Composition, film, laminate and display device

By using a combination of a compound with a maximum absorption wavelength in the range of 420nm to 520nm and a polymerizable liquid crystal compound or a liquid crystalline polymer compound, the problem of reduced dichroic ratio of polarizing plates caused by UV exposure is solved and achieved Wider manufacturing process options and higher polarizing film performance.

CN114127232BActive Publication Date: 2024-10-29SUMITOMO CHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202080052261.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-22
Publication Date
2024-10-29
Estimated Expiration
2040-06-22

Smart Images

  • Figure BDA0003475495610000091
    Figure BDA0003475495610000091
  • Figure BDA0003475495610000101
    Figure BDA0003475495610000101
  • Figure BDA0003475495610000111
    Figure BDA0003475495610000111
Patent Text Reader

Abstract

The present invention is a composition comprising a compound of formula (1) and a polymerizable liquid crystal compound or a liquid crystal polymer compound. n represents 1 or 2. Ar 1 ,Ar 2 and Ar 3 represents 1,4-phenylene or a divalent sulfur-containing aromatic heterocyclic group. 1 and Ar 2 At least one of R has a fluorine atom. 1 represents a single bond or a group selected from -OC(=O)-, -C(=O)O-, -C≡C-, -CH=CH-, -CH=N-, -N=N- and -N=CH-. R 2 represents an alkylamino group or an alkoxy group. 3 represents a group selected from the group consisting of an alkanediyl group, an alkanediyloxy group, an alkanediyloxycarbonyl group and an alkanediylcarbonyloxy group. 4 represents a polymerizable group or a hydrogen atom. 4 ‑R 3 ‑Ar 1 ‑(‑R 1 ‑Ar 2 ‑) n ‑N=N‑Ar 3 ‑R 2 (1).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composition, a film, a laminate and a display device. Background Art

[0002] There is a continuous demand for thinner displays such as image display panels, and further thinning is also required for polarizing plates and polarizers, which are one of their components. In response to such a demand, for example, a thin guest-host polarizer has been proposed, which includes a polarizing film containing a polymerizable liquid crystal compound and a pigment compound showing dichroism (for example, see Patent Documents 1 and 2).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application No. 2007-510946

[0006] Patent Document 2: Japanese Patent Application Publication No. 2013-37353 Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, when ultraviolet (UV) exposure is used in the process of manufacturing a polarizing film constituting a polarizing plate, the dichroic ratio (DR) of the obtained polarizing plate may decrease.

[0009] An object of the present invention is to provide a composition capable of suppressing a decrease in the dichroic ratio of a manufactured polarizing plate.

[0010] Means for solving problems

[0011] The present invention provides the following [1] to

[10] .

[0012] [1] A composition comprising: a compound represented by the following formula (1) and having a maximum absorption wavelength in the range of 420 nm to 520 nm; and at least one compound selected from the group consisting of a polymerizable liquid crystal compound and a liquid crystal polymer compound.

[0013] R 4 -R 3 -Ar 1 -(-R 1 -Ar 2 -) n -N=N-Ar 3 -R 2 (1)

[0014] [In formula (1), n ​​represents an integer of 1 or 2.

[0015] Ar1 ,Ar 2 and Ar 3 Each independently represents a 1,4-phenylene group which may have a substituent or a divalent sulfur-containing aromatic heterocyclic group which may have a substituent, Ar 1 and Ar 2 At least one of them has a fluorine atom as a substituent. 1 It represents a single bond, or at least one group selected from the group consisting of -OC(=O)-, -C(=O)O-, -C≡C-, -CH=CH-, -CH=N-, -N=N-, and -N=CH-.

[0016] R 2 It represents an alkylamino group which may have a polymerizable group, or an alkoxy group which may have a polymerizable group.

[0017] R 3 It represents at least one group selected from the group consisting of an alkanediyl group having 4 to 20 carbon atoms, an alkanediyloxy group having 2 to 20 carbon atoms, an alkanediyloxycarbonyl group having 2 to 20 carbon atoms, and an alkanediylcarbonyloxy group having 2 to 20 carbon atoms.

[0018] R 4 represents a polymerizable group or a hydrogen atom.

[0019] When n is 2, there are 2 R 1 They can be the same or different. There are two Ar 2 They may be the same or different from each other.]

[0020] [2] The composition according to [1], wherein the polymerizable liquid crystal compound and the liquid crystalline polymer compound are a polymerizable smectic liquid crystal compound and a smectic liquid crystalline polymer compound.

[0021] [3] The composition according to [1] or [2], wherein the polymerizable liquid crystal compound is a compound represented by the following formula (A).

[0022] U 1 -V 1 -W 1 -(X 1 -Y 1 ) m -X 2 -Y 2 -X 3 -W 2 -V 2 -U 2 (A)

[0023] [In formula (A), m is an integer of 1 to 3.

[0024] X 1 , X 2 and X 3 Each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group. When m is 2 or 3, there are a plurality of X 1 They may be the same or different from each other. 1 , X 2 and X 3 At least three of the group consisting of these groups represent a divalent 6-membered hydrocarbon ring group.

[0025] Y 1 , Y 2 , W 1 and W 2 Each independently represents a single bond or a divalent linking group.

[0026] When m is 2 or 3, there are multiple Y 1 They can be the same or different from each other.

[0027] V 1 and V 2 Each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent. At least one of the -CH2- groups constituting the alkanediyl group may be replaced by -O-, -CO-, -S- or -NH-.

[0028] U 1 and U 2 Each independently represents a polymerizable group or a hydrogen atom, and at least one of them represents a polymerizable group.]

[0029] [4] The composition according to any one of [1] to [3], wherein in the formula (1), Ar 1 and Ar 2 At least one of them has 1 to 4 fluorine atoms as a substituent.

[0030] [5] The composition according to any one of [1] to [4], wherein in the formula (1), Ar 1 and Ar 2 At least one of them has 1 or 2 fluorine atoms as a substituent.

[0031] [6] The composition according to any one of [1] to [5], wherein in the formula (1), n ​​is 1.

[0032] [7] The composition according to any one of [1] to [6], wherein the polymerizable group is a radical polymerizable group.

[0033] [8] A film formed from the composition according to any one of [1] to [7] as a forming material.

[0034] [9] A laminate comprising the film described in [8].

[0035]

[10] A display device comprising the laminate according to [9].

[0036] Effects of the Invention

[0037] According to the present invention, a composition capable of suppressing a decrease in the dichroic ratio of a manufactured polarizing plate can be provided. DETAILED DESCRIPTION

[0038] In this specification, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes as long as the desired purpose of the process can be achieved. In addition, for the content of each component in the composition, when there are multiple substances belonging to each component in the composition, unless otherwise specified, it refers to the total amount of the multiple substances present in the composition. Below, the embodiments of the present invention are described in detail. It should be noted that the scope of the present invention is not limited to the embodiments described herein, and various changes can be made within the scope of not damaging the main purpose of the present invention.

[0039] <Composition>

[0040] The composition involved in this embodiment includes: a compound represented by the following formula (1) and having a maximum absorption wavelength in the range of 420 nm to 520 nm; and a polymerizable liquid crystal compound. The composition can be used as a forming material of a polarizing film, for example. That is, the composition can be a composition for forming a polarizing film. A polarizing plate having a polarizing film obtained by using the composition as a forming material can effectively suppress the reduction of the dichroic ratio of the polarizing plate from the manufacturing process.

[0041] Compound represented by formula (1)

[0042] The composition contains at least one compound represented by the following formula (1). The compound represented by the formula (1) has a maximum absorption wavelength (λ MAX ), for example, can be used as a pigment compound in the composition.

[0043] R 4 -R 3 -Ar 1 -(-R 1 -Ar 2 -) n -N=N-Ar 3 -R 2 (1)

[0044] In formula (1), n ​​represents an integer of 1 or 2, and n is preferably 1. The geometrical isomerism of the azo group in formula (1) may be either cis or trans, and is preferably trans. In addition, the number of azo groups may be 1 to 3 depending on n, and may be 1, 2, or 3.

[0045] Ar in formula (1) 1 ,Ar 2 and Ar 3 Each of the following independently represents a 1,4-phenylene group which may have a substituent or a divalent sulfur-containing aromatic heterocyclic group which may have a substituent, Ar 1 and Ar 2 At least one of them has a fluorine atom as a substituent.

[0046] As Ar 1 ,Ar 2 and Ar 3 The substituents in include alkyl groups having 1 to 10 carbon atoms, such as methyl, ethyl and butyl groups; alkoxy groups having 1 to 10 carbon atoms, such as methoxy, ethoxy and butoxy groups; fluoroalkyl groups having 1 to 10 carbon atoms, such as trifluoromethyl groups; cyano groups; nitro groups; halogen atoms, such as chlorine atoms and fluorine atoms; substituted or unsubstituted amino groups, such as amino groups, diethylamino groups and pyrrolidinyl groups. Here, the so-called substituted amino group refers to an amino group having 1 or 2 alkyl groups having 1 to 10 carbon atoms on the nitrogen atom, or an amino group in which two alkyl groups on the nitrogen atom are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. In addition, the unsubstituted amino group is -NH2. It should be noted that, as the alkyl group having 1 to 10 carbon atoms, methyl, ethyl, hexyl and the like can be mentioned. Examples of the alkane diyl group having 2 to 8 carbon atoms include ethylene, propane-1,3-diyl, butane-1,3-diyl, butane-1,4-diyl, pentane-1,5-diyl, hexane-1,6-diyl, heptane-1,7-diyl and octane-1,8-diyl.

[0047] In the compound according to this embodiment, Ar 1 and Ar 2 At least one of them has a fluorine atom as a substituent, preferably Ar 1 and Ar 2 Any one of has a fluorine atom as a substituent. 1 and Ar 2 The total number of fluorine atoms present is preferably 1 or more and 4 or less, more preferably 1 or 2, and still more preferably 1. 1 and Ar 2 Any one of the above preferably has 1 or more and 4 or less fluorine atoms, more preferably has 1 or 2 fluorine atoms, and still more preferably has 1 fluorine atom.

[0048] The compound represented by formula (1) has Ar1 and Ar 2 At least one of the compounds has a fluorine atom as a substituent, and thus can exhibit excellent ultraviolet durability. Thus, in the manufacturing process of a polarizing plate having a polarizing film formed by a composition comprising a compound represented by formula (1), even if ultraviolet exposure is used, the dichroic ratio of the manufactured polarizing plate can be suppressed from decreasing, and the restrictions on the manufacturing process can be relaxed, thereby expanding the range of options for the manufacturing process.

[0049] As Ar 1 ,Ar 2 and Ar 3 The substituents other than fluorine atoms are preferably methyl or methoxy. Thus, the compound represented by formula (1) is more easily included in a highly ordered liquid crystal structure such as a smectic liquid crystal. 1 ,Ar 2 and Ar 3 The number of substituents other than fluorine atoms is preferably 1 or 2. Thus, the compound represented by formula (1) is more easily included in a highly ordered liquid crystal structure such as a smectic liquid crystal.

[0050] When n is 1, Ar is preferably selected from the viewpoints of both the simplicity of molecular synthesis and high performance. 1 ,Ar 2 and Ar 3 At least two of them are 1,4-phenylene.

[0051] As Ar 1 ,Ar 2 and Ar 3 The divalent sulfur-containing aromatic heterocyclic group in the formula (I) may be a group formed by removing two hydrogen atoms from a sulfur-containing aromatic heterocyclic compound selected from the group consisting of thiophene, benzothiophene, dibenzothiophene, benzodithiophene, thienofuran, thienothiophene, furothiazole, thienothiazole, and benzothiazole.

[0052] When the compound according to the present embodiment includes a structure in which a divalent sulfur-containing aromatic heterocyclic group and a 1,4-phenylene group are directly bonded, the dichroic ratio of a film including the compound is improved.

[0053] R 1 R represents a single bond, or at least one linking group selected from the group consisting of -OC(=O)-, -C(=O)O-, -C≡C-, -CH=CH-, -CH=N-, -N=N-, and -N=CH-. 1 When there are multiple Rs, they may be the same or different. 1It is preferably at least one selected from the group consisting of a single bond, -OC(=O)-, -C(=O)O-, and -N=N-, and more preferably a single bond or -N=N-.

[0054] R 2 represents an alkylamino group which may have a polymerizable group, or an alkoxy group which may have a polymerizable group. 2 The polymerizable group in R is preferably a radical polymerizable group, for example, a (meth)acrylate group ((meth)acryloyloxy group), a styryl group (vinylphenyl group) and the like. Among them, a (meth)acrylate group is preferred. 2 When the polymerizable group is present, the number of the polymerizable group is, for example, 1 or 2, and preferably 1.

[0055] As R 2 The alkylamino group in the above-mentioned group includes, for example, an amino group having one or two alkyl groups having 1 to 10 carbon atoms on the nitrogen atom, or a cyclic amino group in which two alkyl groups on the nitrogen atom are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. 2 Specific examples of the alkylamino group in R include methylamino, ethylamino, dimethylamino, diethylamino, dipropylamino, methylethylamino, methylhexylamino, pyrrolidinyl, piperidinyl, and morpholinyl. 2 The alkylamino group in is preferably at least one selected from the group consisting of a dimethylamino group, a diethylamino group, a diisopropylamino group, a methylethylamino group, and a methylhexylamino group.

[0056] As R 2 The alkoxy group in the formula (R) may be, for example, an alkoxy group having 1 to 10 carbon atoms. 2 Specific examples of the alkoxy group in R include methoxy, ethoxy, propyloxy, butyloxy, pentyloxy, hexyloxy, cyclopentyloxy, and cyclohexyloxy. 2 The alkoxy group in is preferably at least one selected from the group consisting of an ethoxy group and a propyloxy group.

[0057] R in formula (1) 3 It represents at least one divalent group selected from the group consisting of an alkanediyl group having 4 to 20 carbon atoms, an alkanediyloxy group having 2 to 20 carbon atoms, an alkanediyloxycarbonyl group having 2 to 20 carbon atoms, and an alkanediylcarbonyloxy group having 2 to 20 carbon atoms.

[0058] Examples of the alkanediyl group having 4 to 20 carbon atoms include alkanediyl groups formed by removing one hydrogen atom from an unsubstituted (unsubstituted) linear or branched alkyl group having 4 to 20 carbon atoms, such as n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl. The alkanediyl group preferably has 4 to 16 carbon atoms, and more preferably 4 to 12 carbon atoms.

