Pressurizing rotating member and production method, fixing device and image forming device
By designing a specific hole orientation degree and orientation angle in the surface layer of the rotating member for pressing and forming a hole in the perfluoropolyether, the contradiction between durability and thermal insulation of the pressing member in the prior art is solved, and the result is achieved. Shorter first printout time and higher durability.
Patent Information
- Application Number
- CN202111588896.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-11-30
- Filing Date
- 2021-12-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-12-23
AI Technical Summary
Increased surface layer hollow particles of existing pressurized members lead to improved thermal insulation, but reduced strength and cracks appear, making it difficult to find a balance between maintaining durability and thermal insulation.
The construction of a base layer, an elastic layer and a surface layer, wherein the surface layer has a specific pore orientation and orientation angle, is produced by cylindrical extrusion and impregnated in perfluoropolyether to form pores to improve thermal insulation and maintain strength.
A high level of surface layer durability and thermal insulation are achieved, the first print output time is shortened, and the overall performance of the rotating member for pressurization is improved.
Smart Images

Figure CN114690605B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure is directed to providing a pressing rotating member and a production method thereof, a fixing apparatus, and an electrophotographic image forming apparatus. Background Art
[0002] Examples of fixing devices used in electrophotographic image forming apparatuses (hereinafter, "image forming apparatuses") such as copiers or laser printers include fixing devices having a heating rotating member and a pressing rotating member configured to be in pressure contact with the heating rotating member. In such fixing devices, paper on which an unfixed toner image is held is introduced into a nip formed by the heating rotating member and the pressing rotating member, and the toner is heated and pressed, and as a result, the image becomes fixed to the paper. The pressing rotating member may be referred to as a pressing roller when it has a roller shape, or may be referred to as a pressing belt when it has an endless belt shape.
[0003] Japanese Patent Application Publication No. 2014-232208 discloses a fixing pressure member in which the surface of a pressure member serving as a pressing rotation member is composed of a layer containing a fluororesin and hollow particles having an outer shell formed of an inorganic material in an amount of 10 parts by weight or more relative to 100 parts by weight of the fluororesin.
[0004] The surface layer of the pressurizing member according to Japanese Patent Application Publication No. 2014-232208 contains a fluororesin and is porous by containing hollow particles; therefore, the pressurizing member can be expected to show an inhibitory effect on toner adhesion on the member surface and an inhibitory effect on heat transfer from the heating member toward the pressurizing member. Considering the demand for achieving a shorter first print out time (FPOT) in an electrophotographic device, it is necessary to further improve the thermal insulation of the pressurizing member. It is presumed that a higher thermal insulation of the surface layer constituting the surface of the pressurizing member that is in direct contact with paper (hereinafter, also referred to as the "outer surface") will be effective in further shortening the FPOT.
[0005] Therefore, the inventors have proposed a method of increasing the amount of hollow particles added to the surface layer of the pressurized member according to Japanese Patent Application Publication No. 2014-232208, and increasing the porosity by using hollow particles with a large particle size. However, it was found that as a result, the strength of the surface layer of the pressurized member was reduced, and cracks or breakage occurred in the surface layer during long-term use. Therefore, the inventors recognized that in order to further improve the thermal insulation while maintaining the durability of the surface layer, it is necessary to develop a technology that aims to achieve a pressurized rotating member having a structure that improves the thermal insulation of the surface layer of the pressurized rotating member according to a method other than introducing hollow particles. Summary of the invention
[0006] At least one aspect of the present disclosure is directed to providing a pressurizing rotating member capable of exhibiting both surface layer durability and excellent thermal insulation at a high level. Another aspect of the present disclosure is directed to providing a fixing device that helps shorten the first printout time. Yet another aspect of the present disclosure is directed to providing an image forming device having a first printout time that is shorter than conventional technologies. Yet another aspect of the present disclosure is directed to providing a method for producing a pressurizing rotating member capable of exhibiting both surface layer durability and excellent thermal insulation at a high level.
[0007] According to one aspect of the present disclosure, there is provided a pressurizing rotating member, which includes a base layer, an elastic layer and a surface layer in sequence.
[0008] The surface layer has pores,
[0009] When an observation region of 8 μm in length and 11 μm in width is set in a cross section of the surface layer in the direction perpendicular to the circumferential direction of the pressing rotating member in the thickness direction of the surface layer, and the orientation degree of the pores observed in the observation region is defined as f, and the orientation angle of the pores observed in the observation region is defined as Φ, f and Φ satisfy the following relationship:
[0010] f is greater than 0.20;
[0011] Φ is 0° to 10°.
[0012] According to another aspect of the present disclosure, there is provided a fixing device including the above-mentioned pressing rotating member, a fixing belt, and a heating means for the fixing belt.
[0013] According to still another aspect of the present disclosure, there is provided an electrophotographic image forming apparatus including the above-mentioned fixing apparatus.
[0014] According to another aspect of the present disclosure, a method for producing a pressurizing rotating member is provided, wherein the pressurizing rotating member sequentially comprises a base layer, an elastic layer and a surface layer, wherein the surface layer has holes,
[0015] The above method comprises the following steps:
[0016] (i) providing a resin tube produced by a cylindrical extrusion method;
[0017] (ii) obtaining a laminated body having an endless belt-shaped or roller-shaped substrate, an elastic layer covering the outer peripheral surface of the substrate, and a resin tube covering the outer peripheral surface of the elastic layer;
[0018] (iii) immersing the laminate in perfluoropolyether to allow the perfluoropolyether to impregnate into the resin tube; and
[0019] (iv) The perfluoropolyether that has penetrated into the resin tube of the laminate obtained in step (iii) is removed with a solvent to form pores in the resin tube to obtain a surface layer.
[0020] Further features of the present invention will become apparent from the following description of exemplary embodiments with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram showing a method for confirming the degree of orientation f and the orientation angle Φ of a hole;
[0022] Figure 2 An observation image observed in a cross section parallel to the longitudinal direction of the pressurizing rotating member of the surface layer of the pressurizing rotating member described in Example 1;
[0023] Figure 3 A schematic cross-sectional view of one aspect of a pressurizing rotating member;
[0024] Figure 4 is a schematic cross-sectional view of one aspect of a fixing device using a pressing rotating member; and
[0025] Figure 5 is a schematic diagram showing one aspect of an electrophotographic image forming apparatus. DETAILED DESCRIPTION
[0026] In addition, in the present disclosure, the expression "from XX to YY" or "XX to YY" indicating a numerical range refers to a numerical range including a lower limit and an upper limit as endpoints, unless otherwise specified. When the numerical range is set in segments, the upper and lower limits of each numerical range can be combined in any combination.
[0027] In the present disclosure, the term “longitudinal direction” means a direction perpendicular to the circumferential direction of the pressing rotating member.
[0028] The present inventors have conducted repeated studies with the aim of obtaining a pressurizing rotating member capable of exhibiting both surface layer durability and excellent heat insulation at a high level. As a result, the present inventors have found that by orienting the pores in the surface layer so that the orientation degree f and the orientation angle Φ of the pores exhibit specific values as observed in a cross section of the thickness of the surface layer-a direction perpendicular to the circumferential direction of the pressurizing rotating member, it is possible to reduce heat transfer in the thickness direction of the surface layer while reducing a decrease in the strength of the surface layer.
[0029] That is, the pressurizing rotation member according to one aspect of the present disclosure includes a base layer, an elastic layer, and a surface layer in this order, and the surface layer has holes.
[0030] Furthermore, when an observation area of 8 μm in length and 11 μm in width is set in the cross-section of the surface layer in the thickness direction of the surface layer - the direction perpendicular to the circumferential direction of the pressurizing rotating member, and the orientation degree of the holes observed in the observation area is defined as f, and the orientation angle of the holes observed in the observation area is defined as Φ, f is greater than 0.20, and Φ is 0° to 10°.
