Comfort eTPU
By using thermoplastic elastomer foam material with energy storage modulus and density specific to the range of 0.01 to 0.5MPa, the problem of sudden increase in stiffness of seat materials during compression is solved, and good shock absorption and rebound characteristics are achieved, which improves the Seat comfort.
Patent Information
- Application Number
- CN202080078534.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-13
- Filing Date
- 2020-11-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-11-13
AI Technical Summary
The stiffness of existing seat materials suddenly increases when compressed, causing discomfort to the user and making it difficult to provide good shock absorption and rebound characteristics for a long time.
A foam material composed of thermoplastic elastomer (TPE-1) has an energy storage modulus in the range of 0.01 to 0.5MPa, a molding density in the range of 20 to 400 kg/m3, and a comfort factor greater than 4. By adjusting the density of the foam and structure to achieve slow hardening properties of the material.
It provides good shock absorption and rebound characteristics, while improving seat comfort, avoiding sudden hardening of the material during compression, and enhancing the user's comfort experience.
Smart Images

Figure BDA0003640032310000181 
Figure BDA0003640032310000191 
Figure BDA0003640032310000201
Abstract
Description
[0001] The present invention relates to a molded article comprising a foam composed of a thermoplastic elastomer (TPE-1), wherein the foam has a storage modulus (G modulus) at 25° C. and 1 Hz in the range of 0.01 to 0.5 MPa and a molded density in the range of 20 to 400 kg / m 3 and the comfort factor determined according to Reference Example 3, i.e., the compression hardness ratio (StH65% / StH25%), is greater than 4. The present invention also relates to a method for producing such a molded article, and the use of the molded article of the present invention for producing floors, mats, seating furniture, bicycle saddles, car seats, motorcycle seats, parts of shoes, as insoles, packaging, shock absorbers, protectors, anti-fall pads, elastic insulating materials or sealing materials.
[0002] Foams, including in particular bead foams, have long been known and are described many times in the literature, for example in Ullmann's " der technischen Chemie” [Encyclopedia of Industrial Chemistry], 4th edition, Vol. 20, pp. 416 ff.
[0003] Highly elastic, largely closed-cell foams, such as bead foams made of thermoplastic elastomers, produced, for example, in an autoclave or by extrusion, exhibit exceptional dynamic properties and, in some cases, also good resilience. Hybrid foams made of thermoplastic elastomer beads and system foams or adhesives are also known. Depending on the foam density, the production method and the matrix material, it is possible to produce a relatively wide range of overall stiffness levels. Post-treatment of the foam, such as heat treatment, can also influence the properties of the foam.
[0004] Foamed particulate materials based on thermoplastic polyurethane or other elastomers, also called bead foams (or particle foams), and moldings produced therefrom are known (e.g. WO 94 / 20568, WO 2007 / 082838 A1, WO 2017 / 030835, WO 2013 / 153190 A1, WO 2010 / 010010) and have a wide variety of possible uses.
[0005] For the purposes of the present invention, "expanded particulate material" or "bead foam" or "particulate foam" refers to a foam in the form of beads, wherein the average diameter of the beads is from 0.2 to 20 mm, preferably from 0.5 to 15 mm, in particular from 1 to 12 mm. In the case of non-spherical, such as elongated or cylindrical beads, the diameter refers to the longest dimension.
[0006] Polymers based on thermoplastic elastomers (TPE) have found applications in various fields. The properties of the polymer can vary depending on the application. Thermoplastic polyurethanes in particular are used in a variety of ways.
[0007] In upholstery, good shock absorption is necessary to ensure a high level of seating comfort. However, when sitting on soft seating materials, strong material compression often occurs and, above a relatively high compression level, the material (usually open-cell polyurethane foam) suddenly stiffens, with the result that the material becomes uncomfortably hard for the user.
[0008] It is therefore an object of the present invention to provide a thermoplastic elastomer-based molding which has good shock-absorbing and adjustable rebound properties while providing a high level of seating comfort. Particularly suitable materials are those whose stiffness increases slowly with increasing compression, so as to provide more stability when sitting. Another object of the present invention is to provide a method for producing a corresponding molding.
[0009] This object is achieved according to the invention by a molding comprising a foam composed of a thermoplastic elastomer (TPE-1), wherein the foam has a storage modulus (G modulus) at 25° C. and 1 Hz in the range from 0.01 to 0.5 MPa, determined according to Reference Example 1 (TPE molding), and a molding density in the range from 20 to 400 kg / m 3 The range is determined according to Reference Example 2, wherein the foam is a foamed particle material.
