A lithium titanate graphene electrode and preparation method thereof

Prepared by hydrothermal compounding and ball milling of lithium titanate and graphene oxide, the problem of insufficient stability and conductivity of electrode materials in lithium-ion batteries at high and low temperatures is solved, and high specific capacity and excellent cycle and rate performance are achieved. .

CN114725358BActive Publication Date: 2024-10-11ARMY ENG UNIV OF PLA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210494341.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-07
Publication Date
2024-10-11
Estimated Expiration
2042-05-07

AI Technical Summary

Technical Problem

Lithium-ion batteries exhibit problems such as low capacity, poor rate performance, poor cycle stability, obvious lithium precipitation, and unbalanced lithium deintercalation in high and low temperature environments, mainly due to insufficient stability and conductivity of electrode materials, especially the negative electrode. Materials Graphite-based carbon materials have poor safety and conductivity.

Method used

Lithium titanate and graphene oxide are used to generate composite electrode materials through hydrothermal reaction. Li4Ti5O12 is prepared by ball milling and compounded with graphene. The mass ratio of Li4Ti5O12 and graphene oxide is controlled to (70-90): (10-30). To improve electronic conductivity and structural stability, a "point-surface" contact structure is formed to promote electron transmission and buffer volume expansion.

Benefits of technology

Under high and low temperature conditions, lithium titanate graphene electrode material exhibits high specific capacity and excellent cycle and rate performance, improves the high and low temperature performance of the electrode material, and reduces the solid electrolyte interface impedance and lithium ion diffusion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114725358B_ABST
    Figure CN114725358B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium ion battery electrode materials, and in particular to a lithium titanate graphene electrode and a preparation method thereof, wherein the electrode material is a composite electrode material generated by hydrothermal reaction of lithium titanate and graphene oxide, and the lithium titanate is Li4Ti5O 12 ; wherein the Li4Ti5O 12 The mass ratio of graphene oxide to graphene oxide is (70-90): (10-30). The present invention uses graphene oxide as a reinforcement and Li4Ti5O 12 As raw materials, a uniform and tightly combined lithium titanate / graphene (LTO / G) composite electrode material was prepared by hydrothermal synthesis process. 12 Composite with graphene can not only avoid direct contact between the negative electrode and the electrolyte, improve the compatibility between the electrolyte and the negative electrode, but also increase the Li4Ti5O 12 The conductivity of graphene can be improved, providing more lithium embedding sites and reducing the irreversible capacity; at the same time, the introduction of graphene can also promote the diffusion of lithium ions and reduce the SEI film impedance, thereby improving the high / low temperature performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery electrode materials, and in particular to a lithium titanate graphene electrode and a preparation method thereof. Background Art

[0002] Lithium-ion batteries are widely used in electronic products, electric vehicles, and field power sources due to their high energy density, high operating voltage, and no memory effect. Lithium-ion batteries are usually used at room temperature, and the working environment generally does not exceed 40°C, which is conducive to the performance of electrode materials and performance. However, with the needs of electric vehicles, aerospace, and polar combat readiness, lithium-ion batteries with excellent performance at high and low temperatures will become an inevitable development demand. However, when lithium-ion batteries are used at high or low temperatures, there are problems such as low capacity, poor rate performance, poor cycle stability, obvious lithium precipitation, and unbalanced lithium insertion and extraction.

[0003] Lithium-ion batteries mainly include positive and negative electrode materials, electrolytes, and separators, among which the negative electrode material is the core component of lithium-ion batteries and directly determines the energy storage performance of the battery. It is reported that the discharge capacity of commercial lithium-ion batteries at a high temperature of 40°C is about 80% of that at room temperature, and at a low temperature of -10°C, the discharge capacity is about 35.5% of that at room temperature. Figure 1 The figure is a schematic diagram of the discharge capacity curve of lithium-ion batteries at different low temperatures (here used to indicate the general trend of change). Compared with room temperature, the capacity decay at -20°C is already quite obvious. The factors that restrict the low-temperature performance of lithium-ion batteries are mainly the following: ① The viscosity of the electrolyte increases, and even partially solidifies, resulting in a decrease in the conductivity of the lithium-ion battery; ② The compatibility between the electrolyte and the negative electrode and the separator deteriorates under low temperature conditions; ③ The negative electrode of the lithium-ion battery under low temperature conditions has serious lithium precipitation, and the precipitated metal lithium reacts with the electrolyte, and the product deposition leads to an increase in the thickness of the solid electrolyte interface (SEI); ④ The diffusion system of the lithium-ion battery in the active material under low temperature conditions is reduced, and the charge transfer impedance (Rct) increases significantly. The factors that restrict the high-temperature performance of lithium-ion batteries mainly include the decomposition of the electrolyte and the reduction in the stability of the electrode material. It can be seen that, in addition to the influencing factors of the electrolyte, the stability and activity of the electrode material itself have a significant impact on the high / low temperature performance of the battery.

[0004] At present, the negative electrode material of lithium-ion batteries in practical application is mainly graphite. Graphite has a layered structure and can react with Li during charging. + The reaction generates Li x C, and during the discharge process, Li ions escape from the negative electrode and return to the positive electrode ( Figure 2 ). With graphite as the negative electrode, Li y-x Mn 2 O 4The full battery reaction process assembled for the positive electrode is as follows:

[0005] Positive electrode: Li y-x Mn 2 O 4 -xe - =L y Mn 2 O 4 +xLi -

[0006] Negative electrode: C+xLi + +xe - =Li x C

[0007] However, due to the poor safety of graphite-based carbon negative electrode materials, researchers have been looking for new negative electrode materials to replace commercial graphite-based carbon negative electrode materials in recent years. 4 Ti 5 O 12 ) is a promising lithium-ion battery negative electrode material that is expected to replace graphite-based carbon negative electrode materials in the future. 4 Ti 5 O 12 It neither reacts with the electrolyte to form a solid electrolyte interface film (SEI film) nor forms lithium dendrites to cause safety hazards. 4 Ti 5 O 12 It is in a zero strain state during the phase change process of charge and discharge, has very good cycle efficiency, and can maintain structural stability at high and low temperatures; Li 4 Ti 5 O 12 According to the crystal form, it belongs to the spinel structure, and its space group is Fd3m. Its structural diagram is as follows Figure 3 In this crystal structure, O 2- Occupies position 32e, Li + Occupies the tetrahedral gap at the 8a position, Li + and Ti 4+ Together they occupy the octahedral gaps at the 16d position. + First, it occupies the 16c position. The three Li originally in the 8a position + Migrate to the 16c position to form a lithium-intercalated rock salt structure Li 7 Ti 5 O 12 After lithium insertion, the unit cell parameter changes from 0.836nm to 0.837nm, and its volume changes by less than 0.2%. 4 Ti 5 O 12Also known as "zero strain material", this tiny change makes Li 4 Ti 5 O 12 The structure of the material remains basically stable during the charge and discharge process. As lithium is further inserted, positions 8a, 8b and 48f can also store lithium ions. 7 Ti 5 O 12 Gradually transform into Li 9 Ti 5 O 12 Although the capacity increases, the material structure will be damaged and the cycle life will be affected. 4 Ti 5 O 12 There is a stable charge and discharge platform at about 1.55 V, which indicates that Li + In Li 4 Ti 5 O 12 The insertion and extraction of lithium ions is a two-phase process. At the same time, the 1.55V lithium insertion potential also avoids decomposition with the electrolyte, and has very good safety performance.