[0059] One or more hydrogen atoms constituting the aforementioned alkyl group having 4 to 20 carbon atoms may be substituted by a halogen atom (e.g., a fluorine atom), a hydroxyl group, an amino group, or a substituted amino group. Here, as the substituted amino group, for example, there may be mentioned an amino group substituted by one or two alkyl groups having 1 to 20 carbon atoms, such as N-methylamino, N-ethylamino, N,N-dimethylamino, N,N-diethylamino, etc. As the alkyl group having one or more hydrogen atoms substituted by a halogen atom, a hydroxyl group, an amino group, etc., there may be mentioned a halogenated alkyl group having 4 to 20 carbon atoms, such as a fluorobutyl group, an octafluorobutyl group, etc.; a hydroxyalkyl group having 4 to 20 carbon atoms, such as a hydroxybutyl group, a hydroxypentyl group, a hydroxyhexyl group, etc.; an alkyl group having 4 to 20 carbon atoms and having an unsubstituted or substituted amino group, such as an aminobutyl group, a 2-(N,N-dimethylamino)butyl group, etc.

[0060] -O- or -NR- may be inserted between the carbon atoms constituting the above alkyl group. * -. Here, R * represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms, and examples of the alkyl group having 1 to 6 carbon atoms include methyl, ethyl, butyl, hexyl, and the like. * -alkyl group includes 2-ethoxyethyl, 2-(2-ethoxyethoxy)ethyl, 2-[2-(ethylamino)ethyl)amino]ethyl and the like.

[0061] Examples of the alkanediyloxy group having 2 to 20 carbon atoms include alkanediyloxy groups formed by removing one hydrogen atom from an unsubstituted linear or branched alkoxy group having 2 to 20 carbon atoms, such as ethoxy, n-propoxy, isopropyloxy, n-butoxy, isobutyloxy, tert-butoxy, n-pentyloxy, isopentyloxy, neopentyloxy, n-hexyloxy, n-heptyloxy, n-octyloxy, n-nonyloxy, and n-decyloxy. The alkanediyloxy group preferably has 2 to 16 carbon atoms, and more preferably has 2 to 12 carbon atoms.

[0062] One or more hydrogen atoms constituting the alkoxy group having 2 to 20 carbon atoms may be substituted by a halogen atom (e.g., a fluorine atom), a hydroxyl group, an amino group, or an amino group having a substituent. The amino group having a substituent is the same as above. As alkoxy groups in which one or more hydrogen atoms are substituted by a halogen atom, a hydroxyl group, an amino group, etc., there can be mentioned halogenated alkoxy groups having 2 to 20 carbon atoms such as tetrafluoroethoxy and octafluorobutoxy; hydroxyalkoxy groups having 2 to 20 carbon atoms such as 2-hydroxyethoxy; alkoxy groups having 2 to 20 carbon atoms containing an unsubstituted or substituted amino group such as aminoethoxy and 2-(N,N-dimethylamino)ethoxy.

[0063] -O- or -NR- may be inserted between the carbon atoms constituting the alkoxy group. * -. -O- or -NR is inserted between carbon atoms * -alkoxy group, for example, methoxymethoxy, 2-ethoxyethoxy, 2-(2-ethoxyethoxy) group, etc. * As described.

[0064] Examples of the alkanediyloxycarbonyl group having 2 to 20 carbon atoms include alkanediyloxycarbonyl groups obtained by removing one hydrogen atom from an unsubstituted alkoxycarbonyl group having 2 to 20 carbon atoms, such as methoxycarbonyl, ethoxycarbonyl, n-propoxycarbonyl, isopropoxycarbonyl, n-butoxycarbonyl, isobutoxycarbonyl, tert-butoxycarbonyl, n-pentyloxycarbonyl, isopentyloxycarbonyl, neopentyloxycarbonyl, n-hexyloxycarbonyl, n-heptyloxycarbonyl, n-octyloxycarbonyl, n-nonyloxycarbonyl and n-decyloxycarbonyl. The alkanediyl moiety of the alkanediyloxycarbonyl group preferably has 1 to 16 carbon atoms, more preferably 1 to 12 carbon atoms.

[0065] One or more hydrogen atoms constituting the alkoxycarbonyl group having 2 to 20 carbon atoms may be substituted by a halogen atom (e.g., a fluorine atom), a hydroxyl, an amino group, or an amino group having a substituent. The amino group having a substituent is the same as above. As the alkoxycarbonyl group having one or more hydrogen atoms replaced by a halogen atom, a hydroxyl, an amino group, etc., halogenated alkoxycarbonyl groups having 2 to 20 carbon atoms such as fluoroethoxycarbonyl, trifluoroethoxycarbonyl, tetrafluoroethoxycarbonyl, octafluorobutoxycarbonyl, etc. may be enumerated.

[0066] Examples of the alkanediylcarbonyloxy group having 2 to 20 carbon atoms include alkanediylcarbonyloxy groups formed by removing one hydrogen atom from an unsubstituted alkanoyloxy group having 2 to 20 carbon atoms, such as acetyloxy, ethylcarbonyloxy, n-propylcarbonyloxy, isopropylcarbonyloxy, n-butylcarbonyloxy, isobutylcarbonyloxy, tert-butylcarbonyloxy, n-pentylcarbonyloxy, isopentylcarbonyloxy, neopentylcarbonyloxy, n-hexylcarbonyloxy, n-heptylcarbonyloxy, n-octylcarbonyloxy, n-nonylcarbonyloxy and n-decylcarbonyloxy. The alkanediyl moiety of the alkanediylcarbonyloxy group preferably has 1 to 16 carbon atoms, more preferably 1 to 12 carbon atoms.

[0067] One or more hydrogen atoms constituting the alkanoyloxy group having 2 to 20 carbon atoms may be substituted with a halogen atom (e.g., a fluorine atom), a hydroxyl group, an amino group, or an amino group having a substituent. The amino group having a substituent is the same as described above. Examples of the alkanoyloxy group in which one or more hydrogen atoms are substituted with a halogen atom, a hydroxyl group, or the like include halogenated acyloxy groups having 2 to 20 carbon atoms, such as a tetrafluoroethylcarbonyloxy group and an octafluorobutylcarbonyloxy group.

[0068] R in formula (1) 4 represents a polymerizable group or a hydrogen atom. 4 The polymerizable group in is preferably a radical polymerizable group, and examples thereof include a (meth)acrylate group and a styryl group. Among them, a (meth)acrylate group is preferred.

[0069] Specific examples of the compound represented by formula (1) include compounds represented by the following formulae (2-2) to (2-192), but the present invention is not limited thereto.

[0070] [Chemical formula 1]

[0071]

[0072] [Chemical formula 2]

[0073]

[0074] [Chemical formula 3]

[0075]

[0076] [Chemical formula 4]

[0077]

[0078] [Chemical formula 5]

[0079]

[0080] [Chemical formula 6]

[0081]

[0082] [Chemical formula 7]

[0083]

[0084] [Chemical formula 8]

[0085]

[0086] [Chemical formula 9]

[0087]

[0088] [Chemical formula 10]

[0089]

[0090] [Chemical formula 11]

[0091]

[0092] [Chemical formula 12]

[0093]

[0094] [Chemical formula 13]

[0095]

[0096] [Chemical formula 14]

[0097]

[0098] [Chemical formula 15]

[0099]

[0100] [Chemical formula 16]

[0101]

[0102] [Chemical formula 17]

[0103]

[0104] [Chemical formula 18]

[0105]

[0106] [Chemical formula 19]

[0107]

[0108] [Chemical formula 20]

[0109]

[0110] [Chemical formula 21]

[0111]

[0112] [Chemical formula 22]

[0113]

[0114] [Chemical formula 23]

[0115]

[0116] [Chemical formula 24]

[0117]

[0118] [Chemical formula 25]

[0119]

[0120] [Chemical formula 26]

[0121]

[0122] [Chemical formula 27]

[0123]

[0124] [Chemical formula 28]

[0125]

[0126] [Chemical formula 29]

[0127]

[0128] [Chemical formula 30]

[0129]

[0130] [Chemical formula 31]

[0131]

[0132] [Chemical formula 32]

[0133]

[0134] [Chemical formula 33]

[0135]

[0136] [Chemical formula 34]

[0137]

[0138] [Chemical formula 35]

[0139]

[0140] [Chemical formula 36]

[0141]

[0142] The compound represented by formula (1) (hereinafter also referred to as compound (1)) is preferably at least one selected from the group consisting of compounds represented by any one of (2-2) to (2-7), (2-9) to (2-30), (2-34) to (2-106), and (2-111) to (2-192) among formulas (2-2) to (2-192), and more preferably at least one selected from the group consisting of compounds represented by formulas (2-3) to (2-7), (2-9) to (2-30), (2-34) to (2-106), and (2-111) to (2-192). At least one selected from the group consisting of compounds represented by any one of formulas (2-4) to (2-7), (2-9) to (2-30), (2-39) to (2-47), (2-49) to (2-83), (2-85) to (2-101), (2-104), and (2-111) to (2-192), particularly preferably selected from the group consisting of compounds represented by any one of formulas (2-4) to (2-7), (2-9) to (2-30), (2-39) to (2-47), (2-49) to (2-83), (2-85) to (2-101), (2-104), and (2-111) to (2-192) At least one of the above, more preferably selected from any one of (2-4) to (2-7), (2-9) to (2-30), (2-39) to (2-47), (2-49) to (2-83), (2-85) to (2-101), (2-104), (2-111) to (2-130), (2-132), (2-135), (2-146) to (2-155), and (2-165) to (2-192) At least one of the group of compounds is more preferably at least one of the group of compounds represented by any one of the formulae (2-4) to (2-7), (2-9) to (2-30), (2-39) to (2-47), (2-59), (2-67), (2-111) to (2-113), (2-116) to (2-127), (2-146) to (2-153), and (2-165) to (2-192).

[0143] The content of the compound represented by formula (1) in the composition is preferably less than 50 parts by mass relative to 100 parts by mass of the solid content of the composition, more preferably in the range of more than 0.1 parts by mass and less than 10 parts by mass, and further preferably in the range of more than 0.1 parts by mass and less than 5 parts by mass. If within the above range, the dispersion of the compound represented by formula (1) can be fully carried out. Thus, a film in which the generation of defects is fully suppressed and the compound represented by formula (1) is used as a forming material can be efficiently obtained. It should be noted that in this specification, the so-called solid content refers to the total amount of the components after removing volatile components such as solvents from the composition.

[0144] Method for producing compound (1)

[0145] A method for producing a compound represented by formula (1) [hereinafter also referred to as compound (1)] is described. Compound (1) can be produced, for example, from a compound represented by formula (1X) [hereinafter also referred to as compound (1X)] and a compound represented by formula (1Y) [hereinafter also referred to as compound (1Y)] by the steps shown in the following reaction formula.

[0146] [Chemical formula 37]

[0147]

[0148] In the above reaction formula, Ar 1 ,Ar 2 ,Ar 3 , R 1 , R 2 , R 3 , R 4 and n have the same meanings as those in formula (1). 1 and Re 2 To react with each other to form R 1 Re represents a group or a combination of groups having a single bond. 1 and Re 2 The combination of, for example, the following combinations can be mentioned. 1 In the case of a single bond, examples thereof include a combination of a dihydroxyboryl group or a dialkoxyboryl group and a halogen atom. 1 In the case of -C(=O)O- or -OC(=O)-, examples thereof include a combination of a carboxyl group and a hydroxyl group, a combination of a carbonyl halide group and a hydroxyl group, and a combination of a carbonyloxyalkyl group and a hydroxyl group. 1 In the case of -C≡C-, examples thereof include a combination of a halogen atom and an ethynyl group (-C≡CH). 1 In the case of -CH=CH-, examples thereof include a combination of a halogen atom and a vinyl group (-CH=CH2). 1In the case of -CH=N- or -N=CH-, examples thereof include a combination of a formyl group and an amino group.

[0149] In the above reaction formula, the 4 -R 3 -compound (1X) and having R 2 - has been described, but it is also possible to make the compound (1Y) 4 -R 3 - a compound protected with an appropriate protecting group, and R 2 - Compounds protected with appropriate protecting groups are reacted with each other, followed by appropriate deprotection reaction, thereby producing compound (1).

[0150] Regarding the reaction conditions when reacting Compound (1X) and Compound (1Y), the most appropriate known conditions can be appropriately selected according to the types of Compound (1X) and Compound (1Y) used.

[0151] For example, in R 1 is a single bond, and Re 1 is a dihydroxyboryl or dialkoxyboryl group, Re 2 In the case of a halogen atom, the reaction conditions of Suzuki coupling can be used with reference to, for example, Netherton, MR; Fu, GC Org. Lett. 2001, 3 (26), 4295-4298. A mixed solvent of diethylene glycol dimethyl ether and water can be used as a solvent, and a Pd catalyst such as PdCl2dppf can be added in the presence of potassium acetate and heated to obtain compound (1). The reaction temperature can be selected according to the types of compound (1X) and compound (1Y), and for example, the range from room temperature to 160°C can be cited, and the range from 60°C to 150°C is preferably cited. As for the reaction time, for example, the range from 15 minutes to 48 hours can be cited. It should be noted that at Re 1 is a halogen atom, Re 2 The same method can be applied to the case of a dihydroxyboryl group or a dialkoxyboryl group.

[0152] It should be noted that Re 1 The compound (1X) in which Ar is dihydroxyboryl or dialkoxyboryl can be obtained, for example, by reacting Ar with n-butyl lithium or the like. 1 After the bromine group in the reaction is lithiated, a trialkoxyborane is reacted to introduce a dihydroxyboryl group or a dialkoxyboryl group. 2 The compound (1Y) in which Ar is dihydroxyboryl or dialkoxyboryl can be obtained, for example, by reacting Ar with n-butyl lithium or the like. 2After the bromine group in the reaction mixture is lithiated, a trialkoxyborane is allowed to act thereon to introduce a dihydroxyboryl group or a dialkoxyboryl group.

[0153] The azo structure in compound (1Y) can be constructed, for example, by referring to the description of the production examples in paragraphs

[0220] to

[0268] of International Publication No. WO2016 / 136561, converting an aromatic amine compound having a primary amino group into a diazonium salt using sodium nitrite or the like, and subjecting it to diazo coupling with an aromatic compound.

