Aging method for composite insulator core rod
Through the high and low temperature cycle aging test, the problems of long aging test time of composite insulators and insufficient consideration of the extreme cold environment were solved, the experimental time was shortened, the performance changes of the composite insulator core rod in the extremely cold environment were explored, and the research efficiency and safety were improved. sex.
Patent Information
- Application Number
- CN202111292751.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-03
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-11-03
AI Technical Summary
Existing aging test methods for composite insulators suffer from long aging times, high economic costs, and failure to fully consider the impact of extreme cold environments on the performance of core rod materials, especially in the extremely cold areas of eastern Mongolia, resulting in insufficient research and potential safety hazards.
The high and low temperature cycle aging method is adopted, and the temperature cycle between -60°C and 140°C is set to alternate, and a 1440-hour aging test is conducted to test the changes in the hydrophobic performance, electrical performance and mechanical properties of the mandrel to simulate the extremely cold environment of Eastern Mongolia. Effect on composite insulator core rod.
It significantly shortens the aging test time, simplifies the experimental procedures, satisfies the equivalence between the aging experiment and the simulated operating environment, explores the performance degradation rules of composite insulator core rods in extremely cold environments, and makes up for the core rod performance in existing tests. The lack of changes improves research efficiency and safety.
Smart Images

Figure CN114400118B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite insulator core rods, in particular to an aging method for composite insulator core rods. Background Art
[0002] Composite insulators are mainly composed of core rods and silicone rubber umbrellas. They have the advantages of light weight, high pollution flashover voltage, strong hydrophobicity, etc., which play an important role in reducing pollution flashover and maintaining the safe operation of power grids. They have been widely used in transmission lines at home and abroad. Due to the complex operating environment faced by composite insulators, many environmental factors such as light conditions, temperature and humidity conditions, rainfall in the area, and types of pollutants will affect the operating performance of composite insulators. The environmental factor aging test of composite insulators has become the focus of researchers.
[0003] At present, the artificial accelerated aging test methods include: (1) Professor Li Qingfeng conducted a 5000h artificial accelerated aging test on DC composite insulators in accordance with the aging procedure of standard IEC 61109, and designed an artificial aging test including DC stress, sunshine, high temperature, high humidity, heavy pollution and other factors to study the influence on the aging performance of composite insulators. However, the disadvantage of this aging method is that the aging time is too long, the research economy is poor, and the cost is high. (2) Based on the IEC 61109 multi-factor test method, the team of Professor Liang Xidong of Tsinghua University added diatomaceous earth pollution components and adjusted the time arrangement of aging factors, and proposed the "Tsinghua 5000h multi-factor test method" for composite insulators. This method simulates the hydrophobic migration and hydrophobic recovery of silicone rubber materials of composite insulators under multi-factor aging and the hardening of sheds through the accelerated aging under the action of artificial multi-factors, and reproduces the accelerated failure process of composite insulators. However, this method focuses on simulating the long-term operating reliability of composite insulator silicone rubber materials in a large inland area. The temperature of the 5000h multi-factor aging method is set at 50°C, which fails to take into account the temperature factor of -60°C in the extremely cold weather in eastern Inner Mongolia. In addition, the artificial multi-factor aging tests conducted by the above two methods examine the impact of environmental factors on the composite insulator shed and sheath materials, and fail to reflect the performance changes of the composite insulator core rod materials in an artificial accelerated aging environment.
[0004] However, the above two methods have the following defects and shortcomings:
[0005] (1) Professor Li Qingfeng used a 5000h multi-factor artificial accelerated aging test method to evaluate the long-term performance of composite insulators. The disadvantage of this aging method is that the aging time is too long, the research economy is poor, and the cost is high.
[0006] (2) The shortcoming of the 5000h multi-factor aging method proposed by Professor Liang Xidong's team at Tsinghua University is that this method focuses on simulating the long-term operating reliability of composite insulator silicone rubber materials in large inland areas. The temperature of the 5000h multi-factor aging method is set at 50℃, which fails to take into account the temperature factor of the extremely cold weather in eastern Inner Mongolia, where the lowest temperature reaches -60℃.