[0008] Although Li 4 Ti 5 O 12 The material has many advantages mentioned above, but Li 4 Ti 5 O 12 Negative electrode materials have not been widely used as expected. Their intrinsic defects, such as poor intrinsic electronic conductivity (<10~13S·cm -1 ) and the lithium ion diffusion coefficient is also low (10 -9 ~10 -13 cm 2 ·s -1 ) and other factors have limited the large-scale use of lithium titanate. At present, scientists have explored different methods to improve the above defects: ① The concentration of migrating ions can be increased by introducing elements of other valence states through doping. When lithium titanate is embedded with ions, the lattice requires charge compensation to maintain the overall electrical neutrality. Generally speaking, the process of charge compensation is provided by the change of the lattice band structure. However, the Ti in lithium titanate is +4, and its 3d orbital lacks electrons, so its band gap is relatively large, about 2eV, and it is difficult to provide enough electrons; ② By introducing a composite material with good conductivity, external electrons can be quickly migrated to the surrounding of the lithium titanate lattice.

[0009] Carbon materials generally have high electrical conductivity. Carbon materials can be combined with lithium titanate by coating or in-situ growth to improve the conductivity between lithium titanate particles; or carbon materials and lithium titanate can be designed to form a composite structure that is conducive to ion transmission to improve the rate performance and cycle stability of lithium titanate materials. Among the many carbon allotropes, graphene is a carbon atom with sp 2 The two-dimensional layered structure composed of hybrid orbitals has a thickness of only 0.35nm. It is precisely because of its unique single-atom-layer six-membered ring structure that it has a high specific surface area (~2600m 2 g -1 ), high conductivity (~8×10 5 sm -1 ), high thermal conductivity (~5×10 3 W m -l k -1 ) and high strength, and are widely used in optical devices, energy storage, and lithium-ion batteries.

[0010] At present, the preparation methods of graphene have been widely developed, such as mechanical exfoliation, graphite oxide-reduction method, chemical vapor deposition method, heating silicon carbide method, epitaxial growth method and organic synthesis method. However, the price and yield should be fully considered in the preparation and application of graphene. In addition, graphene is a two-dimensional material and is prone to agglomeration. Therefore, the key to solving the problem of graphene / lithium titanate composite materials is to reduce the production cost while suppressing the stacking and agglomeration of graphene during use and maintaining the close contact between graphene and Li. 4 Ti 5 O 12 Close contact between. Summary of the invention

[0011] The first object of the present invention is to provide a lithium titanate graphene electrode material having high specific capacity and excellent cycle and rate performance at high and low temperatures;

[0012] The second object of the present invention is to provide a method for preparing a lithium titanate graphene electrode material, which effectively solves the agglomeration of graphene and its interaction with Li 4 Ti 5 O 12 The problem of loose connection.

[0013] The present invention provides a method for preparing a lithium titanate graphene electrode material, comprising the following steps: a composite electrode material generated by hydrothermal reaction of lithium titanate and graphene oxide, wherein the lithium titanate is Li 2 CO 3 With TiO 2 Li prepared by ball milling 4 Ti5 O 12 ;

[0014] Among them, the Li 4 Ti 5 O 12 The mass ratio of graphene oxide to graphene oxide is (70-90):(10-30).

[0015] The present invention uses hydrothermal treatment to bond graphene and Li 4 Ti 5 O 12 The composite can effectively improve the shortcomings of lithium titanate itself, such as poor electronic conductivity and rapid attenuation under high / low temperature conditions. 4 Ti 5 O 12 With stable internal structure, Li 4 Ti 5 O 12 It can maintain a stable spatial structure, thereby improving electrode performance. In addition, the study found that graphene and Li 4 Ti 5 O 12 The performance of the composite material is related to the amount of graphene doped. 4 Ti 5 O 12 When the mass ratio of graphene oxide to graphene oxide is (70-90): (10-30), the prepared composite electrode material presents "point-surface" contact, which is more conducive to the transport of electrons and buffering volume expansion. Under high temperature conditions, the liquid phase mass transfer rate is accelerated, and the electrons in the electrode structure and Li + It diffuses faster in the electrolyte and has a faster kinetic process; and under low temperature conditions, due to the wrapping of graphene sheets, its ion diffusion efficiency is higher than that of pure lithium titanate. Therefore, the graphene / lithium titanate composite material of the present invention has high specific capacity and excellent cycle and rate performance at both high and low temperatures.

[0016] As the preferred embodiment of this technical solution, 4 Ti 5 O 12 The preparation comprises the following steps: 2 CO 3 With TiO 2 After mixing evenly, low-temperature pre-sintering, ball milling and high-temperature calcination are carried out in sequence, and Li 4 Ti 5 O 12 ;

[0017] Preferably, Li 2 CO 3 With TiO 2The ratio is based on a Li / Ti molar ratio of 0.8-0.9

[0018] Li 2 CO 3 With TiO 2 During the pre-burning stage, Li 2 CO 3 With TiO 2 Alloying reaction occurs to form lithium-rich compound Li 2 TiO 3 ; Ball milling stage, Li 2 TiO 3 Will further with TiO 2 The reaction generates Li 4 Ti 5 O 12 Among them, Li generated by the pre-calcination reaction 2 TiO 3 Encapsulated in TiO 2 surface, hindering Li 2 CO 3 With TiO 2 Further reaction leads to the partial inclusion of impurity TiO in the final product. 2 The ball milling can break up the large particles generated by the pre-calcination step, exposing the encapsulated TiO 2 , creating a new reaction interface and promoting Li 2 TiO 3 With TiO 2 Further reaction can improve the purity of the product. At the same time, ball milling of the precursor can enhance the activation energy of the precursor, improve the reaction activity of the precursor material, and further promote Li 2 TiO 3 With TiO 2 The reaction improves the purity of the product. And the research shows that when the Li / Ti molar ratio is 0.8-0.9, the prepared Li 4 Ti 5 O 12 The purity and yield are the highest.

[0019] As a preferred embodiment of the present technical solution, during the low-temperature pre-firing, the temperature is controlled to be 600-700°C and the time is 7-9h;

[0020] Preferably, during the low-temperature pre-firing, the temperature is 650°C and the time is 8 hours;

[0021] Preferably, before the low-temperature pre-calcination, Li 2 CO 3 With TiO 2 The mixture is thoroughly dried.

[0022] As a preferred embodiment of the present technical solution, the specific steps of the ball milling treatment are: adding the mixture pre-sintered at low temperature into anhydrous ethanol and performing ball milling treatment in a ball mill;

[0023] Preferably, during the ball milling treatment, the material-ball ratio is controlled to be 1:(9-11), the rotation speed is 350-450r / min, and the ball milling time is 3-8h;

[0024] Preferably, the ball milling time is 6 hours;

[0025] Preferably, the ball mill is a planetary ball mill.

[0026] Studies have shown that with the extension of ball milling time, the battery charge and discharge capacity of different materials first increases and then decreases. When the ball milling time is less than 6 hours, reducing the particle diameter is beneficial to shortening the migration path of lithium ions and improving the electrochemical properties of the material; when the ball milling time is greater than 6 hours, the reduction in particle size will lead to the appearance of agglomeration, thereby increasing the diffusion and migration resistance of lithium ions and limiting the capacity of the material. Therefore, in the invention, the ball milling time is preferably 6 hours.

[0027] As a preferred embodiment of the present invention, the high temperature calcination specifically comprises: leaving the ball milled mixture to stand for 5-7 hours, filtering, drying, high temperature calcining and cooling in sequence to obtain Li 4 Ti 5 O 12 powder;

[0028] Preferably, during the calcination, the temperature is controlled to be 700-900° C. and the time is 9-11 hours.

[0029] As a preferred embodiment of the present technical solution, the hydrothermal reaction specifically comprises: dissolving graphene oxide in deionized water, and adding Li 4 Ti 5 O 12 After stirring and mixing evenly, a hydrothermal reaction is carried out, and after the reaction is completed, washing, drying, calcining and cooling are carried out in sequence to obtain a composite electrode material;

[0030] Preferably, during the hydrothermal reaction, the temperature is controlled to be 170-190° C. and the time is 8-10 h.