[0010] The present invention also relates to a molded article comprising a foam composed of a thermoplastic elastomer (TPE-1), wherein the foam has a storage modulus (G modulus) at 25° C. and 1 Hz in the range of 0.01 to 0.5 MPa, determined according to Reference Example 1 (TPE molding), and a molding density in the range of 20 to 400 kg / m 3 within the range determined according to Reference Example 2, wherein the comfort factor of the foam is greater than 4, determined according to Reference Example 3.
[0011] When the foam is present in the molded article in the form of non-connected beads, the molding density determined according to Reference Example 2 corresponds in the context of the present invention to the bulk density determined by Reference Example 4 or a value greater than this bulk density.
[0012] Surprisingly, it has been found that when using substantially closed-cell foams based on thermoplastic elastomers, in particular expanded particles, which have a low storage modulus and a relative high elasticity of 20 to 400 kg / m 3When the molding density is within the range of , a foam with low stiffness can be obtained, which does not suddenly compress when sitting, but stably hardens according to the degree of compression. By using a foamed particle material with defined properties according to the present invention, that is, the storage modulus (G modulus) at 25° C. and 1 Hz determined according to Reference Example 1 (TPE molding) is in the range of 0.01 to 0.5 MPa, and the molding density determined according to Reference Example 2 is in the range of 20 to 400 kg / m 3 In the range of , the obtained molded articles have a particularly advantageous combination of properties, for example for seating furniture. It is found that only the comfort factor determined according to reference example 3 is greater than 4, which has a significant effect on the comfort when sitting. By combining the properties of the foam used according to the present invention, a molded article with a comfort factor greater than 4 determined according to reference example 3 can be obtained.
[0013] The compression behavior of the molded part is initially similar to that of open-cell flexible foam and later to that of closed-cell bead foam; hardening does not take effect suddenly like open-cell flexible foam, but rather the back pressure continues to build, slowing the user down.
[0014] Surprisingly, it is not just the G modulus of the thermoplastic elastomer that is critical to the initial stiffness, but also the G modulus of the foam and the density of the foam. In addition, a regular foam structure is also advantageous because it experiences uniform compression and is therefore softer at the outset.
[0015] Thus, for example, the stress-strain curves of the examples according to the invention are compared with those of the comparative examples. Figure 1 The graph shown shows that the initial stage is flat and gradually rises.
[0016] The molded article of the present invention comprises a foam composed of a thermoplastic elastomer (TPE-1), wherein the storage modulus (G modulus) of the foam at 25° C. and 1 Hz is in the range of 0.01 to 0.5 MPa, determined according to Reference Example 1 (TPE molding), and the molding density is in the range of 20 to 400 kg / m 3In the range of , determined according to Reference Example 2, and preferably also with a comfort factor of greater than 4, determined according to Reference Example 3. According to the invention, the foam in the context of the present invention may be a slabstock foam or consist of or contain a foamed particulate material. According to the invention, the moldings here may comprise beads of foamed particulate material in the form of individual beads or in molten form, for example in the form of welded or bonded beads of foamed particulate material. According to the invention, the beads of foamed particulate material may also be surrounded by a matrix, i.e. embedded in, for example, a foam or a dense polymer. In the context of the present invention, a foam as a foamed particulate material is understood to mean an embodiment in which the foam consists of or comprises a foamed particulate material. According to the invention, a foam as a foamed particulate material may also be a foamed particulate material surrounded by a matrix.
[0017] According to the invention, the foam preferably has a comfort factor of greater than 4, determined according to Reference Example 3, preferably a comfort factor in the range of 4 to 12, for example in the range of 5 to 11, or in the range of 5 to 10, in each case determined according to Reference Example 3.
[0018] The method of producing foamed particles from thermoplastic elastomers is known per se to those skilled in the art. When a foamed particle material consisting of a thermoplastic elastomer (TPE-1) is used according to the invention, the bulk density of the foamed particle material is, for example, in the range of 20 g / l to 250 g / l, preferably 50 g / l to 180 g / l, more preferably 60 g / l to 150 g / l.
[0019] For example, the diameter of the expanded particles is between 0.2 and 20 mm, preferably 1 to 15 mm, in particular 3 to 12 mm. In the case of non-spherical, for example elongated or cylindrical expanded particles, the diameter refers to the longest dimension.
[0020] In one embodiment, the present invention also relates to a molding as described above, wherein the foam is a foamed particulate material.