[0154] For example, as R 1 is -C(=O)O-, and Re 1 For carboxyl, Re 2 The reaction conditions in the case of a hydroxyl group can refer to Jiang, L.; Lu, X.; Zhang, H.; Jiang, Y.; Ma, D. J. Org. Chem. 2009, 74 (3), 4542-4546., etc., and a dehydration condensation reaction can be used. For example, conditions for condensation in a solvent in the presence of an esterification condensation agent can be mentioned. As the solvent, a solvent such as chloroform in which both compound (1X) and compound (1Y) are soluble can be mentioned. As the esterification condensation agent, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC·HCl), diisopropylcarbodiimide (IPC), etc. can be mentioned. Here, it is more preferred to use a base such as N,N-dimethylaminopyridine (DMAP) in combination. The reaction temperature can be selected according to the types of compound (1X) and compound (1Y), and for example, the range of -15°C to 70°C can be mentioned, and the range of 0°C to 40°C is preferably mentioned. The reaction time may be, for example, in the range of 15 minutes to 48 hours. 1 is -OC(=O)-, and Re 1 Hydroxyl, Re 2 The same can be applied to the case of a carboxyl group.

[0155] For example, in R 1 For -C≡C-, and Re 1 For ethynyl (-C≡CH), Re 2 When Re is a halogen group, the compound (1) can be synthesized by using Sonogashira coupling using a Pd or Cu catalyst. 1 is a halogen atom, Re 2 The same method can be applied to the case of an ethynyl group (—C≡CH).

[0156] For example, in R 1 is -C=C-, and Re 1Vinyl (-CH=CH2), Re 2 When Re is a halogen atom, the compound (1) can be synthesized by applying the Heck reaction using a Pd catalyst and a phosphorus ligand. 1 is a halogen atom, Re 2 The same can be applied to the case of a vinyl group (-CH=CH2).

[0157] For example, in R 1 is -CH=N-, and Re 1 is formyl, Re 2 When R is an amino group, the compound (1) can be synthesized by applying a conventional dehydration condensation reaction. 1 is -N=CH-, and Re 1 Amino group, Re 2 The same can be applied to the case of a formyl group.

[0158] In the obtained compound (1), R 3 In the case of an alkanediyloxycarbonyl group having 2 to 20 carbon atoms, R 3 Change to other alkanediyloxycarbonyl groups with 2 to 20 carbon atoms. In the transesterification reaction, for example, the following method can be applied: refer to Chen, C.-T.; Kuo, J.-H.; Ku, C.-H.; Weng, S.-S.; Liu, C.-YJ Org. Chem. 2005, 70 (4), 1328-1339., etc., use TiO (acac) 2 (name: bis (2,4-pentanedione) titanium (IV) oxide) as a Lewis acid catalyst, and heat it together with an alcohol compound in a solvent. As a solvent, a hydrocarbon aromatic compound such as xylene and toluene can be used. It should be noted that other alkanediyloxycarbonyl groups with 2 to 20 carbon atoms include groups with different alkanediyl moieties, and the number of carbon atoms and substituents may be different.

[0159] The reaction time in the method for producing compound (1) can also be determined by appropriately sampling the reaction mixture during the reaction and confirming the extent of disappearance of compound (1X) and compound (1Y), the extent of generation of compound (1), etc. using known analytical means such as liquid chromatography and gas chromatography.

[0160] The compound (1) can be isolated from the reaction mixture after the reaction by known methods such as recrystallization, reprecipitation, extraction and various chromatography, or by a suitable combination of these operations.

[0161] The composition may further include other pigment compounds other than the compound represented by formula (1), such as at least one of dichroic pigments. As other pigment compounds, for example, azo pigments such as monoazo pigments, disazo pigments, triazo pigments, tetrazo pigments, stilbene azo pigments can be cited, preferably at least one selected from the group consisting of them. The composition may contain one other pigment compound alone, or may contain two or more in combination. For example, in the case of being used as a coating type polarizing plate material, the other pigment compounds contained in the composition preferably have a maximum absorption wavelength in a wavelength range different from the compound represented by formula (1). For example, in the case of being used as a coating type polarizing plate material, the composition preferably includes a compound represented by formula (1) and a combination of more than three dichroic pigments, more preferably a combination of more than three azo pigments. By making the composition combination contain more than three pigment compounds with different maximum absorption wavelengths, for example, it is possible to obtain absorption in the entire visible light domain using a film formed by the composition.

[0162] When composition comprises other pigment compounds, its content is preferably below 50 mass parts, more preferably the scope below 10 mass parts above 0.1 mass parts, further preferably the scope below 5 mass parts above 0.1 mass parts relative to 100 mass parts of the solid component of composition.If within the above-mentioned range, the dispersion of other pigment compounds can be fully carried out.

[0163] The composition includes at least one of a polymerizable liquid crystal compound and a liquid crystal polymer compound in addition to the compound represented by formula (1). The composition may include both a polymerizable liquid crystal compound and a liquid crystal polymer compound, and the polymerizable liquid crystal compound and the liquid crystal polymer compound included in the composition may each be two or more. By making the composition include at least one of a polymerizable liquid crystal compound and a liquid crystal polymer compound, a composition in which compound (1) is dispersed in a polymerizable liquid crystal compound and a liquid crystal polymer compound can be formed.

[0164] The liquid crystalline polymer compound may be a polymer compound constituting a thermotropic liquid crystalline polymer or a polymer compound constituting a lyotropic liquid crystalline polymer. From the viewpoint of enabling precise film thickness control, the liquid crystalline polymer compound is preferably a polymer compound constituting a thermotropic liquid crystalline polymer.

[0165] As a classification of liquid crystal, according to the structure of molecular arrangement in the liquid crystal state, it can be divided into smectic liquid crystal, nematic liquid crystal, and cholesteric liquid crystal. Among them, in the use of polarizing film, smectic liquid crystal is preferably used. Therefore, the polymerizable liquid crystal compound is preferably a polymerizable smectic liquid crystal compound, and the liquid crystal polymer compound is preferably a smectic liquid crystal polymer compound.

[0166] By using a polymerizable liquid crystal compound showing smectic liquid crystal properties and a polymer compound showing smectic liquid crystal properties, a polarizing film with a high degree of orientation order can be formed. The liquid crystal state displayed by the polymerizable liquid crystal compound and the liquid crystal polymer compound is preferably a smectic phase (smectic liquid crystal state), and from the viewpoint of being able to achieve a higher degree of orientation order, a higher order smectic phase (higher order smectic liquid crystal state) is more preferably used. Here, the so-called higher order smectic phase refers to smectic B phase, smectic D phase, smectic E phase, smectic F phase, smectic G phase, smectic H phase, smectic I phase, smectic J phase, smectic K phase and smectic L phase, among which smectic B phase, smectic F phase and smectic I phase are more preferably used. A polarizing film with a high degree of orientation order can obtain Bragg peaks derived from higher-order structures such as hexagonal phases and crystalline phases in X-ray diffraction measurements. The so-called Bragg peak refers to the peak of the planar periodic structure derived from molecular orientation.

[0167] The periodic interval (ordered period) of the polarizing film obtained from the composition is preferably 0.3 nm or more and 0.6 nm or less. The polymerizable liquid crystal compound or liquid crystalline polymer compound may be a polymerizable smectic liquid crystal compound or a smectic liquid crystalline polymer compound showing a Bragg peak derived from a higher order structure in an X-ray diffraction measurement.

[0168] The compound represented by formula (1) can show high dichroism even when dispersed in a state of close molecular chains formed by at least one of a polymerizable liquid crystal compound exhibiting smectic liquid crystal properties and a polymer compound of smectic liquid crystal properties. Therefore, a composition comprising a compound represented by formula (1) and at least one of a polymerizable liquid crystal compound and a liquid crystal polymer compound (particularly a polymerizable liquid crystal compound exhibiting a smectic liquid crystal phase and at least one of a smectic liquid crystal polymer compound) can provide a polarizing film with a high dichroic ratio.

[0169] <Polymerizable liquid crystal compound>

[0170] The polymerizable liquid crystal compound is a compound having at least one polymerizable group in the molecule and capable of exhibiting a liquid crystal phase by orientation. The polymerizable liquid crystal compound is preferably a compound capable of exhibiting a liquid crystal phase by orientation alone.

[0171] The so-called polymerizable group refers to a group that participates in the polymerization reaction, preferably a photopolymerizable group. Here, the so-called polymerizable group refers to a group that can participate in the polymerization reaction using active free radicals, acids, etc. generated by the polymerization initiator described later. As the polymerizable group, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxacyclopropyl, and oxetanyl can be cited. Among them, the polymerizable group is preferably selected from at least one of the group consisting of acryloyloxy, methacryloyloxy, vinyloxy, oxacyclopropyl, and oxetanyl, and more preferably acryloyloxy.

[0172] As a polymerizable liquid crystal compound, as long as it is a liquid crystal compound having at least one polymerizable group and preferably showing smectic liquid crystal properties, it is not particularly limited, and known polymerizable liquid crystal compounds can be used. As a polymerizable liquid crystal compound, specifically, for example, a compound represented by the following formula (A) (hereinafter, also referred to as "polymerizable liquid crystal compound (A)") can be preferably cited.

[0173] U 1 -V 1 -W 1 -(X 1 -Y 1 ) m -X 2 -Y 2 -X 3 -W 2 -V 2 -U 2 (A)

[0174] In formula (A), m is an integer from 1 to 3. 1 , X 2 and X 3 Each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group. When m is 2 or 3, X 1 They may be the same or different from each other. 1 , X 2 and X 3 At least three of the group consisting of Y represent a divalent 6-membered hydrocarbon ring group. 1 , Y 2 , W 1 and W 2 Each independently represents a single bond or a divalent linking group. When m is 2 or 3, Y 1 They may be the same or different from each other. 1 and V 2Each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent. At least one of the -CH2- groups constituting the alkanediyl group may be replaced by -O-, -CO-, -S- or -NH-. 1 and U 2 Each independently represents a polymerizable group or a hydrogen atom, and at least one of them represents a polymerizable group.

[0175] As X 1 , X 2 and X 3 Examples of the divalent aromatic group in X include 1,4-phenylene and 1,4-naphthylene. Examples of the divalent alicyclic hydrocarbon group include cyclohexane-1,4-diyl and the like. 1 , X 2 and X 3 At least one of the divalent aromatic group and the divalent alicyclic hydrocarbon group may have a substituent. As the substituent, alkyl groups having 1 to 4 carbon atoms such as methyl, ethyl, and n-butyl, cyano, and halogen atoms may be mentioned. At least one of -CH2- constituting the divalent alicyclic hydrocarbon group may be replaced by -O-, -S-, or -NR-. Here, R represents an alkyl group having 1 to 6 carbon atoms or a phenyl group.

[0176] Choose Free X 1 , X 2 and X 3 At least three of the group consisting of these groups are divalent 6-membered cyclic hydrocarbon groups. Examples of the divalent 6-membered cyclic hydrocarbon group include 1,4-phenylene which may have a substituent, and cyclohexane-1,4-diyl which may have a substituent.

[0177] X 1 , X 2 and X 3 The divalent aromatic group in is preferably an optionally substituted 1,4-phenylene group, and more preferably an unsubstituted 1,4-phenylene group.

[0178] The divalent alicyclic hydrocarbon group is preferably a cyclohexane-1,4-diyl group which may have a substituent, more preferably a trans-cyclohexane-1,4-diyl group which may have a substituent, and still more preferably an unsubstituted trans-cyclohexane-1,4-diyl group.

[0179] Y 1 and Y 2 Each independently represents a single bond or a divalent linking group. For example, a divalent linking group is selected from -CH2CH2-, -CH2O-, -(C=O)O-, -O(C=O)O-, -N=N-, -CR a =CR b -, -C≡C- and -CR a = At least one of the group consisting of N-. Here, Ra and R b Each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 Preferably, Y is -CH2CH2-, -(C=O)O- or a single bond. 2 Preferred is -CH2CH2- or -CH2O-.

[0180] W 1 and W 2 Each independently represents a single bond or a divalent linking group. For example, the divalent linking group is at least one selected from the group consisting of -O-, -S-, -(C=O)O-, and -O(C=O)O-. 1 and W 2 Each independently is preferably a single bond or -O-.

[0181] V 1 and V 2 Each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent. At least one of the -CH2- groups constituting the alkanediyl group may be replaced by -O-, -CO-, -S- or -NH-.

[0182] As V 1 and V 2 Examples of the alkane diyl represented by V include methylene, ethylene, propane-1,3-diyl, butane-1,3-diyl, butane-1,4-diyl, pentane-1,5-diyl, hexane-1,6-diyl, heptane-1,7-diyl, octane-1,8-diyl, decane-1,10-diyl, tetradecane-1,1-diyl, and eicosane-1,20-diyl. 1 and V 2 The alkanediyl group is preferably an alkanediyl group having 2 to 12 carbon atoms, and the alkanediyl group is more preferably an alkanediyl group having 6 to 12 carbon atoms.

[0183] Examples of the substituent that the optionally substituted alkanediyl group having 1 to 20 carbon atoms may have include a cyano group and a halogen atom. The alkanediyl group is preferably an alkanediyl group having no substituent, and more preferably an alkanediyl group having no substituent and being linear.

[0184] U 1 and U 2 Each independently represents a polymerizable group or a hydrogen atom, and at least one of them represents a polymerizable group. 1 and U 2 Preferably, it is a polymerizable group. Preferably, U 1 and U 2 All are polymerizable groups, preferably all are free radical polymerizable groups. 1 The polymerizable group represented by U 2The polymerizable groups represented by may be different from each other, but are preferably groups of the same type. 1 and U 2 The polymerizable groups in U can be the same as those exemplified above as the polymerizable groups possessed by the polymerizable liquid crystal compound. 1 and U 2 The polymerizable group represented by is preferably at least one selected from the group consisting of a vinyloxy group, an acryloyloxy group, a methacryloyloxy group, an oxirane group, and an oxetanyl group, and more preferably an acryloyloxy group.

[0185] Specific examples of the polymerizable liquid crystal compound (A) include compounds represented by the following formulae (A-1) to (A-25). When the polymerizable liquid crystal compound (A) has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans-type.