[0031] In the case where the orientation degree f and the orientation angle Φ of the pores observed in the observation area fall within the above ranges, the pores exist in a layered manner in the longitudinal direction of the pressing rotating member in the surface layer (see Figure 2 ). This configuration effectively blocks the flow of heat from the surface of the pressurizing rotating member opposite to the surface layer toward the base layer side of the pressurizing rotating member. As a result, it becomes possible to improve the thermal insulation of the surface layer in the thickness direction while avoiding an excessive increase in the porosity of the surface layer that causes a decrease in the strength of the surface layer.
[0032] One aspect of a pressurizing rotating member according to the present disclosure will be described below.
[0033] 1. Pressurizing rotating member
[0034] The pressing rotating member includes a base layer, an elastic layer and a surface layer in sequence.
[0035] Figure 3 1 is a cross-sectional schematic diagram of one aspect of a pressurizing rotating member (hereinafter, referred to as "pressurizing rotating member 19"). The pressurizing rotating member 19 has a cylindrical or columnar base layer 19a and an elastic layer 19b formed as a cylindrical tube concentric with the base layer 19a on the outer peripheral surface of the base layer 19a. The outer peripheral surface of the elastic layer 19b is covered with a surface layer 19c as the outermost layer. The elastic layer 19b can be bonded to the outer peripheral surface of the base layer 19a via an adhesive layer not shown. The surface layer 19c can be bonded to the outer peripheral surface of the elastic layer 19b via an adhesive layer not shown.
[0036] The shape of the pressing rotating member is not particularly limited, and for example, the pressing rotating member may be a pressing belt having an endless belt shape or may be a pressing roller having a roller shape.
[0037] 1-1. Grassroots
[0038] A substrate made of iron or aluminum is preferably used as the base layer 19a. The surface of the substrate may be activated in advance by sandblasting or the like, or may be degreased with, for example, methylene chloride, a hydrocarbon-based cleaning agent, or an aqueous cleaning agent.
[0039] In the case where the elastic layer 19b including silicone rubber is provided on the surface of the base layer 19a, in order to improve the adhesion between the base layer 19a and the elastic layer 19b, the surface of the base layer 19a is preferably subjected to primer treatment.
[0040] Examples of primers used in the primer treatment include coatings in which a silane coupling agent, an organic silicon polymer, hydromethylsiloxane, an alkoxysilane, a reaction accelerating catalyst, and / or a colorant such as red iron oxide are appropriately blended and dispersed in an organic solvent.
[0041] The primer can be appropriately selected according to the material of the base layer 19a, the type of the elastic layer 19b, and the form of the cross-linking reaction. In particular, when the elastic layer 19b contains a large number of unsaturated aliphatic groups, in order to impart adhesion derived from the reaction of the unsaturated aliphatic groups, it is preferable to use a primer containing a hydrosilyl group. When the elastic layer 19b contains a large number of hydrosilyl groups, it is preferable to use a primer containing an unsaturated aliphatic group.
[0042] Other primers include primers containing alkoxy groups. Commercially available products can be used as primers. The primer treatment includes the steps of applying the primer to the outer surface of the base layer 19a (the surface to be bonded to the elastic layer 19b), and drying or baking.
[0043] Commercially available products can be used as the primer. Specifically, for example, a primer which is an equal amount mixture of "Liquid A" and "Liquid B" of DY35-051 manufactured by Dow Corning Toray Co., Ltd. can be used.
[0044] 1-2. Elastic layer
[0045] The material of the elastic layer 19b is not particularly limited, and a known material used as an elastic layer of a pressurizing rotating member can be used. The elastic layer 19b is a layer for forming the fixing nip portion N described below in "2. Fixing device", and can be a solid rubber layer or a foamed rubber layer. The thickness of the elastic layer 19b used in the pressurizing rotating member 19 is not particularly limited as long as the fixing nip portion N of a desired width can be formed, but is preferably 2 mm to 10 mm.
[0046] Any of the following is preferably used as the main polymer of the elastic layer 19b. For example, high temperature vulcanized (HTV) silicone rubber, addition reaction curable (LTV; low temperature vulcanized) silicone rubber, condensation reaction curable (RTV; room temperature vulcanized) silicone rubber, addition type liquid silicone rubber, fluorocarbon rubber, and mixtures thereof. Specifically, silicone rubbers such as dimethyl silicone rubber, fluorosilicone rubber, methylphenyl silicone rubber or vinyl silicone rubber can be used here; or fluorocarbon rubbers such as vinylidene fluoride rubber, tetrafluoroethylene-propylene rubber, tetrafluoroethylene-perfluoromethyl vinyl ether rubber, phosphazene fluorocarbon rubber or fluoropolyether can be used. Commercially available polymers can be used as the main polymer; specifically, a polymer that is an equal mixture of "Liquid A" and "Liquid B" of DY35-1349SC made by Dow Corning Toray Co., Ltd. can be used. These main polymers can be used as a single one or in combination of two or more.
[0047] As required, reinforcing fillers such as carbon black, wet silica or dry silica, or extending fillers such as calcium carbonate or quartz powder may be added to the main polymer.
[0048] The adhesive layer may be formed on the outer periphery of the elastic layer 19b. Although not limited thereto, an addition curable silicone rubber adhesive such as a mixture of equal amounts of "Liquid A" and "Liquid B" of SE1819CV manufactured by Dow Corning Toray Co., Ltd. may be used as the adhesive layer.
[0049] Furthermore, the adhesive layer may be used together with an antistatic agent such as potassium pentafluoroethanesulfonate. When the antistatic agent is used together, the amount of the antistatic agent added may be set to 0.1 to 5 parts by mass relative to 100 parts by mass of the adhesive used in the adhesive layer.
[0050] The thickness of the adhesive layer formed on the outer periphery of the elastic layer 19 b can be set to, for example, 0.5 μm to 20 μm.
[0051] 1-3. Surface layer
[0052] The surface layer 19c has pores. As observed in a region of 8 μm in length and 11 μm in width in a cross section in the thickness direction of the surface layer and in the length direction of the pressurizing rotating member (i.e., in a direction perpendicular to the circumferential direction), the pores of the surface layer 19c have an orientation degree f of 0.20 or more, and an orientation angle Φ of the pores of 0° to 10°.
[0053] The orientation angle Φ and the orientation degree f of the pores calculated according to the above method are parameters indicating the orientation direction and the orientation degree with respect to the length direction of the pores in the surface layer.
[0054] 1-3-1. Calculation method of orientation angle Φ and orientation degree f of pores in the surface layer
[0055] The sample is cut out from the pressurizing rotating member using a slice preparation device (e.g., a cryo-ultramicrotome (product name: manufactured by Leica Microsystems GmbH)) so that a cross section of the thickness of the pressurizing rotating member-the length direction of the pressurizing rotating member appears on the surface of the sample. As necessary, a portion of the cross section corresponding to the total thickness of the surface layer is milled using an ion beam. For example, a cross-section milling machine can be used to mill the obtained cross section using an ion beam.
[0056] Then, the cross section is observed under a scanning electron microscope, and an image (SEM image) of a rectangular observation area of 8 μm in length and 11 μm in width is collected at a predetermined position of the cross section. Image collection is adjusted so that the length direction of the image is the thickness direction of the surface layer and the transverse direction of the image is parallel to the length direction of the pressurizing rotating member. The resolution (e.g., 717 pixels × 986 pixels) is set so that the pores appearing in the cross section can be analyzed.