[0007] (3) The current artificial multi-factor aging test examines the impact of environmental factors on the shed and sheath materials of composite insulators, but fails to reflect the performance changes of the composite insulator core rod materials in an artificial accelerated aging environment.
[0008] The eastern part of Inner Mongolia is located in the northeast of Inner Mongolia. Genhe City in the eastern part of Inner Mongolia is known as the "Cold Pole of China". The average annual temperature is only -5.3℃, the extreme temperature is as low as -58℃, and the annual freezing period is more than 210 days. Such severe weather conditions seriously affect the operating safety of composite insulators.
[0009] In order to effectively simulate the influence of the extreme cold environment in eastern Inner Mongolia on the performance of composite insulator core rods, the present invention proposes an aging method for composite insulator core rods.
[0010] After searching, no prior art documents identical or similar to the present invention were found. Summary of the invention
[0011] The purpose of the present invention is to overcome the shortcomings of the prior art and to propose an aging method for a composite insulator core rod, which can explore the performance degradation of the composite insulator core rod after high and low temperature cycle aging.
[0012] The present invention solves the practical problem by adopting the following technical solutions:
[0013] An aging method for a composite insulator core rod comprises the following steps:
[0014] Step 1, preparing high and low temperature cycle aging composite insulator core rod samples;
[0015] Step 2, grouping the composite insulator core rod samples manufactured in step 1 and performing a high and low temperature cycle aging test;
[0016] Step 3, after the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out to test the change of the hydrophobicity of the core rod samples;
[0017] Step 4: After the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out to test the changes in the electrical properties of the core rod samples;
[0018] Step 5: After the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out to test the mechanical changes of the core rod samples.
[0019] Moreover, the specific method of step 1 is:
[0020] A composite insulator core rod sample with a diameter of 25 mm and a length of 30 mm was selected to detect the changes in the hydrophobicity and electrical properties of the core rod after aging; a composite insulator core rod with a diameter of 25 mm ± 0.1 mm was selected and cut into a sample of 310 mm in length to detect the changes in the mechanical properties of the core rod after aging;
[0021] Moreover, the specific method of step 2 is:
[0022] The temperature points of the high and low temperature cycle aging scheme are set to alternate between extremely low temperatures of -60℃±3℃ and high temperatures of 140℃±3℃ to simulate the impact of temperature changes on the performance of composite insulator core rods. The high and low temperature cycle aging time is 1440h in total, with each 24h as a cycle, for a total of 60 cycle aging cycles; within one aging cycle, 0-12h is used for high temperature 140℃ aging, and 12-24h is used for -60℃ aging.
[0023] Moreover, the specific steps of step 3 include:
[0024] (1) After the high and low temperature cycle aging test is completed, take out the sample for water contact angle measurement: first wash it with distilled water, then dry it naturally, and finally dip anhydrous ethanol with a dry cotton ball and apply it on the side wall of the sample to ensure the cleanliness of the sample. After the anhydrous ethanol on the side wall is completely evaporated, start the hydrophobicity test;
[0025] (2) Each time, 5 μL of deionized water was dropped onto the side wall of the mandrel sample. After the water drop was stationary on the side wall, an image was quickly taken in the hydrophobicity measurement software. Multiple locations of each sample were selected for measurement.
[0026] (3) Obtain a graph showing the relationship between the hydrophobicity of the core rod and the aging time.
[0027] Moreover, the specific steps of step 4 include:
[0028] (1) After the high and low temperature cycle aging test is completed, samples with different aging times are taken out for the core rod power frequency withstand voltage test. When flashover occurs on the sample surface, the surface flashover voltage of each group of multiple samples is recorded;
[0029] (2) After the high and low temperature cycle aging test is completed, samples with different aging times are taken out for the core rod DC withstand voltage test. When flashover occurs on the sample surface, the surface flashover voltage of each group of multiple samples is recorded;
[0030] (3) Take out samples with different aging times to conduct core rod lightning impulse flashover test to determine the lightning impulse flashover voltage;
[0031] (4) Draw a graph showing the relationship between the core rod flashover voltage and aging time;
[0032] (5) Samples with different aging times are taken out, the core rod volume resistance is measured, and a relationship diagram between the core rod volume resistance and the aging time is obtained.
