A method for manufacturing an electrolyte for ultra-low temperature lithium-ion battery
By using a combination of low melting point cyclic carbonate and chain ether mixed solvents and specific lithium salts and additives, the problem of poor performance of lithium-ion batteries at low temperatures is solved, and efficient use and operation in -60°C environments are achieved. Improvement of low-temperature electrochemical performance.
Patent Information
- Application Number
- CN202111487985.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-12-08
AI Technical Summary
Existing lithium-ion batteries have poor performance under low temperature conditions. In particular, the viscosity of the electrolyte increases sharply at low temperatures, the ion diffusion efficiency decreases, and the charge transfer resistance increases. As a result, lithium-ion batteries cannot be used normally in ultra-low temperature environments of -60°C. .
Using a mixed solvent of low melting point cyclic carbonates and ultra-low melting point chain ethers, combined with lithium hexafluorophosphate and lithium difluorophosphate as lithium salts and additives, a simple configuration of ultra-low temperature electrolysis was prepared through a specific stirring sequence and process. liquid to ensure low viscosity and high ionic conductivity in a -60°C environment.
It realizes the normal use of lithium-ion batteries in ultra-low temperature environments of -60°C and maintains high discharge capacity and cycle stability. In particular, batteries equipped with low-temperature lithium iron phosphate cathode materials and graphite anode materials still have good performance at -40°C. 70% capacity retention rate, significantly improving low-temperature electrochemical performance.
Smart Images

Figure CN114156542B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a method for manufacturing an electrolyte for manufacturing ultra-low temperature lithium ion batteries. Background Art
[0002] As the country attaches great importance to the new energy industry, lithium-ion batteries, as an indispensable energy storage part of the new energy system, have become one of the key research objects of researchers. However, the current application of lithium-ion batteries has certain requirements for low temperature conditions, especially in new energy vehicles. Therefore, the improvement of the low temperature performance of lithium-ion batteries is of great significance for their widespread application across the country.
[0003] The poor performance of lithium-ion batteries under low temperature conditions is largely related to the electrolyte. Although the positive electrode materials, negative electrode materials, and current collectors are all restricted under low temperature conditions, the rapid increase in electrolyte viscosity, the sharp decrease in ion diffusion efficiency, and the significant increase in charge transfer impedance at low temperatures have the greatest impact on the low temperature performance of lithium-ion batteries. Therefore, ultra-low temperature electrolytes have become the most important part of low-temperature lithium-ion battery technology.
[0004] CN113036223B discloses an ultra-low temperature lithium-ion battery electrolyte, wherein the solvent is a mixed solvent composed of carbonates, ethers, and acetates; the lithium salt is a mixed lithium salt composed of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, and lithium bis(trifluoromethanesulfonyl)imide; and the additive is a mixed additive composed of vinylene carbonate, fluoroethylene carbonate, lithium nitrate, and dichloromethane. The ultra-low temperature electrolyte prepared in this invention has an electrical conductivity increased by more than 400% compared with conventional electrolytes, and effectively improves the interface film of the negative electrode of the lithium battery and reduces polarization. However, the electrolyte of this invention uses a variety of mixed lithium salts, and the complex formula configuration process is cumbersome, and the anions have little effect on improving the battery performance. This method is not suitable for large-scale industrial production.
[0005] CN113328141A discloses a low-temperature electrolyte, including a lithium salt, an organic solvent and an additive, wherein the lithium salt is a sulfur-containing and oxygen-containing fluoroalkyl lithium phosphate, and the additive includes a conventional additive, an acid binding agent and a bis(tetrafluorophosphoryl)imide salt. The electrolyte of the invention has high ion conductivity under ultra-low temperature conditions of -45°C. However, although the electrolyte involved in the invention has greatly improved the low-temperature performance of the electrolyte, it still cannot be used at an ultra-low temperature of -60°C to meet the use requirements in some special environments. Summary of the invention
[0006] Based on the above problems, the present invention designs a method for manufacturing an electrolyte for ultra-low temperature lithium-ion batteries. The method has a simple formula, is easy to configure, and can be used in an ultra-low temperature environment of -60°C, which is of great significance.
