Polymer electrolyte and preparation method thereof and application in wide temperature range, high rate solid-state lithium battery

By using polymer electrolytes with high ionic conductivity and high thermal stability in lithium batteries, the problem of insufficient working ability of lithium batteries at low or high temperatures is solved, and high-rate charge and discharge in a wide temperature range are achieved, and through freeze-drying The method recycles solvents, reducing production costs and environmental pollution.

CN114597501BActive Publication Date: 2024-10-22INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210199650.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-02
Publication Date
2024-10-22
Estimated Expiration
2042-03-02

AI Technical Summary

Technical Problem

Existing lithium batteries cannot work at low or high temperatures, and can only be charged and discharged at low rates, unable to meet the application requirements of fast charge and discharge, and the organic liquid electrolyte used has safety hazards.

Method used

A polymer electrolyte preparation method is adopted. By dissolving the polymer and lithium salt in a solvent, freeze-drying and then removing the solid solvent, a polymer electrolyte with high ionic conductivity and high thermal stability is prepared for use in a wide temperature range. , high-rate solid-state lithium metal battery, realizing fast charging and discharging.

Benefits of technology

The polymer electrolyte exhibits high capacity and high ionic conductivity in a wide temperature range from -10°C to 100°C, enabling fast charging and discharging of lithium metal batteries, and realizes solvent recovery and reuse through freeze-drying methods, reducing costs. production costs and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003528791640000011
    Figure HDA0003528791640000011
  • Figure HDA0003528791640000012
    Figure HDA0003528791640000012
  • Figure HDA0003528791640000021
    Figure HDA0003528791640000021
Patent Text Reader

Abstract

The present invention discloses a polymer electrolyte and a preparation method thereof and an application in a wide temperature range and high rate solid-state lithium battery, belonging to the field of solid-state battery technology. The polymer electrolyte is composed of a polymer skeleton, a lithium salt and a small amount of confined solvent, and has the characteristics of high ionic conductivity, high thermal stability and stable electrolyte / electrode interface. The solid-state lithium metal battery assembled by the polymer electrolyte maintains high capacity in a wide temperature range (-10 to 100°C) and a high rate (1 to 50°C). The preparation method of the present invention is compatible with existing processes, can effectively simplify the production matching process of solid-state lithium metal batteries, significantly improve battery performance, and further realize the recovery and reuse of solvents in the electrolyte preparation process, thus having good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The present invention relates to the technical field of solid-state batteries, and in particular to a polymer electrolyte and a preparation method thereof, and applications in wide-temperature-range, high-rate solid-state lithium metal batteries. Background technology:

[0002] Currently, commercial lithium batteries often use volatile and flammable organic liquid electrolytes, which can easily lead to safety hazards such as battery fire and explosion. Using polymer electrolytes instead of liquid electrolytes is an effective way to improve battery safety. At present, a variety of polymer electrolyte systems have been reported in the literature, such as polyethylene oxide, polycarbonate, and polymethacrylate. However, although the above electrolyte systems have shown certain application potential, their application scenarios are usually limited. For example, the battery cannot work at low or high temperatures, and the assembled batteries usually only work at low rates, which cannot meet the battery's fast charging and discharging application requirements. Therefore, it is of great significance to develop high-performance solid electrolytes and solid-state batteries that can be charged and discharged over a wide temperature range and at high rates. Summary of the invention:

[0003] In order to solve the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a polymer electrolyte and a preparation method thereof and its application in wide temperature range, high rate solid-state lithium batteries. The polymer electrolyte of the present invention has the characteristics of high ionic conductivity, high thermal stability and stable electrolyte / electrode interface, can be applied to solid-state lithium metal batteries, and can have a high capacity in the low temperature (-10°C) and high temperature (100°C) range, and can realize fast charging and discharging of solid-state lithium metal batteries.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0005] A method for preparing a polymer electrolyte comprises the following steps:

[0006] (1) dissolving the polymer and the lithium salt in a solvent in proportion, and stirring to obtain a mixed solution;

[0007] (2) freezing the mixed solution obtained in step (1) in a low-temperature environment, and removing the solid solvent through a vacuum freeze-drying device after the solvent is completely solidified, thereby obtaining the polymer electrolyte; heating and melting the solvent captured in the cold trap of the vacuum freeze-drying device, and recycling it.

