Electrolyte and lithium ion battery

By using an electrolyte containing benzoquinone and phloroglucinol in lithium metal batteries, combined with lithium salts and organic solvents, the problem of LiH generation caused by LiFSI is solved, and the battery cycle performance and specific capacity are improved.

CN114583262BActive Publication Date: 2024-10-11BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011373527.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-30
Publication Date
2024-10-11
Estimated Expiration
2040-11-30

AI Technical Summary

Technical Problem

In lithium metal batteries, lithium bisfluorosulfanimide (LiFSI) leads to the generation of LiH, which affects the cycle performance and rate performance of the battery. Existing methods such as the use of fluorinated solvents cannot completely solve this problem.

Method used

An electrolyte is used, containing a lithium salt, an organic solvent, a first additive (such as substituted or unsubstituted benzoquinone or phenylhydrazine) and a second additive (such as substituted or unsubstituted phloroglucinol), and the first additive is in the negative electrode The film forms and combines with the anionic radicals of the lithium salt to reduce the generation of LiH. The second additive is oxidized and polymerized at the positive electrode to form a film, protecting the first additive and synergistically forming a stable positive and negative electrode interface film.

Benefits of technology

Significantly reduce the generation of LiH, improve the cycle performance and specific capacity of the battery, and improve the long cycle performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002807512030000046
    Figure BDA0002807512030000046
  • Figure BDA0002807512030000111
    Figure BDA0002807512030000111
  • Figure BDA0002807512030000121
    Figure BDA0002807512030000121
Patent Text Reader

Abstract

The present application provides an electrolyte, including a lithium salt, an organic solvent, a first additive and a second additive, wherein the first additive includes one or more of substituted or unsubstituted benzoquinone, substituted or unsubstituted phenylhydrazine; the second additive includes substituted or unsubstituted pyrogallol; and the lithium salt includes lithium bis(fluorosulfuryl)imide. Under the synergistic effect of the above two types of additives, the electrolyte can stably and efficiently reduce LiH generation, stabilize the positive and negative electrode SEI films, improve battery cycle performance, increase specific capacity, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to an electrolyte and a lithium-ion battery. Background Art

[0002] Lithium bis(fluorosulfuryl)imide (LiFSI) has become a widely used lithium salt in the electrolyte of lithium metal batteries due to its good film-forming effect on the surface of lithium metal negative electrodes. However, studies have found that after multiple cycles of the battery system using LiFSI, LiH is produced in the negative electrode byproduct, and the output is far greater than the amount of LiH that may be introduced by water, which indicates that its formation pathway must have other pathways besides water. The formation of LiH consumes the active metal lithium of the negative electrode, and its ionic conductivity is poor, thereby reducing the cycle performance and rate performance of the battery; in addition, LiH is very brittle and is prone to brittle fracture and enter the electrolyte to form "dead lithium", thereby reducing the negative electrode capacity. Therefore, in order to improve the electrochemical performance of lithium metal batteries, inhibiting or eliminating the formation of LiH is an urgent problem to be solved.

[0003] At present, the industry is still unclear about other formation mechanisms besides the formation of LiH by LiFSI reacting with water. The industry generally considers using fluorinated solvents to avoid the formation of LiH, such as using fluoroethylene carbonate (FEC) to replace ethylene carbonate (EC). However, FEC has poor thermal stability and poor film-forming effect on the surface of lithium metal negative electrodes. It also has many side reactions with metallic lithium. Although it can reduce the generation of LiH to a certain extent, it will still have an adverse effect on the cycle performance of the battery. Summary of the invention

[0004] In view of this, the present application provides an electrolyte for a lithium metal battery system using LiFSI as a lithium salt, which can reduce the generation of LiH and improve the cycle performance of the battery.

[0005] Specifically, the first aspect of the present application provides an electrolyte, which includes a lithium salt, an organic solvent, a first additive and a second additive, wherein the first additive includes one or more of substituted or unsubstituted benzoquinone, substituted or unsubstituted phenylhydrazine; the second additive includes substituted or unsubstituted pyrogallol; and the lithium salt includes lithium bis(fluorosulfuronimide) (LiFSI).