[0057] Figure 2 FIG. 2 is an enlarged schematic diagram of a portion of a SEM image, in which pores 202 exist in the resin portion 201 of the surface layer. Figure 2 As shown, the pores in the surface layer according to one aspect of the present disclosure produced according to the method described later have no shell, and thus the walls of the pores are constituted by the resin portion 201 .
[0058] The obtained SEM image was binarized using numerical calculation software (product name: MATLAB; manufactured by The MathWorks, Inc.) so as to be able to distinguish two regions corresponding to the resin portion 201 and the hole 202, respectively. The Otsu method disclosed in "IEEE Transactions on SYSTEMS, MAN, AND CYBERNETICS, vol. SMC-9, No. 1, Jan 1979, pp. 62-66" was adopted herein for binarization. Then, the binarized image obtained as a result of the above binarization process was subjected to two-dimensional Fourier transform analysis using the above numerical analysis software, and the obtained power spectrum was integrated in each direction, thereby obtaining a plot representing the orientation of the hole ( Figure 1 ).
[0059] The two-dimensional Fourier transform has a peak in a direction orthogonal to the periodicity of the image, so when the two-dimensional Fourier transform is applied to an image of a thickness-length cross section, the 90° to 270° direction represents the length direction of the surface layer. In this figure, the angle (0° to 90°) formed by the longest diameter relative to the 90° to 270° direction is taken as the orientation angle Φ. The closer the orientation angle Φ is to 0°, the greater the degree of orientation of the hole in the length direction. That is, the orientation angle Φ is a parameter representing the orientation of the hole relative to the length direction.
[0060] Furthermore, the degree of orientation f is defined as f=1-(y / x), where x represents the length of a line segment having the longest diameter and y represents the length of a line segment perpendicular to the longest diameter. Figure 1 The method for confirming the orientation angle Φ and the orientation degree f is shown. The orientation degree f takes a value of 0.00 and less than 1.00. In the case of non-oriented, completely random pores, the orientation degree f is 0.00; that is, as the orientation degree of the pores increases, the orientation degree f approaches 1.00. Therefore, the orientation degree is a parameter indicating the degree of orientation of the pores in the length direction.
[0061] The SEM images are collected from the cross section of the sample at the three positions specified below. Specifically, the upper end of the observation area is located at a position 1 μm in the depth direction of the surface layer from the outer surface of the surface layer constituting the outer surface of the pressurizing rotating member that constitutes the contact surface with the heating rotating member in the self-fixing device; the lower end of the observation area is located at a position 1 μm toward the outer surface from the surface of the surface layer on the opposite side of the outer surface (that is, 1 μm away from the surface facing the base layer side); and the central part of the surface layer in the thickness direction is located at a position that coincides with the center of the observation area. In the case where the thickness of the surface layer is less than 26 μm, the collection position is adjusted so that the observation areas do not overlap with each other. The orientation angle and orientation degree according to the present disclosure are set to the average value of each value obtained from the SEM image in each observation area collected at the above-mentioned three positions.
[0062] In the pressurizing rotating member according to one aspect of the present disclosure, the orientation angle Φ is 10° or less, preferably 7° or less, and more preferably 5° or less. The orientation angle Φ is 0° or more, and may be, for example, 1° or more, or 2° or more. That is, for example, the preferred range of the orientation angle Φ is 0° or more and 10° or less, and the more preferred range of the orientation angle Φ is 1° or more and 7° or less, and the further preferred range of the orientation angle Φ is 2° or more and 5° or less.
[0063] The orientation degree f is 0.20 or more, preferably 0.25 or more, and more preferably 0.30 or more. The upper limit of the orientation degree f is not particularly limited, and the larger the value, the more preferred the orientation degree f; for example, the upper limit may be lower than 1.00, or may be 0.80 or less, or 0.60 or less. That is, for example, the preferred range of the orientation degree f is 0.20 or more and less than 1.00, the more preferred range of f is 0.25 or more and 0.80 or less, and the further preferred range of f is 0.30 or more and 0.60 or less.
[0064] When the orientation angle Φ and the orientation degree f in the length direction of the pores take the above values, a heat insulating effect in the thickness direction of the surface layer derived from the orientation of the pores in the length direction can be achieved.
[0065] Hereinafter, a method for producing such a surface layer will be further described.
[0066] The material of the surface layer 19c is not particularly limited, and known materials used as the surface layer of the pressurizing rotating member can be used herein. Preferably, the surface layer contains fluororesin. This makes it possible to suppress the adhesion of the colorant to the surface of the pressurizing rotating member. In this case, the content ratio of the fluororesin in the surface layer is preferably 60% by mass or more, particularly 80% by mass or more, relative to the surface layer. This is because in this case, a more significant inhibitory effect of the film formation of the colorant on the outer surface of the pressurizing rotating member caused by the fluororesin is achieved. The upper limit of the content ratio is not particularly limited, and is less than 100% by mass, and considering the presence of other optional components (conductive fillers, etc.) in the surface layer, it can be less than 95% by mass.
[0067] Examples of fluororesins include copolymers (hereinafter, PFA) of tetrafluoroethylene and perfluoroalkyl vinyl ether (hereinafter, PAVE). As PAVE, for example, PAVE containing a perfluoroalkyl chain having 1 to 6 carbon atoms, particularly 1 to 4 carbon atoms, and further 1 to 3 carbon atoms can be suitably used. Specific examples of PAVE include, for example, perfluoromethyl vinyl ether (CF2=CF-O-CF3), perfluoroethyl vinyl ether (CF2=CF-O-CF2CF3) and perfluoropropyl vinyl ether (CF2=CF-O-CF2CF2CF3).
[0068] The following commercially available products can be used as such PFA.
[0069] "451HP-J", "959HP-Plus", "350-J" and "950HP-Plus" (all product names, manufactured by Chemours-Mitsui Fluoroproducts Co., Ltd.);
[0070] "P-66P", "P-66PT" and "P-802UP" (all product names, manufactured by AGC Inc.);
[0071] "AP-230" and "AP-231SH" etc. (all product names, manufactured by Daikin Industries, Ltd.);
[0072] "6502N" (product name, manufactured by The 3M Company).
[0073] The melting point of PFA generally falls within the range of 280°C to 320°C, such as 290°C to 310°C.
[0074] Production method of rotating member for pressurizing
[0075] A non-limiting example production method of a pressing rotating member (pressing belt or pressing roller) having a base layer, an elastic layer and a surface layer in order and wherein the surface layer has holes according to one aspect of the present disclosure includes, for example, a method having the following steps (i) to (iv).
[0076] (i) providing a resin tube produced according to a cylindrical extrusion method (hereinafter, also referred to as a "cylindrical extruded resin tube");
[0077] (ii) a step of obtaining a laminated body having an endless belt-shaped or roller-shaped substrate, an elastic layer covering the outer peripheral surface of the substrate, and a cylindrically extruded resin tube covering the outer peripheral surface of the elastic layer;
[0078] (iii) immersing the laminate in perfluoropolyether heated to a temperature close to the melting point of the resin tube to allow the perfluoropolyether (PFPE) to penetrate into the resin tube;
[0079] (iv) A step of removing the PFPE that has penetrated into the resin tube of the laminate obtained in step (iii) with a solvent to form pores in the resin tube.
[0080] The present inventors' studies have revealed that by impregnating a cylindrically extruded resin tube with liquid PFPE and then removing the PFPE, pores having a predetermined orientation angle and a predetermined orientation degree can be formed in the resin tube.
[0081] The conceivable reasons why the above method is considered to form holes oriented to a certain extent in the direction perpendicular to the circumferential direction of the pressurizing rotating member in the resin layer include the following. Hereinafter, as an example, a PFA tube obtained by cylindrical extrusion of PFA is used as a resin tube. However, the resin tube according to the present disclosure is not limited to the PFA tube.