[0008] In the above step (1), the polymer is at least one of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyethylene oxide (PEO), polypropylene oxide (PPO), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), polymethacrylate (PMMA) and polypropylene carbonate (PPC).

[0009] In the above step (1), the lithium salt is lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium perchlorate (LiClO 4 ), lithium hexafluorophosphate (LiPF 6 ), lithium chloride (LiCl), lithium nitrate (LiNO 3 ), lithium tetrafluoroborate (LiBF 4 ) and lithium hexafluoroarsenate (LiAsF 6 ) at least one of.

[0010] In the above step (1), the solvent is at least one of dimethyl sulfoxide, sulfolane, water, N-methylpyrrolidone, benzene, tert-butanol, cyclohexane, acetic acid and N,N-dimethylformamide.

[0011] In the above step (1), the weight of the lithium salt is 10wt.% to 60wt.% of the total weight of the polymer and the lithium salt; and the weight of the solvent is 5 to 100 times the weight of the polymer.

[0012] In the above step (2), the vacuum freeze drying device comprises a drying chamber, a vacuum pump and a cold trap. Preferably, the vacuum freeze drying device is a freeze dryer.

[0013] In the above step (1), the stirring time is 12 to 48 hours; in the step (2), the freezing temperature is -50 to 0°C, and the insulation time is 1 to 48 hours; and the drying time in the vacuum freeze-drying device is 12 to 60 hours.

[0014] The polymer electrolyte prepared by the present invention is applied to solid-state lithium metal batteries under a wide temperature range, wherein the wide temperature range is -10 to 100°C, and the fast charge and discharge is charge and discharge at a rate of 1 to 50C.

[0015] The design principle of the present invention is as follows:

[0016] In the process of preparing polymer electrolytes by freeze-drying, free solvent molecules are sublimated and removed, while the residual trace solvent is confined inside the polymer skeleton. The electrochemical / chemical activity of the confined trace solvent is fully suppressed, thereby constructing a stable electrolyte / electrode interface, so that the polymer electrolyte can be used in high-voltage solid-state lithium metal batteries. In addition, the polymer, lithium salt and trace solvent constitute a fast lithium ion transmission channel inside the polymer electrolyte, so that the solid-state battery assembled by the polymer electrolyte has a high capacity in a wide temperature range from low to high temperature. The ternary structure of lithium salt anions, solvent and polymer skeleton can effectively inhibit the migration of lithium salt anions, thereby significantly increasing the number of lithium ion migrations, and further realizing the high-rate performance of fast charging and discharging of solid-state lithium metal batteries. In addition, the process of preparing polymer electrolytes by freeze-drying (liquid-solid-gas-solid-liquid transformation of solvents) can achieve efficient recovery and reuse of solvents.

[0017] The advantages and beneficial effects of the present invention are as follows:

[0018] 1. The method of the present invention has the characteristics of low cost and green environmental protection.

[0019] 2. The polymer electrolyte proposed in the present invention has the characteristics of high thermal stability, high ionic conductivity and wide electrochemical stability window.

[0020] 3. The polymer electrolyte prepared by the method proposed in the present invention exhibits a high capacity in a wide temperature range (-10 to 100° C.) for solid-state lithium metal batteries.

[0021] 4. The polymer electrolyte prepared by the method proposed in the present invention can be used in solid-state lithium metal batteries to achieve fast charging and discharging of the battery.

[0022] 5. The polymer electrolyte preparation process proposed in the present invention can realize the recycling and reuse of organic solvents in the preparation process, solving the problems of high cost, difficult recycling and high pollution caused by the use of volatile organic solvents in the existing polymer electrolyte production process. Description of the drawings:

[0023] Figure 1 Schematic diagram of the polymer electrolyte preparation process and solvent recovery.