[0021] Suitable thermoplastic elastomers for producing the foam or molding of the present invention are known per se to those skilled in the art. For example, suitable thermoplastic elastomers are described in Handbook of Thermoplastic Elastomers, 2nd edition, June 2014. For example, thermoplastic elastomer (TPE-1) can be a thermoplastic polyurethane, a thermoplastic polyetheramide, a polyetherester, a polyesterester, a thermoplastic olefin-based elastomer, a crosslinked thermoplastic olefin-based elastomer, or a thermoplastic sulfide or a thermoplastic styrene-butadiene block copolymer. According to the present invention, thermoplastic elastomer (TPE-1) is preferably a thermoplastic polyurethane, a thermoplastic polyetheramide, a polyetherester, a polyesterester or a thermoplastic styrene-butadiene block copolymer.
[0022] In the context of the present invention, the thermoplastic elastomer (TPE-1) is further preferably a thermoplastic polyurethane, a thermoplastic polyetheramide or a polyester ester or a polyether ester.
[0023] In another embodiment, the present invention accordingly also relates to a molded article as described above, wherein the thermoplastic elastomer (TPE-1) is selected from thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters, thermoplastic olefin-based elastomers, crosslinked thermoplastic olefin-based elastomers, thermoplastic sulfides or thermoplastic styrene-butadiene block copolymers, in particular selected from thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters or thermoplastic styrene-butadiene block copolymers.
[0024] Suitable thermoplastic elastomers are especially those whose G modulus in the densified state is in the range of 0.8 to 8.5 MPa, as determined according to Reference Example 6. In another embodiment, the present invention accordingly also relates to the molded article described above, wherein the thermoplastic elastomer (TPE-1) has a G modulus in the densified state in the range of 0.8 to 8.5 MPa, as determined according to Reference Example 6.
[0025] Suitable processes for producing these thermoplastic elastomers or foams or foamed particles composed of these thermoplastic elastomers are also known per se to the person skilled in the art.
[0026] Suitable thermoplastic polyetheresters and polyesteresters can be produced by transesterification or esterification of aromatic and aliphatic dicarboxylic acids or their esters having 4 to 20 carbon atoms with suitable aliphatic and aromatic diols and polyols by any standard process known in the literature (see "Polymer Chemistry", Interscience Publishers, New York, 1961, pp. 111-127; Kunststoffhandbuch [Plastics Handbook], Vol. 8, C. Hanser Verlag, Munich 1973 and Journal of o f Polymer Science, Part A1, 4, pages 1851-1859 (1966).
[0027] Examples of suitable aromatic dicarboxylic acids include phthalic acid, isophthalic acid and terephthalic acid and their esters. Examples of suitable aliphatic dicarboxylic acids include cyclohexane-1,4-dicarboxylic acid, adipic acid, sebacic acid, azelaic acid and decanedicarboxylic acid as saturated dicarboxylic acids, and maleic acid, fumaric acid, aconitic acid, itaconic acid, tetrahydrophthalic acid and tetrahydroterephthalic acid as unsaturated dicarboxylic acids.
[0028] Examples of suitable diol components include those of the general formula HO-(CH2) n -OH diols, where n = 2 to 20, such as ethylene glycol, propane-1,3-diol, butane-1,4-diol or hexane-1,6-diol, polyether alcohols of the general formula HO-(CH2)nO-(CH2)m-OH, where n is equal to or not equal to m and n and m = 2 to 20, unsaturated diols and polyethers, such as butene-1,4-diol; diols and polyether alcohols containing aromatic units; and polyester alcohols.
[0029] Besides the carboxylic acids and their esters and the alcohols mentioned, it is also possible to use any other standard representatives of these classes of compounds to provide the polyetheresters and polyesteresters used according to the invention.
[0030] Thermoplastic polyetheramides can be obtained by reaction of amines and carboxylic acids or their esters according to any standard method known in the literature. Amines and / or carboxylic acids here also include ether units of the ROR type, where R=organic radicals (aliphatic and / or aromatic). Typically, monomers of the following classes of compounds are used: HOOC-R′-NH2, where R′ can be aromatic and aliphatic, preferably including ether units of the ROR type, where R=organic radicals (aliphatic and / or aromatic); aromatic dicarboxylic acids, including, for example, phthalic acid, isophthalic acid and terephthalic acid or their esters, and aromatic dicarboxylic acids, including ether units of the ROR type, where R=organic radicals (aliphatic and / or aromatic); aliphatic dicarboxylic acids, including, for example, cyclohexane-1,4-dicarboxylic acid, adipic acid, sebacic acid, azelaic acid and Decanedicarboxylic acid as a saturated dicarboxylic acid, and maleic acid, fumaric acid, aconitic acid, itaconic acid, tetrahydrophthalic acid and tetrahydroterephthalic acid as unsaturated and aliphatic dicarboxylic acids comprising ROR type ether units, wherein R=organic free radical (aliphatic and / or aromatic); diamines of the general formula H2N-R″-NH2, wherein R″ can be aromatic and aliphatic, preferably comprising ROR type ether units, wherein R=organic free radical (aliphatic and / or aromatic); lactams, such as ε-caprolactam, pyrrolidone or laurolactam; and amino acids.
