[0189]

[0190] Examples of sliding curves are shown in the attached Figure 1 (Example C1) and Figure 2 (Example V6). The stress (MPa) was measured as strain [%] at 50 mm / min according to the tensile test ISO 527-2:2012 of 2019. Different temperatures such as Figure 1 and Figure 2 As shown, the upper part is low temperature and the lower part is high temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0191] Figure 1 Refers to composition C1, which has a theoretical thermoforming window of 210 to 220°C.

[0192] Figure 2 Refers to composition V6, which has a theoretical thermoforming window of 120 to 220°C.

[0193] Figure 3 The dimensions of the tensile rod are shown in mm.

[0194] The following figure shows the sliding curves for other embodiments: Figure 4 - Example V1

[0195] Figure 5 - Example V2

[0196] Figure 6 - Example V3

[0197] Figure 7 - Example C2

[0198] Figure 8 - Example C3

[0199] Fig. 9 - Example V4

[0200] Fig.10 - Example V5

Claims

1. Use of a thermoplastic polymer with a melting point below 220° C. as an additive in a polybutylene terephthalate molding composition for reducing the necking of a sheet or film of the polybutylene terephthalate molding composition during elongation in a thermoforming process, wherein the thermoplastic polymer with a melting point below 220° C. is selected from polyesters based on aliphatic and aromatic dicarboxylic acids and aliphatic dihydroxy compounds.

2. The method according to claim 1, wherein the amount of the thermoplastic polymer having a melting point below 220° C. is 5 to 40% by weight, based on the total weight of the polybutylene terephthalate molding composition (100% by weight).

3. The use according to claim 1 or 2, wherein the polybutylene terephthalate molding composition comprises: a) 50 to 95% by weight of polybutylene terephthalate as component A, b) 5 to 50% by weight of a thermoplastic polymer having a melting point below 220° C. as component B, c) 0 to 45% by weight of fillers as component C, d) 0 to 20% by weight of other additives as component D, Therein the total amount of components A to D is 100% by weight and wherein component B is a polyester based on aliphatic and aromatic dicarboxylic acids and aliphatic dihydroxy compounds.

4. The method according to claim 3, wherein the polybutylene terephthalate molding composition comprises 50 to 94.9% by weight of component A and component D comprises 0.1 to 2% by weight of a copolymer containing epoxy groups and based on styrene, acrylate and / or methacrylate; bisphenol A epoxide; or a fatty acid ester containing epoxy groups or a fatty acid amide of a natural oil; or a mixture thereof, each based on 100% by weight of the total amount of components A to D.

5. The use according to claim 4, wherein component D comprises 0.1 to 2% by weight of styrene-acrylic acid-glycidyl methacrylate copolymer, based on the total amount of components A to D (100% by weight).

6. The method according to claim 3, wherein 50 to 90% by weight of component A and 5 to 30% by weight of component C are present in the molding composition.

7. The use according to claim 3, wherein the semiaromatic polyester used for component B is a polyester comprising the following important components: BA) an acid component consisting of: a1) 30 to 99 mol % of at least one aliphatic or at least one cycloaliphatic dicarboxylic acid, or its ester-forming derivatives, or mixtures thereof, a2) 1 to 70 mol % of at least one aromatic dicarboxylic acid or an ester-forming derivative thereof, or a mixture thereof, and a3) 0 to 5 mol% of a compound containing a sulfonate group, BB) a diol component selected from at least one C2-C 12 Alkanediol and at least one C5-C 10 Cycloalkane diols, or mixtures thereof, and, if necessary, one or more components selected from the following: BC) is selected from the following components: c1) at least one dihydroxy compound containing an ether function and having the formula I HO-[(CH2) n -Oh m -H (I) wherein n is 2, 3 or 4 and m is an integer from 2 to 250, c2) at least one hydroxycarboxylic acid of the formula IIa or IIb wherein p is an integer from 1 to 1500 and r is an integer from 1 to 4, and G is a group selected from the following: phenylene; -(CH2) q —, wherein q is an integer from 1 to 5; —C(R)H— and —C(R)HCH2, wherein R is methyl or ethyl, c3) at least one amino-C2-C 12 Alkanol, or at least one amino-C5-C 10 Cycloalkanol, or a mixture thereof, c4) at least one diamino-C1-C8 alkane, c5) at least one 2,2'-dioxazoline of formula III Where R 1 is a single bond, (CH2) Z - alkylene, wherein z is 2, 3 or 4, or phenylene c6) at least one aminocarboxylic acid selected from naturally occurring amino acids, polyamides obtainable by polycondensation of dicarboxylic acids having 4 to 6 carbon atoms with diamines having 4 to 10 carbon atoms, compounds of the formula IVa and IVb wherein s is an integer from 1 to 1500 and t is an integer from 1 to 4, and T is a group selected from the following: phenylene; -(CH2) u —, where u is an integer from 1 to 12; —C(R 2 )H— and—C(R 2 )HCH2—, where R 2 is methyl or ethyl, and a polyoxazoline having a repeating unit V Where R 3 is hydrogen, C1-C6-alkyl, C5-C8-cycloalkyl, phenyl which may be unsubstituted or substituted by up to 3 C1-C4-alkyl substituents, or tetrahydrofuranyl, or a mixture consisting of C1 to C6, as well as BD) is selected from the following components: d1) at least one compound having at least three groups capable of forming esters, d2) at least one isocyanate, d3) at least one divinyl ether, Or a mixture consisting of d1) to d3).

8. The use according to claim 7, wherein the semiaromatic polyester used for component B is based on the following components: BA, BB, d1 BA, BB, d2 BA, BB, d1, d2 BA, BB, d3 BA, BB, c1 BA, BB, c1, d3 BA, BB, c3, c4 BA, BB, c3, c4, c5 BA, BB, d1, c3, c5 BA, BB, c3, d3 BA, BB, c3, d1 BA, BB, c1, c3, d3 BA, BB, c2.

9. A method for preparing a molded article comprising or made of the polybutylene terephthalate molding composition as claimed in any one of claims 3 to 8, by heating a sheet or film comprising or made of the polybutylene terephthalate molding composition to a soft molding temperature, and thermoforming the heated sheet or film into a desired shape in a mold, cooling the molded molded article to solidify it and optionally trimming the molded molded article, wherein the polybutylene terephthalate molding composition does not contain a copolyetherester elastomer.

10. The process according to claim 9, wherein the sheet made from the polybutylene terephthalate molding composition is heated to a temperature of 170 to 220°C.

11. The polybutylene terephthalate molding composition as defined in any one of claims 3 to 8, wherein the amount of the thermoplastic polymer having a melting point below 220° C. is 15 to 25% by weight, based on 100% by weight of the total amount of the polybutylene terephthalate molding composition, and wherein the polybutylene terephthalate molding composition does not contain a copolyetherester elastomer.

12. The polybutylene terephthalate molding composition according to claim 11, comprising less than 15% by weight, based on the polybutylene terephthalate molding composition, of a biodegradable homopolyester or copolyester selected from the group consisting of polylactide, polycaprolactone, polyhydroxyalkanoate and polyesters composed of aliphatic dicarboxylic acids and aliphatic diols.

13. The polybutylene terephthalate molding composition according to claim 11 or 12, which contains no polymers other than the styrene-acrylic acid-glycidyl methacrylate copolymer which contain repeating units containing acrylic acid and / or styrene.

14. Thermoformed moldings of the polybutylene terephthalate molding composition according to any one of claims 11 to 13.