A lithium ion battery composite diaphragm with uniform pore structure and preparation method thereof
Ultra-fine spherical alumina powder prepared by thermal plasma technology forms a lithium-ion battery composite separator with a uniform pore structure, which solves the problems of low porosity and complex process of existing ceramic separators, and achieves high safety performance and low-cost lithium ion battery separator. Ion battery separator preparation.
Patent Information
- Application Number
- CN202210250708.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-15
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-03-15
AI Technical Summary
The porosity of existing ceramic separators is low, which limits the safety of lithium-ion batteries. The preparation process is complex and costly, making it difficult to obtain a composite separator with a uniform pore structure.
Using ultra-fine spherical alumina powder prepared based on thermal plasma technology, it is dispersed in an organic solvent to form an alumina coating slurry, which is evenly coated on the polypropylene separator to form a composite separator with a uniform pore structure, avoiding The step of adding pore-forming agent simplifies the process flow.
A composite separator with uniform pore size and moderate air permeability is obtained, which meets the requirements of high-safety lithium-ion batteries. The process is simple, low-cost, and suitable for large-scale production.
Smart Images

Figure CN114597595B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery composite diaphragm preparation, and in particular relates to a lithium ion battery composite diaphragm with a uniform pore structure and a preparation method thereof. Background Art
[0002] As a secondary battery, lithium-ion batteries have the characteristics of high energy density, long cycle life, high open circuit voltage, and no memory effect. They are widely used in mobile electronic devices and new energy vehicles. In particular, benefiting from the rapid growth of new energy vehicles, the lithium-ion battery industry has ushered in a new round of development opportunities. Safety issues are the core of the promotion of new energy vehicles and the sustainable development of the power battery industry. The diaphragm is a key component that affects the safety of lithium-ion batteries. The diaphragm provides a large number of tortuous micropores for the free passage of electrolyte ions to form a discharge circuit. At the same time, under uncontrolled conditions such as increased battery temperature, the closed-cell barrier function separates the positive and negative electrodes of the battery to prevent short circuits. Therefore, the safety of lithium-ion batteries depends to a large extent on the performance of the diaphragm.
[0003] The commonly used diaphragm is a ceramic diaphragm, but the existing ceramic diaphragms such as Separion diaphragms are made of cellulose non-woven fabrics and have compacted Al2O3 on the surface, so their porosity is low, which limits their performance. Improving the structure of the ceramic coating (including continuity, porosity, pore size, etc.) can improve the performance of the diaphragm and the safety of lithium-ion batteries. Application No. 201810673343.2 discloses a composite ceramic porous lithium-ion battery diaphragm, a preparation method and its application. The diaphragm is prepared by a wet process, and a nano-scale ceramic diaphragm is evenly added during the raw material preparation process. It is extruded and stretched together with the polyethylene raw material, and the pore-forming agent is removed by soaking in an organic solvent to form a diaphragm with a porous structure. However, this process generally has the defects of uneven pore structure, complicated process, and high cost. There is an urgent need for a preparation method for a lithium-ion battery composite diaphragm with a simple process and low cost to obtain a uniform pore structure. Summary of the invention
[0004] The purpose of the present invention is to provide a lithium-ion battery composite diaphragm with a uniform pore structure and a preparation method thereof, which is simple and easy to operate. Ultrafine spherical alumina powder prepared based on thermal plasma technology is used as a raw material to prepare a coating slurry to obtain a lithium-ion battery composite diaphragm with a uniform pore structure. This process is simple to operate, does not require the addition of a pore-forming agent, and the obtained pore structure is uniform and controllable, meeting the requirements for the application of high-safety power lithium-ion batteries.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A lithium ion battery composite diaphragm with a uniform pore structure comprises a polypropylene base layer and an aluminum oxide coating layer, wherein the aluminum oxide coating layer is a porous structure formed by the accumulation of spherical ultrafine aluminum oxide particles.