[0033] Moreover, the specific method of step 5 is:
[0034] After the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out for maximum load and tensile strength tests, and a relationship diagram of the maximum load and tensile strength of the core rod sample with aging time is obtained.
[0035] Advantages and beneficial effects of the present invention:
[0036] 1. The present invention places the composite insulator core rod in a constant temperature test chamber for 1440h (60 days) of high and low temperature cycle aging, selects the hydrophobicity, electrical properties, and mechanical properties of the composite insulator core rod after different aging times as the research objects, and explores the performance degradation law of the composite insulator core rod after high and low temperature cycle aging. In addition, the present invention fully considers the influence of the natural environment of the extremely cold temperature conditions in the extremely cold area of eastern Mongolia on the composite insulator core rod, and sets the environmental factor of -60℃, which is more in line with the special extremely cold climate environment in the extremely cold area of eastern Mongolia.
[0037] 2. Compared with the 5000h artificial accelerated aging test scheme, the aging time of the scheme adopted by the present invention is 1440h, and the electrical, mechanical and hydrophobic properties of the composite insulator core rod are significantly deteriorated. On the premise of meeting the equivalence of the aging experiment with the simulated operating environment and the repeatability of the aging experiment, the aging experiment time is greatly shortened and the experimental procedure is simplified.
[0038] 3. The research object of the present invention is the performance change of the composite insulator core rod in the artificial accelerated aging test, which makes up for the shortcomings of the core rod performance change in the composite insulator core aging test research. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a sample diagram of the hydrophobicity and electrical performance test of the core rod of the present invention;
[0040] Figure 2 This is a sample diagram of the mandrel mechanical property test of the present invention;
[0041] Figure 3 Schematic diagram of static contact angle of mandrel at different aging times of the present invention;
[0042] Figure 4 is a graph showing the relationship between the static contact angle of the mandrel of the present invention and the aging time;
[0043] Figure 5This is a diagram of a composite insulator core rod withstand voltage test device of the present invention;
[0044] Figure 6 is a graph showing the relationship between the core rod flashover voltage and the aging time of the present invention;
[0045] Figure 7 It is a schematic diagram of a device for measuring the volume resistance of a mandrel by a voltammetric method of the present invention;
[0046] Figure 8 is a graph showing the relationship between the core rod volume resistance and the aging time of the present invention;
[0047] Fig. 9 is a graph showing the relationship between the maximum load and the aging time of the mandrel sample of the present invention;
[0048] Fig.10 It is a curve diagram showing the relationship between the tensile strength of the core rod sample of the present invention and the aging time. DETAILED DESCRIPTION
[0049] The embodiments of the present invention are further described in detail below with reference to the accompanying drawings:
[0050] An aging method for a composite insulator core rod comprises the following steps:
[0051] Step 1, preparing high and low temperature cycle aging composite insulator core rod samples;
[0052] The specific method of step 1 is:
[0053] A composite insulator core rod sample with a diameter of 25 mm and a length of 30 mm was selected to detect the changes in the hydrophobicity and electrical properties of the core rod after aging; a composite insulator core rod with a diameter of 25 mm ± 0.1 mm was selected and cut into a sample of 310 mm in length to detect the changes in the mechanical properties of the core rod after aging;
[0054] In this embodiment, a composite insulator core rod is selected as the research object to study the degradation law of the core rod's hydrophobicity and electrical performance after high and low temperature cycle aging. A total of 119 core rod cylindrical samples with a diameter of 25 mm and a length of 30 mm are selected, such as Figure 1 As shown, Figure 1 This is a sample diagram of the core rod hydrophobicity and electrical performance test.
