A lithium ion battery antistatic glue-coated diaphragm and preparation method thereof and a lithium ion battery
By applying an antistatic coating layer on the lithium-ion battery separator, which contains antistatic agents, polymer binders and ceramic particles, the problem of electrostatic adsorption of dust and hardness is solved, reducing static electricity and improving production efficiency, while maintaining battery life. performance.
Patent Information
- Application Number
- CN202111594544.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-23
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-12-23
AI Technical Summary
The glued separators of lithium-ion batteries are prone to electrostatic effects during the manufacturing process, adsorbing air dust and causing short circuits, affecting battery performance and production efficiency. Existing solutions such as static removal rods and antistatic agents have limitations or performance impacts.
Design an antistatic glue-coated separator for lithium-ion batteries. The glue layer contains antistatic agents, polymer binders and ceramic particles. By forming an antistatic glue layer on the separator substrate, it reduces the electrostatic effect and improves the hardness of the separator. .
It effectively reduces the static electricity of the separator to below 200V, prevents dust adsorption, improves lamination efficiency, and maintains battery hardness during the thermal lamination process without affecting other battery performance.
Smart Images

Figure CN114388982B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of secondary batteries, and specifically relates to an antistatic glue-coated diaphragm for a lithium ion battery and a preparation method thereof, and a lithium ion battery. Background Art
[0002] Lithium-ion batteries are currently the most popular new energy storage devices. According to the different packaging methods of lithium-ion batteries, they can be divided into soft-pack lithium-ion batteries and metal-shell lithium-ion batteries. Among them, soft-pack lithium-ion batteries use aluminum-plastic film as packaging materials. As the size of batteries develops towards longer and narrower trends, soft-pack lithium-ion batteries are increasingly unfavorable for subsequent group assembly. In the process of grabbing and translating batteries by the manipulator, the battery is prone to fall and collide, causing safety accidents. Therefore, special processes are required to improve the hardness of the battery. The thermal composite process uses a diaphragm with glue to stick the positive and negative electrodes and the diaphragm together under high temperature and high pressure conditions, making the core package a whole, which can effectively improve the hardness of the battery. However, this diaphragm with glue has a large electrostatic effect, which will absorb dust in the air during the battery manufacturing process, causing battery short circuits and affecting battery performance. In addition, during the lamination or winding process, the diaphragm will be adsorbed on the equipment due to the electrostatic effect, which not only affects the battery alignment, but also affects the production efficiency. Therefore, it is particularly important to effectively remove the static electricity of the diaphragm for battery production.
[0003] One solution is to start with the equipment, such as setting up a static-eliminating rod or an ion blower in front of the stacking table. Both methods can effectively remove static electricity from the diaphragm, but they need to be placed near the stacking table, which requires a certain amount of space and location. In addition, static-eliminating rods and ion blowers can only remove static electricity in a local area. After the static-eliminating diaphragm enters the stacking table, it will generate new static electricity as it moves on the rollers, and the effect is average.
[0004] Another solution is to start with the diaphragm, for example, adding antistatic agent polyether ester amide monomer during the base film processing. This method has a significant antistatic effect and is more durable. However, the antistatic agent has poor compatibility with the masterbatch and is easy to precipitate, which will affect the performance of the base film and has a high cost. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention proposes an antistatic coated diaphragm for lithium-ion batteries. The static electricity of the diaphragm can be reduced to below 200V, which can effectively alleviate the short circuit caused by the diaphragm's electrostatic adsorption of dust, and alleviate the adsorption of the static diaphragm on the equipment rollers and the stacking table, thereby effectively improving the stacking efficiency.
[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides an antistatic coated diaphragm for lithium-ion batteries, wherein the diaphragm comprises a diaphragm substrate and an antistatic coating layer coated on the diaphragm substrate; the antistatic coating layer contains an antistatic agent, a polymer binder and ceramic particles.
[0007] The second aspect of the present invention provides a method for preparing an antistatic coated diaphragm for lithium ion batteries, comprising: forming an antistatic coated layer on the surface of a diaphragm substrate; the antistatic coated layer contains an antistatic agent, a polymer binder and ceramic particles.
[0008] A third aspect of the present invention provides a lithium ion battery, which comprises positive and negative electrodes and a separator, wherein the separator is the antistatic glue-coated separator for the lithium ion battery.
[0009] The antistatic glue-coated diaphragm for lithium-ion batteries designed by the present invention has the following advantages:
[0010] 1) The antistatic coated lithium ion battery diaphragm of the present invention can reduce static electricity to below 200V, effectively alleviate the short circuit caused by the diaphragm due to static adsorption of dust, alleviate the adsorption of the static diaphragm on the equipment roller and the stacking table, and effectively improve the stacking efficiency.