[0006] In the electrolyte provided in the first aspect of the present application, the first additive can form a film on the negative electrode of the battery, and can present a high cation density in a polar solvent, and form a strong electrostatic force with anions and anion radicals derived from the lithium salt LiFSI, significantly reducing the shuttling effect of anion radicals between the positive and negative electrodes, reducing the attack of these anion radicals on H atoms in the solvent to produce hydrogen ions, and then reducing the generation of LiH on the negative electrode surface, thereby improving the cycle performance of the battery. However, the first additive is easily oxidized at the positive electrode, and after the introduction of the second additive, based on the second additive can be oxidized and polymerized at a lower oxidation potential on the positive electrode surface to form a film, the first additive can be avoided from being oxidized at the positive electrode, which plays a protective role. Therefore, the first additive and the second additive have a synergistic effect in electrode film formation, so that the electrolyte containing them can reduce the formation of LiH in the lithium metal battery and improve the battery cycle performance under the premise of forming a stable positive and negative electrode interface film.

[0007] Optionally, the substituent groups in the substituted benzoquinone, the substituted phenylhydrazine and the substituted benzyltriol include at least one of a halogen atom, a hydroxyl group, a nitro group, a cyano group, an isothiocyano group, an amine group, an acyloxy group, an alkyl group, a halogenated alkyl group, an alkoxy group, a halogenated alkoxy group, an alkenyl group, a halogenated alkenyl group, an alkenyloxy group, a halogenated alkenyloxy group, an aryl group, a halogenated aryl group, an aryloxy group, and a halogenated aryloxy group.

[0008] The halogen atoms include chlorine atoms (Cl), bromine atoms (Br), and iodine atoms (I). The amine groups include primary amine groups (-NH2), secondary amine groups (or alkylamino groups, -NHR), and tertiary amine groups (or dialkylamino groups, -NRR').

[0009] In the embodiment of the present application, the benzoquinone includes o-benzoquinone (1,2-benzoquinone) and p-benzoquinone (1,4-benzoquinone, ).

[0010] In some embodiments of the present application, the substituted benzoquinone may include methyl para-benzoquinone 2-tert-Butyl-p-benzoquinone Nitrobenzoquinone Hydroxybenzoquinone, 2,5-dihydroxybenzoquinone Tetrahydroxy-p-benzoquinone, tetraamino-p-benzoquinone Tetrafluoro-o-benzoquinone 3,5-Dichloro-2-methyl-p-benzoquinone 2,6-Dibromobenzoquinone 2,3-Difluoro-1,4-benzoquinone 2,3-Dicyanobenzoquinone Dichlorodicyanobenzoquinone (DDQ, ), 2,3-dimethoxy-5-methyl-1,4-benzoquinone 4-Methoxy-1,2-benzoquinone 2,5-Dibutoxy-1,4-benzoquinone 2-Phenoxy-1,4-benzoquinone 2,5-Biphenyl-p-benzoquinone 2-Allyloxy-1,4-benzoquinone

[0011] In the present application, the structural formula of the phenylhydrazine is In some embodiments of the present application, the substituted phenylhydrazine may include 2-ethylphenylhydrazine 4-Fluorophenylhydrazine m-Bromophenylhydrazine 4-Fluoro-3-methylphenylhydrazine 4-Chloro-2-fluorophenylhydrazine p-Nitrophenylhydrazine 3-Benzylphenylhydrazine etc., but not limited to.

[0012] In the present application, the above-mentioned pyrogallol includes pyrogallol and phloroglucinol. Among them, phloroglucinol has a high structural symmetry, a small steric hindrance in the polymerization reaction, and can easily form a polymer protective film with a higher degree of polymerization through oxidative polymerization. Preferably, the second additive is substituted or unsubstituted phloroglucinol.

[0013] In some embodiments of the present application, the substituents in the substituted benzyltriol include electron-donating groups such as nitro, acyl, halogen, amine, alkyl, alkoxy, acyloxy, and aryl. The introduction of electron-donating groups can improve the reduction resistance of the second additive, making it less likely to have side reactions with the negative electrode, and reduce its positive electrode film-forming potential (i.e., oxidation potential), so that the second additive can form a film on the positive electrode as early as possible.

[0014] In some embodiments of the present application, the substituted phloroglucinol includes one or more of 2,4-dimethyl phloroglucinol, 2-nitro phloroglucinol, 2,4-dinitro phloroglucinol, 2,4-diformyl phloroglucinol, trimethyl phloroglucinol, tribromo phloroglucinol, triiodo phloroglucinol, etc., but is not limited thereto. Among them, 2,4-dimethyl phloroglucinol and trimethyl phloroglucinol are preferred substituted phloroglucinols.