[0031] Besides the carboxylic acids and their esters and the amines, lactams and amino acids, it is also possible to use any other standard representatives of these classes of compounds to provide the polyetheramines used according to the invention.
[0032] The thermoplastic elastomer having a block copolymer structure used according to the present invention preferably comprises vinyl aromatic units, butadiene units and isoprene units, as well as polyolefin units and vinyl units, such as ethylene, propylene and vinyl acetate units. Styrene-butadiene copolymers are preferred.
[0033] Thermoplastic elastomers, polyetheramides, polyetheresters and polyesteresters with block copolymer structure used according to the invention are preferably selected such that their melting point is ≤300° C., preferably ≤250° C., in particular ≤220° C.
[0034] Thermoplastic elastomers, polyetheramides, polyetheresters and polyesteresters having a block copolymer structure used according to the invention may be semicrystalline or amorphous.
[0035] Suitable thermoplastic olefin-based elastomers (TPO) have, in particular, hard segments, which are, for example, polyolefins such as polypropylene and polyethylene, and soft segments, which are rubber components such as ethylene-propylene rubber. Blends, dynamic crosslinking types, and polymerization types of polyolefins and rubber components are suitable.
[0036] Suitable structures are, for example, structures in which ethylene-propylene rubber (EPM) is dispersed in polypropylene; structures in which crosslinked or partially crosslinked ethylene-propylene-diene rubber (EPDM) is dispersed in polypropylene; random copolymers of ethylene and α-olefins (such as propylene and butene); or block copolymers of polyethylene blocks and ethylene / α-olefin copolymer blocks. Examples of suitable α-olefins are propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-n-decene, 3-methyl-1-butene and 4-methyl-1-pentene or mixtures of these olefins.
[0037] Suitable semicrystalline polyolefins are, for example, homopolymers of ethylene or propylene or copolymers comprising monomeric ethylene and / or propylene units. Examples are copolymers of ethylene and propylene or α-olefins having 4 to 12 carbon atoms and copolymers of propylene and α-olefins having 4 to 12 carbon atoms. Here, the concentration of ethylene or propylene in the copolymer is preferably high enough to render the copolymer semicrystalline.
[0038] In the case of a random copolymer, an ethylene content or a propylene content of, for example, about 70 mol% or more is suitable.
[0039] Suitable polypropylenes are propylene homopolymers or also polypropylene block copolymers, such as random copolymers of propylene and up to about 6 mol % of ethylene.
[0040] Suitable thermoplastic styrene block copolymers generally include polystyrene blocks and elastomer blocks. Suitable styrene blocks are, for example, selected from polystyrene, substituted polystyrene, poly(α-methylstyrene), ring halogenated styrene and ring alkylated styrene. Suitable elastomer blocks are, for example, polydiene blocks, such as polybutadiene and polyisoprene, poly(ethylene / butylene) copolymers and poly(ethylene / propylene) copolymers, polyisobutylene, or polypropylene sulfide or polydiethylsiloxane.
[0041] In the context of the present invention, the thermoplastic elastomer (TPE-1) is particularly advantageously a thermoplastic polyurethane.
[0042] Thermoplastic polyurethanes are known in the prior art. They are usually obtained by reacting a polyisocyanate composition with a polyol composition, wherein the polyol composition usually includes a polyol and a chain extender.
[0043] The thermoplastic elastomers used according to the invention may contain further additives, for example customary auxiliaries, such as surface-active substances, fillers, flame retardants, nucleating agents, oxidation stabilizers, lubricants and demoulding aids, dyes and pigments, optionally stabilizers, for example against hydrolysis, light, heat or discoloration, inorganic and / or organic fillers, reinforcing agents and plasticizers. Suitable auxiliaries and additives may be found in Kunststoffhandbuch [Plastics Handbook], Volume 7, by Vieweg and ed., Carl Hanser Verlag, Munich 1966 (pp. 103-113).
[0044] In the context of the present invention, it was found that the comfort factor, in addition to the storage modulus (G modulus) and the density of the foam, has a significant influence, in particular, on the seating comfort.
[0045] According to the present invention, it has been found to be advantageous that after the 4th cycle in the measurement according to Reference Example 5, the compression hardness of the foam at 10% compression is less than or equal to 22 kPa, more preferably less than 20 kPa or less than 15 kPa. In the context of the present invention, "after the 4th cycle" is understood to mean that the corresponding value may also have been reached in the previous measurement cycle, i.e. the measured value falls within the scope of the present invention no later than at the 4th measurement or after the 4th cycle.