[0007] In order to achieve the above object, the technical solution of the present invention is as follows:
[0008] A method for manufacturing an electrolyte for manufacturing an ultra-low temperature lithium-ion battery, wherein the electrolyte comprises 50% to 93.5% of a solvent, 5% to 30% of a lithium salt and 1.5% to 20% of an additive, calculated by mass ratio in the electrolyte; the solvent is a mixed solvent composed of low-melting-point cyclic carbonates such as propylene carbonate PC and ultra-low-melting-point chain ethers such as dipropylene glycol dimethyl ether DMM, and the mass ratios of carbonates and ethers in the mixed solvent are 60% to 90% and 10% to 40%, respectively; the lithium salt is lithium hexafluorophosphate LiPF6; and the additive is a lithium salt-type film-forming aid lithium difluorophosphate LiPO2F2;
[0009] The method comprises the following steps: mixing and stirring the above electrolyte components in any one of the following addition orders:
[0010] Sequence 1: mixed solvent, lithium salt, additive;
[0011] Sequence 2: mixed solvent, additive, lithium salt;
[0012] Sequence three: low melting point cyclic carbonate solvents, additives, low melting point chain ethers, lithium salts;
[0013] Each component in the above sequence needs to be stirred for 30 minutes to 240 minutes after being added.
[0014] Furthermore, the method comprises the following steps: firstly, carbonates and ethers are mixed and stirred to form a mixed solvent A, then lithium salt is added to the mixed solvent A and stirred until the lithium salt is completely dissolved to form a mixed solution B, and finally additives are added.
[0015] Furthermore, carbonate and ether solvents are both distilled under reduced pressure and dried with 4A grade molecular sieves in order to reduce the water content in the solvent to below 30 ppm.
[0016] Furthermore, lithium salt is added in portions so that the concentration of the prepared electrolyte is 1 to 3 mol / L.
[0017] The advantages and positive effects of the present invention are:
[0018] Cyclic carbonate solvents generally have a large polarity, a high dielectric constant, and a high viscosity. The high dielectric constant makes them very capable of dissolving lithium salts, which is beneficial to improving the ionic conductivity of the electrolyte. Chain ether solvents are just the opposite. They have a lower dielectric constant, but their lower viscosity can effectively prevent the problem of a sharp increase in electrolyte viscosity at low temperatures. The mixed solvent obtained by mixing two low-melting-point solvents in a certain proportion has a very low melting point to ensure its normal use under ultra-low temperature conditions, and can maintain a low viscosity and high ionic conductivity at low temperatures. The use of lithium difluorophosphate effectively improves the co-embedding phenomenon of solvent molecules caused by the embedding of solvated ions into the graphite layer when PC is used in the graphite negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is the first charge and discharge curve of Example 4 at -60°C 1C rate;
[0020] Figure 2 This is the 300 cycle curve of Example 4 at -40°C and 1C rate. DETAILED DESCRIPTION
[0021] In order to further understand the content, features and effects of the present invention, the following embodiments are given as examples and described in detail with reference to the accompanying drawings:
[0022] A method for manufacturing an electrolyte for manufacturing an ultra-low temperature lithium-ion battery. The electrolyte comprises 50% to 93.5% of a solvent, 5% to 30% of a lithium salt and 1.5% to 20% of an additive, calculated by mass ratio in the electrolyte; the solvent is a mixed solvent composed of low-melting-point cyclic carbonates such as propylene carbonate PC and ultra-low-melting-point chain ethers such as dipropylene glycol dimethyl ether DMM, and the mass ratios of carbonates and ethers in the mixed solvent are 60% to 90% and 10% to 40%, respectively; the lithium salt is lithium hexafluorophosphate LiPF6; and the additive is a lithium salt-type film-forming aid, lithium difluorophosphate LiPO2F2.