[0055] In order to study the effect of high and low temperature cycle aging on the mechanical properties of the core rod, a core rod with a diameter of 25 mm ± 0.1 mm was selected and cut into a specimen with a length of 310 mm. According to GB / T13096, the diameter of the middle part of the specimen was turned to 5.0 mm ± 0.5 mm using a lathe. Figure 2 Shown. Total 7 Figure 2 sample.
[0056] The samples were divided into seven groups, each containing 17 Figure 1 Sample, one Figure 2 sample. Figure 1 The samples are used to detect the changes in the hydrophobicity and electrical properties of the core rod after aging; Figure 2 The samples are used to detect the changes in the mechanical properties of the core rod after aging. The grouped samples are named sample group 1 to group 7. The seven groups of samples are subjected to high and low temperature cycle aging tests in step 2.
[0057] Step 2: Group the composite insulator core rod samples manufactured in step 1 and perform a high and low temperature cycle aging test.
[0058] The specific method of step 2 is:
[0059] The temperature points of the high and low temperature cycle aging scheme are set to alternate between extremely low temperatures of -60℃±3℃ and high temperatures of 140℃±3℃ to simulate the impact of temperature changes on the performance of composite insulator core rods. The high and low temperature cycle aging time is 1440h in total, with each 24h as a cycle, for a total of 60 cycle aging cycles; within one aging cycle, 0-12h is used for high temperature 140℃ aging, and 12-24h is used for -60℃ aging.
[0060] In this embodiment, sample groups 1 to 6 are placed in an aging box for high and low temperature cycle aging, and sample group 7 is used as a control group and is not aged.
[0061] After aging to the 10th cycle (aging for 10 days), sample group 1 was taken out.
[0062] After aging to the 20th cycle (aging for 20 days), sample group 2 was taken out.
[0063] After aging to the 30th cycle (aging for 30 days), sample group 3 was taken out.
[0064] After aging to the 40th cycle (aging for 40 days), sample group 4 was taken out.
[0065] After aging to the 50th cycle (aging for 50 days), sample group 5 was taken out.
[0066] After aging to the 60th cycle (aging for 60 days), sample group 6 was taken out.
[0067] The aging test is ended in step 2. After the sample is taken out, the performance change of the core rod is tested.
[0068] Step 3, after the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out to test the change of the hydrophobicity of the core rod samples;
[0069] The specific steps of step 3 include:
[0070] (1) After the high and low temperature cycle aging test is completed, take out the sample for water contact angle measurement: first wash it with distilled water, then dry it naturally, and finally dip anhydrous ethanol with a dry cotton ball and apply it on the side wall of the sample to ensure the cleanliness of the sample. After the anhydrous ethanol on the side wall is completely evaporated, start the hydrophobicity test;
[0071] In this example, one sample was taken from each of the seven sample groups. Figure 1 The sample shown in the figure is subjected to water contact angle measurement. First, it is cleaned with distilled water, then naturally dried, and finally, anhydrous ethanol is dipped into a dry cotton ball and applied to the side wall of the sample to ensure the cleanliness of the sample. After the anhydrous ethanol on the side wall is completely evaporated, the hydrophobicity test is started.
[0072] (2) Each time, a volume of 5 μL of deionized water was dropped onto the side wall surface of the core rod sample. After the water drop was stationary on the side wall, an image was quickly captured in the hydrophobicity measurement software. Multiple locations were selected for each sample for measurement.
[0073] In this embodiment, 5 μL of deionized water was dropped onto the side wall surface of the core rod sample each time. After the water drop was stationary on the side wall, an image was quickly taken in the hydrophobicity measurement software. Five locations were selected for measurement on each sample.
[0074] (3) Obtain a graph showing the relationship between the hydrophobicity of the core rod and the aging time.