[0031] As a preferred embodiment of the present technical solution, when the graphene oxide is dissolved, it is first mechanically stirred for 20-40 minutes, and then ultrasonicated using a pulverizer for 20-40 minutes; the Li 4 Ti 5 O 12 After addition, stir magnetically for 5-7 hours.

[0032] As a preferred embodiment of the present technical solution, after the graphene oxide is dissolved, a polymer electrolyte is added;

[0033] Preferably, the polymer electrolyte is PDDA.

[0034] Graphene and Li 4 Ti 5 O 12 The full dissolution and mixing of graphene and Li is the prerequisite for the hydrothermal reaction and also the 4 Ti 5 O 12 The seamless connection between particles is the key to the "point-to-surface" bridge. Therefore, they need to be fully stirred and dissolved before the hydrothermal reaction. In addition, in order to further improve the bonding between graphene and Li 4 Ti 5 O 12 The dispersion effect can also be improved by adding an appropriate amount of PDDA polymer electrolyte to react with Li 4 Ti 5 O 12 The compound.

[0035] As a preferred embodiment of the present technical solution, during the calcination, the material is heated to 800-900° C. at a heating rate of 4-6° C. / min in an Ar atmosphere and kept at that temperature for 5-7 hours.

[0036] The lithium titanate graphene electrode material prepared by the above method should also fall within the protection scope of the present invention.

[0037] Compared with the prior art, the preparation method of the lithium titanate graphene electrode of the present invention has the following technical effects:

[0038] The present invention uses graphene oxide as a reinforcement and Li 2 CO 3 With TiO 2 Li prepared by ball milling 4 Ti 5 O 12 As raw materials, a uniform and tightly combined lithium titanate / graphene (LTO / G) composite electrode material was prepared by hydrothermal synthesis process. 4 Ti 5 O 12 With stable internal structure, Li 4 Ti 5 O 12 It can maintain a stable spatial structure, thereby improving electrode performance; and Li 4 Ti 5 O 12 Composite with graphene can not only avoid direct contact between the negative electrode and the electrolyte, improve the compatibility between the electrolyte and the negative electrode, but also increase the Li 4 Ti 5O 12 The conductivity of graphene can provide more lithium embedding sites, which reduces the irreversible capacity. At the same time, the introduction of graphene can also promote the diffusion of lithium ions and reduce the SEI film impedance, thereby improving the high / low temperature performance of the battery. 4 Ti 5 O 12 During the hydrothermal reaction with graphene, the aggregation of graphene and its interaction with Li 4 Ti 5 O 12 The problem of loose bonding keeps graphene and Li 4 Ti 5 O 12 The bridge structure of graphene and Li 4 Ti 5 O 12 The bonding effect of the interface makes the composite material present a "point-surface" contact state, which makes the lithium titanate graphene composite electrode material have high specific capacity and excellent cycle and rate performance at high and low temperatures. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the specific implementation methods of the invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0040] Figure 1 To invent the discharge curve of lithium-ion batteries under 1C conditions at low temperatures;

[0041] Figure 2 To invent the working principle diagram of lithium-ion battery;

[0042] Figure 3 For the invention of embedded + The crystal structure of LTO changes during the process;

[0043] Figure 4 Schematic diagram of the invention of the Hummers method for preparing reduced graphene oxide;

[0044] Figure 5 For the invention of 4 Ti 5 O 12 Ball milling preparation process;

[0045] Figure 6 Schematic diagram for the preparation of the invented LTO / G composite electrode material;

[0046] Figure 7 To invent the overall design;

[0047] Figure 8 To invent TiO 2 and XRD pattern of LTO;

[0048] Fig. 9 To invent Raman spectra of composite materials with different graphene doping amounts;

[0049] Fig.10 SEM images of the precursors obtained after low-temperature calcination at different ball milling times: (a) not ball milled, (b) ball milled for 2 h, (c) ball milled for 4 h, (d) ball milled for 6 h, (e) ball milled for 8 h, (f) ball milled for 10 h;

[0050] Fig.11 SEM images of the microscopic morphology of the electrode materials obtained by adding different amounts of graphene after ball milling for 6 hours: (a) LTO morphology before ball milling, (b) LTO / G-3 morphology with 0.01g graphene added, (c) LTO / G-2 morphology with 0.015g graphene added; (d) LTO / G-3 morphology with 0.02g graphene added;

[0051] Fig.12 TEM images of the invented LTO / G-2 sample at different magnifications: (a, b) low-magnification microscopic morphology, (c) lattice distribution at high magnification;

[0052] Fig.13 (a)Li 4 Ti 5 O 12 Cyclic voltammetry curve of particles; (b) Li 4 Ti 5 O 12 Particle charge and discharge curves;

[0053] Fig.14 To invent the spinel structure and schematic diagrams of octahedral and tetrahedral interstices;

[0054] Fig.15 To invent the charge and discharge curves of LTO electrode under different ball milling times;

[0055] Fig.16 To invent the electrode performance after LTO and graphene are combined;

[0056] Fig.17 To invent LTO and compare the rate performance of different doped graphene materials;

[0057] Fig.18 Comparison of cycle stability and Coulomb efficiency under different conditions: (a) 2C; (b) 10C;

[0058] Fig.19 The CV (0.1 mV s -1 ) Graphs: (a) LTO, (b) LTO / G-2;

[0059] Fig. 20 The rate performance tests of different electrodes at room temperature, 40°C, 50°C and 60°C were performed: (a) LTO, (b) LTO / G-2;

[0060] Fig.21 To invent the cycling characterization of LTO and LTO / G-2 electrodes at high temperature (40°C);

[0061] Fig. 22 To invent the AC impedance diagram of LTO / G-2 composite material sample (the embedded diagram is the equivalent circuit diagram);

[0062] Fig.23 To invent the low frequency region Z' with ω at different temperatures -1 / 2 Graph of changes in data;

[0063] Fig.24 To invent different high temperature 6 Chemical migration of Li and relative intensities at different structural sites;

[0064] Fig.25 To invent CV characterization of LTO and LTO / G-2 electrodes under different low temperature conditions;

[0065] Fig.26 To invent the rate performance of different electrodes at low temperature: (a) LTO, (b) LTO / G-2;

[0066] Fig. 27 To characterize the cycling performance of different electrodes at low temperature (-20°C);

[0067] Fig.28 To invent the low frequency region Z' with ω at different temperatures -1 / 2 Graph of changes in data;

[0068] Fig.29 To invent the performance of the full battery at different temperatures: (a) rate, (b) cycle, (c) charge and discharge curves after different number of cycles at -10°C, (d) charge and discharge curves after different number of cycles at 40°C. DETAILED DESCRIPTION

[0069] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0070] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0071] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0072] 1. Experimental process

[0073] Example 1

[0074] S1. Preparation of graphene oxide by Hummers method

[0075] ① First, graphite and potassium persulfate were mixed in a mass ratio of 0.83:1 (6.0 g graphite and 7.2 g potassium persulfate) and slowly added to 276 mL of concentrated H 2 SO 4 and stirred with magnetic stirring for 15 min for later use;

[0076] ② Then slowly add 36g of strong oxidant potassium permanganate (KMnO 4 ), control the reaction temperature not to exceed 20°C;

[0077] ③ The mixture obtained above was stirred in an ice bath for 1.5 h, then heated to 40°C and kept at this temperature for 6 h to obtain a turquoise viscous solution. After the reaction was completed, the turquoise solution was added to 4 L of deionized water under vigorous stirring;

[0078] ④ Then add a certain amount of H 2 O 2 The solution was stirred until no more bubbles were generated and the stirring was continued for 5 min. Finally, the mixed solution was centrifuged and washed until the pH value was close to 5.0 to obtain graphene oxide, which was then freeze-dried to obtain graphene oxide powder. Figure 4 shown.