[0023] The method comprises the following steps: mixing and stirring the above electrolyte components according to any one of the following adding sequences: sequence one: mixed solvent, lithium salt, additive; sequence two: mixed solvent, additive, lithium salt; sequence three: low melting point cyclic carbonate solvent, additive, low melting point chain ether, lithium salt; the stirring time after each part is added is 30 minutes to 240 minutes.
[0024] The preferred order of addition is order 1; specifically, firstly, carbonates and ethers are mixed and stirred to form a mixed solvent A, then lithium salt is added to the mixed solvent A and stirred until the lithium salt is completely dissolved to form a mixed solution B, and finally the additive is added.
[0025] The electrolyte was prepared in a glove box protected by argon. Carbonate and ether solvents were distilled under reduced pressure and dried with 4A molecular sieves to reduce the water content of the solvent to below 30 ppm.
[0026] Lithium salt needs to be added in portions so that the concentration of the prepared electrolyte is 1 to 3 mol / L.
[0027] Embodiment 1
[0028] A method for manufacturing an electrolyte for an ultra-low temperature lithium-ion battery comprises the following steps:
[0029] Taking the order of adding mixed solvent, lithium salt and additive as an example, the following operations are performed:
[0030] In a glove box filled with argon (H2O≤0.01ppm, O2≤0.01ppm), 295.5g of propylene glycol carbonate (PC) and 197g of dipropylene glycol dimethyl ether (DMM) were weighed respectively, put into a beaker and stirred for 30min, and mixed evenly to obtain solvent A1; then 85g of lithium hexafluorophosphate was slowly added and stirred for 4h to completely dissolve to form a mixed solution B1, and finally 22.5g of lithium difluorophosphate was added and stirred for 60min to obtain an ultra-low temperature electrolyte L1 with a lithium salt concentration of 1 mol / L.
[0031] Embodiment 2
[0032] Taking the order of adding mixed solvent, additives, and lithium salt as an example, the following operations are performed:
[0033] In a glove box filled with argon (H2O≤0.01ppm, O2≤0.01ppm), weigh 295.5g of propylene glycol carbonate (PC) and 197g of dipropylene glycol dimethyl ether (DMM), put them into a beaker and stir for 30min, mix them evenly to obtain a mixed solvent A2; then add 22.5g of lithium difluorophosphate and stir for 60min to obtain a mixed solution B2, and finally slowly add 85g of lithium hexafluorophosphate and stir for 4h. After complete dissolution, an ultra-low temperature electrolyte L2 with a lithium salt concentration of 1 mol / L is obtained.
[0034] Embodiment 3
[0035] Taking the order of adding low melting point cyclic carbonate solvent, additive, low melting point chain ether and lithium salt as an example, the following operation is performed:
[0036] In a glove box filled with argon (H2O≤0.01ppm, O2≤0.01ppm), weigh 295.5g of propylene glycol carbonate (PC) into a beaker, then add 22.5g of lithium difluorophosphate and stir for 60min to obtain solution A3, add 197g of dipropylene glycol dimethyl ether (DMM) and stir for 30min to obtain solution B3, finally slowly add 85g of lithium hexafluorophosphate and stir for 4h to completely dissolve to obtain an ultra-low temperature electrolyte L3 with a lithium salt concentration of 1 mol / L.
[0037] Embodiment 4
[0038] Taking the order of adding mixed solvent, lithium salt and additive as an example, the following operations are performed:
[0039] In a glove box filled with argon (H2O≤0.01ppm, O2≤0.01ppm), 238.1g of propylene glycol carbonate (PC) and 79.4g of dipropylene glycol dimethyl ether (DMM) were weighed respectively, put into a beaker and stirred for 30min, and mixed evenly to obtain solvent A4; then 160g of lithium hexafluorophosphate was slowly added and stirred for 4h to completely dissolve to form a mixed solution B4, and finally 22.5g of lithium difluorophosphate was added and stirred for 60min to obtain an ultra-low temperature electrolyte L4 with a lithium salt concentration of 2mol / L.