[0015] The organic solvent in the electrolyte of the present application may include at least one of an ester solvent, an ether solvent, and a nitrile-based solvent, but is not limited thereto.

[0016] Among them, the ester solvent may include one or more of dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate (MPC), dipropyl carbonate (DPC), ethyl propyl carbonate, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, γ-butyrolactone (GBL), etc. The ether solvent may include one or more of cyclic ether tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane and 1,4-dioxane, chain ether dimethoxymethane, 1,2-dimethoxyethane and diethylene glycol dimethyl ether, etc. The nitrile-containing solvent may include one or more of acetonitrile, propionitrile, succinonitrile, etc.

[0017] Preferably, the organic solvent is the above-mentioned ether solvent. Ether solvents have a lower reduction potential, higher reduction resistance, and are less likely to have side reactions with metallic lithium; in addition, ether solvents are less polar than ester solvents, and are more conducive to improving the solubility of lithium salts and the above-mentioned additives therein.

[0018] Optionally, the mass of the first additive is 0.5%-10% of the mass of the organic solvent. In some embodiments of the present application, the mass of the first additive is 1.5%-5% of the mass of the organic solvent. In this case, the amount of the first additive is more appropriate, and it can fully capture anion radicals and reduce LiH generation without causing side reactions with the negative electrode.

[0019] Optionally, the mass of the second additive is 1%-20% of the mass of the organic solvent, preferably 1.2%-8%, which can ensure that the second additive forms a film of suitable thickness on the positive electrode, and will neither form a film insufficiently due to too low a dosage nor increase the impedance of the battery and be detrimental to the cycle performance of the battery due to too thick a film.

[0020] Further optionally, the mass of the second additive may be 1-6 times the mass of the first additive. In this case, the lithium-ion battery using the electrolyte may have better cycle performance. Preferably, the mass of the second additive may be 1.5-5 times the mass of the first additive.

[0021] Optionally, the concentration of the lithium salt in the electrolyte may be 0.7-5 mol / L, preferably 1-3 mol / L.

[0022] In some other embodiments of the application, the lithium salt may contain, in addition to LiFSI, lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium hexafluoroantimonate (LiSbF6), lithium perchlorate (LiClO4), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiDFOB), lithium trifluoromethylsulfonate (LiCF3SO3), lithium perfluorobutylsulfonate (LiC4F9SO3), lithium bis(trifluoromethylsulfonyl)imide (Li(CF3SO2)2N), lithium bis(perfluoroethylsulfonyl)imide (Li(C2F5SO2)2N), and the like. One or more.

[0023] In some other embodiments of the application, the electrolyte may also include one or more of the following additives: vinylene carbonate (VC), vinyl vinyl carbonate (VEC), phenyl vinyl carbonate (PhEC), styrene vinyl carbonate (PhVC), fluoroethylene carbonate (FEC), catechol carbonate (CC), phenyl methyl carbonate (AMC), vitamin A (VA) and 2-hydrofuran (CN-F).

[0024] The electrolyte provided in the first aspect of the present application contains a lithium salt containing LiFSI, and the above-mentioned first additive and second additive, wherein the first additive can capture anion free radicals and reduce the generation of negative electrode LiH, and the second additive can be easily oxidized to form a film at the positive electrode, and when it protects the positive electrode SEI film, it can also prevent the first additive from being oxidized and failing at the positive electrode. Under the synergistic effect of these two types of additives, it can play a role in stably and efficiently reducing the generation of LiH, stabilizing the positive and negative electrode SEI films, improving the battery cycle performance, and increasing the specific capacity. The electrolyte is particularly suitable for battery systems with metallic lithium and lithium-silicon alloys as negative electrodes.

[0025] The preparation method of the above electrolyte is relatively simple, and the preparation method comprises: adding the first additive and the second additive after drying and the lithium salt into an organic solvent, stirring to fully dissolve and evenly disperse the components, and obtaining the above electrolyte. There is no requirement for the order of adding the lithium salt, the first additive, and the second additive, and they can be added in batches or simultaneously.

[0026] In a second aspect, the present application provides a lithium-ion battery, in which the electrolyte described in the first aspect of the present application is built-in.