[0082] A laminate consisting of a substrate having an endless belt shape or a roller shape, an elastic layer covering the outer peripheral surface of the substrate, and a PFA tube covering the outer peripheral surface of the elastic layer is immersed in PFPE heated to a temperature near the melting point of PFA (the temperature is 300°C ± 50°C (preferably 290°C to 325°C)), and the heated PFPE is brought into contact with the outer peripheral surface of the PFA tube, so that the PFPE is impregnated into the PFA tube. As the amount of PFPE in the PFA tube increases, a state of aggregated / linked PFPE is generated in the PFA tube. It is believed that the aggregation / linking of PFPE occurs preferentially in the non-crystalline region of PFA. If the non-crystalline region of PFA is oriented, the region of PFPE is also formed accordingly, while being oriented in the orientation direction of the non-crystalline region. In the PFA tube formed by cylindrical extrusion, the non-crystalline region is oriented in a direction parallel to the extrusion direction, that is, in a direction perpendicular to the circumferential direction of the PFA tube. Therefore, when the cylindrically extruded PFA tube is impregnated with PFPE, the PFPE region becomes oriented in a direction perpendicular to the circumferential direction of the PFA tube.
[0083] Then, the PFPE in the PFA tube is removed using a solvent, and as a result, holes are formed in the PFA tube at the location where the PFPE exists. Therefore, holes oriented in a direction perpendicular to the circumferential direction of the PFA tube are formed in the PFA tube. The inventors' research has shown that the smaller the thickness of the resin tube, the higher the degree of orientation f of the holes can be made, and the closer the orientation angle Φ can be made to zero. The above-mentioned conceivable fundamental reason is that the thinner the cylindrically extruded resin tube is, the easier it is for the non-crystalline region to be oriented in a direction parallel to the extrusion direction.
[0084] In the present disclosure, the thickness of the resin tube can be appropriately selected as long as the orientation degree f and orientation angle Φ according to the present disclosure are achieved; however, the value of the resin tube thickness that orients the holes in the extrusion direction herein is preferably 12 μm to 100 μm, more preferably 20 μm to 50 μm.
[0085] In terms of the preferred amount of pores in the resin layer described later, the perfluoropolyether is preferably impregnated into the resin tube in the following manner: the amount of perfluoropolyether impregnated into the resin tube in step (iii) is 25% to 60% by mass, particularly 30% to 45% by mass, relative to the mass of the resin tube after impregnation with the perfluoropolyether.
[0086] The vicinity of the melting point of the resin tube in step (iii) includes, for example, a range of Tm±50 (°C), wherein Tm (°C) is the melting point of the resin tube. In the case where the resin tube is a PFA tube, Tm of PFA falls within the range of 280 to 320°C, and thus the temperature of the PFPE in contact with the outer surface of the resin tube in step (iii) is, for example, 250 to 350°C, preferably 290 to 325°C.
[0087] The higher the temperature of the PFPE in step (iii) and the lower the viscosity of the PFPE, the greater the degree to which the amount of PFPE that can be impregnated into the resin tube can be increased. The contact time between the outer peripheral surface of the resin tube and the PFPE varies depending on the viscosity and the amount of PFPE that has penetrated into the resin tube; however, as a guide, the contact time ranges from 20 seconds to 5 minutes, and particularly from 30 seconds to 2 minutes. Within this range, as time passes, the resin tube can be impregnated with a sufficient amount of PFPE to form holes in the resin tube. In the production of the pressurized rotating member of step (iii), the contact method between the resin tube and the PFPE can be any method as long as the PFPE can be in contact with the outer peripheral surface of the resin tube at a temperature near the melting point of the resin tube.
[0088] The contact between the outer peripheral surface of the resin tube and the PFPE can be performed in a state where the base layer, the elastic layer, and the surface layer have been previously laid to obtain a laminate; alternatively, the contact can be performed in a state where the surface (inner peripheral surface) of the resin tube on the side in contact with the elastic layer is shielded. The above can be produced by adopting, for example, an immersion method as a contact method.
[0089] In step (iv), the laminated body in which the resin tube is impregnated with PFPE is taken out from the perfluoropolyether bath, cooled to room temperature, and then the PFPE impregnated into the resin tube is removed using a fluorinated solvent. This operation forms pores in the resin tube.
[0090] The laminated body may be simply immersed in the fluorine solvent; however, in order to more effectively remove PFPE from the resin tube, it is preferred to apply ultrasonic waves and / or heat the fluorine solvent.
[0091] A solvent capable of dissolving PFPE but not dissolving the resin constituting the resin tube is preferably used as the fluorine solvent. The term "solvent that dissolves PFPE" includes, for example, a solvent in which PFPE is dissolved in 100 g of the solvent at 25° C. in an amount of 10 g or more. Meanwhile, the term "solvent that does not dissolve PFA" includes a solvent in which PFA is dissolved in 100 g of the solvent at 25° C. in an amount of 1 g or less.
[0092] For example, when the resin tube is a PFA tube, hydrofluoroether dissolves PFPE. In contrast, PFA is almost insoluble in hydrofluoroether, and therefore, hydrofluoroether is a preferred fluorine solvent herein. For example, commercially available hydrofluoroethers such as "Novec 7300" (product name, manufactured by The 3M Company) can be used as hydrofluoroether.
[0093] In the surface layer according to the present disclosure, in the binarized image used for calculating the orientation angle Φ and the orientation degree f, the arithmetic mean of the ratio of the sum of the surface areas of the pores relative to the surface area of the observation area of 8 μm long×11 μm wide (having pores) (hereinafter, "pore area ratio") is preferably 15% to 50%, more preferably 25% to 45%. Setting the pore area ratio within the above range enables both the strength of the pressurizing rotating member according to the present disclosure and the thermal insulation in the thickness direction to be achieved at a higher level.
[0094] In order to achieve such a pore area ratio as described above, it is preferred that the resin tube is impregnated with a sufficient amount of PFPE in step (iii). The amount of PFPE impregnated into the resin tube can be adjusted, for example, according to the temperature of the PFPE in contact with the outer peripheral surface of the resin tube and the viscosity of the PFPE. Specifically, the amount of PFPE impregnated into the resin tube can be increased by increasing the temperature of the PFPE in contact with the outer peripheral surface of the resin tube. By using a low-viscosity PFPE, the amount of PFPE impregnated into the resin tube can be increased. However, in the case of a PFPE with too low viscosity, it is ostensibly due to an increase in affinity for PFA, so that the PFPE region derived from aggregation / linking in the resin tube is not easily formed, and it may be difficult to achieve a high pore surface area ratio.
[0095] The surface layer is preferably a single-layer film. Considering that the orientation angle Φ and the orientation degree f of the pores are easily adjusted to fall within the scope of the present disclosure, and considering the durability of the pressurizing rotating member, the thickness of the surface layer is preferably 12 μm or more, more preferably 20 μm or more, and preferably 100 μm or less, more preferably 50 μm or less. The thickness of the surface layer can be set in the range of, for example, 12 μm to 100 μm.
[0096] Perfluoropolyether (PFPE)
[0097] The perfluoropolyether is not particularly limited as long as it can penetrate into the resin tube, and known perfluoropolyethers can be used herein. Preferably, PFPE has a structure represented by the following formula. PFPE is preferably in an oily state at the melting point of PFA.
[0098]
[0099] In formula (1), a, b, c, d, e and f are each independently 0 or a positive integer, satisfying 1≤a+b+c+d+e+f≤600, and at least one of a, b, c and d represents a positive integer.
[0100] In addition, the order in which each repeating unit in formula (1) exists is not limited to the above order. In addition, each repeating unit in formula (1) may exist at multiple positions in the PFPE. That is, the PFPE represented by formula (1) may be a block copolymer or a random copolymer.