[0024] Figure 2 is the electrochemical impedance of the polymer film prepared according to Example 1.

[0025] Figure 3 The charge and discharge curves of the solid-state battery prepared according to Example 5 at 100°C.

[0026] Figure 4 The charge and discharge curves of the solid-state battery prepared according to Example 5 at -10°C.

[0027] Figure 5 The charge and discharge curves of the solid-state battery prepared according to Example 7 at 25°C.

[0028] Figure 6 This is a safety test of the soft-pack battery prepared according to Example 6. Specific implementation method:

[0029] The following is an exemplary description of the various steps for preparing the polymer electrolyte and the solid-state lithium metal battery of the present invention.

[0030] Embodiment 1:

[0031] This embodiment is the preparation of a polymer electrolyte, and the process is as follows:

[0032] PVDF-HFP with a molecular weight of 400,000 and LiTFSI were dissolved in dimethyl sulfoxide solvent and stirred for 24 hours to obtain a uniform solution. Among them, the mass fraction of PVDF-HFP in the solution was 7.9wt.%, and the weight of LiTFSI accounted for 40wt.% of the total mass of LiTFSI and PVDF-HFP. Subsequently, the uniform solution was transferred to a polytetrafluoroethylene sheet, frozen at -18°C for 24 hours, and freeze-dried in a freeze dryer for 48 hours before being taken out to obtain a polymer electrolyte.

[0033] Figure 1 Shown is a schematic diagram of the polymer electrolyte preparation and solvent recovery process.

[0034] Embodiment 2:

[0035] This embodiment is the preparation of a polymer electrolyte, and the process is as follows:

[0036] PVDF with a molecular weight of 500,000 and LiTFSI were dissolved in N-methylpyrrolidone solvent and stirred for 24 hours to obtain a uniform solution. Among them, the mass fraction of PVDF in the solution was 7.9wt.%, and the weight of LiTFSI accounted for 40wt.% of the total mass of LiTFSI and PVDF. Subsequently, the uniform solution was transferred to a polytetrafluoroethylene sheet, frozen at -30°C for 24 hours, and freeze-dried in a freeze dryer for 48 hours before being taken out to obtain a polymer electrolyte.

[0037] Embodiment 3:

[0038] This embodiment is the preparation of a polymer electrolyte, and the process is as follows:

[0039] PAN with a molecular weight of 150,000 and LiFSI were dissolved in dimethyl sulfoxide solvent and stirred for 24 hours to obtain a uniform solution. Among them, the mass fraction of PAN in the solution was 5wt.%, and the weight of LiFSI accounted for 30wt.% of the total mass of LiFSI and PAN. Subsequently, the uniform solution was transferred to a polytetrafluoroethylene sheet, frozen at -18°C for 24 hours, and freeze-dried in a freeze dryer for 48 hours to obtain a polymer electrolyte.

[0040] Embodiment 4:

[0041] This embodiment is the preparation of a polymer electrolyte, and the process is as follows:

[0042] PVDF-HFP, LiTFSI and LiFSI with a molecular weight of 500,000 were dissolved in dimethyl sulfoxide solvent and stirred for 24 hours to obtain a uniform solution. Among them, the mass fraction of PVDF-HFP in the solution was 8wt.%, and LiTFSI and LiFSI accounted for 20wt.% of the total mass of lithium salt and PVDF-HFP, respectively. Subsequently, the uniform solution was transferred to a polytetrafluoroethylene sheet, frozen at -18°C for 24 hours, and freeze-dried in a freeze dryer for 48 hours before being taken out to obtain a polymer electrolyte.

[0043] Embodiment 5:

[0044] This embodiment is to prepare a high-performance lithium metal battery that works in a wide temperature range (-10 to 100° C.), and the process is as follows:

[0045] Lithium iron phosphate, polyvinylidene fluoride and conductive carbon black were mixed in N-methylpyrrolidone at a mass ratio of 8:1:1 to obtain a positive electrode slurry, which was coated on one side of the carbon-coated aluminum foil, and dried in a vacuum at 60°C to remove the N-methylpyrrolidone to obtain a positive electrode.