[0046] Preferably, the foam has a compression hardness at 25% compression after the 4th cycle less than or equal to 65 kPa, as determined according to Reference Example 5.
[0047] In another embodiment, the present invention accordingly also relates to a molded article as described above, wherein the compression hardness of the foam at 10% compression after the 4th cycle is less than or equal to 22 kPa, determined according to Reference Example 5.
[0048] In another embodiment, the present invention accordingly also relates to a molded article as described above, wherein the compression hardness of the foam at 25% compression after the 4th cycle is less than or equal to 65 kPa, determined according to Reference Example 5.
[0049] In one embodiment, the present invention also relates to a molded article as described above, wherein the compression hardness of the foam at 65% compression is in the range of 300 to 700 kPa, determined according to Reference Example 5 after the 4th cycle.
[0050] In one embodiment, the present invention also relates to a molded article as described above, wherein the compression hardness of the foam at 10% compression is in the range of 1 to 20 kPa, determined according to Reference Example 5 after the 4th cycle.
[0051] According to the invention, it was found that the compression hardness of the molded article is influenced by a combination of the G modulus of the foam of the thermoplastic elastomer (TPE-1) employed and the density of the foam adjusted within the scope of the invention. According to the invention, the density of the foam can be influenced, for example, by appropriate conditions during the foam production process.
[0052] In the context of the present invention, it is also possible to use foamed particulate materials which have been melted by suitable means, wherein during melting the foam or the molding is adjusted to a suitable density.
[0053] According to the invention, the moulding may comprise beads of foamed particulate material in loose form. In this case, the moulding may, for example, comprise a suitable shell which substantially determines the shape of the moulding.
[0054] In one embodiment, the present invention also relates to a molded article as described above, wherein the molded article comprises a shell and beads of foamed particulate material.
[0055] Within the scope of the invention, the material and shape of the shell may vary within wide limits, provided that the shell is enclosed and suitable for forming a moulding of loose beads of expanded particulate material.
[0056] According to the invention, beads of foamed particulate material can for example be welded to form a foam of suitable density. It is also possible within the scope of the invention to treat the foamed particulate material before welding or bonding, for example heat-treating, irradiating or treating with a solvent.
[0057] In one embodiment, the present invention also relates to a molding as described above, wherein the foam consists of welded beads.
[0058] According to the invention, it is also possible for the foamed particulate material to be embedded in the matrix and for the foam to be a hybrid foam.
[0059] In one embodiment, the present invention also relates to a molding as described above, wherein the foam is a hybrid foam comprising a foamed particle material consisting of a thermoplastic elastomer (TPE-1).
[0060] In the context of the present invention, a material comprising a foamed particle material and a matrix material is referred to as a hybrid material. Here, the matrix material may be composed of a dense material or a foam.
[0061] Polymers (PM) suitable as matrix materials are known per se to the person skilled in the art. In the context of the present invention, suitable are, for example, ethylene-vinyl acetate copolymers, epoxy resin-type adhesives or other polyurethanes. According to the invention, polyurethane foams or other dense polyurethanes, for example elastic polyurethanes, are suitable here. According to the invention, the polymer used as matrix material may comprise further additives, for example customary auxiliaries, such as surfactants, fillers, flame retardants, nucleating agents, oxidation stabilizers, lubricants and demoulding aids, dyes and pigments, optionally stabilizers, for example stabilizers against hydrolysis, light, heat or discoloration, inorganic and / or organic fillers, reinforcing agents and plasticizers. Suitable auxiliaries and additives may be found in Kunststoffhandbuch [Plastics Handbook], Volume VII, by Vieweg and ed., Carl Hanser Verlag, Munich 1966 (pp. 103-113).
[0062] According to the invention, the polymer (PM) is selected to ensure sufficient bonding between the foamed particulate material and the matrix, so that a mechanically stable hybrid material is obtained, at least on the surface.
[0063] The matrix may completely or partially surround the foamed particle material. According to the invention, the mixed material may include other components, such as other fillers or particles. According to the invention, the mixed material may also include a mixture of different polymers (PM). The mixed material may also include a mixture of foamed particles.
[0064] Besides the foamed particle materials according to the invention, the foamed particles which can be used are known per se to the person skilled in the art. In the context of the present invention, foamed particles composed of thermoplastic elastomers, in particular thermoplastic polyurethanes, are particularly suitable.
[0065] In the context of the present invention, therefore, mixed materials comprising a matrix consisting of a polymer (PM), a foamed particle material consisting of a thermoplastic elastomer (TPE-1) and a further foamed particle material consisting of a thermoplastic polyurethane are also suitable.