[0101] Specifically, the perfluoropolyether preferably has at least one structure selected from the group consisting of the following formulae (2) to (5).
[0102]
[0103] In the formula (2), n is a positive number, and n falls within a range such that the viscosity of PFPE at a temperature of 40° C. is 30 mPa·s to 400 mPa·s.
[0104]
[0105] In the formula (3), n' is a positive number, and n' falls within a range such that the viscosity of PFPE at a temperature of 40°C is 10 mPa·s to 400 mPa·s.
[0106]
[0107] In formula (4), n" and m are each independently a positive number, m / n" is a number from 0.5 to 2, and n"+m is a number within a range such that the viscosity of PFPE at a temperature of 40°C is from 20 mPa·s to 400 mPa·s.
[0108]
[0109] In formula (5), n'' and m' are each independently a positive number, m' / n'' is a number from 20 to 1000, and n''+m' is a number within a range such that the viscosity of PFPE at a temperature of 40° C. is from 20 to 400 mPa·s.
[0110] From the viewpoint of good penetration into the resin tube, the viscosity of PFPE at a temperature of 40°C is preferably in the range of 10 mPa·s to 400 mPa·s, more preferably 30 mPa·s to 350 mPa·s. As used herein, the term viscosity means the viscosity of PFPE at 100 s using a dynamic viscoelasticity measuring device (rheometer) using a cone plate having a cone angle of 1° and a cone radius of 20 mm. -1 The value is measured after rotating for 60 seconds at a shear rate of 1000 rpm and a measuring temperature of 40° C. Examples of the rheometer include, for example, “DHR-2” (product name, manufactured by TA Instruments Inc.).
[0111] Examples of commercially available PFPE include, for example, PFPE having a structure represented by formula (2) (e.g., Demnum S-200 and Demnum S-65 (both are product names); manufactured by Daikin Industries, Ltd.), PFPE having a structure represented by formula (3) (e.g., Krytox GPL-105, Krytox GPL-104, Krytox GPL-103, Krytox GPL-102, and Krytox GPL-101 (all are product names); manufactured by The Chemours Company), PFPE having a structure represented by formula (4) (e.g., Fomblin M07 and Fomblin M15 (both are product names); manufactured by Solvay Specialty Polymers Co., Ltd.), and PFPE represented by formula (5) (e.g., Fomblin Y15 and Fomblin Y25 (both are product names); manufactured by Solvay Specialty Polymers Co., Ltd.).
[0112] For example, the viscosity of "Demnum S-200" is 377 mPa·s, the viscosity of "Krytox GPL-105" is 301 mPa·s, the viscosity of "Krytox GPL-104" is 111 mPa·s, the viscosity of "Krytox GPL-103" is 54 mPa·s, the viscosity of "Krytox GPL-102" is 26 mPa·s, and the viscosity of "Krytox GPL-101" is 12 mPa·s. The above viscosity values all represent the viscosity at a temperature of 40°C.
[0113] 2. Fixing equipment
[0114] The fixing device includes the pressing rotating member described above as the pressing rotating member, a fixing belt, and a heating device for the fixing belt.
[0115] Figure 4 It is a schematic diagram showing a cross section in one example of a schematic configuration of a fixing device of a belt heating type.
[0116] The fixing belt 11 is loosely fitted to the belt guide member 16. The pressurizing rigid stay 18 is inserted into the inner side of the belt guide member 16. The belt guide member 16 is formed of, for example, a heat-resistant / heat-insulating resin.
[0117] The heating device is, for example, a heater configured to contact the inner peripheral surface of the fixing belt. A ceramic heater 17 as a heat source is provided at a position where the inner surface of the belt guide member 16 and the fixing belt 11 contact each other. The ceramic heater 17 is fitted and fixed in a groove provided in the length direction of the belt guide member 16. The ceramic heater 17 generates heat by energizing by a device not shown.
[0118] The roller-shaped pressure-applying rotating member 19 is the pressure-applying rotating member described as the above-mentioned pressure-applying rotating member. By arranging a pressure spring (not shown) between both ends of the pressure-applying rigid support 18 and a spring receiving member (not shown) on the side of the device chassis, downward pressure is applied to the pressure-applying rigid support 18. As a result, the lower surface of the ceramic heater 17 arranged on the lower surface of the belt guide member 16 and the upper surface of the pressure-applying rotating member 19 are pressed against each other, with the fixing belt 11 being sandwiched therebetween, to form a predetermined fixing roller nip portion N. That is, the lower surface of the ceramic heater 17 is arranged in contact with the inner peripheral surface of the fixing belt 11.
[0119] The recording medium P as a heated body on which an image is formed by the unfixed toner G is nipped and conveyed in the fixing nip portion N at a conveying speed V. As a result, the toner image is heated and pressurized. Therefore, the toner image is melted and the colors are mixed; thereafter, the toner image is cooled, so that the toner image is fixed on the recording medium P.
[0120] In addition, in a method other than the belt heating type method in this example, for example, a heat roll method, the same effect can be obtained by adopting a structure having the pressing rotating member described as the above-mentioned pressing rotating member.
[0121] 3. Image forming equipment
[0122] A known configuration can be adopted as the image forming apparatus. Such apparatuses include multifunctional devices, copiers, fax machines, and printers using an electrophotographic system. Here, a color laser printer will be used as an example to schematically illustrate the overall structure of the image forming apparatus.
[0123] Figure 5 is a schematic cross-sectional view of the laser printer 40 . Figure 5 The laser printer 40 shown has respective electrophotographic photosensitive member drums 39 (hereinafter, referred to as "photosensitive member drums 39") that rotate at a constant speed for respective colors including yellow (Y), magenta (M), cyan (C), and black (K). The laser printer 40 also has an intermediate transfer member 38 that holds a color image that is developed in an image forming portion and produced by multiple transfers, and transfers the color image onto a recording medium P fed from a feeding unit.
[0124] Each photosensitive member drum 39 (39Y, 39M, 39C, 39K) is driven by a driving device (not shown). Figure 5 Counterclockwise rotation drive shown.
[0125] Around each photosensitive member drum 39, corresponding charging devices 21 (21Y, 21M, 21C, 21K) for uniformly charging the surface of the photosensitive member drum 39, corresponding scanner units 22 (22Y, 22M, 22C, 22K) for projecting laser beams based on image information to form electrostatic latent images on the photosensitive member drum 39, corresponding developing units 23 (23Y, 23M, 23C, 23K) for making colorants adhere to the electrostatic latent images to develop the colorants in the form of colorant images, corresponding primary transfer rollers 24 (24Y, 24M, 24C, 24K) for transferring the colorant images on the photosensitive member drum 39 to the intermediate transfer member 38 at the primary transfer section T1, and corresponding cleaning units 25 (25Y, 25M, 25C, 25K) having cleaning scrapers for removing untransferred colorants remaining on the surface of the photosensitive member drum 39 after transfer.
[0126] At the time of image formation, a belt-like intermediate transfer member 38 stretched around rollers 26, 27 and 28 rotates and the color toner images formed on the respective photosensitive member drums 39 are primarily transferred and superimposed on each other on the intermediate transfer member 38, resulting in a color image being formed.
[0127] Then, the recording medium P is conveyed to the secondary transfer portion T2 by a conveying device in synchronization with the primary transfer to the intermediate transfer member 38. The conveying device includes a feed cassette 29 that accommodates a plurality of recording media P, a feed roller 30, a separation pad 31, and a resist roller pair 32. At the time of image formation, the feed roller 30 is rotationally driven in accordance with the image forming operation, and the recording media P in the feed cassette 29 are separated one by one and conveyed to the secondary transfer portion T2 by the resist roller pair 32 at a timing synchronized with the image forming operation.