[0046] The obtained composite positive electrode was cut into positive electrode sheets, and the negative electrode was a lithium sheet. The polymer electrolyte in Example 1 was sandwiched between the positive electrode sheet and the negative electrode sheet and loaded into a 2025 battery shell to form a button battery for testing.

[0047] Example 6

[0048] This embodiment is to prepare a high-performance lithium metal battery that works in a wide temperature range (-10 to 100° C.), and the process is as follows:

[0049] Lithium iron phosphate, polyvinylidene fluoride and conductive carbon black were mixed in N-methylpyrrolidone at a mass ratio of 8:1:1 to obtain a positive electrode slurry, which was coated on one side of the carbon-coated aluminum foil, and dried in a vacuum at 60°C to remove the N-methylpyrrolidone to obtain a positive electrode.

[0050] The obtained positive electrode was cut into a positive electrode sheet, and the negative electrode was made of lithium foil. The polymer electrolyte in Example 1 was sandwiched between the positive electrode sheet and the negative electrode sheet for aluminum-plastic packaging to obtain a soft-pack battery, which was then tested.

[0051] Example 7

[0052] This embodiment is to prepare a high-performance lithium metal battery that works in a wide temperature range (-10 to 100° C.), and the process is as follows:

[0053] NCM811, polyvinylidene fluoride and conductive carbon black were mixed uniformly in N-methylpyrrolidone at a mass ratio of 8:1:1 to obtain a positive electrode slurry, and the positive electrode slurry was coated on one side of the carbon-coated aluminum foil. The positive electrode was dried at 60° C. in a vacuum to remove the N-methylpyrrolidone to obtain a positive electrode.

[0054] The obtained composite positive electrode was cut into positive electrode sheets, and the negative electrode was a lithium sheet. The polymer electrolyte in Example 1 was sandwiched between the positive electrode sheet and the negative electrode sheet and loaded into a 2025 battery shell to form a button battery for testing.

[0055] The following is the performance test of the samples prepared in each embodiment:

[0056] 1. Ionic conductivity test:

[0057] The polymer electrolyte prepared in Example 1 was punched out with a punching machine to obtain a polymer electrolyte disc. The sample thickness was found to be about 80 microns and the film diameter was 19 mm. The ionic conductivity of the sample in Example 1 was tested. The specific test method was as follows: stainless steel sheets were added to both ends of the sample to form a battery test. The diameter of the stainless steel sheet was 12 mm. The test frequency range was 0.1 Hz-1 MHz (electrochemical workstation). The impedance diagram at -10 to 80 ° C was shown in FIG. Figure 2 . Finally, the ionic conductivity of the sample is calculated based on parameters such as electrochemical impedance, sample thickness and electrode area. The ionic conductivity of the sample of Example 1 measured at 80°C is 2.43mS / cm; the ionic conductivity measured at 25°C is 0.353mS / cm; and the ionic conductivity measured at -10°C is 0.0317mS / cm. Therefore, the polymer electrolyte has high ionic conductivity in a wide temperature range (-10 to 80°C).

[0058] 2. Charge and discharge test:

[0059] The lithium metal battery prepared in Example 5 was tested at 100°C. The charge cut-off voltage was 3.9V, and the discharge cut-off voltage was 2.5V. The charge and discharge current was set to 1-50C. Figure 3As shown in the figure, it is a charge and discharge curve of the lithium metal battery prepared according to Example 5 at 100°C. As can be seen from the figure, the discharge specific capacity of the lithium metal battery containing the polymer electrolyte at 30C and 50C is as high as 141.6mAh / g and 102.2mAh / g respectively. Therefore, this type of solid-state lithium metal battery has fast charge and discharge capabilities.