[0007] Furthermore, the pore size of the porous structure of the alumina coating is 300-800nm, the thickness of the alumina coating is 3-15μm, the air permeability of the composite membrane is 15-25s / 100ml, the porosity of the composite membrane is 40-60%, the puncture strength is greater than 350gf, the tensile strength is greater than 170MPa, and the thermal shrinkage rate (105℃ / 2 hours) is less than 1.2%.
[0008] A method for preparing a lithium ion battery composite diaphragm with a uniform pore structure comprises the following steps:
[0009] (1) dispersing spherical ultrafine alumina powder in an organic solvent to obtain a dispersion and collecting the upper suspension after settling to obtain an alumina dispersion;
[0010] (2) adding PVDF to the alumina dispersion obtained in step (1) and stirring the mixture to obtain an alumina coating slurry;
[0011] (3) The aluminum oxide coating slurry is evenly coated on the surface of the polypropylene diaphragm and dried to obtain a lithium ion battery composite diaphragm with a uniform pore structure.
[0012] Furthermore, in the step (1), the particle size of the spherical ultrafine alumina powder is 10-1000nm, and the spherical ultrafine alumina is obtained by loading aluminum powder raw material into a high-temperature plasma arc with oxygen-containing gas and undergoing gas phase reaction deposition; the organic solvent is at least one of N-methylpyrrolidone, dimethylformamide, and acetone, and the standing time in the step (1) is 10-30min. The purpose of the standing time is to improve the uniformity of the dispersion by settling out the agglomerates in the alumina powder and reduce the defects of the alumina coating in the composite diaphragm.
[0013] Furthermore, the content of aluminum oxide in the aluminum oxide dispersion in step (2) is 20-50 wt %, and the content of PVDF in the aluminum oxide coating slurry is 5 wt %-30 wt %, and the addition of PVDF acts as an adhesive.
[0014] Furthermore, in the step (3), the coating process adopts a flat scraping process, and after scraping, the coating is dried at 80° C. for 1 to 4 hours.
[0015] A lithium ion battery composite separator with uniform pore structure is used in the manufacture of lithium ion batteries.
[0016] The advantages of the present invention are: the composite diaphragm obtained by the present invention has a uniform pore structure, can be used for high-end diaphragms for lithium-ion batteries with high safety performance, and a thinner alumina coating can be obtained by using ultrafine spherical alumina powder instead of ordinary spherical alumina. In addition, the ultrafine alumina powder has a relatively low melting and sintering temperature, and can start safety protection at a relatively low temperature compared to ordinary alumina. The formation of the uniform pore structure is mainly based on the solvent volatilization mechanism. In this process, there is no need to add pore-forming agents and surfactants. The process is simple, low-cost, and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a scanning electron microscope photograph of the surface of the composite diaphragm obtained in Example 1;
[0018] Figure 2 is a scanning electron microscope photograph of the surface of the composite diaphragm obtained in Example 2;
[0019] Figure 3 is a scanning electron microscope photograph of the surface of the composite diaphragm obtained in Example 3;
[0020] Figure 4 is a scanning electron microscope photograph of the surface of the composite diaphragm obtained in Example 5;
[0021] Figure 5 is a scanning electron microscope photograph of the surface of the composite diaphragm obtained in Example 6;
[0022] Figure 6 1 is a scanning electron microscope photograph of the surface of the polypropylene diaphragm used in Examples 1 to 6. DETAILED DESCRIPTION
[0023] Example 1
[0024] First, 100 g of ultrafine spherical alumina powder prepared based on thermal plasma technology was weighed, added to 200 mL of N-methylpyrrolidone, and stirred and dispersed for 10 min to obtain a dispersion of ultrafine spherical alumina in N-methylpyrrolidone; then, the above dispersion was allowed to stand for 5 min, and 180 mL of the upper dispersion was poured out; then, 10 g of PVDF was added to the upper dispersion, and the mixture was dispersed at a stirring speed of 1500 rpm for 30 min to obtain an alumina coating slurry; finally, a lithium-ion battery composite diaphragm was obtained by scraping on a heated coating machine, the coating thickness was set to 15 μm, the heating temperature was 80 ° C, and the insulation time was 60 min. The prepared composite diaphragm was subjected to performance testing, and the specific results are shown in Table 1.