[0079] S2, Li 2 CO 3 With TiO 2 Preparation of Li by ball milling 4 Ti 5 O 12

[0080] Weigh Li with a stoichiometric ratio of n(Li / Ti)=0.85 2 CO 3 and TiO 2 A total of 20g of powder was mixed and mixed, and after being fully dried, it was pre-calcined at low temperature (650℃) in a muffle furnace for 8h. Then it was added to an appropriate amount of anhydrous ethanol and ball-milled in a planetary ball mill at a material-ball ratio of 1:10 and a speed of 400r / min for 6h. After standing for 6h, it was filtered and dried. The dried sample was calcined at a high temperature of 800℃ for 10h and cooled in the furnace to obtain the product Li 4 Ti 5 O 12 Powder. Process as Figure 5 shown.

[0081] S3, Li 4 Ti 5 O 12 Preparation of composite electrode materials by hydrothermal reaction of LTO and graphene oxide (GO)

[0082] ①According to Li 4 Ti 5 O 12 After LTO was quantified, the corresponding mass of freeze-dried GO was weighed and dissolved in 100 mL of deionized water according to the above calculation results, stirred evenly for 30 min, and then ultrasonicated for 30 min using a pulverizer, and an appropriate amount of PDDA was added for standby use.

[0083] ② Then weigh LTO according to the proportion and add it to the solution in step ①, then stir it magnetically for 6 hours, transfer it to the polytetrafluoroethylene liner after the suspension is evenly mixed, cover it with the polytetrafluoroethylene liner cover and the stainless steel cover, and put it into a blast drying oven preheated at 180°C for hydrothermal reaction. The reaction time is controlled to be 9 hours. After the reaction is completed, the temperature is lowered to room temperature (the temperature of the reactor should also be room temperature), taken out, washed, and dried;

[0084] ③After drying, the composite material is placed in a quartz crucible, placed in a tube furnace, heated to 800-900°C at a heating rate of 5°C / min in an Ar atmosphere and kept warm for 6 hours, and then cooled to room temperature with the furnace to obtain a composite thin film electrode material. Design and synthesis diagram of lithium titanate / graphene electrode material ( Figure 6) and specific processes ( Figure 7 ).

[0085] Example 2

[0086] The ball milling time was 3 h, and other parameters and steps were the same as in Example 1.

[0087] Example 3

[0088] The ball milling time was 4 h, and other parameters and steps were the same as in Example 1.

[0089] Example 4

[0090] The ball milling time was 5 h, and other parameters and steps were the same as in Example 1.

[0091] Example 5

[0092] The ball milling time was 7 h, and other parameters and steps were the same as in Example 1.

[0093] Example 6

[0094] Li 4 Ti 5 O 12 :GO (mass ratio) is 70:30 (denoted as LTO / G3), and other parameters and steps are the same as in Example 1.

[0095] Example 7

[0096] Li 4 Ti 5 O 12 :GO (mass ratio) is 90:10 (denoted as LTO / G1), and other parameters and steps are the same as in Example 1.

[0097] Example 8

[0098] The hydrothermal reaction time was 8 h, and other parameters and steps were the same as in Example 1.

[0099] Example 9

[0100] The hydrothermal reaction time was 10 h, and other parameters and steps were the same as in Example 1.

[0101] 2. Structural and electrochemical characterization

[0102] 2.1 Morphology Characterization

[0103] X-ray diffractometer (XRD, Rigaku D / Max-2400, working conditions: Cu target Ka ray, 40kV, 110mA current) was used to analyze TiO 2, the phase structure and crystal morphology of Li4Ti5O12 samples with different ball milling times; the Raman spectrometer (Raman, HORIBA LabRAM HR) was used to test the graphitization degree and defect content of graphene and the characteristic peaks of Li4Ti5O12; the scanning electron microscope (SEM, Hitachi S4800) was used to analyze the micromorphology of TiO2, Li4Ti5O12, LTO / G-1, LTO / G-2, and LTO / G-3; the transmission electron microscope (TEM, FEI Tecnai F20) was used to characterize the micromorphology of the optimal sample obtained; the X-ray photoelectron spectrometer (XPS, Thermo Kalpha) was used to test the bonding form of different elements in the sample and the valence distribution of Ti element.

[0104] 2.2 Electrochemical characterization

[0105] (1) Battery packaging: In the experiment, the electrodes prepared under different conditions were packaged into half-cells (button cell, 2032 type), that is, Li sheet was used as the counter electrode, the prepared material was used as the working electrode, the solute was LiPFs, the solvent was an organic solution prepared by dimethyl carbonate, diethyl carbonate and ethylene carbonate in a volume ratio of 1:1:1 as the electrolyte, and the diaphragm was a commercial Celgard2320 diaphragm. The entire packaging process was completed in an Ar atmosphere glove box to avoid the influence of oxygen and moisture. After packaging, it was left to stand for 12 hours before testing.

[0106] (2) Cyclic voltammetry (CVs) test: The equipment used was a Biologic electrochemical workstation (VMP-300, France). The scan rate was set to 0.1 mV s -1 , the scanning voltage range is 1.0-3.0 V. The cyclic voltammetry curve test can indirectly characterize the redox reaction process occurring on the electrode surface, and verify the phase and process of the reaction based on the redox peak.

[0107] (3) Charge / discharge test: Wuhan The test was carried out using the LAND CT2001A multi-channel battery test equipment of Blue Electric Electronics. The charge and discharge curves can characterize the redox reaction of the electrode, the charge and discharge platform voltage, and the first cycle coulomb efficiency.

[0108] (4) Rate capacity test: Based on the charge and discharge curve, by setting different current densities, the capacitance at different current densities is analyzed, and the rate curve is obtained by statistically plotting the discharge / charge specific capacity obtained at different current densities. Generally, as the rate increases, the capacity decays more slowly, and the rate performance is better; conversely, the rate will be worse. The rate performance characterization directly reflects the practical applicability at different current densities.

[0109] (5) Cyclic stability test: Based on charge and discharge, the curve obtained by multiple cycles at a uniform current density is the cyclic performance. Generally, the better the cyclic performance, the slower the capacity decay, which is more conducive to extending the service life of lithium-ion batteries.

[0110] (6) Electrochemical impedance spectroscopy (EIS) test: The equipment is a Biologic electrochemical workstation (VMP-300, France). The frequency range is set to 0.01 Hz to 100 kHz, and the step is 5 mV for the electrochemical impedance spectroscopy test. In general, the low-frequency region of the electrochemical impedance curve is diffusion-controlled, and the high-frequency region is kinetic-controlled. By fitting the electrochemical curve, the interface contact resistance, reaction kinetic resistance, and diffusion resistance can be determined, which indirectly indicates the electron transport capacity.

[0111] 3. Results and Discussion

[0112] 3.1 Structure and morphology characterization

[0113] Figure 8 a is the purchased TiO 2 XRD diagram of the powder. It can be seen from the figure that the TiO 2 It presents an rutile structure, and there are also a small amount of impurity peaks. Analysis shows that the reason may be caused by impurities in the powder during the preparation process, but the impurity peaks are very small and do not affect the practical application.