[0040] Embodiment 5
[0041] Taking the order of adding mixed solvent, additives, and lithium salt as an example, the following operations are performed:
[0042] In a glove box filled with argon (H2O≤0.01ppm, O2≤0.01ppm), 238.1g of propylene glycol carbonate (PC) and 79.4g of dipropylene glycol dimethyl ether (DMM) were weighed respectively, put into a beaker and stirred for 30min, and mixed evenly to obtain a mixed solvent A5; then 22.5g of lithium difluorophosphate was added and stirred for 60min to obtain a mixed solution B5, and finally 160g of lithium hexafluorophosphate was slowly added and stirred for 4h. After complete dissolution, an ultra-low temperature electrolyte L5 with a lithium salt concentration of 2mol / L was obtained.
[0043] Embodiment 6
[0044] Taking the order of adding low melting point cyclic carbonate solvent, additive, low melting point chain ether and lithium salt as an example, the following operation is performed:
[0045] In a glove box filled with argon (H2O≤0.01ppm, O2≤0.01ppm), weigh 238.1g of propylene glycol carbonate (PC) into a beaker, then add 22.5g of lithium difluorophosphate and stir for 60min to obtain solution A6, add 79.4g of dipropylene glycol dimethyl ether (DMM) and stir for 30min to obtain solution B6, finally slowly add 160g of lithium hexafluorophosphate and stir for 4h to completely dissolve to obtain ultra-low temperature electrolyte L6 with a lithium salt concentration of 2mol / L.
[0046] Embodiment 7
[0047] Taking the order of adding mixed solvent, lithium salt and additive as an example, the following operations are performed:
[0048] In a glove box filled with argon (H2O≤0.01ppm, O2≤0.01ppm), weigh 218.25g of propylene glycol carbonate (PC) and 24.25g of dipropylene glycol dimethyl ether (DMM), put them into a beaker and stir for 30min, mix them evenly to obtain solvent A7; then slowly add 225g of lithium hexafluorophosphate, stir for 4h, and completely dissolve to form a mixed solution B7, finally add 22.5g of lithium difluorophosphate and stir for 60min to obtain an ultra-low temperature electrolyte L7 with a lithium salt concentration of 3mol / L.
[0049] Embodiment 8
[0050] Taking the order of adding mixed solvent, additives, and lithium salt as an example, the following operations are performed:
[0051] In a glove box filled with argon (H2O≤0.01ppm, O2≤0.01ppm), weigh 218.25g of propylene glycol carbonate (PC) and 24.25g of dipropylene glycol dimethyl ether (DMM), put them into a beaker and stir for 30min, mix them evenly to obtain a mixed solvent A8; then add 22.5g of lithium difluorophosphate and stir for 60min to obtain a mixed solution B8, and finally slowly add 225g of lithium hexafluorophosphate and stir for 4h. After complete dissolution, an ultra-low temperature electrolyte L8 with a lithium salt concentration of 2 mol / L is obtained.
[0052] Embodiment 9
[0053] Taking the order of adding low melting point cyclic carbonate solvent, additive, low melting point chain ether and lithium salt as an example, the following operation is performed:
[0054] In a glove box filled with argon (H2O≤0.01ppm, O2≤0.01ppm), weigh 218.25g of propylene glycol carbonate (PC) into a beaker, then add 22.5g of lithium difluorophosphate and stir for 60min to obtain solution A9, add 24.25g of dipropylene glycol dimethyl ether (DMM) and stir for 30min to obtain solution B9, finally slowly add 225g of lithium hexafluorophosphate and stir for 4h to completely dissolve to obtain ultra-low temperature electrolyte L9 with a lithium salt concentration of 2mol / L.
[0055] Comparative Example 1
[0056] Taking ethyl carbonate (EC) and dimethyl carbonate (DMC) as a mixed solvent and lithium hexafluorophosphate (LiPF6) as a traditional electrolyte as an example, the following operations are performed:
[0057] In a glove box filled with argon (H2O≤0.01ppm, O2≤0.01ppm), 120g of ethyl carbonate (EC) and 260g of dimethyl carbonate (DMC) were weighed and placed in a beaker and stirred for 30 minutes to obtain solvent A10. Then, 75g of lithium hexafluorophosphate was slowly added and stirred for 4 hours to obtain ultra-low temperature electrolyte L10 with a lithium salt concentration of 1 mol / L.