[0186] [Chemical formula 38]

[0187]

[0188] [Chemical formula 39]

[0189]

[0190] [Chemical formula 40]

[0191]

[0192] [Chemical formula 41]

[0193]

[0194] [Chemical formula 42]

[0195]

[0196] Among them, the polymerizable liquid crystal compound (A) is preferably at least one selected from the group consisting of compounds represented by any one of formula (A-2), formula (A-3), formula (A-4), formula (A-5), formula (A-6), formula (A-7), formula (A-8), formula (A-13), formula (A-14), formula (A-15), formula (A-16) and formula (A-17). The polymerizable liquid crystal compound (A) can be used alone or in combination of two or more.

[0197] The polymerizable liquid crystal compound (A) can be produced by the method described in known documents such as Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996) and Japanese Patent No. 4719156.

[0198] <Liquid crystal polymer compounds>

[0199] The so-called liquid crystalline polymer compound may be a compound obtained by polymerizing the aforementioned polymerizable liquid crystal compound (hereinafter also referred to as a polymer of the polymerizable liquid crystal compound), or may be other liquid crystalline polymer compounds, but is preferably a compound obtained by polymerizing the aforementioned polymerizable liquid crystal compound.

[0200] The polymer of the polymerizable liquid crystal compound may contain two or more of the polymerizable liquid crystal compounds as raw material monomers. In addition, the polymer of the polymerizable liquid crystal compound may contain other monomers other than the polymerizable liquid crystal compound as raw material monomers.

[0201] The content ratio of the aforementioned polymerizable liquid crystal compound in the polymer of the aforementioned polymerizable liquid crystal compound is generally from 1 mol % to 100 mol % relative to the total amount of structural units derived from the aforementioned polymerizable liquid crystal compound constituting the polymer of the aforementioned polymerizable liquid crystal compound. From the viewpoint of improving the orientation of the polymer of the aforementioned polymerizable liquid crystal compound, it is preferably from 30 mol % to 100 mol %, more preferably from 50 mol % to 100 mol %, and further preferably from 80 mol % to 100 mol %.

[0202] As the aforementioned other liquid crystal polymer compounds, polymer compounds having liquid crystal groups can be cited. For example, as polymer compounds forming the mother skeleton, polyolefins such as polyethylene and polypropylene; cyclic olefin resins such as norbornene polymers; polyalkylene ethers, polyvinyl alcohols; polymethacrylates; polyacrylates; etc., these polymer compounds have liquid crystal groups. Among them, polymethacrylates and polyacrylates having liquid crystal groups are preferred.

[0203] The aforementioned other liquid crystal polymer compounds may include more than two liquid crystal groups. The liquid crystal group may be included in the main chain of the polymer compound forming the mother skeleton, may be included in the side chain of the polymer compound forming the mother skeleton, or may be included in both the main chain and the side chain of the polymer compound forming the mother skeleton. As the liquid crystal group, a group formed by removing one hydrogen atom from a compound having at least two 6-membered cyclic hydrocarbon structures or a group formed by removing two hydrogen atoms from the compound may be cited.

[0204] The content ratio of the liquid crystal groups in the aforementioned other liquid crystal polymer compounds is generally from 1 mol % to 100 mol % relative to the total amount of the structural units of the polymer compounds constituting the mother skeleton of the aforementioned other liquid crystal polymer compounds. From the viewpoint of improving the orientation of the aforementioned other liquid crystal polymer compounds, it is preferably from 30 mol % to 100 mol %, more preferably from 50 mol % to 100 mol %, and further preferably from 80 mol % to 100 mol %.

[0205] In the case of combining more than two polymerizable liquid crystal compounds in the composition, it is preferred that at least one of them is a polymerizable liquid crystal compound (A), and more preferably more than two of them are polymerizable liquid crystal compounds (A). By combining more than two polymerizable liquid crystal compounds, the liquid crystal phase can sometimes be temporarily maintained even at a temperature below the liquid crystal-crystallization phase transition temperature. Relative to the total mass of all polymerizable liquid crystal compounds in the composition, the content of the polymerizable liquid crystal compound (A) contained in the composition is preferably more than 40% by mass, more preferably more than 60% by mass, and all polymerizable liquid crystal compounds can also be polymerizable liquid crystal compounds (A). If the content of the polymerizable liquid crystal compound (A) is within the above range, the polymerizable liquid crystal compound is easily arranged with a high degree of orientation order, and the compound represented by formula (1) is oriented along it, thereby being able to obtain a polarizing film with excellent polarization performance.

[0206] From the viewpoint of improving the orientation of polymerizable liquid crystal compounds and liquid crystalline polymer compounds, the total content ratio of polymerizable liquid crystal compounds and liquid crystalline polymer compounds in the composition relative to 100 parts by mass of the solid content of the composition is, for example, 50 parts by mass or more, preferably 70 parts by mass or more and 99.9 parts by mass or less, more preferably 70 parts by mass or more and 99.5 parts by mass or less, further preferably 80 parts by mass or more and 99 parts by mass or less, particularly preferably 80 parts by mass or more and 94 parts by mass or less, and further preferably 80 parts by mass or more and 90 parts by mass or less.

[0207] Relative to the total amount of 100 parts by mass of the polymerizable liquid crystal compound and the liquid crystal polymer compound, the content of the compound (1) in the composition is usually 0.1 parts by mass or more and 50 parts by mass or less, preferably 0.1 parts by mass or more and 20 parts by mass or less, more preferably 0.1 parts by mass or more and 10 parts by mass or less, and further preferably 0.1 parts by mass or more and 5 parts by mass or less. If the content of the compound (1) relative to the total amount of the polymerizable liquid crystal compound and the liquid crystal polymer compound is 50 parts by mass or less, the orientation disorder of the polymerizable liquid crystal compound, the liquid crystal polymer compound and the compound (1) is small, and there is a tendency to obtain a polarizing film with a high degree of orientation order.

[0208] By making the composition contain compound (1) and at least one of a polymerizable liquid crystal compound and a liquid crystal polymer compound, the dichroic ratio of the composition is not easily reduced even if UV exposure is used in the middle process of manufacturing a guest-host polarizing plate using the composition. Therefore, photocuring can be used in the processing technology, which can reduce the restrictions on the process.

[0209] <Polymer compounds>

[0210] The composition may include a polymer compound in addition to compound (1), a polymerizable liquid crystal compound and a liquid crystal polymer compound. By making the composition include a polymer compound, compound (1) is sometimes easily dispersed in the composition. There is no particular limitation on the polymer compound that can be included in the composition as long as it can disperse compound (1). From the perspective of making it easy to evenly disperse compound (1), acrylic polymers such as polymethyl methacrylate (PMMA) are preferred. In addition, the polymer compound may also be a polymer compound obtained by polymerizing the polymerizable liquid crystal compound described above. The weight average molecular weight of the polymer compound converted to polystyrene is, for example, more than 10,000 and less than 200,000, preferably more than 20,000 and less than 150,000.

[0211] When the composition contains a polymer compound, its content can be appropriately selected according to the purpose, etc. The content of the polymer compound is preferably 10 parts by mass or less, more preferably 5.0 parts by mass or less, and further preferably 3.0 parts by mass or less relative to 100 parts by mass of the solid content of the composition.

[0212] The composition preferably further contains a liquid medium such as a solvent and a polymerization initiator, and may further contain a photosensitizer, a polymerization inhibitor, a leveling agent, and the like as necessary.

[0213] <Solvent>

[0214] The solvent is preferably a solvent that can completely dissolve the compound (1), the polymerizable liquid crystal compound, the liquid crystal polymer compound, and the polymer compound. In addition, the solvent is preferably inactive with respect to the polymerization reaction of the polymerizable liquid crystal compound.

[0215] As the solvent, there can be mentioned alcohol solvents such as methanol, ethanol, ethylene glycol, isopropanol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol monomethyl ether, etc.; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, ethyl lactate, etc.; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, methyl isobutyl ketone, etc.; aliphatic hydrocarbon solvents such as pentane, hexane, heptane, etc.; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane, etc.; and chlorinated solvents such as chloroform and chlorobenzene. These solvents can be used alone or in combination of two or more.

[0216] When the composition includes a solvent, the content of the solvent is preferably 50% by mass or more and 98% by mass or less relative to the total amount of the composition. In other words, the content of the solid component in the composition is preferably 2% by mass or more and 50% by mass or less. If the solid component is 50% by mass or less, the viscosity of the composition decreases, and the film obtained by the composition, such as the thickness of the film, becomes roughly uniform, and there is a tendency that it is not easy to produce unevenness in the film. The content of the solid component can be determined by considering the thickness of the film to be manufactured.

[0217] <Polymerization initiator>

[0218] The polymerization initiator is a compound that can initiate the polymerization reaction of the polymerizable liquid crystal compound. From the aspect of being able to initiate the polymerization reaction under lower temperature conditions, the polymerization initiator is preferably a photopolymerization initiator. Specifically, a photopolymerization initiator that can generate active free radicals or acids by the action of light can be cited, among which a photopolymerization initiator that generates free radicals by the action of light is preferred.

[0219] As the polymerization initiator, benzoin compounds, benzophenone compounds, alkylphenone compounds, acylphosphine oxide compounds, triazine compounds, iodonium salts, and sulfonium salts can be mentioned. The polymerization initiator can be appropriately selected from known polymerization initiators according to the purpose, etc. In addition, the polymerization initiator can be used alone or in combination of two or more.

[0220] Examples of the benzoin compound include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether and benzoin isobutyl ether.

[0221] Examples of the benzophenone compound include benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4′-methyldiphenyl sulfide, 3,3,4,4-tetrakis(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.

[0222] Examples of the alkylphenone compound include diethoxyacetophenone, 2-methyl-2-morpholinyl-1-(4-methylthiophenyl)propane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinylphenyl)butane-1-one, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1,2-diphenyl-2,2-dimethoxyethane-1-one, 2-hydroxy-2-methyl-1-〔4-(2-hydroxyethoxy)phenyl〕propane-1-one, 1-hydroxycyclohexylphenyl ketone and oligomers of 2-hydroxy-2-methyl-1-〔4-(1-methylvinyl)phenyl〕propane-1-one.

[0223] Examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

[0224] Examples of the triazine compound include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)ethyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)vinyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)vinyl]-1,3,5-triazine, and the like.

[0225] Examples of the iodonium salt and the sulfonium salt include salts represented by the following formulas.

[0226] [Chemical formula 43]

[0227]

[0228] As the polymerization initiator, a commercially available product may be used. Examples of commercially available polymerization initiators include Irgacure (registered trademark) 907, "Irgacure (registered trademark) 184", "Irgacure (registered trademark) 651", "Irgacure (registered trademark) 819", "Irgacure (registered trademark) 250", and "Irgacure (registered trademark) 369" (manufactured by BASF Japan Ltd.); "SEIKUOL (registered trademark) BZ", "SEIKUOL (registered trademark) Z", and "SEIKUOL (registered trademark) BEE" (manufactured by Seiko Chemical Co., Ltd.); "Kayacure (registered trademark) BP100" and "Kayacure (registered trademark) UVI-6992" (manufactured by Dow Chemical Company); "ADEKA OPTOMER SP-152", "ADEKA OPTOMER SP-170" (manufactured by ADEKA Co., Ltd.); "TAZ-A", "TAZ-PP" (manufactured by Nihon SiberHegner KK); and "TAZ-104" (manufactured by Sanwa Chemical Co., Ltd.); and the like.

[0229] When the composition contains a polymerization initiator, its content can be appropriately determined according to the type and amount of the polymerizable liquid crystal compound contained in the composition. Relative to 100 parts by mass of the polymerizable liquid crystal compound, the content of the polymerization initiator is, for example, 0.001 parts by mass or more, 0.01 parts by mass or more, 0.1 parts by mass or more, or 0.5 parts by mass or more, for example, 30% by mass or less, 10% by mass or less, or 8% by mass or less. In addition, relative to 100 parts by mass of the polymerizable liquid crystal compound, the content of the polymerization initiator is preferably 0.001 parts by mass or less and 30 parts by mass or less, more preferably 0.01 parts by mass or less and 10 parts by mass or less, and further preferably 0.1 parts by mass or less and 8 parts by mass or less. If the content of the polymerization initiator is within the above range, polymerization can be performed without disturbing the orientation of the polymerizable liquid crystal compound.

[0230] <Photosensitizer>

[0231] When the composition contains a photopolymerization initiator, the composition may preferably contain at least one of the photosensitizers. By making the composition contain a photopolymerization initiator and a photosensitizer, there is a tendency that the polymerization reaction of the polymerizable liquid crystal compound is further promoted. As the photosensitizer, xanthone compounds such as xanthone and thioxanthone (for example, 2,4-diethylthioxanthone, 2-isopropylthioxanthone); anthracene compounds such as anthracene and anthracene containing an alkoxy group (for example, dibutoxyanthracene); phenothiazine and rubrene; and the like. The photosensitizer can be used alone or in combination of two or more.

[0232] When the composition includes a photosensitizer, the content of the photosensitizer in the composition can be appropriately determined according to the type and amount of the photopolymerization initiator and the polymerizable liquid crystal compound. The content of the photosensitizer in the composition is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and further preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound.

[0233] <Polymerization inhibitor>

[0234] The composition may contain at least one of the polymerization inhibitors. Examples of the polymerization inhibitor include free radical scavengers such as hydroquinone, hydroquinone containing an alkoxy group, catechol containing an alkoxy group (e.g., butyl catechol), pyrogallol, and 2,2,6,6-tetramethylpiperidin-1-oxyl free radical; thiophenols; β-naphthylamines and β-naphthols; and the like.

[0235] By making the composition contain a polymerization inhibitor, the degree of progress of the polymerization reaction of the polymerizable liquid crystal compound can be controlled.

[0236] When the composition contains a polymerization inhibitor, the content of the polymerization inhibitor in the composition is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound.

[0237] <Leveling agent>

[0238] The composition may contain at least one of the leveling agents. The leveling agent has the function of adjusting the fluidity of the composition and making the coating obtained by applying the composition flatter. Specifically, a surfactant may be mentioned. As the leveling agent, at least one selected from the group consisting of a leveling agent with a polyacrylate compound as a main component and a leveling agent with a compound containing a fluorine atom as a main component is preferred. The leveling agent may be used alone or in combination of two or more.