[0011] 2) The antistatic coated lithium ion battery diaphragm of the present invention has no effect on other properties of the battery except for its obvious antistatic effect. The battery assembled with the diaphragm can combine the positive and negative electrodes with the diaphragm through a thermal composite process, so that the battery maintains a certain hardness.
[0012] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present invention.
[0014] Figure 1 Schematic diagram of the cross-section and planar structure of the double-coated diaphragm.
[0015] 1-diaphragm substrate, 2-mixed coating layer of polymer binder and ceramic particles, 3-antistatic agent coating DETAILED DESCRIPTION
[0016] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein.
[0017] The invention provides an antistatic glue-coated diaphragm for lithium ion batteries. The diaphragm comprises a diaphragm substrate and an antistatic glue-coated layer coated on the diaphragm substrate. The antistatic glue-coated layer contains an antistatic agent, a polymer binder and ceramic particles.
[0018] Preferably, the antistatic coating layer is a single coating or a double coating.
[0019] When the antistatic coating layer is a double coating layer, the mixed coating layer including the binder and the ceramic particles is disposed near the diaphragm substrate, and the antistatic agent coating layer is disposed on the mixed coating layer. Figure 1 shown.
[0020] According to the present invention, the antistatic coating layer is coated on one side or both sides of the diaphragm substrate.
[0021] Specifically, the single coating layer and the mixed coating layer of the binder and ceramic particles are coated by any one of roller coating, dip coating and gap coating. The antistatic agent coating is coated by any one of gravure coating, spray coating and gap coating.
[0022] According to a preferred embodiment of the present invention, the thickness of the antistatic coating layer is 1 to 7 μm, preferably 2 to 4 μm.
[0023] According to a preferred embodiment of the present invention, when the antistatic coating layer is a double coating, the thickness of the mixed coating layer of the binder and ceramic particles is 0.8-5 μm, preferably 1.5-3 μm; the thickness of the antistatic agent coating is 0.2-2 μm, preferably 0.5-1 μm.
[0024] According to the present invention, the weight percentage of the antistatic agent in the antistatic coating layer is 1% to 20%, preferably 5% to 10%.
[0025] The weight percentage of the polymer binder in the antistatic coating layer is 10% to 50%, preferably 20% to 30%.
[0026] The weight percentage of the ceramic particles in the antistatic coating layer is 50% to 90%, preferably 70% to 75%.
[0027] Optionally, the antistatic agent includes a cationic antistatic agent and a nonionic antistatic agent.
[0028] The cationic antistatic agent can be selected from at least one of ammonium salt type, quaternary ammonium salt type, heterocyclic type, and pyrochlore salt type antistatic agents.
[0029] The nonionic antistatic agent may be selected from at least one of ethoxylated aliphatic alkylamines, ethoxylated alkylamines, and ethoxylated alkyl acid ammoniums.
[0030] According to the present invention, the polymer binder may be selected from at least one of polyacrylonitrile, polyvinylidene fluoride and polymethyl methacrylate, preferably polyvinylidene fluoride.
[0031] The ceramic particles may be selected from at least one of aluminum oxide, magnesium hydroxide, layered composite hydroxides, layered composite oxides, boehmite, silicon dioxide, and silicon carbide.
[0032] Preferably, the diaphragm substrate is at least one of PE, PP, cellulose, PET, PI, non-woven fabric and electrospinning.
[0033] The thickness of the diaphragm substrate may be 5 to 15 μm, preferably 7 to 12 μm; the porosity may be 10% to 50%, preferably 35% to 45%.
[0034] The present invention also provides a method for preparing an antistatic coated diaphragm for lithium ion batteries, comprising: forming an antistatic coated layer on the surface of a diaphragm substrate; the antistatic coated layer contains an antistatic agent, a polymer binder and ceramic particles.
[0035] Specifically, the preparation method is selected from any one of the following methods:
[0036] Method 1:
[0037] (1) adding a binder and ceramic particles into an organic solvent to prepare a slurry of a mixed coating layer of a polymer binder and ceramic particles, and applying the slurry on the surface of a diaphragm substrate to form a mixed coating layer;
[0038] (2) coating the antistatic agent coating slurry on the mixed adhesive layer to prepare the lithium ion battery antistatic adhesive coating diaphragm;
[0039] Method 2:
[0040] (1) adding an antistatic agent, a polymer binder and ceramic particles into an organic solvent to prepare a mixed slurry;
[0041] (2) The mixed slurry is coated on the surface of a diaphragm substrate to prepare the antistatic coated diaphragm for lithium-ion batteries.
[0042] The organic solvent is preferably N-methylpyrrolidone (NMP).