[0066] In the context of the present invention, the matrix may consist of, for example, a polymer (PM). In the context of the present invention, examples of suitable matrix materials are elastomers or foams, in particular polyurethane-based foams, for example elastomers such as ethylene-vinyl acetate copolymers or other thermoplastic or elastomeric polyurethanes.
[0067] Suitable matrix materials are known per se to the person skilled in the art. For example, epoxy-based or polyurethane-based adhesive systems known per se can be used.
[0068] Suitable thermoplastic polyurethanes and elastomeric polyurethanes are known per se to the person skilled in the art. Suitable polyurethanes are described, for example, in "Kunststoffhandbuch" [Plastics Handbook], Volume 7 "Polyurethane" [Polyurethane], Carl Hanser Verlag, 3rd edition, 1993, Chapter 3.
[0069] In the context of the present invention, polymer (PM) is preferably polyurethane. In the present invention, term "polyurethane" includes all known polyisocyanate polyaddition products. These include particularly solid polyisocyanate polyaddition products, such as viscoelastic gel or thermoplastic polyurethane, and elastic foams based on polyisocyanate polyaddition products, such as flexible foam, semi-rigid foam or integral foam. For purposes of the present invention, "polyurethane" is also understood to include elastic polymer blends of polyurethane and other polymers, and the foams formed by these polymer blends. Matrix is preferably a hardened dense polyurethane adhesive, elastic polyurethane foam or gel.
[0070] In the context of the present invention, "polyurethane adhesive" is understood to mean a mixture consisting of at least 50% by weight, preferably at least 80% by weight, in particular at least 95% by weight, of prepolymers having isocyanate groups, hereinafter referred to as isocyanate prepolymers. The viscosity of the polyurethane adhesive of the invention is preferably in the range of 500 to 4000 mPa.s, more preferably 1000 to 3000 mPa.s, determined at 25° C. in accordance with DIN 53019-1: 2008-09.
[0071] Suitable polyurethane foams in the context of the present invention are known per se to the person skilled in the art.
[0072] The density of the matrix material is preferably between 2 and 0.001 g / cm 3 The matrix material is particularly preferably an elastic foam or integral foam with a density of 0.8 to 0.1 g / cm 3 In the range of 0.6 to 0.1 g / cm 3 , or dense materials such as hardened polyurethane adhesives.
[0073] Foam is particularly suitable as matrix material. A hybrid material comprising a matrix material consisting of polyurethane foam preferably has good adhesion between the matrix material and the foamed particle material.
[0074] A suitable mixed material according to the present invention, which comprises a polymer (PM) as a matrix and a foamed particulate material, can be prepared, for example, by mixing the components for producing the polymer (PM) and the foamed particulate material, optionally with other ingredients, and reacting them to obtain a mixed material, the reaction preferably being carried out under conditions where the foamed particulate material is substantially stable.
[0075] Suitable processes and reaction conditions for producing polymers (PM), in particular ethylene-vinyl acetate copolymers or polyurethanes, are known per se to the person skilled in the art.
[0076] In a preferred embodiment, a suitable hybrid material according to the invention is an integral foam, in particular an integral foam based on polyurethane. Suitable methods for producing integral foams are known per se to the person skilled in the art. The integral foam is preferably produced by a one-shot process in a closed, advantageously temperature-controlled mold using low-pressure or high-pressure technology. The mold is usually made of metal, for example aluminum or steel. For example, Piechota and These procedures are described in "Integralschaumstoff" [Integral Foam], Carl-Hanser-Verlag, Munich, Vienna, 1975, or in "Kunststoff-Handbuch" [Plastics Handbook], Volume 7, "Polyurethane" [Polyurethane], 3rd edition, 1993, Chapter 7.
[0077] Thus, a hybrid material having a matrix consisting of a polymer (PM) can be produced, in which the expanded particle material of the invention is present. The expanded particle material of the invention can be easily used in a process for producing a hybrid material, for example by compression molding.
[0078] In the mixed material suitable according to the invention, the volume proportion of the foamed particle material is preferably 20% by volume or more, more preferably 50% by volume or more, preferably 80% by volume or more, in particular 90% by volume or more, in each case based on the volume of the mixed system.
[0079] Hybrid materials suitable as foams in the context of the present invention are, in particular, hybrid materials with a matrix consisting of cellular polyurethane, which are characterized in that the matrix material has very good adhesion to the foamed particle material of the present invention. The hybrid materials of the present invention are therefore preferably free of tearing at the interface between the matrix material and the foamed particle material. This makes it possible to produce hybrid materials whose mechanical properties, such as tear propagation resistance and elasticity, are improved compared to conventional polymer materials, in particular conventional polyurethane materials, of the same density.