[0239] Examples of leveling agents having a polyacrylate compound as a main component include "BYK-350", "BYK-352", "BYK-353", "BYK-354", "BYK-355", "BYK-358N", "BYK-361N", "BYK-380", "BYK-381" and "BYK-392" (BYK Chemie).

[0240] Examples of leveling agents containing a fluorine atom-containing compound as a main component include "Megafac (registered trademark) R-08", Megafac "R-30", Megafac "R-90", Megafac "F-410", Megafac "F-411", Megafac "F-443", Megafac "F-445", Megafac "F-470", Megafac "F-471", Megafac "F- "477", Megafac "F-479", Megafac "F-482" and Megafac "F-483" (DIC (Co., Ltd.); "SURFLON (registered trademark) S-381", SURFLON "S-382", SURFLON "S-383", SURFLON "S-393", SURFLON "SC-101", SURFLON "SC-105", "KH-40" and "SA-100" (AGC Seimi Chemical Co., Ltd.); "E1830", "E5844" (DAIKIN FINECHEMICAL LABORATORIES); "F-top EF301", "F-top EF303", "F-top EF351" and "F-top EF352" (Mitsubishi Materials Electronic Chemicals Co., Ltd.); etc.

[0241] When the composition includes a leveling agent, the content of the leveling agent is preferably 0.05 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, relative to the total amount of 100 parts by mass of the polymerizable liquid crystal compound and the liquid crystal polymer compound. If the content of the leveling agent is within the above range, it is easy to horizontally align the polymerizable liquid crystal compound and the liquid crystal polymer compound, and there is a tendency that unevenness is not easy to occur and a smoother film (such as a polarizing film) can be obtained.

[0242] If the content of the leveling agent is within the above range, it is easy to horizontally align the polymerizable liquid crystal compound and the liquid crystal polymer compound, and there is a tendency for the obtained film to become smoother. If the content of the leveling agent relative to the polymerizable liquid crystal compound and the liquid crystal polymer compound exceeds the above range, there is a tendency to easily produce unevenness in the obtained film.

[0243] <Antioxidants>

[0244] The composition may contain an antioxidant. As long as the composition can exert the effect of the present invention, there is no particular limitation on the antioxidant, and known antioxidants can be used. From the viewpoint of having a high inhibitory effect on the photodegradation of the compound represented by formula (1), the antioxidant is preferably a so-called primary antioxidant that captures free radicals and thus has the effect of preventing auto-oxidation. Therefore, the antioxidant contained in the composition is more preferably at least one selected from the group consisting of phenolic compounds, alicyclic alcohol compounds and amine compounds. The antioxidant may be used alone or in combination of two or more.

[0245] Relative to 100 parts by mass of the composition, the content of the above-mentioned antioxidant in the composition is preferably 0.1 parts by mass or more and 15 parts by mass or less, more preferably 0.3 parts by mass or more, further preferably 0.5 parts by mass or more, more preferably 12 parts by mass or less, and further preferably 10 parts by mass or less. If the content of the antioxidant is above the above lower limit, the photodegradation of the compound represented by formula (1) can be more effectively suppressed. In addition, if the content of the antioxidant is below the above upper limit, it is less likely to disturb the orientation of the polymerizable liquid crystal compound, and a higher inhibitory effect on the photodegradation of the compound represented by formula (1) can be expected.

[0246] The composition may contain other additives other than those mentioned above. Examples of other additives include mold release agents, stabilizers, colorants such as bluing agents, flame retardants, and lubricants. When the composition contains other additives, the content of the other additives is preferably greater than 0% and less than 20% by mass, more preferably greater than 0% and less than 10% by mass, relative to the solid content of the composition.

[0247] The composition can be prepared by a method for preparing a composition known in the art. Generally, the composition can be prepared by mixing and stirring a compound represented by formula (1) and having a maximum absorption wavelength in the range of 420 nm to 520 nm, a polymerizable liquid crystal compound, and additives such as an antioxidant and a leveling agent used as needed.

[0248] When the guest-host polarizing plate is manufactured using the composition, the dichroic ratio is not easily reduced even if UV exposure is used in the middle of the manufacturing process. Therefore, photocuring can be used in the processing technology. Therefore, the composition can be preferably used to manufacture a polarizing film.

[0249] <Film>

[0250] The film involved in the present embodiment is obtained by using a composition comprising a compound represented by formula (1) and having a maximum absorption wavelength in a range of more than 420nm and less than 520nm, and a polymerizable liquid crystal compound and at least one compound in a liquid crystal polymer compound as a forming material. The film formed by the composition can be formed by imparting the composition to a substrate and forming a film. In addition, in the case where the composition comprising the compound represented by formula (1) includes a polymerizable liquid crystal compound, a film comprising a cured product obtained by polymerizing the polymerizable liquid crystal compound can be formed by imparting the composition to a substrate, and after film formation, the polymerizable liquid crystal compound is polymerized to solidify it.

[0251] The composition can form a film with a high degree of orientation order, such as a polarizing film. Therefore, the film involved in the present embodiment includes a polarizing film formed by a composition comprising a compound represented by formula (1) and having a maximum absorption wavelength in a wavelength range of 420 nm to 520 nm, and at least one of a polymerizable liquid crystal compound and a liquid crystal polymer compound, and the polarizing film has a high degree of orientation order. As described later, a polarizing film with a high degree of orientation order shows a Bragg peak derived from a high-order structure in an X-ray diffraction measurement.

[0252] Here, for a polarizing film with a high degree of orientation order, a Bragg peak derived from a higher-order structure such as a hexagonal phase and a crystalline phase can be obtained in an X-ray diffraction measurement. Therefore, for a polarizing film formed by a composition, it is preferred that a polymerizable liquid crystal compound or a liquid crystal polymer compound is oriented in a manner that shows a Bragg peak in an X-ray diffraction measurement, and more preferably a "horizontal orientation" in which the molecules of a polymerizable liquid crystal compound or a liquid crystal polymer compound are oriented in the direction of absorbing light. The orientation order that shows a high degree of Bragg peak can be achieved by controlling the type of the polymerizable liquid crystal compound or liquid crystal polymer compound used, the amount of the compound having a maximum absorption wavelength within a wavelength range of more than 420nm and less than 520nm represented by formula (1), etc.

[0253] As polymerizable liquid crystal compounds, liquid crystalline polymer compounds and compounds represented by formula (1) and having a maximum absorption wavelength in the wavelength range of not less than 420 nm and not more than 520 nm constituting the composition for forming a film, there can be cited compounds similar to the polymerizable liquid crystal compounds, liquid crystalline polymer compounds and compound (1) that can be used in the composition described above.

[0254] The membrane can be produced, for example, by a method comprising the following steps:

[0255] forming a coating film of a composition comprising compound (1) and at least one of a polymerizable liquid crystal compound and a liquid crystal high molecular compound, and further comprising a solvent;

[0256] removing at least a portion of the solvent from the coating film;

[0257] Raising the temperature to a temperature above the temperature at which the polymerizable liquid crystal compound or the liquid crystal polymer compound undergoes phase transition to a liquid phase, and then lowering the temperature to transform the polymerizable liquid crystal compound or the liquid crystal polymer compound into a smectic phase (smectic liquid crystal state); and

[0258] The polymerizable liquid crystal compound is polymerized while maintaining the above-mentioned smectic phase (smectic liquid crystal state).

[0259] The coating film of the composition can be formed by, for example, applying the composition on a substrate, an alignment film described later, etc. Alternatively, the composition may be directly applied on a retardation film or other layers constituting a polarizing plate.

[0260] The substrate is usually a transparent substrate. It should be noted that when the substrate is not disposed on the display surface of the display element, for example, when a laminate obtained by removing the substrate from the film is disposed on the display surface of the display element, the substrate may not be transparent. The so-called transparent substrate refers to a substrate having transparency that allows light, especially visible light, to pass through, and the so-called transparency refers to a property of having a transmittance of 80% or more relative to light within a wavelength range of 380 nm to 780 nm. As a specific transparent substrate, a translucent resin substrate can be cited.

[0261] As the resin constituting the light-transmitting resin substrate, polyolefins such as polyethylene and polypropylene can be cited; cyclic olefin resins such as norbornene polymers; polyvinyl alcohol; polyethylene terephthalate; polymethacrylate; polyacrylate; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide and polyphenylene ether, etc. From the viewpoint of ease of acquisition and transparency, polyethylene terephthalate, polymethacrylate, cellulose ester, cyclic olefin resin or polycarbonate is preferred. Cellulose ester is a product obtained by esterification of part or all of the hydroxyl groups contained in cellulose, and can be easily obtained from the market. In addition, cellulose ester substrates can also be easily obtained from the market. Examples of commercially available cellulose ester substrates include "Fujitac Film" (Fujifilm Corporation); "KC8UX2M", "KC8UY", and "KC4UY" (Konica Minolta Opto Co., Ltd.).

[0262] The characteristics required for the substrate vary depending on the composition of the film, but it is generally preferred to use a substrate with as little phase difference as possible. As a substrate with as little phase difference as possible, cellulose ester films such as Zero tack (Konica Minolta Opto Co., Ltd.) and Ztack (Fujifilm Corporation) that do not have a phase difference can be cited. In addition, unstretched cyclic olefin resin substrates are also preferred. Hard coating treatment, anti-reflection treatment, antistatic treatment, etc. can be applied to the surface of the substrate without laminated film.

[0263] The thickness of the substrate is usually 5 μm to 300 μm, preferably 20 μm to 200 μm, and more preferably 20 μm to 100 μm. When it is at least the lower limit, a decrease in strength is suppressed and workability tends to be good.

[0264] Examples of a method for applying the composition to a substrate include known methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator coating, and printing methods such as flexographic printing.

[0265] Next, the solvent contained in the coating film obtained by the composition is removed by drying, etc., thereby forming a dried coating film. In addition, when the coating film contains a polymerizable liquid crystal compound, the dried coating film is formed by drying under the condition that the polymerizable liquid crystal compound does not polymerize. As the drying method of the aforementioned coating film, natural drying method, ventilation drying method, heating drying method and reduced pressure drying method, etc. can be cited.

[0266] In addition, in order to make the polymerizable liquid crystal compound or the liquid crystal polymer compound phase transition to the liquid phase, the temperature is raised to a temperature above the temperature at which the polymerizable liquid crystal compound or the liquid crystal polymer compound phase transitions to the liquid phase, and then the temperature is lowered to make the polymerizable liquid crystal compound or the liquid crystal polymer compound phase transition to the smectic phase (smectic liquid crystal state). The phase transition can be performed after removing the solvent in the coating film, or it can be performed simultaneously with the removal of the solvent.

[0267] By polymerizing the polymerizable liquid crystal compound while maintaining the smectic liquid crystal state of the polymerizable liquid crystal compound, a film of a solidified layer containing a polymerizable liquid crystal composition is formed. As a polymerization method, photopolymerization is preferably used. In photopolymerization, as the light irradiated to the dry coating, it can be appropriately selected according to the type of photopolymerization initiator contained in the dry coating, the type of polymerizable liquid crystal compound (especially the type of polymerizable group possessed by the polymerizable liquid crystal compound) and its amount. As a specific example, one or more light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α rays, β rays and γ rays, and active electron rays can be cited. Among them, from the aspect of easy control of the progress of the polymerization reaction, the aspect of being able to use a device widely used in this field as a photopolymerization device, it is preferably ultraviolet light, and it is preferably selected in advance in a way that ultraviolet light can be used for photopolymerization. The type of polymerizable liquid crystal compound and photopolymerization initiator contained in the composition is selected. In addition, during polymerization, light irradiation can also be performed while the dry coating is cooled using a suitable cooling means, thereby controlling the polymerization temperature. If the polymerizable liquid crystal compound is polymerized at a lower temperature by using such cooling means, a film can be suitably formed even when a substrate with low heat resistance is used. During photopolymerization, a patterned film can also be obtained by performing masking, development, etc.

[0268] As the light source of the aforementioned active energy rays, for example, there can be mentioned a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source that emits light in a wavelength range of not less than 380 nm and not more than 440 nm, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, a metal halide lamp, and the like.

[0269] The UV radiation intensity is usually 10mW / cm 2 Above 3,000mW / cm 2 the following.

[0270] The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating the photopolymerization initiator. The irradiation time is usually 0.1 second to 10 minutes, preferably 0.1 second to 5 minutes, more preferably 0.1 second to 3 minutes, and further preferably 0.1 second to 1 minute. When irradiating once or more times with such an ultraviolet irradiation intensity, the cumulative light amount is preferably 10 mJ / cm 2 Above 3,000mJ / cm 2 the following.

[0271] By photopolymerization, the polymerizable liquid crystal compound is polymerized while maintaining a liquid crystal state of a smectic phase, preferably a higher-order smectic phase, to form a film. The film obtained by polymerizing the polymerizable liquid crystal compound while maintaining a liquid crystal state of a smectic phase is also accompanied by the effect of a dichroic pigment, and thus has the advantage of high polarization performance compared to a conventional guest-host polarizing film, that is, a film formed by a liquid crystal state of a nematic phase. In addition, it also has the advantage of excellent strength compared to a film coated only with a dichroic pigment or a lyotropic liquid crystal.

[0272] The thickness of the film can be appropriately selected depending on the display device to which it is applied, and is preferably 0.5 μm to 10 μm, more preferably 1 μm to 5 μm, and further preferably 1 μm to 3 μm.

[0273] When the film is used as a polarizing film, it is preferably formed on an alignment film. An alignment film is a film with an alignment control force that allows a polymerizable liquid crystal compound and a liquid crystal polymer compound to be oriented in a desired direction. As an alignment film, it is preferably a film having solvent resistance that does not dissolve due to the coating of a composition containing at least one compound of a polymerizable liquid crystal compound and a liquid crystal polymer compound, and having heat resistance in a heating treatment for removing a solvent and orienting a polymerizable liquid crystal compound. As the alignment film, an alignment film comprising an oriented polymer, a photo-aligned film, and a groove-aligned film having a concave-convex pattern and a plurality of grooves on the surface can be cited. From the perspective of the accuracy and quality of the orientation angle, a photo-aligned film is preferably used.