[0128] A movable secondary transfer roller 33 is disposed in the secondary transfer portion T2. The secondary transfer roller 33 can be moved approximately in the vertical direction. At the time of image transfer, the secondary transfer roller 33 is pressed against the intermediate transfer member 38 via the recording medium P at a predetermined pressure. At the same time, a bias is applied to the secondary transfer roller 33, and the toner image on the intermediate transfer member 38 is transferred to the recording medium P.
[0129] The intermediate transfer member 38 and the secondary transfer roller 33 are driven separately, so that the recording medium P sandwiched between the intermediate transfer member 38 and the secondary transfer roller 33 is moved along the Figure 5The recording medium P is conveyed in the left arrow direction at a predetermined conveying speed V; then, as a subsequent process, the recording medium P is further conveyed to the fixing unit 35 by the conveying belt 34. In the fixing unit 35, the transferred toner image is fixed on the recording medium P by applying heat and pressure. Then, the recording medium P is discharged to a discharge tray 37 on the top surface of the apparatus by a discharge roller pair 36.
[0130] One aspect of the present disclosure allows for obtaining a pressurizing rotating member capable of exhibiting both surface layer durability and excellent thermal insulation at a high level. Another aspect of the present disclosure allows for obtaining a fixing device that helps shorten the first printout time. Yet another aspect of the present disclosure allows for obtaining an image forming device having a shorter first printout time than conventional devices. Another aspect of the present disclosure allows for a method for producing a pressurizing rotating member capable of exhibiting both surface layer durability and excellent thermal insulation at a high level.
[0131] Example
[0132] The present disclosure will be specifically described based on examples. The present disclosure is not limited to the following examples. Unless otherwise specifically stated, the unit of part in the examples and comparative examples refers to the mass basis in all cases.
[0133] In this embodiment, the following fluororesin and perfluoropolyether were used to produce a pressurizing rotating member.
[0134] (Fluororesin)
[0135] PFA-1: "959HP-Plus" (product name, manufactured by Chemours-Mitsui Fluoroproducts Co., Ltd., melting point 296°C)
[0136] PFA-2: "451HP-J" (product name, manufactured by Chemours-Mitsui Fluoroproducts Co., Ltd., melting point 305°C)
[0137] (Perfluoropolyether)
[0138] PFPE-1: "Krytox GPL104" (product name, manufactured by The Chemours Company, viscosity: 111 mPa·s (40° C.)
[0139] PFPE-2: "Krytox GPL105" (product name, manufactured by The Chemours Company, viscosity: 301 mPa·s (40° C.)
[0140] PFPE-3: "Krytox GPL103" (product name, manufactured by The Chemours Company, viscosity 54 mPa·s (40° C.)
[0141] Example 1
[0142] Preparation of laminates
[0143] First, a 23 mm diameter iron substrate with sandblasted surface was prepared as a base layer. The periphery of the substrate was sprayed with addition curing liquid silicone rubber (product name: DY35-051 A&B; an equal mixture of "liquid A" and "liquid B", manufactured by Dow Corning Toray Co., Ltd.) to a dry thickness of 3 μm, and then baked at a temperature of 150° C. for 30 minutes.
[0144] Then, an addition-curable liquid silicone rubber (product name: DY35-1349SC, manufactured by Dow Corning Toray Co., Ltd.) (volume resistance value 10 5 50 parts by mass of liquid A (main agent) and 50 parts by mass of liquid B (curing agent) with a relative humidity of 20 Ω·cm) are cast into a forming mold with an inner diameter of 30 mm in which the above-mentioned iron substrate is mounted at the center, and the mold is heated at a temperature of 150°C for 1 hour to cause primary vulcanization, and then the product is demolded from the mold to form an elastic layer on the outer peripheral surface of the substrate.
[0145] The outer peripheral surface of the elastic layer was coated with an addition-curable silicone rubber adhesive (product name: SE1819CV, manufactured by Dow Corning Toray Co., Ltd.; an equal mixture of "Liquid A" and "Liquid B") so as to have an average thickness of 5 μm.
[0146] Next, a PFA-1 tube formed into a thickness of 20 μm by extrusion molding was applied, and the tube surface was uniformly pressed to remove excess adhesive from between the elastic layer and the fluororesin tube. Then, the base layer coated with the elastic layer and the surface layer was placed in an electric furnace set at a temperature of 200° C. and heated as a whole for 4 hours to cause curing of the adhesive and adhesion of the tube to the elastic layer, thereby obtaining a laminated body A1.
[0147] Production of rotating components for pressurization
[0148] Soaking Steps
[0149] PFPE-1 was placed in a measuring cylinder made of borosilicate glass. An electric heating wire covered with a heat insulating material was wound around the entire measuring cylinder, and the measuring cylinder was heated to 310°C, the temperature of PFPE. The stack A1 was attached to a dipping device, the entire stack was dipped in the heated PFPE, and the stack A1 was taken out after 1 minute.
[0150] The amount of PFPE in the obtained PFA tube impregnated with PFPE is measured according to the following method. Specifically, a multilayer sample of an elastic layer and a resin layer is cut out from the laminate. The multilayer sample is immersed in a silicone resin dissolving agent (product name: e-Solve21RS, manufactured by Kaneko Chemical Co., Ltd.) to dissolve the silicone rubber in the elastic layer. As a result, the elastic layer is removed from the multilayer sample to prepare a measurement sample consisting only of the entire thickness portion of the PFA tube. The measurement sample is measured using a thermogravimetric analyzer (TGA). The content ratio (mass %) of PFPE relative to the PFPE-containing resin layer is calculated under the following measurement conditions.
[0151] Instrument: TGA851 (manufactured by Mettler-Toledo International Inc.)
[0152] Atmosphere: In the air
[0153] Temperature: 425℃
[0154] In the measurement time-weight loss rate curve obtained based on the above-mentioned thermogravimetric analysis, a linear least squares approximation expression was found from the region where the slope was constant and only PFA decreased; the intercept of the linear least squares approximation expression was taken as the PFA amount (mass %), and the PFPE content was calculated as PFPE content (mass %) = 100 - PFA amount.
[0155] Hole Forming Process
[0156] Then, the laminate A1 was placed in a measuring cylinder filled with a fluorine solvent having a hydrofluoroether structure (product name: Novec7300, manufactured by The 3M Company) prepared separately, and then the measuring cylinder was placed in a water bath of an ultrasonic applying device (product name: Bransonic (model 2510J-DTH); manufactured by Emerson Japan, Ltd.), and irradiated with ultrasonic waves for 60 minutes. After the treatment, the laminate was taken out of the measuring cylinder and dried by leaving it in an environment at a temperature of 25° C. for 60 minutes. In this way, the PFPE present on the surface and inside of the surface layer of the laminate A1 was removed to obtain a pressurizing rotating member according to the present embodiment. The visual appearance of the obtained laminate was white, and pores were found to be formed in the resin layer.
[0157] Three sets of measurement samples for measuring the following physical properties were prepared as follows.
[0158] Preparation of measurement samples
[0159] The base was separated from the pressing rotating member to obtain a laminate B1 of an elastic layer and a surface layer. The laminate B1 was immersed in a silicone resin dissolving agent (product name: e-Solve 21RS, manufactured by Kaneko Chemical Co., Ltd.) to dissolve the silicone rubber in the elastic layer, and as a result, the elastic layer was removed from the laminate B1 to prepare a measurement sample of the entire thickness portion including the surface layer.