[0080] The rebound elasticity of the hybrid material according to the invention in the form of integral foam is preferably greater than 30%, more preferably greater than 50%, according to DIN 53512: 2000-04.
[0081] The properties of the hybrid material can vary within a wide range depending on the polymer (PM) used and can be adjusted within a wide range, in particular by varying the size, shape and properties of the expanded particulate material, or by adding other additives, for example also other non-foamed particulate materials such as plastic particles, for example rubber particles.
[0082] In another aspect, the present invention also relates to a method for producing a molded article, the method comprising the steps of:
[0083] (i) providing a foam composed of a thermoplastic elastomer (TPE-1), wherein the foam has a storage modulus (G modulus) at 25° C. and 1 Hz in the range of 0.01 to 0.5 MPa, determined according to Reference Example 1 (TPE molding), and a molding density in the range of 20 to 400 kg / m 3 within the range determined according to Reference Example 2, wherein the comfort factor of the foam is greater than 4, determined according to Reference Example 3;
[0084] (ii) processing the foam into a molded article.
[0085] With regard to the preferred embodiments, reference is made to the above statements.
[0086] In the context of the present invention, the method of the present invention comprises steps (i) and (ii). The foam composed of a thermoplastic elastomer (TPE-1) provided according to step (i) can be a block foam or a foamed granular material. According to the present invention, the foam can also be processed before being provided to step (i). In the context of the present invention, the foam can also be, for example, a welded or bonded foamed granular material, or a foamed granular material embedded in a matrix foam or a matrix polymer. Therefore, within the scope of the present invention, it is also possible, for example, to initially use a foam composed of a thermoplastic elastomer (TPE-1) whose density and / or G modulus and / or comfort factor are not within the scope of the present invention, and to adjust the density, G modulus and comfort factor by appropriate treatment.
[0087] In one embodiment, the present invention also relates to a process for producing the above-mentioned moldings, wherein the foam is a foamed particulate material.
[0088] The present invention also relates to a method for producing a molded article, comprising the following steps:
[0089] (i) providing a foam composed of a thermoplastic elastomer (TPE-1), wherein the foam has a storage modulus (G modulus) at 25° C. and 1 Hz in the range of 0.01 to 0.5 MPa, determined according to Reference Example 1 (TPE molding), and a molding density in the range of 20 to 400 kg / m 3 Within the range determined according to Reference Example 2, wherein the foam is a foamed particle material;
[0090] (ii) processing the foam into a molded article.
[0091] Suitable processes for producing moldings from foamed particulate materials are known per se to the person skilled in the art.
[0092] When the molded article comprises a shell and beads of foamed particulate material in loose form, according to step (ii), the shell can, for example, be filled to form the molded article. Suitable measures for filling the shell with foamed particulate material are known per se to the person skilled in the art. For example, the shell can be filled by pouring, layering, pushing, pressing, robot positioning, rotating or suctioning.
[0093] Within the scope of the present invention, steps (i) and (ii) of the method can also be carried out simultaneously, that is, for example, first a foamed particle material is provided according to step (i) and then processed according to step (ii) to give a molding by welding, bonding or foaming.
[0094] In one embodiment, the present invention also relates to the process described above, wherein the processing according to step (ii) is carried out by welding, foaming or bonding beads of foamed particulate material.
[0095] According to the present invention, a molded article is produced, for example, by first providing a mold and then pouring the expanded particle material into the mold. The amount of expanded particle material poured into the mold is determined according to the size of the mold and the desired molding density. Within the scope of the present invention, the method may also include other steps, such as temperature regulation. Within the scope of the present invention, the molded article may also include other components. Accordingly, other molded articles or expanded beads composed of different materials may be used in production.
[0096] The processing in step (ii) is preferably carried out in a closed mold, wherein melting can be achieved by steam, hot air (eg as described in EP1979401B1), variable temperature welding or high energy radiation (eg microwaves or radio waves).
[0097] The temperature at which the foamed particle material is melted is preferably below or close to the melting point of the polymer used to produce the foamed particle material.
[0098] Welding by high-energy radiation is generally carried out in the frequency range of microwaves or radio waves, optionally in the presence of water or other polar liquids such as microwave-absorbing hydrocarbons having polar groups (e.g., carboxylic acids and esters of diols or triols or ethylene glycol and liquid polyethylene glycols), and can be carried out in a manner similar to the methods described in EP3053732A or WO16146537.
[0099] For example, the molded article is produced by performing the welding at a temperature in the range of 100 to 170° C. The temperature at which the expanded beads are welded is preferably between 100° C. and 140° C.