[0274] <Laminated body>

[0275] The laminated body involved in the present embodiment includes a film containing the aforementioned composition. The laminated body may include a substrate, and a film formed of the aforementioned composition disposed on the substrate, or may include a substrate, an oriented film disposed on the substrate, and a film formed of the aforementioned composition disposed on the oriented film. The film formed of the aforementioned composition may constitute a polarizing film. In addition, the substrate may also be a phase difference film. The laminated body may, for example, constitute a polarizing plate. The laminated body may, for example, be manufactured by the above-mentioned film manufacturing method.

[0276] From the viewpoint of the bendability and visibility of the display device, the thickness of the laminate is preferably 10 μm to 300 μm, more preferably 20 μm to 200 μm, and further preferably 25 μm to 100 μm.

[0277] When the laminated body includes a retardation film as a substrate, the thickness of the retardation film can be appropriately selected according to the display device to be applied.

[0278] The laminated body according to the present embodiment can be produced by a production method including the following steps A and B, and optionally step C. When the composition contains a liquid crystalline polymer compound in addition to the compound represented by formula (1), it is preferred to further align the liquid crystalline polymer compound in step B. When the composition contains a polymerizable liquid crystal compound in addition to the compound represented by formula (1), it is preferred to further include step C.

[0279] The laminate can be produced by a production method including the following steps.

[0280] Step A: a step of applying the composition of the present invention on the surface of a substrate to form a coating film;

[0281] Step B: a step of heating to remove the solvent and aligning at least one of the polymerizable liquid crystal compound and the liquid crystalline polymer compound and the compound (1) contained in the formed coating film; and

[0282] Step C: a step of irradiating the aligned polymerizable liquid crystal compound with active energy rays to polymerize the polymerizable liquid crystal compound.

[0283] (Process A)

[0284] The substrate may be any of a glass substrate and a resin substrate, and is preferably a resin substrate. In addition, by using a film substrate formed of a resin, a thin laminate can be obtained.

[0285] The resin substrate is preferably a transparent resin substrate. The so-called transparent resin substrate refers to a substrate having light transmittance that allows light, especially visible light, to pass through, and the so-called light transmittance refers to the property that the visibility-corrected transmittance is 80% or more relative to light within the wavelength range of 380nm to 780nm.

[0286] Examples of the resin constituting the substrate include polyolefins such as polyethylene, polypropylene, and norbornene polymers; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylate; polyacrylate; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyethersulfone; polyetherketone; polyphenylene sulfide; polyphenylene ether; and the like. Preferably, the resin is at least one selected from the group consisting of cellulose esters, cyclic olefin resins, polycarbonate, polyethersulfone, polyethylene terephthalate, and polymethacrylate.

[0287] The substrate thickness is preferably thinner as long as it can be handled practically, but if it is too thin, the strength may decrease and the processability may be poor. The substrate thickness is usually 5 μm to 300 μm, preferably 20 μm to 200 μm.

[0288] (Process B)

[0289] When the composition contains a solvent, the solvent is usually removed from the formed coating film. Examples of the method for removing the solvent include natural drying, ventilation drying, heating drying, and reduced pressure drying.

[0290] When the formed coating film contains at least one of a polymerizable liquid crystal compound and a liquid crystalline high molecular compound, it is usually heated to a temperature higher than a solution state and then cooled to a temperature for liquid crystal alignment to form a liquid crystal phase.

[0291] In the case where the formed coating film contains at least one of a polymerizable liquid crystal compound and a liquid crystal polymer compound, the temperature at which the polymerizable liquid crystal compound and the liquid crystal polymer compound are oriented can be obtained in advance by observing the texture of a composition containing the polymerizable liquid crystal compound. In addition, the removal of the solvent and the liquid crystal orientation can also be performed simultaneously. As the temperature at this time, although it also depends on the type of the solvent, polymerizable liquid crystal compound or liquid crystal polymer compound to be removed, it is preferably in the range of 50°C to 200°C, and in the case where the substrate is a resin substrate, it is more preferably in the range of 80°C to 130°C.

[0292] (Process C)

[0293] When the formed coating film contains a polymerizable liquid crystal compound, the aligned polymerizable liquid crystal compound is irradiated with active energy rays to polymerize the polymerizable liquid crystal compound.

[0294] By polymerizing the aligned polymerizable liquid crystal compound, a film containing the polymerizable liquid crystal compound polymerized in an aligned state and the compound (1) aligned together with the polymerizable liquid crystal compound can be obtained.

[0295] The film containing a polymerizable liquid crystal compound polymerized while maintaining a smectic liquid crystal phase has higher polarization performance than the conventional guest-host polarizing film, that is, the polarizing film obtained by polymerizing a polymerizable liquid crystal compound while maintaining a nematic liquid crystal phase. In addition, compared with the polarizing film coated with only a dichroic pigment or a lyotropic liquid crystal compound, it has excellent polarization performance and strength.

[0296] The active energy ray source may be a ray source that generates ultraviolet rays, electron rays, X-rays, etc. Preferably, it is a light source having a luminescence distribution within a wavelength range of 400 nm or less, such as a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, or a metal halide lamp.

[0297] <Display device>

[0298] The display device of the present embodiment has the aforementioned laminate, and the laminate can be a polarizing plate. The display device can be obtained, for example, by attaching the laminate as a polarizing plate to the surface of the display device via an adhesive layer. The so-called display device is a device having a display element, and is a device comprising a light-emitting element or a light-emitting device as a light source. As a display device, for example, a liquid crystal display device, an organic electroluminescent (EL) display device, an inorganic electroluminescent (EL) display device, an electron emission display device (for example, a field emission display device (FED), a surface field emission display device (SED)), an electronic paper (a display device using electronic ink, an electrophoretic element, etc.), a plasma display device, a projection type display device (for example, a grating light valve (GLV) display device, a display device having a digital micromirror device (DMD)), and a piezoelectric ceramic display, etc. The liquid crystal display device includes any device in a transmissive liquid crystal display device, a semi-transmissive liquid crystal display device, a reflective liquid crystal display device, a direct-view liquid crystal display device, and a projection type liquid crystal display device. These display devices may be display devices that display two-dimensional images or stereoscopic display devices that display three-dimensional images. In particular, as the display device, an organic EL display device and a touch panel display device are preferred, and an organic EL display device is particularly preferred.

[0299] Example

[0300] Hereinafter, the present invention will be specifically described by way of Examples, but the present invention is not limited to these Examples.

[0301] Synthesis Example 1: Synthesis of Compound (2-1)

[0302] To synthesize compound (2-1), compound (2-1-a) is first synthesized. Compound (2-1-c) is then synthesized via compound (2-1-b). Compound (2-1-a) and compound (2-1-c) are then subjected to Suzuki coupling to obtain compound (2-1).

[0303] Synthesis of compound (2-1-a)

[0304] To a chloroform (240 mL) solution of EDC·HCl (1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride. 4.83 g, 25.2 mmol), and DMAP (N,N-dimethylaminopyridine. 0.29 g, 2.4 mmol), n-butanol (3.57 g, 48.1 mmol), and 4-bromobenzoic acid (4.83 g, 24.0 mmol) were added in sequence. After stirring at room temperature for 6 hours, the reaction solution was washed with water, then washed with saturated brine, dried with magnesium sulfate, and concentrated with an evaporator to obtain compound (2-1-a) (5.38 g, yield 87%).

[0305] [Chemical formula 44]

[0306]

[0307] Synthesis of compound (2-1-b)

[0308] 4-Bromoaniline (13.2 g, 77.6 mmol), 35% hydrochloric acid (22.0 mL, 249 mmol), and water (200 mL) were mixed and cooled to 0°C to 5°C. A solution of sodium nitrite (13.0 g, 189 mmol) in water (26 mL) was added dropwise thereto. Thereafter, the mixture was stirred for 30 minutes while being kept at 0°C to 5°C, and aminosulfonic acid (11.0 g, 113 mmol) was further added to prepare a diazo solution. On the other hand, N,N-dimethylaniline (14.0 mL, 111 mmol), sodium acetate (24.8 g, 302 mmol), methanol (200 mL), and water (100 mL) were mixed, cooled to 0°C to 5°C, and the entire amount of the diazo solution just prepared was added dropwise. After the addition was completed, the mixture was heated to room temperature, and the precipitated solid was separated by filtration to obtain compound (2-1-b) (21.0 g, yield 90%).

[0309] [Chemical formula 45]

[0310]

[0311] Synthesis of compound (2-1-c)

[0312] A THF (450 mL) solution of compound (2-1-b) (18.3 g, 60.0 mmol) was cooled to -78°C, and a 1.57 M n-butyl lithium hexane solution (38.0 mL, 59.7 mmol) was added dropwise thereto. Thereafter, the mixture was stirred for 30 minutes while being kept at -78°C, and iPrOBpin (abbreviation for 2-isopropoxy-4,4,5,5-tetramethyl-1,3,2-dioxaborolane) was further added dropwise. 11.0 mL, 64.8 mmol). After the addition was completed, the mixture was heated to room temperature and stirred for 30 minutes. A solution of ammonium chloride (60 g) in water (400 mL) was added to stop the reaction, the organic layer was separated, washed with saturated brine, dried with magnesium sulfate, and concentrated with an evaporator. The obtained solid was purified by reprecipitation from chloroform / hexane to obtain compound (2-1-c) (16.7 g, yield was 79%).

[0313] [Chemical formula 46]

[0314]

[0315] Synthesis of compound (2-1)

[0316] Pd2(dba)3 (22.7 mg, 0.0248 mmol) and P(t-Bu)3·HBF4 (15.3 mg, 0.0527 mmol) were added to a THF (10 mL) solution of compound (2-1-a) (286 mg, 1.10 mmol) and compound (2-1-c) (352 mg, 1.00 mmol), and the mixture was stirred. A 3M potassium phosphate aqueous solution (1.0 mL, 3.0 mmol) was further added, and the mixture was heated and stirred at 60°C for 3.6 hours. Methanol (20 mL) was added to the reaction solution, and the precipitated solid was filtered out and purified by silica gel column chromatography using chloroform as a developing solvent to obtain compound (2-1) (256 mg, yield: 71%).

[0317] 1 H-NMR (400MHz, CDCl3): δ (ppm) = 8.14-8.10 (m, 2H), 7.95-7.89 (m, 4H), 7.76-7.71 (m, 4H), 6 .80-6.76(m, 2H), 4.36(t, 2H), 3.11(s, 6H), 1.78(tt, 2H), 1.55-1.46(m, 2H), 1.00(t, 3H).

[0318] UV visible spectrum: λmax=436nm (in acetonitrile)

[0319] [Chemical formula 47]

[0320]

[0321] Synthesis Example 2: Synthesis of Compound (3)

[0322] In order to synthesize compound (3), compound (3-a) is first synthesized, and then compound (3-a) is subjected to Suzuki coupling with the aforementioned compound (2-1-c) to obtain compound (3).

[0323] Synthesis of compound (3-a)

[0324] To a solution of EDC·HCl (1.36 g, 7.10 mmol) and DMAP (0.083 g, 0.68 mmol) in dichloromethane (60 mL) were added n-hexanol (0.90 mL, 7.2 mmol) and 4-bromobenzoic acid (1.36 g, 6.76 mmol) in sequence. After stirring at room temperature for 6 hours, the reaction solution was washed with water, then with saturated brine, dried over magnesium sulfate, and concentrated with an evaporator to obtain compound (3-a) (1.70 g, yield 88%).

[0325] [Chemical formula 48]

[0326]

[0327] Synthesis of compound (3)

[0328] PdCl2dppf (41.0 mg, 0.0502 mmol) was added to a mixed solution of compound (3-a) (285 mg, 1.00 mmol), compound (2-1-c) (457 mg, 1.30 mmol), diethylene glycol dimethyl ether (13 mL), and water (2 mL) with potassium acetate (650 mg, 6.63 mmol), and the mixture was heated and stirred at 140°C for 4 hours. THF was added to the reaction solution, and after passing through a short silica gel column, it was concentrated by an evaporator. The obtained solid was washed with methanol / water and purified by silica gel column chromatography (chloroform / toluene = 20 / 80) to obtain compound (3) (238 mg, yield 55%).

[0329] 1 H-NMR (400MHz, CDCl3): δ (ppm) = 8.14-8.11 (m, 2H), 7.95-7.89 (m, 4H), 7.76-7.71 (m, 4H), 6.80-6.76 (m, 2H), 4.35 (t, 2H), 3.11 (s, 6H), 1.79 (tt, 2H), 1.51-1.44 (m, 2H), 1.37-1.33 (m, 4H), 0.92 (t, 3H).

[0330] UV visible spectrum: λmax=430nm (in acetonitrile)

[0331] [Chemical formula 49]

[0332]

[0333] Synthesis Example 3: Synthesis of Compound (2-3)

[0334] In order to synthesize compound (2-3), compound (2-3-a) is first synthesized, and then compound (2-3-a) is subjected to Suzuki coupling with the aforementioned compound (2-1-c) to obtain compound (2-3).

[0335] Synthesis of compound (2-3-a)

[0336] To a chloroform (80 mL) solution of EDC·HCl (1.61 g, 8.41 mmol) and DMAP (0.098 g, 0.80 mmol) were added ethanol (1.85 g, 40.1 mmol) and 4-bromo-2,6-difluorobenzoic acid (1.90 g, 8.01 mmol) in sequence. After stirring at room temperature for 4 hours, the reaction solution was washed with water, then washed with saturated brine, dried with magnesium sulfate, and concentrated with an evaporator. The mixture was dissolved in a chloroform / hexane = 1 / 1 mixed solvent, passed through a silica gel short column, and concentrated with an evaporator to obtain compound (2-3-a) (1.32 g, yield 62%).

[0337] [Chemical formula 50]

[0338]

[0339] Synthesis of compound (2-3)

[0340] Pd2(dba)3 (22.7 mg, 0.0248 mmol) and P(t-Bu)3·HBF4 (15.2 mg, 0.0524 mmol) were added to a THF (10 mL) solution of compound (2-3-a) (292 mg, 1.10 mmol) and compound (2-1-c) (351 mg, 1.00 mmol), and the mixture was stirred. A 3M potassium phosphate aqueous solution (1.0 mL, 3.0 mmol) was further added, and the mixture was heated and stirred at 60°C for 4.5 hours. Methanol (20 mL) was added to the reaction solution, and the precipitated solid was filtered out and purified by silica gel column chromatography using chloroform as a developing solvent to obtain compound (2-3) (161 mg, yield: 39%).