[0060] The lithium metal battery prepared in Example 5 was tested at -10°C. The charge cut-off voltage was 4.2V, and the discharge cut-off voltage was 2.5V. The charge and discharge currents were set to 0.05C and 0.1C. Figure 4 As shown, it is a charge and discharge curve of the lithium metal battery prepared according to Example 5 at -10°C. As can be seen from the figure, the discharge specific capacity of the lithium metal battery containing the polymer electrolyte at 0.05C and 0.1C is as high as 135mAh / g and 109.2mAh / g respectively. Therefore, this type of solid-state lithium metal battery has a higher charge and discharge capacity at low temperatures.

[0061] The lithium metal battery prepared in Example 7 was tested at 25°C. The charge cut-off voltage was 4.3V, and the discharge cut-off voltage was 3.0V. The charge and discharge current was set to 0.2C. Figure 5 The figure shows the charge and discharge curve of the lithium metal battery prepared according to Example 4 at room temperature. As can be seen from the figure, the discharge capacity of the lithium metal battery containing the polymer electrolyte is as high as 167.7 mAh / g. Therefore, the polymer electrolyte is suitable for high-voltage solid-state lithium metal batteries.

[0062] 3. Soft pack battery safety test:

[0063] The safety test of the soft-pack battery prepared in Example 6 was carried out, and the specific test method was: using scissors to destructively cut the soft-pack battery, and then lighting the LED light board. Figure 6 As shown, the soft pack battery can still supply power to the LED light board normally even if it is cut several times. Therefore, the soft pack battery containing the polymer electrolyte has higher safety.

[0064] The above description is only a preferred embodiment of the present invention. It should be pointed out that the above embodiments are illustrative in nature and cannot be understood as limitations of the present invention. Several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a polymer electrolyte, characterized in that: The method comprises the following steps: (1) dissolving the polymer and lithium salt in a solvent in proportion, and stirring to obtain a mixed solution; (2) freezing the mixed solution obtained in step (1) in a low-temperature environment, and after the solvent in the mixed solution is completely solidified, removing the solid solvent through a vacuum freeze-drying device to obtain the polymer electrolyte; In step (1), the polymer is at least one of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), polymethacrylate (PMMA) and polypropylene carbonate (PPC); The solvent is at least one of dimethyl sulfoxide, sulfolane, N-methylpyrrolidone, benzene, tert-butyl alcohol, cyclohexane, acetic acid and N, N-dimethylformamide.

2. The method for preparing a polymer electrolyte according to claim 1, characterized in that: In step (2), the solid solvent captured in the cold trap of the vacuum freeze-drying device can be heated and melted for recycling.

3. The method for preparing a polymer electrolyte according to claim 1, characterized in that: In step (1), the lithium salt is at least one of lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium chloride (LiCl), lithium nitrate (LiNO3), lithium tetrafluoroborate (LiBF4) and lithium hexafluoroarsenate (LiAsF6).

4. The method for preparing a polymer electrolyte according to claim 1, characterized in that: In step (1), the weight of the lithium salt is 10 wt.% to 60 wt.% of the total weight of the polymer and the lithium salt; and the weight of the solvent is 5 to 100 times the weight of the polymer.

5. The method for preparing a polymer electrolyte according to claim 1, characterized in that: In step (2), the vacuum freeze-drying device includes a drying chamber, a vacuum pump and a cold trap.

6. The method for preparing a polymer electrolyte according to claim 1, characterized in that: In step (1), the stirring time is 12 to 48 hours; in step (2), the freezing temperature is -50 to 0°C, and the insulation time is 1 to 48 hours; and the drying time in the vacuum freeze-drying device is 12 to 60 hours.

7. A polymer electrolyte prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the polymer electrolyte according to claim 7 in a solid-state lithium metal battery, characterized in that: The polymer electrolyte is applied to solid-state lithium metal batteries under a wide temperature range and fast charge and discharge conditions, wherein the wide temperature range is -10 to 100°C, and the fast charge and discharge conditions are charge and discharge at a rate of 1 to 50C.