[0114] Figure 8 b is TiO 2 XRD spectrum of the product obtained after ball milling and calcination at 800℃ with lithium carbonate. As can be seen from the figure, compared with the standard spectrum (JCPDS card 49-0207), after the ball milling time is 2h, the product contains a small amount of TiO 2 (2θ is 27.3°), but the main phase is still lithium titanate. The main reason is that the ball milling time is short, which is not conducive to complete lithiation and formation of lithium titanate. As the ball milling time increases from 4h to 6h, the purity of the product lithium titanate will become higher and higher. When the ball milling time reaches 8h, the 2θ of the XRD spectrum is 25.5° and non-Li 4 Ti 5 O 12 peak, but the main phase is still spinel Li4 Ti 5 O 12 According to the standard spectrum, the phases appearing at 2θ of 18.3°, 35.6°, 43.3°, 47.4°, 57.2°, 62.8° and 66.1° correspond to Li 4 Ti 5 O 12 (111), (311), (400), (331), (333), (440) and (531) crystal planes of (JCPDS Card 49-0207).

[0115] Therefore, the lithiation step can be divided into the following two stages: 1) Under the condition of low temperature pre-burning, Li 2 CO 3 Will be with TiO 2 Alloying reaction occurs to form lithium-rich compound Li 2 TiO 3 Therefore, lithium titanate can be formed even after ball milling for 2h; 2) Under ball milling and high temperature conditions, Li 2 TiO 3 Will further with TiO 2 The reaction generates Li 4 Ti 5 O 12 Among them, Li generated by low-temperature pre-sintering reaction 2 TiO 3 Encapsulated in TiO 2 surface, hindering Li 2 CO 3 With TiO 2 Further reaction leads to the partial inclusion of impurity TiO in the final product. 2 The precursor generated by the low-temperature pre-sintering reaction can break up the large particles generated by the first step reaction and expose the encapsulated TiO 2 , creating a new reaction interface and promoting Li 2 TiO 3 With TiO 2 Further reaction can improve the purity of the product. At the same time, ball milling of the precursor can enhance the activation energy of the precursor, improve the reaction activity of the precursor material, and further promote Li 2 TiO 3 With TiO 2 reaction to improve the purity of the product.

[0116] When reduced graphene oxide and Li 4 Ti 5 O 12After the composite, the presence of graphene could not be detected due to the strong peak of lithium titanate and the large half-peak width and low intensity of graphene. In order to detect whether graphene and lithium titanate form a composite material under hydrothermal conditions, Raman spectroscopy analysis was performed on LTO / G composite materials with different amounts of graphene added. Fig. 9 The Raman spectra of the composite materials with 0.02g, 0.015g and 0.01g of graphene added are shown in the figure. -1 Obvious characteristic peaks were detected at 1353 cm-1, and the intensity was high. Compared with the standard spectrum, it was shown that the characteristic peak was the peak type of LTO. It is worth noting that all three samples have a peak at 1353 cm-1. -1 and 1591cm -1 There are two characteristic peaks near the carbon material: the D peak and the G peak. The G peak represents the presence of graphitized carbon, and the D peak represents the irregularity or defects of graphitized carbon. By comparing the peak intensities, the I D / I G The D peak intensity is significantly lower than the G peak intensity, indicating that graphene is prone to stacking during the hydrothermal process. The results show that this method can be used to introduce graphene into LTO and form an LTO / G composite material.

[0117] Scanning electron microscope (SEM) images can reflect the morphology of lithium titanate and graphene-coated lithium titanate in real time. Fig.10 For Li 2 CO 3 Mixed TiO 2 The morphology distribution after different ball milling time and low temperature calcination. Fig.10 a shows the morphology of the precursor before ball milling. It can be seen that its particle size distribution is relatively uniform, about 1-2um. As the ball milling time continues to increase, the particle size of the obtained material changes significantly. When the ball milling time is 2h, the precursor particles are reduced to about 1um, but the degree of reduction is not large. At the same time, there are also some larger particles, indicating that short ball milling time will lead to uneven particle size distribution. As the ball milling time increases to 10h, the particle size of the precursor particles becomes smaller and smaller. Surface ball milling is an effective way to reduce the particle size of the material. However, when the ball milling time is greater than 8h, the material will show obvious agglomeration, and as the ball milling time increases, the agglomeration phenomenon tends to be more serious. Comprehensively considering different ball milling times, when the ball milling time is 6h, the material obtained is more evenly distributed than the samples obtained under other conditions.

[0118] The tap density of lithium titanate has a certain effect on electrode packaging. The greater the tap density, the higher its application value. Table 1 shows the tap density of the materials obtained by ball milling the precursor at different times. As can be seen from Table 1, the tap density of the sample obtained when the precursor is not ball milled is only 0.96g / cm3 As the ball milling time increases, Li 4 Ti 5 O 12 The tap density of the precursor increases first and then decreases. When the precursor is ball-milled for 6 hours, the tap density of the obtained material reaches a maximum value of 1.72 g / cm 3 . Combined with the SEM test results, it can be seen that this is closely related to the uniform distribution of material particles and the best dispersion effect when ball milled for 6 hours, as well as the spherical morphology. The particle surface of the spherical material is smooth and has good fluidity, resulting in a higher tap density. As the ball milling time increases, the agglomeration phenomenon becomes more and more serious, resulting in poor fluidity of the material and a decrease in tap density.

[0119] Table 1. Tap density of LTO at different ball milling times

[0120]

[0121] The lithium titanate and graphene composites with a ball milling time of 6 h were selected. The scanning electron microscopy of the samples obtained after adding 0.01 g (LTO / G-3), 0.015 g (LTO / G-2) and 0.02 g (LTO / G-3) graphene were as follows: Fig.11 As shown. Fig.11 a is a scanning electron microscope image of uncompounded graphene material, which is convenient for comparison with graphene doping. Fig.11 b is the SEM image of the electrode material obtained after adding 0.01g of graphene, and an obvious lamellar structure can be seen between the particles. As the graphene mass is further increased to 0.015g ( Fig.11 c), the graphene sheet structure is more obvious and evenly distributed between lithium titanate particles, which is conducive to bridging lithium titanate particles and forming "surface-point" contact, providing an electron transmission channel for lithium titanate. When the graphene addition amount is 0.02g ( Fig.11 d), graphene will agglomerate and gradually begin to graphitize. Compared with LTO / G-2, too high an addition amount will affect the performance of graphene and lead to poor electron transmission performance. It can be seen that it is difficult to form a good electron transmission channel when adding a small amount of graphene, while too much addition will cause graphene to tend to graphitize. Therefore, when the addition amount is 0.015g, it can provide better ion transmission performance and is conducive to the performance of lithium titanate.

[0122] Transmission electron microscopy (TEM) images can reflect the interface contact effect between graphene and lithium titanate, so TEM tests were performed on LTO / G-2 samples. Fig.12a shows the sample morphology at low magnification. It can be seen from the figure that the graphene is layered and evenly dispersed, and the lithium titanate particles are dispersed between the graphene sheets. Further magnification shows that the lithium titanate is distributed as a whole between the graphene sheets, and the graphene and lithium titanate particles are seamlessly connected, indicating that the two are "point-to-surface" bridges ( Fig.12 b), which is beneficial to electron transport. Fig.12 c is the lattice fringe distribution under high magnification. By comparing with the standard card, the interplanar spacing is 0.482nm, which belongs to Li 4 Ti 5 O 12 (111) crystal plane. In addition, the number of graphene layers can be clearly obtained under high-magnification TEM, which is about 10-15 layers. Comprehensive scanning electron microscopy and transmission electron microscopy can prove that graphene and lithium titanate meet the expected "point-surface" contact, which is conducive to the subsequent improvement of lithium storage performance.