[0341] 1H-NMR (400MHz, CDCl3): δ (ppm) = 7.95-7.89 (m, 4H), 7.69-7.66 (m, 2H), 7.26-7.22 (m, 2H), 6.79-6.75 (m, 2H), 4.45 (q, 2H), 3.11 (s, 6H), 1.42 (t, 3H).

[0342] UV visible spectrum: λmax=437nm (in acetonitrile)

[0343] [Chemical formula 51]

[0344]

[0345] Synthesis Example 4: Synthesis of Compound (2-106)

[0346] In order to synthesize compound (2-106), compound (2-106-a) is first synthesized.

[0347] Next, compound (2-106-a) is subjected to Suzuki coupling with the aforementioned compound (2-1-c) to obtain compound (2-106).

[0348] Synthesis of compound (2-106-a)

[0349] To a chloroform (80 mL) solution of EDC·HCl (1.61 g, 8.41 mmol) and DMAP (0.098 g, 0.80 mmol) were added n-butanol (1.19 g, 16.0 mmol) and 4-bromo-2,6-difluorobenzoic acid (1.90 g, 8.01 mmol) in sequence. After stirring at room temperature for 3.5 hours, the reaction solution was washed with water and then with saturated brine. The mixture was dried over magnesium sulfate and concentrated using an evaporator to obtain compound (2-106-a) (1.47 g, yield 62%).

[0350] [Chemical formula 52]

[0351]

[0352] Synthesis of Compound (2-106)

[0353] Pd2(dba)3 (23.2 mg, 0.0253 mmol) and P(t-Bu)3·HBF4 (15.8 mg, 0.0545 mmol) were added to a THF (10 mL) solution of compound (2-106-a) (323 mg, 1.10 mmol) and compound (2-1-c) (352 mg, 1.00 mmol), and the mixture was stirred. A 3M potassium phosphate aqueous solution (1.0 mL, 3.0 mmol) was further added, and the mixture was heated and stirred at 60°C for 4 hours. Methanol (20 mL) was added to the reaction solution, and the precipitated solid was filtered out and purified by silica gel column chromatography using chloroform as a developing solvent to obtain compound (2-106) (154 mg, yield: 35%).

[0354] 1 H-NMR (400MHz, CDCl3): δ (ppm) = 7.95-7.89 (m, 4H), 7.69-7.66 (m, 2H), 7.26-7.22 (m, 2H) , 6.79-6.75(m, 2H), 4.39(t, 2H), 3.11(s, 6H), 1.76(tt, 2H), 1.49(tq, 2H), 0.99(t, 3H).

[0355] UV visible spectrum: λmax=436nm (in acetonitrile)

[0356] [Chemical formula 53]

[0357]

[0358] Synthesis Example 5: Synthesis of Compound (2-4)

[0359] To synthesize compound 2-4, compound (2-4-b) is first synthesized via compound (2-4-a). Next, compound (2-4-b) is subjected to Suzuki coupling with ethyl 4-bromobenzoate to obtain compound (2-4).

[0360] Synthesis of compound (2-4-a)

[0361] To a solution of EDC·HCl (1.61 g, 8.41 mmol) and DMAP (0.098 g, 0.80 mmol) in chloroform (80 mL) were added ethanol (1.84 g, 40.0 mmol) and 4-bromo-2-fluorobenzoic acid (1.75 g, 8.00 mmol) in sequence. After stirring at room temperature for 3.5 hours, the reaction solution was washed with water and then with saturated brine. The mixture was dried over magnesium sulfate and concentrated using an evaporator to obtain compound (2-4-a) (1.60 g, yield 81%).

[0362] [Chemical formula 54]

[0363]

[0364] Synthesis of compound (2-4)

[0365] Pd2(dba)3 (46.1 mg, 0.0503 mmol) and P(t-Bu)3·HBF4 (29.0 mg, 0.100 mmol) were added to a THF (10 mL) solution of compound (2-4-a) (552 mg, 2.23 mmol) and compound (2-1-c) (704 mg, 2.01 mmol), and the mixture was stirred. A 3M potassium phosphate aqueous solution (2.0 mL, 6.0 mmol) was further added, and the mixture was heated and stirred at 60°C for 3.5 hours. Water (20 mL) was added to the reaction solution, and the precipitated solid was filtered out and purified by silica gel column chromatography using chloroform as a developing solvent to obtain compound (2-4) (480 mg, yield: 61%).

[0366] 1 H-NMR (400MHz, CDCl3): δ (ppm) = 8.02 (dd, 1H), 7.95-7.89 (m, 4H), 7.74-7.70 (m, 2H), 7 .50(dd, 1H), 7.43(dd, 1H), 6.80-6.76(m, 2H), 4.43(q, 2H), 3.11(s, 6H), 1.43(t, 3H).

[0367] UV visible spectrum: λmax=436nm (in acetonitrile)

[0368] [Chemical formula 55]

[0369]

[0370] Synthesis Example 6: Synthesis of Compound (2-6)

[0371] In order to synthesize compound (2-6), compound (2-6-b) is first synthesized via compound (2-6-a). Next, compound (2-6-b) is subjected to Suzuki coupling with ethyl 4-bromobenzoate to obtain compound (2-6).

[0372] Synthesis of compound (2-6-a)

[0373] 4-Bromo-2-fluoroaniline (14.3 g, 75.0 mmol), 35% hydrochloric acid (22.0 mL, 249 mmol), and water (200 mL) were mixed and cooled to 0°C to 5°C, and a solution of sodium nitrite (7.76 g, 112 mmol) in water (26 mL) was added dropwise thereto. Thereafter, the mixture was stirred for 30 minutes while maintaining the temperature at 0°C to 5°C, and aminosulfonic acid (4.36 g, 45.0 mmol) was further added to prepare a diazo solution. On the other hand, N,N-dimethylaniline (13.6 g, 113 mmol), sodium acetate (24.6 g, 300 mmol), methanol (200 mL), and water (100 mL) were mixed, cooled to 0°C to 5°C, and the entire amount of the diazo solution just prepared was added dropwise. After the addition was completed, the mixture was heated to room temperature, and the precipitated solid was separated by filtration to obtain compound (2-6-a) (15.8 g, yield 66%).

[0374] [Chemical formula 56]

[0375]

[0376] Synthesis of compound (2-6-b)

[0377] PdCl2dppf (249 mg, 0.305 mmol) was added to a solution of compound (2-6-a) (3.23 g, 10.0 mmol), B2pin2 (bis(pinacolato)diboron. 2.79 g, 11.0 mmol), and potassium acetate (2.99 g, 30.4 mmol) in 1,4-dioxane (60 mL), and heated with stirring at 80°C for 7 hours. The reaction solution was separated using toluene / water, and the organic layer was washed with water, then washed with saturated brine, then dried with magnesium sulfate, and concentrated using an evaporator. The obtained solid was purified by reprecipitation from chloroform / hexane to obtain compound (2-6-b) (2.53 g, yield was 69%).

[0378] [Chemical formula 57]

[0379]

[0380] Synthesis of compound (2-6)

[0381] Pd2(dba)3 (69.8 mg, 0.0762 mmol) and P(t-Bu)3·HBF4 (45.0 mg, 0.155 mmol) were added to a THF (30 mL) solution of ethyl 4-bromobenzoate (0.763 g, 3.33 mmol) and compound (2-6-b) (1.11 g, 3.00 mmol), and the mixture was stirred. A 3M potassium phosphate aqueous solution (4.0 mL, 12.0 mmol) was further added, and the mixture was heated and stirred at 60°C for 4 hours. Methanol (20 mL) was added to the reaction solution, and the precipitated solid was filtered out and purified by silica gel column chromatography using chloroform as a developing solvent to obtain compound (2-6) (904 mg, yield: 77%).

[0382] 1 H-NMR (400MHz, CDCl3): δ (ppm) = 8.15-8.12 (m, 2H), 7.95-7.91 (m, 2H), 7.84 (d, 1H), 7.72- 7.68(m, 2H), 7.52-7.45(m, 2H), 6.79-6.75(m, 2H), 4.42(q, 2H), 3.12(s, 6H), 1.43(t, 3H).

[0383] UV visible spectrum: λmax=452nm (in acetonitrile)

[0384] [Chemical formula 58]

[0385]

[0386] Synthesis Example 7: Synthesis of Compound (2-116)

[0387] In order to synthesize compound 2-116, compound (2-116-b) is first synthesized via compound (2-116-a). Next, compound (2-116-b) is subjected to Negishi coupling with n-butylzinc bromide to obtain compound (2-116).

[0388] Synthesis of compound (2-116-a)

[0389] 4-Bromo-3-fluoroaniline (9.50 g, 50.0 mmol), 35% hydrochloric acid (14.8 mL, 167 mmol), and water (95 mL) were mixed, cooled to 0°C to 5°C, and a solution of sodium nitrite (3.45 g, 50.0 mmol) in water (5 mL) was added dropwise to prepare a diazo solution. On the other hand, sodium (phenylamino)methanesulfonate (11.5 g, 55.0 mmol), sodium acetate (16.4 g, 55.0 mmol), and water (100 mL) were mixed, cooled to 0°C to 5°C, and the entire amount of the diazo solution just prepared was added dropwise. After the addition was completed, the temperature was raised to room temperature, sodium hydroxide (12.0 g, 300 mmol) was added, and the mixture was heated and stirred at 90°C for 2.5 hours. The precipitated solid was filtered to obtain compound (2-116-a) (13.9 g, yield 94%).

[0390] [Chemical formula 59]

[0391]

[0392] Compound (2-116-a) (1.47 g, 10.0 mmol), 35% hydrochloric acid (1.5 mL, 17 mmol), and water (9 mL) were mixed, cooled to 0°C to 5°C, and a solution of sodium nitrite (345 mg, 5.00 mmol) in water (1 mL) was added dropwise. Thereafter, the mixture was stirred for 45 minutes while maintaining the temperature at 10°C to 15°C to prepare a diazo solution. On the other hand, N,N-diethylaniline (895 mg, 6.00 mmol), sodium acetate (1.64 g, 20.0 mmol), methanol (20 mL), and water (10 mL) were mixed, cooled to 10°C to 15°C, and the entire amount of the diazo solution just prepared was added dropwise. After the addition was completed, the mixture was heated to room temperature, the precipitated solid was filtered out, dissolved in chloroform, washed with water, and then washed with saturated brine.

[0393] The residue was dried over magnesium sulfate and concentrated using an evaporator. The obtained solid was purified by silica gel column chromatography (chloroform / hexane=50 / 50) to obtain compound (2-116-b) (1.26 g, yield: 55%).

[0394] [Chemical formula 60]

[0395]

[0396] A mixed solution of compound (2-116-b) (213 mg, 0.500 mmol), PdCl2dppf (8.1 mg, 0.010 mmol), and THF (5.0 mL) was heated and stirred at 55°C, and 0.50 M n-butylzinc bromide (1.2 mL, 0.60 mmol) was added dropwise. Thereafter, the mixture was heated under reflux for 3.5 hours. Water (20 mL) was added to the reaction solution, and the precipitated solid was filtered out and purified by silica gel column chromatography (chloroform / hexane = 50 / 50). Further purification was performed by reprecipitation from chloroform / hexane to obtain compound (2-116) (137 mg, yield 64%).

[0397] 1 H-NMR (400MHz, CDCl3): δ (ppm) = 8.03-8.00 (m, 2H), 7.98-7.95 (m, 2H), 7.92-7.88 (m, 2H), 7.71 (dd, 1H), 7.60 (dd, 1H) ), 7.34(dd, 1H), 6.76-6.72(m, 2H), 3.46(q, 4H), 2.72(t, 2H), 1.65(tt, 2H), 1.41(tq, 2H), 1.25(t, 6H), 0.96(t, 3H).

[0398] UV visible spectrum: λmax=499nm (in acetonitrile)

[0399] [Chemical formula 61]

[0400]

[0401] Synthesis Example 8: Synthesis of Compound (2-166)

[0402] 2-Bromo-5-n-butylthienothiazole is subjected to Suzuki coupling with the aforementioned compound (2-6-b) to obtain compound (2-166).

[0403] Synthesis of compound (2-166)

[0404] To a THF (10 mL) solution of 2-bromo-5-n-butylthienothiazole (0.304 g, 1.10 mmol) and compound (2-6-b) (0.369 g, 1.00 mmol) were added Pd2(dba)3 (0.0367 mg, 0.0400 mmol) and P(t-Bu)3·HBF4 (0.0232 mg, 0.0800 mmol) and stirred.

[0405] 3M potassium phosphate aqueous solution (2.0 mL, 6.0 mmol) was further added, and the mixture was heated and stirred for 16 hours. Methanol was added to the reaction solution, and the precipitated solid was filtered out and purified by silica gel column chromatography (chloroform / toluene=10 / 90) to obtain compound (2-166) (0.127 g, yield: 29%).

[0406] 1 H-NMR (400MHz, CDCl3): δ (ppm) = 9.95-7.91 (m, 2H), 7.87-7.81 (m, 2H), 7.77 (dd, 1H), 6.95 (s , 1H), 6.78-6.74(m, 2H), 3.12(s, 6H), 2.92(t, 2H), 1.74(tt, 2H), 1.44(tq, 2H), 0.97(t, 3H).

[0407] UV visible spectrum: λmax=475nm (in acetonitrile)

[0408] [Chemical formula 62]

[0409]

[0410] Synthesis Example 9: Synthesis of Compound (2-167)

[0411] Compound (2-167) is obtained by subjecting 2-bromo-5-n-butylthienothiazole and compound (2-167-b) synthesized via compound (2-167-a) to Suzuki coupling.

[0412] Synthesis of compound (2-167-a)

[0413] 4-Bromo-3-fluoroaniline (1.90 g, 10.0 mmol), 35% hydrochloric acid (3.0 mL, 34 mmol), and water (25 mL) were mixed and cooled to 0°C to 5°C, and a solution of sodium nitrite (0.69 mg, 10.0 mmol) in water (2.5 mL) was added dropwise to prepare a diazo solution. On the other hand, dimethylaniline (1.33 g, 11.0 mmol), sodium acetate (3.28 g, 40.0 mmol), methanol (25.0 mL), and water (12.5 mL) were mixed, cooled to 0°C to 5°C, and the entire amount of the diazo solution just prepared was added dropwise. After the addition was completed, the mixture was heated to room temperature, and the precipitated solid was separated by filtration to obtain compound (2-167-a) (2.59 g, yield 80%).