[0027] Specifically, the lithium-ion battery includes a battery shell and a battery cell and an electrolyte contained in the battery shell, wherein the battery cell includes a positive electrode sheet, a negative electrode sheet and a separator located between the positive electrode sheet and the negative electrode sheet, and the electrolyte is as described in the first aspect of the present application.

[0028] The preparation method of the lithium ion battery comprises: stacking a positive electrode sheet, a separator and a negative electrode sheet in sequence to form a battery core, accommodating the battery core in a battery shell, injecting the above electrolyte, and then sealing the battery shell to obtain a lithium ion battery.

[0029] Among them, the negative electrode sheet, the positive electrode sheet, and the separator are all conventional choices in the battery field. For example, the separator includes a modified polyethylene felt, a modified polypropylene felt, an ultrafine glass fiber felt, a vinylon felt, or a composite film formed by welding or bonding nylon felt and a wettable polyolefin microporous membrane. The positive electrode sheet includes a current collector and a positive electrode material layer disposed on the current collector, wherein the positive electrode material layer includes a positive electrode active substance, a positive electrode binder, and an optional conductive agent. The positive electrode active material may include one or more of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, ternary materials, etc., but is not limited thereto. The negative electrode sheet includes a current collector and a negative electrode material layer disposed on the current collector, wherein the negative electrode material layer may include a negative electrode active substance, a negative electrode binder, and an optional conductive agent. The negative electrode active material may be metallic lithium, etc. DETAILED DESCRIPTION

[0030] The embodiments of the present application are further described below with reference to a plurality of embodiments.

[0031] Example 1

[0032] A method for preparing an electrolyte comprises: adding 3 g of a first additive - benzoquinone and 5 g of a second additive - pyrogallol after drying to 100 g of dimethoxyethane (DME) solvent, stirring thoroughly, and finally adding lithium salt - lithium bis(fluorosulfuryl)imide (LiFSI), stirring thoroughly, and preparing an electrolyte, which is recorded as E1. The concentration of LiFSI in the electrolyte is 1.2 M.

[0033] A method for preparing a lithium ion battery, comprising:

[0034] Lithium metal negative electrode: A 40um thick lithium metal strip is rolled onto a copper foil current collector to obtain a negative electrode lithium metal strip, which is then cut into a 44mm long and 20mm wide negative electrode sheet;

[0035] Preparation of positive electrode sheet: The positive electrode active material lithium cobalt oxide LiCoO2 is mixed with acetylene black and polyvinylidene fluoride (PVDF) in a mass ratio of 100:3:2 in N-methylpyrrolidone, and the positive electrode slurry is prepared by high-speed dispersion. The positive electrode slurry is coated on both sides of the aluminum foil current collector, and a positive electrode material layer is formed after baking to obtain a positive electrode sheet;

[0036] Preparation of laminated batteries: The above-cut positive and negative electrodes are alternately laminated, with a 45mm wide 9+2 ceramic separator inserted in a Z shape in the middle. The total number of positive and negative electrodes is 33. After being placed in an aluminum-plastic film, the battery L1 is made by known steps such as edge sealing, baking, and electrolyte injection.

[0037] Example 2

[0038] A method for preparing an electrolyte comprises: adding 3 g of a first additive (benzoquinone) and 5 g of a second additive (phloroglucinol) which have been dried to 100 g of a DME solvent, stirring thoroughly, and finally adding lithium salt LiFSI, stirring thoroughly, to prepare an electrolyte having a LiFSI concentration of 1.2 M, recorded as E2.

[0039] According to the battery manufacturing method provided in Example 1, a laminated battery L2 was prepared using electrolyte E2.

[0040] Example 3

[0041] A method for preparing an electrolyte comprises: adding 3 g of a first additive (benzoquinone) and 5 g of a second additive (nitrophloroglucinol) which have been dried to 100 g of a DME solvent, stirring the mixture thoroughly, and finally adding lithium salt LiFSI, stirring the mixture thoroughly, to prepare an electrolyte having a LiFSI concentration of 1.2 M, which is recorded as E3.

[0042] According to the battery manufacturing method provided in Example 1, a laminated battery L3 was prepared using electrolyte E2.

[0043] Example 4

[0044] A method for preparing an electrolyte comprises: adding 3 g of a first additive (benzoquinone) and 5 g of a second additive (specifically 2,4-dimethylphloroglucinol) which have been dried to 100 g of a DME solvent, stirring thoroughly, and finally adding lithium salt LiFSI, stirring thoroughly, to prepare an electrolyte having a LiFSI concentration of 1.2 M, recorded as E4.