[0075] Figure 3 Schematic diagram of static contact angle of mandrel at different aging times. Figure 4 The relationship between the static contact angle of the mandrel and the aging time
[0076] Step 4: After the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out to test the changes in the electrical properties of the core rod samples;
[0077] The specific steps of step 4 include:
[0078] (1) After the high and low temperature cycle aging test is completed, samples with different aging times are taken out for the core rod power frequency withstand voltage test. When flashover occurs on the sample surface, the surface flashover voltage of each group of multiple samples is recorded;
[0079] In this example, 5 samples were taken from each of the seven sample groups. Figure 1 The samples shown were placed Figure 5 A core rod power frequency withstand voltage test was performed between the two electrodes shown, and the test voltage increased at a rate of 1kV / S±0.2kV / S.
[0080] Figure 5This is a diagram of the composite insulator core rod power frequency withstand voltage test device. The device consists of two identical brass electrodes, the upper electrode is the high voltage end, the lower electrode is the ground end, and the core rod sample is between the upper and lower electrodes.
[0081] When flashover occurs on the sample surface, record the surface flashover voltage of each group of 5 samples, conduct 5 experiments on each group of samples, and take the average value as the flashover voltage value of each group of samples. The temperature during the experiment is 25±0.2℃ and the humidity is 35±3%.
[0082] (2) After the high and low temperature cycle aging test is completed, samples with different aging times are taken out for the core rod DC withstand voltage test. When flashover occurs on the sample surface, the surface flashover voltage of each group of multiple samples is recorded;
[0083] In this example, 5 samples were taken from each of the seven sample groups. Figure 1 The samples shown were placed Figure 5 A core rod DC withstand voltage test was conducted between the two electrodes, and the test voltage increased at a rate of 1 kV / S±0.2 kV / S. The temperature during the test was 23±0.2°C and the humidity was 32±3%. Figure 5 This is a diagram of the composite insulator core rod withstand voltage test device.
[0084] When flashover occurs on the sample surface, record the surface flashover voltage of each group of 5 samples, conduct 5 experiments on each group of samples, and take the average value as the flashover voltage value of each group of samples. The temperature during the experiment is 25±0.2℃ and the humidity is 35±3%.
[0085] (3) Take out samples with different aging times to conduct core rod lightning impulse flashover test to determine the lightning impulse flashover voltage;
[0086] In this example, 5 samples were taken from each of the seven sample groups. Figure 1 The sample shown uses an impulse voltage generator to add positive polarity lightning impulse voltage to both ends of the sample to conduct a core rod lightning impulse flashover test. The impulse voltage shape is 1.2 / 50μs. According to the rise and fall method, each sample is tested and determined for 10 effective tests to determine the lightning impulse flashover voltage. 4-6 flashovers in 10 tests are effective experiments.
[0087] (3) Draw a graph showing the relationship between the core rod flashover voltage and aging time.
[0088] Figure 6 This is the relationship between the core rod flashover voltage and aging time.
[0089] The flashover voltage data of the core rod with different aging time is obtained, as shown in Table 1.
[0090] Table 1 AC and DC flashover voltages and lightning impulse flashover voltages of composite insulator core rod samples with different aging times
[0091]
[0092] (5) Samples with different aging times are taken out, the core rod volume resistance is measured, and a relationship diagram between the core rod volume resistance and the aging time is obtained.
[0093] In this example, one sample was taken from each of the seven sample groups. Figure 1 The samples shown are placed Figure 7 The device shown uses the voltammetric method to measure the volume resistance of the core rod. The experimental temperature is 24°C ± 0.2°C and the humidity is 38 ± 3%.
[0094] Figure 7 This is a schematic diagram of the voltammetric method for measuring the volume resistance of the mandrel. As shown in the figure, there are three-electrode systems at both ends of the mandrel sample. The upper end of the mandrel sample is a circular electrode, which is connected to the DC power supply as the high-voltage end; the electrode at the lower end of the mandrel sample is made of a ring with a larger diameter, which serves as the protected electrode; the circular electrode with a small diameter at the lower end of the mandrel sample is the guarding electrode. The high-voltage power supply provides voltage to the mandrel, and the picoammeter measures the current.
[0095] Obtain the relationship between the core rod volume resistance and aging time.
[0096] Figure 8 This is a curve diagram of the relationship between the core rod volume resistance and the aging time.