[0123] 3.2 Characterization of electrochemical performance at room temperature

[0124] Fig.13 The figure shows the Li assembled from the material obtained without ball milling of the precursor. 4 Ti 5 O 12 / Li half-cell at a typical cyclic voltammetry (CV) curve and the charge-discharge curve at 0.1C. In the cyclic voltammetry curve ( Fig.13 a), when the scan rate is 0.2 mV s -1 When the oxidation peak appears at 1.61V, the corresponding reduction peak appears at 1.33V, which is close to the position of the redox peaks reported in many literatures, indicating that the redox peaks are generated by the following redox process:

[0125] [Li] 8a [Li 1 / 3 Ti 5 / 3 ] 16d [O 4 ] 32e +e - —[Li 2 ] 16c [Li 1 / 3 Ti 5 / 3 ] 16d [O 4 ] 32e (Charge)

[0126] [Li 2 ] 16c [Li 1 / 3 Ti 5 / 3 ] 16d [O 4 ] 32e -Li + -e- —[Li] 8a [Li 1 / 3 Ti 5 / 3 ] 16d [O 4 ] 32e (Discharge)

[0127] Since lithium titanate itself does not provide Li + , when in the charging process, the external Li + Will be embedded in Li 4 Ti 5 O 12 The Li embedded in the lattice + Will react with Li at the 8a site + Migrate to the octahedral 16c and eventually form a light blue salt rock phase [Li 2 ] 16c [Li 1 / 3 Ti 5 / 3 ] 16d [O 4 ] 32e During the discharge process, [Li 2 ] 16c [Li 1 / 3 Ti 5 / 3 ] 16d [O 4 ] 32e They will lose electrons, and Li + It will move out from the 16c position and return to the 8a position. Its crystal structure changes as follows Fig.14 shown. Fig.13 In a, when the scan rate increases from 0.2mV / s to 1.6mV / s, the oxidation peak shifts to the left and the reduction peak shifts to the right, but the shift is not large, which indirectly proves that lithium titanate itself has good rate performance. In the charge and discharge curve test, the 1st, 5th and 25th cycles ( Fig.13 b). From the analysis of the first cycle, it can be found that the discharge platform appears at 1.55V and the charge platform appears at about 1.60V; with the increase of the number of cycles, the position of the charge and discharge platform does not change significantly, which shows the structural stability of LTO; in addition, according to the calculation formula, the discharge capacity of the first cycle under 1C condition is 170mAh / g; even after 25 cycles, its discharge capacity can still maintain 168mAh / g.

[0128] Fig.15 The charge-discharge curves obtained under 1C conditions for different ball milling times are shown in Figure 2. When the ball milling time is 0h, the charge-discharge curves and Fig.13 b is basically similar, and the charge and discharge platform is consistent. When the ball milling time is 1h, Li 4 Ti 5O 12 The particle size is significantly reduced, so the capacity increases significantly, and the capacity can reach 192mAh / g. When the ball milling time is 2h and 4h, the particle size will continue to decrease, but it is not obvious, and the resulting capacity is about 210-220mAh / g. When the ball milling time increases to 6h, because the particle size is small and evenly distributed, the discharge capacity can reach 240mAh / g. However, as the ball milling time increases to 10h, due to the smaller particles beginning to agglomerate, it does not have a high capacity like 6h, but a lower specific capacity appears. In general, with the extension of ball milling time, the battery charge and discharge capacity of different materials increases first and then decreases, indicating that reducing the particle diameter is conducive to shortening the migration path of lithium ions and improving the electrochemical properties of the material. When the ball milling time is greater than 6h, the capacity performance of the material decreases. This is because the appearance of agglomeration increases the diffusion and migration resistance of lithium ions and limits the capacity of the material. Therefore, uniform particle size distribution is a necessary condition for obtaining excellent electrochemical properties of the material.

[0129] After lithium titanate and graphene are combined, the charge and discharge curve is tested at a rate of 5C. After the test is stable, the curve obtained by taking the same cycle is as follows: Fig.16 As shown in the figure, it can be seen that Li 4 Ti 5 O 12 The discharge capacity at 2C is still close to 160mAh / g, and compared with Fig.16 In the curve under 1C condition, the charge and discharge platform has not changed significantly (the platform spacing is less than 0.12V). With the introduction of graphene, the specific capacity of LTO / G composite materials has been significantly improved, but the performance is different with different graphene incorporation amounts. When the graphene content is 0.01g, due to the low content of graphene, it is impossible to form a connected two-dimensional layered structure between lithium titanate particles, resulting in a small performance improvement, which can only reach 170mAh / g; when the graphene incorporation amount is 0.015g, because the aforementioned SEM results have shown that graphene can fully integrate with Li 4 Ti 5 O 12 Bridging, so its capacity is the largest, about 178mAh / g; when the amount of graphene added is too much (0.02g), the graphene will agglomerate, causing the bridging form to be destroyed, resulting in a significant decrease in capacity (its capacity is only 173mAh / g). It can be seen that the composite of graphene and lithium titanate can increase the specific capacity of lithium titanate, but the capacity is affected by the amount of graphene added. With the addition of graphene, the capacity shows a trend of first increasing and then decreasing. Therefore, choosing the appropriate amount of graphene added is the key to ensuring the capacity is improved.

[0130] like Fig.17The figure shows the rate performance of LTO / G after different graphene additions. As can be seen from the figure, at the rates of 1, 2, 5, 10, and 20C, the discharge capacity of pure LTO without graphene is 162, 133, 125, 108, and 95 mAh / g, respectively, and the rate retention rate is about 58%; when the rate returns to 1C, its capacity will increase to 170 mAh / g due to polarization; when the graphene addition amount is 0.01g, the LTO / G-3 obtained at the rates of 1, 2, 5, 10, and 20C can reach 175, 142, 133, 115, and 104 mAh / g (rate retention rate is 59.5%); when the graphene addition amount reaches 0.02 The LTO / G-1 obtained at 0.015g has a discharge capacity of 191, 184, 177, 162 and 155 mAh / g at rates of 1, 2, 5, 10 and 20C, respectively (rate retention rate is 81%). Compared with LTO, LTO / G-1 and LTO / G-3, the LTO / G-2 composite material with an incorporation amount of 0.015g can obtain a discharge capacity of 221, 215, 205, 183 and 174 mAh / g at rates of 1, 2, 5, 10 and 20C (rate retention rate is 78.7%). Even when it returns to a rate of 1C, the LTO / G-2 electrode can still recover to a specific capacity of 220 mAh / g, which is much higher than the LTO, LTO / G-1 and LTO / G-3 electrodes. It is also worth noting that both undoped graphene and doped graphene electrode materials show good cycle stability at different rates (the decay of 10 cycles at each rate is not obvious), which indirectly indicates that both LTO and LTO / G have structural stability during the cycle process. It can be seen that the difference between doped and undoped graphene materials lies in whether additional ion / electron transmission paths and buffer volume expansion effects are provided, thereby contributing to the improvement of capacity.

[0131] like Fig.18 a is the cycle performance diagram under 2C conditions. As can be seen from the figure, LTO has obvious attenuation within 200 cycles, while LTO / G-1 and LTO / G-3 have relatively stable performance and no obvious attenuation has occurred during the 200 cycles. It is worth noting that the electrode capacity of LTO / G-2 (graphene doping amount is 0.015g) shows a trend of first decreasing and then increasing. This trend of first decreasing and then increasing is mainly due to the continuous training process due to the Li + During insertion / extraction at different locations, the electrolyte is consumed and the SEI film is formed, which leads to a decrease in the electrolyte and then a decrease in the electrolyte due to Li + The insertion / extraction of Li leads to some defects in the crystal structure, which can accommodate more Li +Therefore, although LTO / G-2 has a downward trend in the early stage, it has more practical advantages because of its high discharge capacity and no attenuation after 200 cycles. In addition, in order to study the cycle performance under high current conditions, the cycle performance of LTO / G-2 and LTO electrodes under 10C conditions was tested. Fig.18 As shown in b. It can be seen that under 10C conditions, the LTO electrode will decay during the cycle, but the decay amplitude is not large. In comparison, LTO / G-2 is more stable and does not decay after 500 cycles.