[0045] According to the battery manufacturing method provided in Example 1, a laminated battery L4 was prepared using electrolyte E2.

[0046] Example 5

[0047] A method for preparing an electrolyte comprises: adding 10 g of a first additive - benzoquinone and 5 g of a second additive - pyrogallol after drying to 100 g of a DME solvent, stirring thoroughly, and finally adding lithium salt LiFSI, stirring thoroughly, to prepare an electrolyte with a LiFSI concentration of 1.2 M, recorded as E5.

[0048] According to the battery manufacturing method provided in Example 1, a laminated battery L5 was prepared using electrolyte E2.

[0049] Example 6

[0050] A method for preparing an electrolyte comprises: adding 3 g of a first additive (benzoquinone) and 15 g of a second additive (pyrogallol) which have been dried to 100 g of a DME solvent, stirring thoroughly, and finally adding lithium salt LiFSI, stirring thoroughly, to prepare an electrolyte having a LiFSI concentration of 1.2 M, recorded as E6.

[0051] According to the battery manufacturing method provided in Example 1, a laminated battery L6 was prepared using electrolyte E2.

[0052] Example 7

[0053] A method for preparing an electrolyte comprises: adding 3 g of a first additive (benzoquinone) and 5 g of a second additive (pyrogallol) which have been dried to 100 g of a DME solvent, stirring thoroughly, and finally adding lithium salt LiFSI, stirring thoroughly, to prepare an electrolyte having a LiFSI concentration of 3 M, recorded as E7.

[0054] According to the battery manufacturing method provided in Example 1, a laminated battery L7 was prepared using electrolyte E2.

[0055] Example 8

[0056] Battery L8 was prepared by referring to the battery preparation method provided in Example 1, which differs from Example 2 in that the solvent in the electrolyte is a mixture of EC, EMC, DEC and DMC in a mass ratio of 34:35:13:18.

[0057] Example 9

[0058] A method for preparing an electrolyte comprises: adding a first additive (specifically 3 g of phenylhydrazine) and a second additive (specifically 5 g of trimethylphloroglucinol) that have been dried to 100 g of 2-methyltetrahydrofuran solvent, stirring thoroughly, and finally adding lithium salt LiFSI, stirring thoroughly, to prepare an electrolyte with a LiFSI concentration of 1.2 M, recorded as E9.

[0059] According to the battery manufacturing method provided in Example 1, a laminated battery L9 was prepared using electrolyte E9.

[0060] Example 10

[0061] A method for preparing an electrolyte comprises: adding a first additive (specifically 3 g of m-bromophenylhydrazine) and a second additive (specifically 5 g of phloroglucinol) that have been dried to 100 g of a 1,3-dioxolane solvent, stirring thoroughly, and finally adding lithium salt LiFSI, stirring thoroughly, to prepare an electrolyte having a LiFSI concentration of 1.2 M, recorded as E10.

[0062] According to the battery manufacturing method provided in Example 1, a laminated battery L10 was prepared using electrolyte E10.

[0063] Embodiment 11

[0064] A method for preparing an electrolyte comprises: adding a first additive (specifically 3 g of tetraaminobenzoquinone) and a second additive (specifically 5 g of phloroglucinol) that have been dried to 100 g of a DME solvent, stirring thoroughly, and finally adding lithium salt LiFSI, stirring thoroughly, to prepare an electrolyte having a LiFSI concentration of 1.2 M, recorded as E11.

[0065] According to the battery manufacturing method provided in Example 1, a laminated battery L11 was prepared using electrolyte E11.

[0066] In order to highlight the beneficial effects of the embodiments of the present application, the following comparative examples 1-3 are provided.

[0067] Comparative Example 1

[0068] The battery DL1 was prepared by referring to the battery preparation method provided in Example 1. The difference between the battery DL1 and Example 1 is that the electrolyte DE1 of the battery DL1 only contains LiFSI and the solvent DME.

[0069] Comparative Example 2

[0070] The battery DL2 was prepared by referring to the battery preparation method provided in Example 1, which differs from Example 2 in that the electrolyte DE2 of the battery DL2 does not contain the second additive. That is, the electrolyte DE2 contains 100 g of solvent DME, 3 g of the first additive-benzoquinone and LiFSI, and the concentration of LiFSI in the electrolyte is 1.2 M.