[0160] Orientation of pores in the surface layer (degree of orientation f and orientation angle Φ)
[0161] The sample is cut out from the pressurizing rotating member using a slice preparation device (e.g., a cryo-ultramicrotome (product name: manufactured by Leica Microsystems GmbH)) so that a cross section of the thickness of the surface layer-the length direction of the pressurizing rotating member appears on the surface of the sample. Then, the cross section is observed under a scanning electron microscope to collect a corresponding image (SEM image) of a rectangular observation area of 8 μm in length×11 μm in width at a predetermined position in the cross section. Image collection is adjusted so that the length direction of the image is parallel to the thickness direction of the surface layer, and the lateral direction of the image is parallel to the length direction of the pressurizing rotating member.
[0162] This SEM image from the cross section was collected at the following three positions. Specifically, the upper end of the observation area was located at a position of 1 μm in the depth direction of the surface layer from the outer surface of the surface layer constituting the outer surface of the pressurizing rotating member that constitutes the contact surface with the heating rotating member in the fixing device; the lower end of the observation area was located at a position of 1 μm from the surface of the surface layer on the opposite side of the outer surface (i.e., from the surface facing the base layer side) toward the outer surface; and the central part of the surface layer in the thickness direction was located at a position that coincided with the center of the observation area. In the case where the thickness of the surface layer was less than 26 μm, the collection position was adjusted so that the observation areas would not overlap with each other.
[0163] Each SEM image obtained was binarized using numerical calculation software (product name: MATLAB; manufactured by The MathWorks, Inc.) so as to distinguish two regions corresponding to the resin portion and the hole portion, respectively. The binarization process relies on the Otsu method. Then, the binarized image obtained as a result of the binarization process was subjected to a two-dimensional Fourier transform analysis using the above numerical calculation software, and the power spectrum was integrated in each direction to obtain a drawing representing the degree and direction of the orientation of the hole. The orientation degree and orientation angle were calculated from the drawing, and the arithmetic mean thereof was taken as the orientation degree f and the orientation angle Φ.
[0164] The ratio of pores in the surface layer
[0165] From each of the above-mentioned binarized images, the hole area ratio is calculated based on the ratio of the number of pixels in the portion corresponding to the hole relative to the total number of pixels in the observation area.
[0166] Evaluation 1: Thermal conductivity in the thickness direction of the surface layer
[0167] The thermal conductivity λ in the thickness direction of the surface layer is calculated based on the following expression.
[0168] λ=α×C p ×ρ
[0169] In the expression, λ is the thermal conductivity of the surface layer in the thickness direction (W / (m·K)), and α is the thermal diffusion coefficient in the thickness direction (m 2 / s), C p is the specific heat at constant pressure (J / (kg·K)) and ρ is the density (kg / m 3 ).
[0170] Thermal diffusion coefficient α in the thickness direction, constant pressure specific heat C p The values of and density ρ are obtained by the following method.
[0171] Thermal diffusion coefficient α
[0172] The thermal diffusion coefficient α in the thickness direction of the surface layer was measured as follows. A total of five sample pieces each having a surface area of 8 mm×12 mm were produced by cutting from the measurement sample using a cutter. A digital length measuring instrument (product name: DIGIMICRO MF-501, flat stylus, Next, each sample piece was measured a total of 5 times at room temperature (25° C.) using a thermal diffusion coefficient measuring device relying on a periodic heating method (product name: FTC-1, manufactured by ADVANCERIKO, Inc.), and the average value (m 2 / s). The measurement was performed while the sample piece was pressurized with a 1 kg weight.
[0173] As a result, it was confirmed that the thermal diffusion coefficient α in the thickness direction of the surface layer was 4.66×10 -8 m 2 / s.
[0174] Specific heat at constant pressure C p
[0175] Specific heat of the surface layer at constant pressure C p The measurement was performed using a differential scanning calorimeter (product name: DSC823e, manufactured by Mettler-Toledo International Inc.).
[0176] Specifically, an aluminum pan was used as a sample pan and as a control pan. First, in blank measurement, measurement was performed according to a procedure in which two empty pans were kept at a constant temperature of 15°C for 10 minutes, then the pans were heated to 215°C at a heating rate of 10°C / min, and kept at 215°C for another 10 minutes.
[0177] Next, 10 mg of synthetic sapphire with known constant pressure specific heat was used as a control, and the same procedure was used for measurement. Next, 10 mg of measurement sample, i.e., the same amount of synthetic sapphire as the control, was cut out from the above measurement sample, placed in a sample pan, and measured according to the same procedure.
[0178] The measurement results were analyzed using the specific heat analysis software attached to the differential scanning calorimeter, and the constant pressure specific heat C at 25°C was calculated based on the average value of 5 measurement results. p .
[0179] Prove that the surface layer has a constant pressure specific heat C p It is 1002.80J / (kg·K).
[0180] Density ρ
[0181] The density ρ of the surface layer is measured with a dry type automatic densitometer (product name: Accupic 1330-01, manufactured by Shimadzu Corporation).
[0182] Specifically, using 10cm 3 A sample cell of , and a sample piece was cut out from the above measurement sample so that it filled about 80% of the cell volume, and after measuring the mass of the sample piece, the sample piece was placed in the sample cell. The sample cell was placed in the measurement part of the device, and after gas replacement using helium as the measurement gas, the volume measurement was performed 10 times. The density of the surface layer was calculated from the mass of the sample piece and each measured volume, and the average value was calculated.
[0183] As a result, the density of the surface layer is 1287.47 kg / m 3 .
[0184] Here, the constant pressure specific heat C is calculated based on the unit conversion. p (J / (kg·K)) and density ρ(kg / m 3 ), and based on the measured thermal diffusion coefficient α(m 2 / s), and the calculated thermal conductivity λ in the thickness direction of the surface layer is 6.01×10 -2 W / (m·K).
[0185] Evaluation 2: Measurement of tensile yield stress of the surface layer
[0186] Each of the above-mentioned measurement samples was cut into a width of 5 mm and a length of 20 mm to prepare each tensile test piece. The test piece was placed on the tensile measurement fixture of the dynamic viscoelasticity measuring device (product name: Reogel-E4000, manufactured by UBM Co.) so that the chuck distance was 10 mm. The test piece was fixed to the fixture with a torque screwdriver so that the tightening torque of the test piece was 5 cN·m.
[0187] Under the conditions of a temperature of 200°C and a tensile speed of 0.055 m / sec, the SS curve in the tensile test was measured until the test piece broke. In the measurement, only the fracture data between the chucks were considered, and the measurement result was taken as the average value of five measurements. In the case where the strain of the SS curve from 0% to 3% was taken as a straight line, an approximate line was drawn, and the stress value at the intersection between the SS curve and the straight line obtained by shifting the approximate curve by 5% of the strain in the positive direction was taken as the value of the tensile yield stress.
[0188] Evaluation 3: Evaluation of first printout time
[0189] Install the produced pressurizing rotating member to Figure 4 The fixing device shown in the figure, wherein the pressing force applied between the fixing member and the pressing rotating member is set to 20 kgf. The ceramic heater 17 of the fixing device starts to be energized at 1200 W, and the time until the surface temperature of the fixing member reaches 200° C., which is a temperature capable of fixing in the fixing device, is measured and taken as the first print output time.
[0190] Evaluation 4: Durability Evaluation
[0191] The following durability test was conducted on the pressurizing rotating member to evaluate the wear resistance of the surface layer. First, the produced pressurizing rotating member was mounted on a Figure 4 The fixing device was built in a laser beam printer capable of high-speed fixing at 60 sheets / minute (process speed of 350 mm / sec), and then 5,000 sheets of A4 size paper were continuously run in a continuous paper-passing mode. The surface temperature of the fixing belt during fixing was set to 200°C, and the paper was run in an environment of a temperature of 15°C and a humidity of 20%. The pressing rotating member was removed after the continuous paper was run, and the surface of the pressing rotating member was visually observed and evaluated according to the following criteria.