[0414] [Chemical formula 63]

[0415]

[0416] Synthesis of compound (2-167-b)

[0417] PdCl2dppf (0.286 g, 0.351 mmol) was added to a 1,4-dioxane (35 mL) solution of compound (2-167-a) (2.26 g, 7.00 mmol), B2pin2 (formal name is bis(pinacolato)diboron. 1.96 g, 7.70 mmol), and potassium acetate (2.06 g, 21.0 mmol), and heated with stirring at 80°C for 15 hours. The reaction solution was separated using toluene / water, and the organic layer was washed with water, then washed with saturated brine, then dried with magnesium sulfate, and concentrated using an evaporator. The obtained solid was purified by reprecipitation from chloroform / hexane to obtain compound (2-167-b) (1.74 g, yield was 67%).

[0418] [Chemical formula 64]

[0419]

[0420] Synthesis of compound (2-167)

[0421] Pd2(dba)3 (0.023 g, 0.0251 mmol) and P(t-Bu)3·HBF4 (0.015 g, 0.0517 mmol) were added to a solution of 2-bromo-5-n-butylthienothiazole (0.307 g, 1.11 mmol) and compound (2-167-b) (0.370 g, 1.00 mmol) in 1,4-dioxane (10 mL), and the mixture was stirred. A 3M potassium phosphate aqueous solution (1.0 mL, 3.0 mmol) was further added, and the mixture was heated and stirred for 4 hours. Methanol was added to the reaction solution, and the precipitated solid was filtered out and purified by silica gel column chromatography using chloroform as a developing solvent, and further purified by reprecipitation from chloroform / methanol to obtain compound (2-167) (0.317 g, yield: 72%).

[0422] 1 H-NMR (400MHz, CDCl3): δ (ppm) = 8.42 (dd, 1H), 7.92-7.89 (m, 2H), 7.78 (dd, 1H), 7.68 (dd, 1H), 6. 97(s, 1H), 6.79-6.75(m, 2H), 3.12(s, 6H), 2.93(t, 2H), 1.75(tt, 2H), 1.45(tq, 2H), 0.97(t, 3H).

[0423] UV visible spectrum: λmax=471nm (in acetonitrile)

[0424] [Chemical formula 65]

[0425]

[0426] Synthesis Example 10: Synthesis of Compound (2-184)

[0427] In order to synthesize compound (2-184), compound (2-184-a) is first synthesized.

[0428] Next, compound (2-184-a) is subjected to Suzuki coupling with the aforementioned compound (2-6-b) to obtain compound (2-184-b). Next, compound (2-184) is obtained by ester exchange reaction.

[0429] Synthesis of compound (2-184-a)

[0430] Isobutyl nitrite (4.40 mL, 37 mmol) and ethyl 2-aminobenzothiazole-6-carboxylate (5.56 g, 25.0 mmol) were added to a solution of copper (II) bromide (6.48 g, 29.0 mmol) in acetonitrile (200 mL) in sequence. After stirring at 65°C for 1.5 hours, the reaction solution was cooled to room temperature and then injected into 0.4 M hydrochloric acid (200 mL) to stop the reaction. After separation using chloroform / water, the organic layer was washed with water, then washed with saturated brine, dried with magnesium sulfate, and concentrated using an evaporator to obtain compound (2-184-a) (6.56 g, yield 92%).

[0431] [Chemical formula 66]

[0432]

[0433] Synthesis of compound (2-184-b)

[0434] Pd2(dba)3 (0.0464 g, 0.0507 mmol) and P(t-Bu)3·HBF4 (0.0290 g, 0.100 mmol) were added to a THF (20 mL) solution of compound 2-184-a (0.631 g, 2.21 mmol) and compound 2-6-b (0.739 g, 2.00 mmol), and the mixture was stirred. A 3M potassium phosphate aqueous solution (2.0 mL, 6.0 mmol) was further added, and the mixture was heated and stirred at 60°C for 12 hours. Methanol was added to the reaction solution, and the precipitated solid was filtered to obtain compound (2-184-b) (0.782 g, yield 87%).

[0435] [Chemical formula 67]

[0436]

[0437] Synthesis of compound (2-184)

[0438] A solution of compound (2-184-b) (0.450 g, 1.00 mmol), TiO(acac)2 (abbreviation for bis(2,4-pentanedione)titanium(IV) oxide. 0.132 g, 0.504 mmol), and n-hexanol (0.512 g, 5.01 mmol) in p-xylene (15 mL) was heated to reflux for 4 hours. Methanol was added to the reaction solution, the precipitated solid was filtered out, and purified by silica gel column chromatography with chloroform as the developing solvent to obtain compound (2-184) (0.366 g, yield was 72%).

[0439] 1 H-NMR (400MHz, CDCl3): δ (ppm) = 8.65 (d, 1H), 8.19 (dd, 1H), 8.11 (d, 1H), 8.02 (dd, 1H), 7.97-7.91 (m, 3H), 7.88 (dd, 1H), 6.79-6.75(m, 2H), 4.38(t, 2H), 3.13(s, 6H), 1.82(tt, 2H), 1.52-1.45(m, 2H), 1.40-1.34(m, 4H), 0.92(t, 3H).

[0440] UV visible spectrum: λmax=482nm (in acetonitrile)

[0441] [Chemical formula 68]

[0442]

[0443] <Example 1>: Preparation of a composition containing compound (2-3)

[0444] The following components were mixed and stirred at 80° C. for 1 hour to obtain composition E1.

[0445]

[0446]

[0447] Polymerizable liquid crystal compound (A-6)

[0448] [Chemical formula 69]

[0449]

[0450] Polymerizable liquid crystal compound (A-7)

[0451] [Chemical formula 70]

[0452]

[0453] The polymerizable liquid crystal compound (A-6) was synthesized by the method described in Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996). In addition, a polymerizable liquid crystal compound (A-7) was produced according to the same method.

[0454] <Example 2>: Preparation of a composition containing compound (2-106)

[0455] Composition E2 was obtained in the same manner as in Example 1 except that compound (2-106) was used instead of compound (2-3).

[0456] <Example 3>: Preparation of a composition containing compound (2-4)

[0457] Composition E3 was obtained in the same manner as in Example 1 except that compound (2-4) was used instead of compound (2-3).

[0458] <Example 4>: Preparation of a composition containing compound (2-6)

[0459] Composition E4 was obtained in the same manner as in Example 1 except that compound (2-6) was used instead of compound (2-3).

[0460] <Example 5>: Preparation of a composition containing compound (2-116)

[0461] Composition E5 was obtained in the same manner as in Example 1 except that compound (2-116) was used instead of compound (2-3).

[0462] <Example 6>: Preparation of a composition comprising compound (2-166)

[0463] Composition E6 was obtained in the same manner as in Example 1 except that compound (2-166) was used instead of compound (2-3).

[0464] <Example 7>: Preparation of a composition containing compound (2-167)

[0465] Composition E7 was obtained in the same manner as in Example 1 except that compound (2-167) was used instead of compound (2-3).

[0466] <Example 8>: Preparation of a composition comprising compound (2-184)

[0467] Composition E8 was obtained in the same manner as in Example 1 except that compound (2-184) was used instead of compound (2-3).

[0468] <Comparative Example 1>: Preparation of a composition containing compound (2-1)

[0469] Composition C1 was obtained in the same manner as in Example 1 except that compound (2-1) was used instead of compound (2-3).

[0470] <Comparative Example 2>: Preparation of a composition containing compound (3)

[0471] Composition C2 was obtained in the same manner as in Example 1 except that compound (3) was used instead of compound (2-3).

[0472] <Manufacturing of polarizing plates>

[0473] 1. Formation of oriented film

[0474] A glass substrate was used as a transparent substrate. A 2 mass % aqueous solution of polyvinyl alcohol (polyvinyl alcohol 1000 completely saponified type, manufactured by Wako Pure Chemical Industries, Ltd.) (composition for forming an alignment layer) was applied to the glass substrate by spin coating, and after drying, a film with a thickness of 100 nm was formed. Next, the surface of the obtained film was subjected to a rubbing treatment to form an alignment film, thereby obtaining a laminate 1 having an alignment film formed on a glass substrate.

[0475] 2. Formation of polarizing film

[0476] The composition obtained above is applied to the oriented film of the stacked body 1 obtained above by spin coating, and after heating and drying on a heating plate at 120°C for 3 minutes, it is rapidly cooled to below 70°C (the temperature at which a smectic liquid crystal phase is exhibited when cooled), thereby obtaining a stacked body 2 having a first dry film formed on the oriented film.

[0477] Next, a UV irradiation device (SPOT CURE SP-7; manufactured by USHIO Inc.) was used at an exposure dose of 2400 mJ / cm 2 The polarizing film is irradiated with ultraviolet rays under the condition of 100 nm (based on 365 nm), thereby polymerizing the polymerizable liquid crystal compound contained in the first dry film while maintaining the liquid crystal state of the composition, and the polarizing film is formed from the first dry film to obtain a polarizing plate as a laminate 3.

[0478] <Evaluation>

[0479] The dichroic ratio of the laminate 2 in which a polarizing film is formed on the oriented film of the laminate 1 is measured as follows. Using a device in which a holder (folder) having the laminate 1 is mounted on a spectrophotometer (UV-3150 manufactured by Shimadzu Corporation), the absorbance in the transmission axis direction (A1) and the absorbance in the absorption axis direction (A2) of the polarizing film of the laminate 2 at the maximum absorption wavelength (λmax) are measured by a double beam method. On the holder, a screen that cuts off 50% of the light is set on the reference side. From the measured values ​​of the absorbance in the transmission axis direction (A1) and the absorbance in the absorption axis direction (A2), the ratio (A2 / A1) is calculated as the dichroic ratio (DR1) before UV exposure.

[0480] For the laminate 3 after UV exposure, the absorbance in the transmission axis direction and the absorbance in the absorption axis direction at the maximum absorption wavelength (λmax) of the polarizing film of the laminate 3 were measured in the same manner as above, and the dichroic ratio (DR2) after UV exposure was calculated. The dichroic ratio (DR2) after UV exposure was divided by the dichroic ratio (DR1) before UV exposure to calculate the dichroic ratio maintenance rate (DR2 / DR1; %). The results are summarized in Table 1. When the dichroic ratio maintenance rate of the laminate 3 is greater than 50%, it is good as a polarizing plate.

[0481] [Table 1]

[0482]

[0483] As can be seen from Table 1, for a polarizing plate having a polarizing film formed by a composition comprising a compound represented by formula (1) and having a maximum absorption wavelength in a wavelength range of not less than 420 nm and not more than 520 nm, and at least one compound among a polymerizable liquid crystal compound and a liquid crystalline polymer compound, when UV irradiation is included in the manufacturing process of the polarizing plate, the maintenance rate of the dichroic ratio before and after UV irradiation is excellent.

Claims

1. A composition comprising: a compound represented by the following formula (1) and having a maximum absorption wavelength in the range of 420 nm to 520 nm; and at least one of a polymerizable liquid crystal compound and a liquid crystal polymer compound, R 4 -R 3 -On 1 -(-R 1 -On 2 -) n -N=N-On 3 -R 2 (1) In formula (1), n ​​represents an integer of 1 or 2; Ar 1 ,Ar 2 and Ar 3 Each independently represents an optionally substituted 1,4-phenylene group or an optionally substituted divalent sulfur-containing aromatic heterocyclic group, Ar 1 and Ar 2 At least one of them has 1 or 2 fluorine atoms as substituents; R 1 represents a single bond, or at least one group selected from the group consisting of -OC(=O)-, -C(=O)O-, and -N=N-; R 2 represents an alkylamino group optionally having a polymerizable group, or an alkoxy group optionally having a polymerizable group; R 3 represents at least one group selected from the group consisting of an alkanediyl group having 4 to 20 carbon atoms, an alkanediyloxy group having 2 to 20 carbon atoms, an alkanediyloxycarbonyl group having 2 to 20 carbon atoms, and an alkanediylcarbonyloxy group having 2 to 20 carbon atoms; R 4 represents a polymerizable group or a hydrogen atom; When n is 2, there are 2 R 1 The same or different, there are 2 Ar 2 The same as or different from each other.

2. The composition according to claim 1, wherein The polymerizable liquid crystal compound and the liquid crystalline polymer compound are a polymerizable smectic liquid crystal compound and a smectic liquid crystalline polymer compound.

3. The composition according to claim 1 or 2, wherein The polymerizable liquid crystal compound is a compound represented by the following formula (A): U 1 -V 1 -W 1 -(X 1 -Y 1 ) m -X 2 -Y 2 -X 3 -W 2 -V 2 -U 2 (A) In formula (A), m is an integer from 1 to 3; X 1 , X 2 and X 3 Each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group; when m is 2 or 3, there are multiple X 1 Same or different from each other; selected from X 1 , X 2 and X 3 At least three of the group consisting of these groups represent divalent 6-membered cyclic hydrocarbon groups; Y 1 , Y 2 , W 1 and W 2 Each independently represents a single bond or a divalent linking group; When m is 2 or 3, there are multiple Y 1 the same as or different from one another; V 1 and V 2 Each independently represents an alkanediyl group having 1 to 20 carbon atoms and optionally having a substituent; optionally, at least one of the -CH2- groups constituting the alkanediyl group is replaced by -O-, -CO-, -S- or -NH-; U 1 and U 2 Each independently represents a polymerizable group or a hydrogen atom, and at least one of them represents a polymerizable group.

4. The composition according to claim 1 or 2, wherein In the formula (1), n ​​is 1.

5. The composition according to claim 1 or 2, wherein The polymerizable group is a free radical polymerizable group.

6. A film formed of the composition according to any one of claims 1 to 5.

7. A laminate comprising the film according to claim 6.

8. A display device comprising the laminate according to claim 7.

Citation Information

Patent Citations

  • JP1972019156U

  • Dichroic Guest-Host Polarizers Containing Oriented Polymer Films

    JP2007510946A

  • Polarizer and method for manufacturing the same

    JP2013037353A

  • Composition

    WO2016136561A1

  • Light absorption anisotropic film, production method thereof, and liquid crystal display device using the same

    JP2011237513A