[0043] The present invention also provides a lithium ion battery, which comprises positive and negative electrodes and a diaphragm, wherein the diaphragm is the antistatic glue-coated diaphragm of the lithium ion battery.
[0044] The present invention is described in more detail below through examples and comparative examples.
[0045] Comparative Example
[0046] Polyvinylidene fluoride and aluminum oxide are added to an organic solvent N-methylpyrrolidone (NMP) in a mass ratio of 2.5:7.5 to prepare a coating liquid, which is then coated on a 9 μm thick polyethylene base film by roller coating to form a diaphragm with a coating layer, and the thickness of the coating layer is controlled to be about 3 μm.
[0047] Example 1
[0048] Polyvinylidene fluoride, aluminum oxide, and hexadecyltrimethylammonium chloride are added to an organic solvent NMP in a mass ratio of 2.5:7:0.5 to prepare a coating liquid, which is applied to a 9 μm thick polyethylene base film by roller coating to form a diaphragm with a coating layer, and the thickness of the coating layer is controlled to be about 3 μm.
[0049] Example 2
[0050] Polyvinylidene fluoride, aluminum oxide, and ethoxylaurylamide are added to an organic solvent NMP in a mass ratio of 2.5:7:0.5 to prepare a coating liquid, and the coating liquid is applied to a 9 μm thick polyethylene base film by roller coating to form a diaphragm with a coating layer, and the thickness of the coating layer is controlled to be about 3 μm.
[0051] Example 3
[0052] Polyvinylidene fluoride and aluminum oxide were added to an organic solvent NMP at a mass ratio of 2.5:7.5 to prepare a coating solution, which was then coated on a 9 μm thick polyethylene base film by roller coating, and the coating layer thickness was controlled to be about 3 μm.
[0053] Hexadecyl trimethyl ammonium chloride is added to NMP to prepare a coating solution, and the mass ratio of hexadecyl trimethyl ammonium chloride to aluminum oxide is 0.5:7. The coating solution is coated on the base film coated with the polymer binder and ceramic particles by gravure coating, and the thickness of the coating layer is controlled to be about 1 μm.
[0054] Example 4
[0055] Polyvinylidene fluoride and aluminum oxide were added to an organic solvent NMP at a mass ratio of 2.5:7.5 to prepare a coating solution, which was then coated on a 9 μm thick polyethylene base film by roller coating, and the coating layer thickness was controlled to be about 3 μm.
[0056] Hexadecyl trimethyl ammonium chloride is added to NMP to prepare a coating liquid, and the mass ratio of hexadecyl trimethyl ammonium chloride to aluminum oxide is 0.5:7. The coating liquid is applied to the base film coated with the polymer binder and ceramic particles by gap coating, with a coating gap of 1000 μm and a coating layer thickness of about 1 μm.
[0057] Test Example 1
[0058] The diaphragm samples prepared in the comparative example and Examples 1-4 were tested for moisture content. The test method was as follows: 3 portions of diaphragm samples weighing about 0.1 g were weighed and sealed in sample bottles. The sealed sample bottles were placed in a heating furnace at a heating temperature of 150°C. The samples were tested using a Karl Fischer moisture meter. After the test was completed, the average of the 3 moisture values was taken. The test results are shown in Table 1.
[0059] Test Example 2
[0060] The membrane samples prepared in the comparative example and Examples 1-4 were subjected to an air permeability test. The test method was: 3 membrane samples were selected to measure the average time required for 100 mL of gas to pass through. The test results are shown in Table 1.
[0061] Test Example 3
[0062] The diaphragm samples prepared in the comparative example and Examples 1-4 were tested for electrostatic values. The test method was: using a Keyence SK-H050 electrostatic meter to test the average electrostatic values of the three diaphragm samples. The test results are shown in Table 1.
[0063] Table 1 Test results of the diaphragms prepared in comparative examples and embodiments 1-4
[0064]
[0065] From the test results of moisture in Table 1, it can be seen that the moisture in the comparative example and the example is significantly different, and the moisture in the comparative example is lower. This is because the addition of the antistatic agent will absorb moisture in the air, and the moisture is basically inversely proportional to the antistatic effect. However, after adding the antistatic agent, the moisture of the diaphragm still meets the use requirements.
[0066] From the test results of air permeability in Table 1, it can be seen that the air permeability of the comparative example and the example is not much different and there is no obvious regularity, indicating that the addition of the antistatic agent will not affect the air permeability of the diaphragm.