[0192] Grade "A": No cracks were found in the surface layer.
[0193] Rank "B": Cracks were observed in the surface layer.
[0194] Examples 2 to 12
[0195] Pressurizing rotating members 2 to 12 according to each Experimental Example were produced in the same manner as in Example 1 except that the PFA resin and thickness of the fluororesin tube used in the surface layer, the kind of PFPE used for impregnation, and the PFPE temperature at the time of contact were changed as shown in Table 1.
[0196] Embodiment 13
[0197] In the method described in Example 1, the iron substrate on which the PFA resin (PFA-1) was laminated was subjected to annealing treatment at 330° C. for 30 minutes to obtain a laminated body. Then, a pressurizing rotating member subjected to the impregnation step and the pore forming step was produced in the same manner as in Example 1 to obtain a pressurizing rotating member 13 according to the present example.
[0198] Comparative Example 1
[0199] A pressurizing rotating member was produced as described in Example 1 until the PFA resin was laid; the obtained member was a pressurizing rotating member C-1 according to this comparative example.
[0200] Comparative Examples 2 to 4
[0201] Pressurizing rotating members C-2 to 4 according to respective comparative examples were produced in the same manner as in Comparative Example 1 except that the thickness of the PFA resin laid as described in Comparative Example 1 was changed as shown in Table 1 herein.
[0202] Comparative Example 5
[0203] A coating material was prepared as a mixture of 65 parts of small hollow spherical particles (product name: Glass Bubbles iM30K; manufactured by The 3M Company) in 100 parts of an aqueous coating material containing a perfluoroethylene-propylene copolymer (product name: EJ-CL500; manufactured by Chemours-Mitsui Fluoroproducts Co., Ltd.).
[0204] An elastic layer and an adhesive layer were formed on the iron substrate in the same manner as in Example 1. Next, the coating prepared above was sprayed on the surface of the adhesive layer so that the film thickness after baking was 20 μm. Then, the whole was baked at a temperature of 340° C. for 30 minutes to produce a pressurizing rotating member C-5 according to this comparative example.
[0205] Table 1 lists the formulations and pore physical properties (pore ratio, orientation degree f and orientation angle Φ) of the pressurizing rotating members produced in Examples 1 to 13 and Comparative Examples 1 to 5. The surface layers of the pressurizing rotating members C-1 to C-4 according to Comparative Examples 1 to 4 had no pores, and therefore, the pore physical properties were not measured.
[0206] [Table 1]
[0207]
[0208] In Table 1, the term "pore ratio" indicates the area ratio (%) occupied by pores in the surface layer.
[0209] Table 2 lists the evaluation results of Evaluations 1 to 4 of the pressurizing rotating members produced in Examples 1 to 13 and Comparative Examples 1 to 5.
[0210] [Table 2]
[0211]
[0212] Table 2 shows that the pressurizing rotating member of the example exhibits excellent thermal conductivity, and the member does not develop cracks even after long-term use. As a result, it was found that the pressurizing rotating member of the example allows shortening the first printout time while maintaining durability.
[0213] While the present invention has been described with reference to exemplary embodiments, it is to be understood that the invention is not limited to the disclosed exemplary embodiments.The scope of the following claims is to be accorded the broadest interpretation so as to encompass all such modifications and equivalent structures and functions.
Claims
1. A pressurizing rotating member, which comprises a base layer, an elastic layer and a surface layer in sequence, The surface layer has pores, It is characterized in that When an observation region of 8 μm in length and 11 μm in width is set in the cross section of the surface layer in the thickness direction of the surface layer and the length direction of the pressurizing rotating member, and the orientation degree of the pores observed in the observation region is defined as f, and the orientation angle of the pores observed in the observation region is defined as Φ, In the case where two-dimensional Fourier transform is applied to an image of a cross section in the thickness direction and the length direction, an angle formed by the longest diameter with respect to a direction of 90° to 270° indicating the length direction of the surface layer is taken as an orientation angle Φ, and The degree of orientation f is defined as f=1-(y / x), where x represents the length of the line segment with the longest diameter and y represents the length of the line segment perpendicular to the longest diameter. f and Φ satisfy the following relationship: f is greater than 0.20; Φ is 0° to 10°. 2 . The pressurizing rotating member according to claim 1 , wherein a ratio of an area occupied by the holes in the region is 15% to 50%. 3 . The pressurizing rotary member according to claim 1 , wherein the surface layer has a thickness of 12 to 100 μm. 4 . The pressurizing rotating member according to claim 1 , wherein the surface layer contains a fluororesin. 5 . The pressurizing rotating member according to claim 1 , wherein the surface layer comprises a copolymer of tetrafluoroethylene and perfluoroalkyl vinyl ether. 6 . The pressurizing rotary member according to claim 5 , wherein the melting point of the copolymer is 280 to 320° C.
7. The pressurizing rotating member according to claim 1 or 2, wherein the pressurizing rotating member has an endless belt shape. 8 . The pressurizing rotating member according to claim 1 , wherein the pressurizing rotating member has a roller shape.
9. A fixing device, characterized in that: The invention comprises the pressing rotating member according to any one of claims 1 to 8, a fixing belt, and a heating device for the fixing belt.
10. An electrophotographic image forming device, characterized in that: Comprising the fixing device according to claim 9.
11. A method for producing a pressurizing rotating member according to any one of claims 1 to 8, characterized in that: The pressurizing rotating member has a base layer, an elastic layer and a surface layer in sequence, wherein the surface layer has holes. The method comprises the following steps: (i) providing a resin tube produced by a cylindrical extrusion method; (ii) obtaining a laminated body of a substrate having an endless belt shape or a roller shape, an elastic layer covering the outer peripheral surface of the substrate, and the resin tube covering the outer peripheral surface of the elastic layer; (iii) immersing the laminate in perfluoropolyether so that the perfluoropolyether penetrates into the resin tube; and (iv) removing the perfluoropolyether that has penetrated into the resin tube of the laminate obtained in the step (iii) with a solvent, thereby forming pores in the resin tube to obtain the surface layer. 12 . The method for producing a pressurizing rotating member according to claim 11 , wherein the perfluoropolyether has a viscosity of 10 to 400 mPa·s at a temperature of 40° C.
13. The method for producing a pressurizing rotating member according to claim 11 or 12, wherein the thickness of the resin tube is 12 to 100 [mu]m.
14. The method for producing a pressurizing rotating member according to claim 11 or 12, in, The step (iii) includes the step of bringing perfluoropolyether into contact with the outer surface of the resin tube, and the temperature of the perfluoropolyether is Tm±50° C., wherein Tm is the melting point of the resin tube.
15. The method for producing a pressurizing rotating member according to claim 11 or 12, wherein in the step (iii), the perfluoropolyether is impregnated into the resin tube such that the amount of the perfluoropolyether impregnated into the resin tube is 25 to 60% by mass relative to the mass of the resin tube after impregnation with the perfluoropolyether.
16. The method for producing a pressurizing rotating member according to claim 11 or 12, wherein the resin tube contains a copolymer of tetrafluoroethylene and perfluoroalkyl vinyl ether.
17. The method for producing a pressurizing rotating member according to claim 16, wherein the step (iii) comprises the step of bringing perfluoropolyether into contact with the outer surface of the resin tube, and the temperature of the perfluoropolyether is 250 to 350°C.
Citation Information
Patent Citations
Pressure member for fixation, fixing device, and image forming apparatus
JP2014232208A
Development device, process cartridge, and image forming apparatus including same
CN102385290A
Image Heating Apparatus And Image Forming Apparatus
CN105759581A
Cleaning device, collecting member, fixing device, and image forming apparatus
CN106200321A
Pressing member and fixing device
CN106662834A