[0097] Step 4 obtains the change of the electrical properties of the core rod with the high and low temperature cycle aging time.
[0098] Step 5: After the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out to test the mechanical changes of the core rod samples.
[0099] The specific method of step 5 is: after the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out to conduct maximum load and tensile strength tests, and a relationship diagram of the maximum load and tensile strength of the core rod sample changing with aging time is obtained.
[0100] In this example, one sample was taken from each of the seven sample groups. Figure 2 Tensile tests were carried out on type samples to study the relationship between the maximum load and tensile strength of the core rod material with high and low temperature cycle aging time.
[0101] The universal testing machine was used to test the Figure 2 The type mandrel specimen is subjected to a tensile load measurement experiment in an environment with a temperature of 25±0.2°C and a humidity of 30±3%.
[0102] The sample was continuously loaded until it was broken, and the displacement speed of the tensile machine was 20 mm / min. The maximum load was recorded after the mandrel was broken. The tensile strength of each sample was calculated, and the calculation of tensile strength is shown in Formula 1.
[0103]
[0104] Where σ is the tensile strength, in MPa, Pb is the maximum load when the sample is damaged, in N, and D is the diameter of the working section of the sample, in mm.
[0105] The relationship diagram between the maximum load and tensile strength of the core rod sample and the aging time was obtained.
[0106] Fig. 9 This is a curve diagram showing the relationship between the maximum load of the core rod sample and the aging time.
[0107] Fig.10 This is a curve diagram of the relationship between the tensile strength of the core rod sample and the aging time.
[0108] In this embodiment, the processing steps of the present invention are further described in combination with specific examples:
[0109] In order to explore the effect of high and low temperature cyclic aging on the hydrophobicity of composite insulator core rods, the water contact angle of the side wall of the core rod sample was selected as the research object. Figure 3 Shown is a schematic diagram of the static contact angle of the mandrel at different aging times. Figure 4 This is the relationship between the static contact angle of the mandrel and the aging time. Figure 4 As shown in the figure, the average static contact angle of the mandrel side wall after aging ranges from 44.7° to 61.65°, and the water contact angle on the mandrel side wall surface shows a downward trend. As the aging time increases, the water contact angle tends to be stable, the hydrophobicity of the mandrel decreases, and the hydrophilicity increases.
[0110] In order to explore the influence of high and low temperature cyclic aging on the electrical properties of composite insulator core rods, the AC and DC flashover voltages and lightning impulse flashover voltages of composite insulator core rods were selected as research objects, and the relationship between the AC and DC flashover voltages and lightning impulse flashover voltages of composite insulator core rods and aging time was studied, so as to obtain the influence of high and low temperature cyclic aging on the electrical properties of composite insulator core rods.
[0111] The experimental results are shown in Table 1. Table 1 shows the AC and DC flashover voltages and lightning impulse flashover voltages of composite insulator core rod samples with different aging times. Figure 6 is the relationship between the core rod flashover voltage and aging time. Figure 6 It can be seen that after high and low temperature cycle aging, the AC and DC flashover voltage and lightning impulse voltage of the composite insulator core rod both show a downward trend, but the downward trend is not obvious. Within the same high and low temperature cycle aging time, the peak value of the core rod impulse flashover voltage is significantly higher than the AC and DC flashover voltage value.
[0112] As a good insulator, the core rod of the composite insulator will have volume resistance changes when defects such as brittle cracking and powdering occur in the core rod. Figure 8The relationship between the core rod volume resistance and aging time. Figure 8 It can be seen that with the increase of aging time, the volume resistance decreases, which is more obvious from aging 20 to 30 days, indicating that the insulation performance of the core rod has deteriorated with the increase of high and low temperature cycle aging time.