[0025] Table 1
[0026] serial number Test items unit Numeric 1 thickness μm 24 2 Porosity % 50 3 Heat shrinkage (MD) (105℃ / 2 hours) % 1.1 4 Puncture strength gf 410 5 Tensile strength (MD) MPa 193
[0027] Example 2
[0028] First, 100 g of ultrafine spherical alumina powder prepared based on thermal plasma technology was weighed, added to 200 mL of N-methylpyrrolidone, and stirred and dispersed for 10 min to obtain a dispersion of ultrafine spherical alumina in N-methylpyrrolidone; then, 10 g of PVDF was added to the above upper dispersion, stirred at 1500 rpm for 30 min, and an alumina coating slurry was obtained; finally, a lithium-ion battery composite diaphragm was obtained by scraping on a heated coating machine, the coating thickness was set to 15 μm, the heating temperature was 80 ° C, and the insulation time was 60 min.
[0029] Example 3
[0030] First, 100 g of ultrafine spherical alumina powder prepared based on thermal plasma technology was weighed, added to 200 mL of acetone, and stirred and dispersed for 10 minutes to obtain a dispersion of ultrafine spherical alumina in acetone; then, the above dispersion was allowed to stand for 5 minutes, and 180 mL of the upper dispersion was poured out; then, 10 g of PVDF was added to the upper dispersion, and the mixture was dispersed at a stirring speed of 1500 rpm for 30 minutes to obtain an alumina coating slurry; finally, a lithium-ion battery composite separator was obtained by scraping on a heated coating machine, and the coating thickness was set to 15 μm, the heating temperature was 80°C, and the insulation time was 60 minutes.
[0031] Example 4
[0032] First, 100 g of ultrafine spherical alumina powder prepared based on thermal plasma technology was weighed, added into 200 mL of a mixed solvent consisting of N-methylpyrrolidone (50 wt%) and acetone (50 wt%), and stirred and dispersed for 10 min to obtain a dispersion of ultrafine spherical alumina in the mixed solvent; then, the above dispersion was allowed to stand for 5 min, and 180 mL of the upper dispersion was poured out; then, 10 g of PVDF was added to the upper dispersion, and the mixture was dispersed at a stirring speed of 1500 rpm for 30 min to obtain an alumina coating slurry; finally, a lithium-ion battery composite separator was obtained by scraping on a heated coating machine, and the coating thickness was set to 15 μm, the heating temperature was 80 ° C, and the insulation time was 60 min.
[0033] Example 5
[0034] First, 100 g of ultrafine spherical alumina powder prepared based on thermal plasma technology was weighed, added to 200 mL of N-methylpyrrolidone, and stirred and dispersed for 10 minutes to obtain a dispersion of ultrafine spherical alumina in N-methylpyrrolidone; then, the above dispersion was allowed to stand for 5 minutes, and 180 mL of the upper dispersion was poured out; then, 10 g of PVDF was added to the upper dispersion, and the mixture was dispersed at a stirring speed of 1500 rpm for 30 minutes to obtain an alumina coating slurry; finally, a polypropylene diaphragm was immersed in the alumina coating slurry and pulled twice by a pulling method, and the alumina coating slurry was coated on the surface of the polypropylene diaphragm, and the mixture was kept warm at 80°C in a drying oven for 60 minutes to obtain a lithium-ion battery composite diaphragm.
[0035] Example 6
[0036] First, weigh 100g of commercially available ultrafine alumina, add it to 200mL of N-methylpyrrolidone, and stir and disperse it for 10min to obtain a dispersion of ultrafine spherical alumina in N-methylpyrrolidone; then, let the above dispersion stand for 5min, pour out 120mL of the upper dispersion; then, add 10g of PVDF to the above upper dispersion, stir at 1500rpm for 30min, and obtain an alumina coating slurry; finally, obtain a lithium-ion battery composite diaphragm by scraping on a heated coating machine, the coating thickness is set to 15μm, the heating temperature is 80℃, and the insulation time is 60min.