[0071] Comparative Example 3

[0072] Battery DL3 was prepared by referring to the battery preparation method provided in Example 1, which differs from Example 2 in that the electrolyte DE3 of battery DL3 does not contain the first additive. That is, the electrolyte DE3 contains 100 g of solvent DME, 5 g of the second additive - resorcinol and LiFSI, and the concentration of LiFSI in the electrolyte is 1.2 M.

[0073] Performance Testing

[0074] The lithium ion batteries prepared in the above examples and comparative examples were tested for cycle performance and initial efficiency respectively:

[0075] At 25°C, charge at 0.5C constant current until the cut-off voltage is 4.2V, leave for 30min, then discharge at 0.5C constant current until the voltage is 3.0V, leave for 30min, and cycle 100 times under this condition, where the ratio of the first discharge capacity of the battery to the first charge capacity is the first efficiency of the battery; the ratio of the discharge capacity after 100 cycles to the first discharge capacity is the capacity retention rate of the battery after 100 cycles at room temperature. The performance test results of each battery are shown in Table 1 below.

[0076] Table 1 Performance test results of each battery

[0077]

[0078]

[0079] It can be seen from the data in Table 1 that the first efficiency of the batteries provided in Examples 1-11 of the present application is higher than that of the battery in Comparative Example 1; the capacity retention rate of the batteries provided in Examples 1-11 of the present application after 100 cycles is much higher than that of the battery in Comparative Example 1. In addition, from the comparison between Example 2 and Comparative Examples 2-3, it can be seen that when the electrolyte contains both the first additive and the second additive, the long-cycle capacity retention rate of the battery can be better improved. Based on the fact that the electrolyte provided in the present application can better inhibit the formation of LiH, stabilize the positive and negative electrode interface films, etc., the cycle performance of the battery using the electrolyte provided in the present application can be greatly improved.

[0080] The above is an exemplary embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made thereto without departing from the principles of the present application. These improvements and modifications are also considered to be within the scope of protection of the present application.

Claims

1. An electrolyte, characterized in that: The electrolyte includes a lithium salt, an organic solvent, a first additive and a second additive, wherein the first additive includes one or more of substituted or unsubstituted benzoquinone, substituted or unsubstituted phenylhydrazine; the second additive includes substituted or unsubstituted benzyltriol; the lithium salt includes lithium bis(fluorosulfuryl)imide; wherein the mass of the first additive is 0.5%-10% of the mass of the organic solvent, the mass of the second additive is 1%-20% of the mass of the organic solvent, and the mass of the second additive is 1-6 times the mass of the first additive.

2. The electrolyte according to claim 1, characterized in that The substituent groups in the substituted benzoquinone, the substituted phenylhydrazine and the substituted benzyltriol include at least one of a halogen atom, a hydroxyl group, a nitro group, a cyano group, an isothiocyano group, an amine group, an acyloxy group, an alkyl group, a halogenated alkyl group, an alkoxy group, a halogenated alkoxy group, an alkenyl group, a halogenated alkenyl group, an alkenyloxy group, a halogenated alkenyloxy group, an aryl group, a halogenated aryl group, an aryloxy group and a halogenated aryloxy group.

3. The electrolyte according to claim 2, characterized in that The second additive includes one or more of pyrogallol, phloroglucinol, 2,4-dimethylphloroglucinol, 2-nitrophloroglucinol, trimethylphloroglucinol, tribromophloroglucinol, and triiodophloroglucinol.

4. The electrolyte according to claim 1, characterized in that The organic solvent includes at least one of an ether solvent, an ester solvent, and a nitrile-based solvent.

5. The electrolyte according to claim 4, characterized in that The ether solvent includes one or more of cyclic ether tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane and 1,4-dioxane, chain ether dimethoxymethane, 1,2-dimethoxyethane and diethylene glycol dimethyl ether.

6. The electrolyte according to claim 1, characterized in that The concentration of the lithium salt in the electrolyte is 0.7-5 mol / L.

7. The electrolyte according to any one of claims 1 to 6, characterized in that The electrolyte also contains other lithium salts and / or other additives.

8. A lithium metal battery, wherein the electrolyte according to any one of claims 1 to 7 is built into the lithium metal battery.