[0113] In order to explore the influence of high and low temperature cycle aging on the mechanical properties of composite insulator core rods, tensile tests were conducted on the core rods of sample 2 of the seventh group (control group) and the other 6 groups of sample 2 core rods with different aging times to study the relationship between the maximum load and tensile strength of the core rod material with high and low temperature cycle aging, so as to evaluate the influence of high and low temperature cycle aging on the mechanical properties of the core rod. Fig. 9 This is a curve diagram showing the relationship between the maximum load of the core rod sample and the aging time. Fig.10 The figure is the relationship between the tensile strength of the core rod sample and the aging time. Fig. 9 Fig.10 It can be seen that the maximum load and tensile strength of the core rod sample show an overall downward trend with the increase of aging time. The above research shows that long-term high and low temperature cycle aging can cause the mechanical properties of the composite insulator core material to deteriorate.
[0114] It should be emphasized that the embodiments of the present invention are illustrative rather than restrictive. Therefore, the present invention includes but is not limited to the embodiments described in the specific implementation modes. Any other implementation modes derived by those skilled in the art based on the technical solutions of the present invention also fall within the scope of protection of the present invention.
Claims
1. A composite insulator core rod aging method, characterized in that: The following steps are involved: Step 1, preparing high and low temperature cycle aging composite insulator core rod samples; Step 2, grouping the composite insulator core rod samples manufactured in step 1 and performing a high and low temperature cycle aging test; Step 3, after the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out to test the change of the hydrophobicity of the core rod samples; Step 4: After the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out to test the changes in the electrical properties of the core rod samples; Step 5: After the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out to test the mechanical changes of the core rod samples; The specific method of step 1 is: A composite insulator core rod sample with a diameter of 25 mm and a length of 30 mm was selected to detect the changes in the hydrophobicity and electrical properties of the core rod after aging; a composite insulator core rod with a diameter of 25 mm ± 0.1 mm was selected and cut into a sample of 310 mm in length to detect the changes in the mechanical properties of the core rod after aging; The specific method of step 2 is: The temperature points of the high and low temperature cycle aging scheme are set to alternate between extremely low temperature of -60℃±3℃ and high temperature of 140℃±3℃ to simulate the influence of temperature change on the performance of composite insulator core rods. The high and low temperature cycle aging time is 1440h in total, and each 24h is a cycle, with a total of 60 cycle aging cycles; in one aging cycle, 0-12h is used as high temperature 140℃ aging, and 12-24h is used as -60℃ aging; The specific steps of step 3 include: (1) After the high and low temperature cycle aging test is completed, take out the sample for water contact angle measurement: first wash it with distilled water, then dry it naturally, and finally dip anhydrous ethanol with a dry cotton ball and apply it on the side wall of the sample to ensure the cleanliness of the sample. After the anhydrous ethanol on the side wall is completely evaporated, start the hydrophobicity test; (2) Each time, 5 μL of deionized water was dropped onto the side wall of the mandrel sample. After the water drop was stationary on the side wall, an image was quickly taken in the hydrophobicity measurement software. Multiple locations of each sample were selected for measurement. (3) Obtaining a graph showing the relationship between the hydrophobicity of the core rod and the aging time; The specific steps of step 4 include: (1) After the high and low temperature cycle aging test is completed, samples with different aging times are taken out for the core rod power frequency withstand voltage test. When flashover occurs on the sample surface, the surface flashover voltage of each group of multiple samples is recorded; (2) After the high and low temperature cycle aging test is completed, samples with different aging times are taken out for the core rod DC withstand voltage test. When flashover occurs on the sample surface, the surface flashover voltage of each group of multiple samples is recorded; (3) Take out samples with different aging times to conduct core rod lightning impulse flashover test to determine the lightning impulse flashover voltage; (4) Draw a graph showing the relationship between the core rod flashover voltage and aging time; (5) taking out samples with different aging times, measuring the volume resistance of the mandrel, and obtaining a relationship diagram between the volume resistance of the mandrel and the aging time; The specific method of step 5 is: After the high and low temperature cycle aging test in step 2 is completed, samples with different aging times are taken out for maximum load and tensile strength tests, and a relationship diagram of the maximum load and tensile strength of the core rod sample with aging time is obtained.
Citation Information
Patent Citations
Method for testing and evaluating high-low temperature circulating ageing of silicone rubber for composite insulator
CN104458552A