[0132] 3.3 Electrochemical performance at high temperature

[0133] The LTO and LTO / G electrodes prepared above were assembled into half-cells, and their performances under high temperature and low temperature conditions were tested. Fig.19 a is LTO and LTO / G-2 at 0.1mVs -1 The CV graph obtained by testing at a scanning rate. For the half-cell assembled with LTO electrode material, it can be found that at room temperature (25°C), the oxidation peak appears at about The reduction peak appears at about The difference between the two And the peak intensity is high, which is basically consistent with the CV tested previously. When the temperature is raised to 40°C, the oxidation peak shifts significantly to the left, the reduction peak shifts significantly to the right, and the peak position deviation decreases to 0.11V. This is mainly because the temperature rises, the ion transport is faster, thereby reducing the polarization internal resistance generated by electron transfer and improving the reversibility of its electrode reaction; when the temperature is raised to 50 or 60°C, the peak position is basically the same as at 40°C, which also proves that the reversibility will be significantly improved at high temperature.

[0134] Fig.19 b shows the CV graph of the LTO / G-2 electrode. It can be seen from the figure that the peak position deviation of the redox peak at room temperature (0.13V) is still greater than the deviation at high temperature (0.10V) after graphene composite, indicating that high temperature also promotes the ion transport of LTO / G. It can be seen that compared with LTO, after composite with graphene, the peak position deviation will be reduced regardless of high temperature or room temperature, and the reversibility will be significantly improved.

[0135] like Fig. 20This is a rate performance test of different electrodes under different high temperature conditions. For the LTO electrode, the rate performance at room temperature is basically similar to the above. When the temperature is 40°C, at the rates of 1C, 2C, 3C, 5C, 10C and 20C, the output capacity of the LTO electrode is 152, 145, 139, 132, 120 and 100mAh / g (the rate retention rate is 65.8%); when the temperature is 50°C, at the same rate, the specific capacity of LTO is 155, 146, 142, 134, 119 and 79mAh / g (the rate retention rate is 50.1%); at 60°C, the specific capacity at the same rate is significantly attenuated, and the attenuated specific capacity is about 142, 139, 130, 122, 116 and 40mAh / g (the rate retention rate is 28.2%). In comprehensive comparison (Table 2), for LTO, the capacity and rate at 40°C are better than those at room temperature and higher temperatures, and LTO can also work normally in a high temperature environment of 60°C, indicating that LTO itself is suitable for high temperatures.

[0136] Fig. 20 b is the rate performance test of LTO / G-2 electrode at different temperatures above room temperature. The LTO / G-2 electrode at 40°C shows higher rate and stability, that is, at current densities of 1C, 2C, 3C, 5C, 10C and 20C, the capacity of the LTO / G-2 electrode can reach 230, 212, 209, 193, 182 and 161 mAh / g respectively (rate retention rate is 70%), and even if it returns to the current density of 1C, its discharge capacity can still reach 210 mAh / g. When the temperature reaches 50°C, the capacity of the LTO / G-2 electrode at the same rate is 221, 209, 203, 188, 172 and 155 mAh / g respectively (rate retention rate is 69.1%), while the capacity at 60°C is 218, 206, 185, 166, 151 and 133 mAh / g (rate retention rate is 61.1%). It can be seen that after LTO and graphene are composited, the formed LTO / G-2 electrode has the highest capacity at different rates at 40°C (Table 3).

[0137] Table 2. Discharge capacity of LTO at 1C, 5C and 10C at different temperatures

[0138]

[0139] Table 3. Discharge capacity of LTO / G-2 at 1C, 5C and 10C at different temperatures

[0140]

[0141] Then the cycling performance of LTO and LTO / G-2 was compared at 40℃ and 1C. Fig.21 As shown in the figure, the capacity of LTO can be maintained at 170 mAh / g in the first cycle at 40°C. As the number of cycles increases, the capacity gradually decays and is only 102 mAh / g after 500 cycles. For the LTO / G-2 electrode, it decays first during the cycle, then the capacity rises, and after 500 cycles, the capacity can still be maintained at nearly 220 mAh / g (the capacity retention rate after 500 cycles is >100%), indicating that it can maintain long-term operation at 40°C.

[0142] Fig. 22 The AC impedance graph at 0.01Hz-100kHz is shown in Table 4. s , R ct and R f It can be seen that as the temperature increases, the charge transfer resistance R of the LTO assembled half-cell increases. ct The value is significantly reduced. This indicates that LTO may have higher electrochemical activity at high temperatures. The charge transfer resistance R of the half-cell assembled with LTO / G-2 ct With similar rules, LTO / G-2 after graphene composite has lower diffusion internal resistance, indicating that LTO / G will provide smaller ion transfer impedance due to the introduction of graphene. In addition, under high temperature conditions, due to the fast movement rate of ions themselves, the electron transfer impedance value will be further reduced.

[0143] In order to verify whether this law exists in the ion transfer process, the AC impedance in the low-frequency region is deformed to obtain Z'-ω -1 / 2 The spectrum of Fig.23 ). Low frequency region LTO and LTO / G-2Z'-ω -1 / 2 The line graph shows a linear correlation and the slope of the line is attributed to the diffusion of lithium ions into the bulk of the electrode material or so-called Warburg diffusion. The lithium ion diffusion coefficient (D) can be calculated from the low frequency graph according to the following equation:

[0144] Z re =R ct +R s +σω -1 / 2 (1)

[0145]

[0146] Where R is the gas constant, T is the absolute temperature, S is the electrode area, n is the number of moles of transferred electrons, F is the Faraday constant, and C is Li + concentration, σ is the Warburg factor. From the diffusion coefficient, it can be found that the diffusion coefficient of lithium ions increases significantly in the range of 25-60°C, which indicates that the kinetics of lithium ion and electron transfer to the electrode at high temperatures is much faster than that at low temperatures.

[0147] Table 4. Impedance coefficient and diffusion coefficient at high temperature

[0148]

[0149] For Li at different temperatures + The embedding and unembedding mechanisms of Fig.24 a It can be seen that with increasing temperature, all three peaks move in the direction of decreasing ppm. This general trend can be attributed to the thermal expansion of the material with temperature. Below 525K, the isotropic chemical shift of the 8a peak changes significantly and moves toward the 16d peak. Above 525K, the 8a peak and the 16d peak are inseparable. All peaks show an increase in line width over the entire temperature range. This shows that the broad peak above 525K is not the result of the merging of the 8a and 16d peaks, but is due to the broadening of the 8a and 16d peaks so that they strongly overlap, indicating that there is no significant lithium exchange between the 8a and 16d sites. Fig.24 b shows three lithium resonances 6 Temperature dependence of Li integrated intensity. The integrated intensity of the 16c peak increases from 12% at 300K to about 40% at 675K, while the integrated intensity of the 8a peak decreases sharply with increasing temperature. This result clearly shows that with increasing temperature, lithium ions are gradually redistributed from the 8a site to the 16c site. This lithium migration will eventually lead to the merging of the various 6Li peaks. The complete migration of lithium from the 8a site to the 16c site will lead to a defective NaCl-type structure (space group), whereby lithium ions and cation vacancies are distributed on the 16c site ( Fig.24 b).

[0150] Based on the performance under different high temperature conditions, it can be found that when the temperature rises, the electron / ion transport performance of LTO and LTO / G-2 electrodes will show a trend of first increasing and then decreasing. For the LTO / G-2 composite sample, its specific capacity can reach 230mAh / g at a current density of 1C in an external environment of 40°C. Even if it is increased to 20C, its capacity can still be maintained at 180mAh / g, with a rate greater than 70%. Even if it is cycled 500 times at high temperature, it still does not decay. Through the analysis of the electron / ion transport efficiency, the higher the temperature, the higher the diffusion kinetics of ions and electrons in the electrolyte and electrode structure respectively, which can significantly improve the diffusion efficiency of ions / electrons.