[0037] The final products prepared in the above-mentioned Examples 1 to 6 were tested, and the results and analysis were as follows:
[0038] The diaphragm prepared in Example 1 was tested for microscopic morphology. The surface of the diaphragm was still relatively flat in the entire field of view, and a regular porous structure appeared. The pore size of the inorganic coating surface was uniform, about 500 nm. The enlarged SEM photo showed that the porous membrane was assembled from nano-alumina particles.
[0039] The diaphragm prepared in Example 2 was tested for microscopic morphology, and compared with Example 1, it was found that large alumina particles and traces of large particles appeared in some places. A simple sedimentation method can remove individual coarse particles in the alumina powder, and the coating slurry prepared on this basis helps to obtain a uniform porous structure.
[0040] The microscopic morphology of the diaphragms prepared in Example 3 and Example 4 was detected, and compared with Example 1, it was found that when N-methylpyrrolidone, acetone, and ethanol were used as dispersion liquids, the film uniformity results showed that N-methylpyrrolidone was the best, acetone was the second, and ethanol was the worst. Therefore, N-methylpyrrolidone is preferred as the dispersion solvent.
[0041] The diaphragm prepared in Example 5 was subjected to microscopic morphology detection. The surface of the organic diaphragm in the product pulled once was not yet covered with aluminum oxide particles, and no porous structure assembled by aluminum oxide particles appeared. As a result of the secondary pulling, the number of aluminum oxide particles on the surface of the organic diaphragm increased, but there was still no porous structure assembled by aluminum oxide particles. This result shows that the scraping method is an important factor in producing a regular and uniform porous structure. The scraping process has low requirements on the concentration, viscosity, adhesion and other parameters of the slurry, and can effectively control the film thickness, which is convenient for scale-up production. Therefore, the scraping method is preferred as the coating process.
[0042] The diaphragm prepared in Example 6 was subjected to microscopic morphology inspection. Compared with Example 1, it was found that the flatness and uniformity were very poor, and the regular porous assembly structure observed in the entire field of view was not very similar to that in Example 1, indicating that the spherical structure, high dispersibility, morphology and particle size consistency of plasma-prepared alumina are key conditions for obtaining a uniform porous structure.
Claims
1. A method for preparing a lithium-ion battery composite diaphragm with a uniform pore structure, wherein the composite diaphragm comprises a polypropylene base layer and an alumina coating layer, wherein the alumina coating layer is a porous structure formed by accumulation of spherical ultrafine alumina particles, characterized in that: The pore size of the porous structure of the alumina coating is 300-800nm, the thickness of the alumina coating is 3-15μm, the air permeability of the composite membrane is 15-25s / 100ml, the porosity of the composite membrane is 40-60%, the puncture strength is greater than 350gf, the tensile strength is greater than 170MPa, and the thermal shrinkage is less than 1.2%. The preparation method comprises the following steps: Step (1), dispersing spherical ultrafine alumina powder in an organic solvent to obtain a dispersion and collecting the upper suspension after standing and settling to obtain an alumina dispersion, wherein the particle size of the spherical ultrafine alumina powder is 10-1000 nm, and the spherical ultrafine alumina is obtained by loading an aluminum powder raw material into a high-temperature plasma arc with oxygen-containing gas and undergoing gas phase reaction deposition; the organic solvent is N-methylpyrrolidone; Step (2), adding PVDF to the alumina dispersion obtained in step (1) and stirring evenly to obtain an alumina coating slurry; Step (3), evenly coating the aluminum oxide coating slurry on the surface of the polypropylene diaphragm and drying it to obtain a lithium ion battery composite diaphragm with a uniform pore structure. The coating process adopts a flat scraping process, and after scraping, it is dried at 80° C. for 1 to 4 hours.
2. The method for preparing a lithium ion battery composite diaphragm having a uniform pore structure according to claim 1, characterized in that: In the step (2), the content of aluminum oxide in the aluminum oxide dispersion is 20-50 wt %, and the content of PVDF in the aluminum oxide coating slurry is 5 wt %-30 wt %.
3. The lithium ion battery composite separator with uniform pore structure as described in any one of claims 1 to 2 is applied to lithium ion batteries.