[0058] The above electrolyte was combined with the low-temperature lithium iron phosphate positive electrode material, hard carbon negative electrode material and traditional PP separator developed by our research group to make 14500 cylindrical batteries, and the low-temperature electrochemical performance was tested.
[0059] Experimental data analysis and discussion
[0060] It can be seen from Table 1 that all nine groups of embodiments can be discharged at a low temperature of -60°C, especially the three groups of embodiments (Example 4, Example 5, Example 6) with PC:DMM=3:1, which still maintain a discharge capacity retention rate of about 50% at a low temperature of -60°C. It is worth noting that the 14500 cylindrical battery made with the low-temperature lithium iron phosphate positive electrode material developed by the present invention still has a capacity retention rate of about 70% after 300 cycles at a low temperature of -40°C. However, after using the electrolyte of the traditional ratio in Comparative Example 1, it can no longer be discharged at a low temperature of -40°C. By comparing the three groups of data with the same formula but different addition orders, it can be found that the addition order has a certain influence on the performance of the electrolyte, and the best effect is achieved by adding the mixed solvent, lithium salt, and additive in the order of mixing.
[0061] Example 4 has the best low-temperature electrochemical performance and low-temperature conductivity. It still has a discharge capacity of 254.8 mAh in an ultra-low temperature environment of -60°C, and still has a capacity retention rate of 72.3% after 300 cycles under an ultra-low temperature condition of -40°C.
[0062] Table 1: 14500 battery low temperature performance and electrolyte low temperature conductivity test record
[0063]
[0064] The embodiments described herein are only some embodiments of the present invention, not all. According to the explanation and guidance of the above specification, those skilled in the art can change, improve, replace, etc. the implementation methods based on the present invention and the embodiments, but all other embodiments obtained without making innovative research are within the protection scope of the present invention.
Claims
1. A method for manufacturing an electrolyte for an ultra-low temperature lithium-ion battery, characterized in that: Calculated according to the mass ratio in the electrolyte, the electrolyte includes 63.5% solvent, 32% lithium salt and 4.5% additive; the solvent is a mixed solvent composed of propylene glycol carbonate and dipropylene glycol dimethyl ether, and the mass ratios of propylene glycol carbonate and dipropylene glycol dimethyl ether in the mixed solvent are 75% and 25% respectively; the lithium salt is lithium hexafluorophosphate LiPF6; the additive is a lithium salt type film-forming aid lithium difluorophosphate LiPO2F2; The method comprises the following steps: mixing and stirring the above electrolyte components in any one of the following addition orders: Sequence 1: mixed solvent, lithium salt, additive; Sequence 2: mixed solvent, additive, lithium salt; Sequence three: propylene glycol carbonate, additives, dipropylene glycol dimethyl ether, lithium salt; Each component in the above sequence needs to be stirred for 30 minutes to 240 minutes after being added.
2. The method for manufacturing an electrolyte for an ultra-low temperature lithium-ion battery according to claim 1, characterized in that: First, propylene glycol carbonate and dipropylene glycol dimethyl ether are mixed and stirred to form a mixed solvent A, and then lithium salt is added to the mixed solvent A and stirred until the lithium salt is completely dissolved to form a mixed solution B, and finally the additive is added.
3. The method for manufacturing an electrolyte for an ultra-low temperature lithium-ion battery according to claim 1, characterized in that: Propylene glycol carbonate and dipropylene glycol dimethyl ether are both subjected to vacuum distillation and dried with a 4A grade molecular sieve to reduce the water content in the solvent to below 30 ppm.
Citation Information
Patent Citations
An ultra-low temperature lithium-ion battery electrolyte
CN113036223B
Low-temperature electrolyte and lithium ion battery thereof
CN113328141A
Novel electrolyte system of lithium ion battery
CN103367806A
Superlow-temperature lithium ion battery electrolyte and lithium ion battery using same
CN108511800A
Electrolyte and preparation method thereof, lithium ion battery and electric vehicle
CN112993408A