[0151] 3.4 Electrochemical performance at low temperature

[0152] Further research on the electrochemical performance at low temperatures is to verify whether lithium titanate and its composite materials can be used in low temperature environments. Fig.25a and b are CV curves of LTO and LTO / G-2 electrode materials at 20, 0, -10 and -20 ° C, respectively. As can be seen from the figure, LTO / G-2 composited with graphene has a smaller redox peak position deviation, which is basically similar to the rules of electrodes at high temperature and room temperature.

[0153] like Fig.26 The rate performance of different electrodes at low temperature is characterized. For LTO electrode, such as Fig.25 As shown in a, when the temperature reaches the freezing point at 0°C, the lithium titanate electrode can still work normally. However, compared with the performance at room temperature, it can be found that the rate of LTO at 0°C is significantly worse, which is mainly caused by the slower migration of ions at low temperatures. As the temperature continues to drop to -10 and -20°C, its initial capacity and rate performance are significantly worse. When graphene and lithium titanate are composited ( Fig.26 b), LTO / G-2 electrode exhibits better specific capacity and rate performance than LTO; the rate is 60% at -10°C, and even in a -20°C temperature environment, it can still output specific capacities of 200, 183, 155, 121, 92 and 78 mAh / g at current densities of 1, 2, 3, 5, 10 and 20C (rate is 40%).

[0154] Fig. 27 The figure shows the cycle performance at low temperature (-20°C). It can be seen that the LTO / G-2 electrode shows a downward trend in the first 70 cycles. As the number of cycles continues to increase, the specific capacity will continue to increase. After 500 cycles, the specific capacity is about 191mAh / g. This is because the consumption of electrolyte and the formation of SEI film in the initial stage cause the capacity to decay. However, as the number of cycles increases, due to the Li + The continuous embedding / de-embedding of graphene will generate more active sites and the strengthening effect of graphene, which will increase the efficiency of ion and electron transport even at low temperatures, resulting in an increase in capacity.

[0155] In addition, the AC impedance test of Li + The transmission efficiency and transport path of Z′ are theoretically analyzed. -1 / 2 Plotting, we can see ω -1 / 2 -Z' is a straight line with a slope of σ ( Fig.28 ). The lithium diffusion coefficient (D) of LTO and LTO / G-2 electrodes was calculated by the calculation formula (Table 5). It can be seen that the reduction of working temperature will significantly affect the lithium diffusion coefficient. By comparing the lithium diffusion coefficients of LTO and LTO / G-2 electrodes, it can be found that after graphene is composited with lithium titanate, the ion transmission efficiency will be improved even under low temperature conditions.

[0156] Table 5. Impedance coefficient and diffusion coefficient at low temperature

[0157]

[0158] The initial discharge capacity of the LTO / G-2 composite sample at low temperature of -20°C is about 200 mAh g -1 (1C), which is higher than the LTO sample under the same conditions. Under low temperature conditions of -10℃, when the rate performance is increased from 1C to 20C, it is still higher than 60%; and there is almost no attenuation after 500 cycles at 1C, which shows the practical applicability of the electrode.

[0159] Finally, LiCoO 2 As the positive electrode, LT / G-2 as the negative electrode, the full battery was assembled and tested at -10 and 40 °C, respectively. Fig.29 a shows the full battery rate test between 1.00 and 2.85V. Among them, the LCO / / LTO / G-2 full battery at 40℃ showed higher capacity than the LCO / / pure LTO full battery at different rates from 0.2 to 10C (Table 6). The LCO / / LTO / G-2 full battery can provide a discharge capacity of 145mAh / g at 40℃, while the LCO / / LTO / G-2 full battery only maintains a discharge capacity of 129mAh / g at -10℃. The cycling performance of the LCO / / LTO / G-2 full battery at -10 and 40℃ is shown in Figure 6. Fig.29 b. The initial discharge capacities of the full battery at -10 and 40°C at 0.5C are 141 and 150 mAh / g, respectively. After 500 cycles, the discharge capacity of the LCO / / LTO / G-2 full battery at 40°C is as high as 144 mAh / g, and the capacity loss is only 4.2%, which is much higher than the capacity loss of the full battery at -10°C (111 mAh / g, capacity loss is 21.8%). The corresponding charge and discharge curves for the 1st, 100th, 300th and 500th cycles are shown in Fig.29 c, d. The results show that the rate and cycle performance of the LCO / LTO-CNTs-2 full cell are better than those of the LCO / pure LTO full cell, which can be attributed to the composite of LTO and graphene, which is consistent with the results of the half cell.

[0160] Table 6 Capacity statistics of full batteries at different temperatures

[0161]

[0162] In summary, the hydrothermal treatment of graphene and lithium titanate can effectively improve the shortcomings of lithium titanate itself, such as poor electronic conductivity and rapid attenuation under high / low temperature conditions. The prepared graphene / lithium titanate composite material has high specific capacity and excellent cycle and rate performance at high and low temperatures.

[0163] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the invention rather than to limit it. Although the invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solution to deviate from the scope of the technical solution of the embodiments of the invention.

Claims

1. A method for preparing a lithium titanate graphene electrode material, It is characterized in that The following steps are involved: A composite electrode material generated by hydrothermal reaction of lithium titanate and graphene oxide, wherein the lithium titanate is Li 2 CO 3 With TiO 2 Li prepared by ball milling 4 Ti 5 O 12 ; Among them, the Li 4 Ti 5 O 12 The mass ratio of graphene oxide is (70-90):(10-30); The Li 4 Ti 5 O 12 The preparation comprises the following steps: 2 CO 3 With TiO 2 After mixing evenly, low-temperature pre-sintering, ball milling and high-temperature calcination are carried out in sequence, and Li 4 Ti 5 O 12 ; Li 2 CO 3 With TiO 2 The ratio is based on a Li / Ti molar ratio of 0.8-0.9; Before the low temperature pre-calcination, Li 2 CO 3 With TiO 2 The mixture is fully dried; During the low temperature pre-firing, the temperature is 650°C and the time is 8 hours; The specific steps of the ball milling treatment are: adding the mixture pre-sintered at low temperature into anhydrous ethanol and performing ball milling treatment in a ball mill; During the ball milling process, the material-ball ratio is controlled to be 1:(9-11), the rotation speed is 350-450r / min, and the ball milling time is 6h; The ball mill is a planetary ball mill; The high temperature calcination specifically includes: leaving the ball-milled mixture to stand for 5-7 hours, filtering, drying, first calcining and cooling in sequence to obtain Li 4 Ti 5 O 12 powder; During the first calcination, the temperature is controlled at 700-900°C and the time is 9-11h; The hydrothermal reaction specifically comprises: dissolving graphene oxide in deionized water, and adding Li 4 Ti 5 O 12 After stirring and mixing evenly, a hydrothermal reaction is carried out, and after the reaction is completed, washing, drying, a second calcination and cooling are carried out in sequence to obtain a composite electrode material; When the graphene oxide is dissolved, it is first mechanically stirred for 20-40 minutes, and then ultrasonicated by a pulverizer for 20-40 minutes; 4 Ti 5 O 12 After addition, stir magnetically for 5-7h; After the graphene oxide is dissolved, a polymer electrolyte is added; The polymer electrolyte is PDDA; During the hydrothermal reaction, the temperature is controlled at 170-190°C and the time is 8-10h; During the second calcination, the material is heated to 800-900° C. at a heating rate of 4-6° C. / min in an Ar atmosphere and kept at that temperature for 5-7 hours.