[0067] As can be seen from Table 1, the electrostatic value of the diaphragm using the antistatic agent formula is significantly lower than that of the comparative example. From the comparison of the electrostatic value test results of Example 2 and Examples 1, 3, and 4 in Table 1, it can be clearly seen that the antistatic effect of ethoxy lauryl amide is better than that of hexadecyl trimethyl ammonium chloride. From the comparison of the electrostatic value test results of Example 1 and Examples 3 and 4 in Table 1, it can be seen that the antistatic effect of the double coating is better than that of the single coating. This is because the antistatic agent is concentrated on the surface of the diaphragm during the double coating, so the antistatic effect is more obvious. From the comparison of the electrostatic value test results of Example 3 and Example 4 in Table 1, it can be seen that the upper antistatic agent has little effect on the antistatic effect by roller coating and interval coating, and the roller coating effect is slightly better, because the roller coating antistatic agent covers the entire diaphragm.
[0068] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A lithium ion battery antistatic glue-coated diaphragm, characterized in that: The diaphragm comprises a diaphragm substrate and an antistatic coating layer coated on the diaphragm substrate; the antistatic coating layer contains an antistatic agent, a polymer binder and ceramic particles; The antistatic coating layer is a double coating; A mixed coating layer including a binder and ceramic particles is arranged near the diaphragm substrate, and an antistatic coating is arranged on the mixed coating layer; The antistatic coating layer is coated on both sides of the diaphragm substrate; The method for preparing the antistatic glue-coated diaphragm for lithium-ion batteries comprises the following steps: (1) adding a binder and ceramic particles into an organic solvent to prepare a slurry of a mixed coating layer of a polymer binder and ceramic particles, and applying the slurry on the surface of a diaphragm substrate to form a mixed coating layer; (2) coating the antistatic agent coating slurry on the mixed adhesive layer to prepare the lithium ion battery antistatic adhesive coating diaphragm; The thickness of the antistatic coating layer is 2 to 4 μm; The thickness of the mixed coating layer of the binder and ceramic particles is 1.5 to 3 μm; The thickness of the antistatic agent coating is 0.5 to 1 μm; The weight percentage of the antistatic agent in the antistatic coating layer is 5% to 10%; The weight percentage of the polymer binder in the antistatic coating layer is 20% to 30%; The weight percentage of the ceramic particles in the antistatic coating layer is 70% to 75%.
2. The antistatic glue-coated diaphragm for lithium-ion batteries according to claim 1, characterized in that: The coating method of the mixed coating layer of the binder and ceramic particles is selected from any one of roller coating, dip coating and gap coating; The coating method of the antistatic agent coating is selected from any one of gravure coating, spray coating and gap coating.
3. The antistatic glue-coated diaphragm for lithium-ion batteries according to any one of claims 1 to 2, characterized in that: The antistatic agent includes a cationic antistatic agent and a nonionic antistatic agent; The cationic antistatic agent is selected from at least one of ammonium salt type, heterocyclic type, and pyrochlore salt type antistatic agents; The nonionic antistatic agent is selected from at least one of ethoxylated alkylamines and ethoxylated alkyl ammonium acids.
4. The antistatic glue-coated diaphragm for lithium-ion batteries according to claim 3, characterized in that: The ammonium salt antistatic agent is a quaternary ammonium salt antistatic agent; The ethoxylated alkylamine is an ethoxylated aliphatic alkylamine.
5. The antistatic glue-coated diaphragm for lithium-ion batteries according to any one of claims 1 to 2, characterized in that: The polymer binder is selected from at least one of polyacrylonitrile, polyvinylidene fluoride and polymethyl methacrylate; The ceramic particles are selected from at least one of layered composite hydroxides, layered composite oxides, boehmite and silicon carbide.
6. The antistatic glue-coated diaphragm for lithium-ion batteries according to claim 5, characterized in that: The layered composite hydroxide is composed of magnesium hydroxide; The components of the layered composite oxide are silicon dioxide and aluminum oxide.
7. The antistatic glue-coated diaphragm for lithium-ion batteries according to claim 5, characterized in that: The polymer binder is polyvinylidene fluoride.
8. The antistatic glue-coated diaphragm for lithium-ion batteries according to any one of claims 1 to 2, characterized in that: The diaphragm substrate is at least one of PE, PP, cellulose, PET, PI, non-woven fabric and electrospinning; The thickness of the diaphragm substrate is 5 to 15 μm, and the porosity is 10% to 50%.
9. The antistatic glue-coated diaphragm for lithium-ion batteries according to claim 8, characterized in that: The thickness of the diaphragm substrate is 7-12 μm, and the porosity is 35% to 45%.
10. A lithium ion battery, comprising positive and negative electrodes and a separator, wherein the separator is the antistatic coated separator for lithium ion batteries according to any one of claims 1 to 9.
Citation Information
Patent Citations
Membrane and secondary battery
CN106299222A
Battery separator, preparation method thereof and lithium ion battery
CN112117421A