[0100] For example, the welding can be achieved by welding the components to each other in a closed mold under the action of heat and optionally under pressure. To this end, the components, i.e. at least the foamed particulate material, are poured into a mold and, after closing the mold, steam or hot air is introduced, which causes the beads of the foamed particulate material to expand further and to weld together to form a foam. According to the invention, the mold can also be heated from the outside with a heating medium such as water or oil to weld the beads, depending on the thickness of the components.
[0101] The method according to the invention may comprise further steps, such as temperature regulation.
[0102] Here, further embodiments according to standard methods are possible; the methods for producing the starting materials can be integrated directly into the production.
[0103] The invention also relates to a molding obtained or obtainable by the process described above.
[0104] The moldings of the invention are particularly suitable as cushioning parts. The moldings of the invention are also suitable as shoe soles, parts of shoe soles, bicycle saddles, cushions, mattresses, padding, backrests, arm pads, pads, underlays, handles, protective films, protectors, damping elements or as components in the field of automotive interior and exterior trim.
[0105] In another embodiment, the present invention accordingly also relates to the molding described above, wherein the molding is a sole, a part of a sole, a bicycle saddle, a cushion, a mattress, a padding, a backrest, an arm pad, a pad, a substrate, a handle, a protective film, a protector, a damping element or a component in the field of automotive interior and exterior.
[0106] In a further aspect, the invention also relates to the use of the moldings according to the invention for producing floor coverings, mattresses, seating furniture, bicycle saddles, car seats, motorcycle seats, parts of shoes, as insoles, packaging or shock absorbers.
[0107] Further embodiments of the invention can be found in the claims and the examples. It is understood that the features of the subject matter / method / use of the invention described above and the features described below can be used not only in the combination specified in each case but also in other combinations without departing from the scope of the invention. Thus, combinations of preferred features with particularly preferred features, or combinations of features not further characterized with particularly preferred features, etc., are also implicitly included, even if such combinations are not explicitly mentioned.
[0108] The illustrative embodiments of the present invention are described in detail below, but the present invention is not limited thereto. In particular, the present invention also includes those embodiments resulting from the related references and the combinations described below.
[0109] 1. A molded article comprising a foam composed of a thermoplastic elastomer (TPE-1), wherein the foam has a storage modulus (G modulus) at 25°C and 1 Hz in the range of 0.01 to 0.5 MPa, determined according to Reference Example 1 (TPE molding), and a molding density in the range of 20 to 400 kg / m 3 within the range determined according to Reference Example 2, wherein the comfort factor of the foam is greater than 4, determined according to Reference Example 3.
[0110] 2. The molded article according to embodiment 1, wherein the foam has a compression hardness at 10% compression of less than or equal to 22 kPa, determined according to Reference Example 5 after the 4th cycle.
[0111] 3. The molded article according to embodiment 1 or 2, wherein the foam has a compression hardness at 25% compression of less than or equal to 65 kPa, determined according to Reference Example 5 after the 4th cycle.
[0112] 4. The molded article according to any one of embodiments 1 to 3, wherein the foam is a foamed particulate material.
[0113] 5. The molded article according to any one of embodiments 1 to 4, wherein the thermoplastic elastomer (TPE-1) is selected from thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters, thermoplastic olefin-based elastomers, crosslinked thermoplastic olefin-based elastomers, thermoplastic sulfides or thermoplastic styrene-butadiene block copolymers.
[0114] 6. The molded article according to any of embodiments 1 to 5, wherein the thermoplastic elastomer (TPE-1) is selected from thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters or thermoplastic styrene-butadiene block copolymers.
[0115] 7. The molded article according to any one of embodiments 1 to 6, wherein the thermoplastic elastomer (TPE-1) has a G modulus in the densified state in the range of 0.8 to 8.5 MPa, determined according to Reference Example 6.
[0116] 8. The molding according to any one of embodiments 1 to 7, wherein the molding comprises a shell and beads of foamed particulate material.
[0117] 9. The molding according to any one of embodiments 1 to 7, wherein the foam consists of fused beads of foamed particulate material.
[0118] 10. The molding according to any one of embodiments 1 to 7, wherein the foam is a hybrid foam comprising a foamed particle material composed of a thermoplastic elastomer (TPE-1).
[0119] 11. A method for producing a molded article, comprising the steps of:
[0120] (i) providing a foam composed of a thermoplastic elastomer (TPE-1), wherein the foam has a storage modulus (G modulus) at 25° C. and 1 Hz in the range of 0.01 to 0.5 MPa, determined according to Reference Example 1 (TPE molding), and a molding density in the range of 20 to 400 kg / m 3 within the range determined according to Reference Example 2, wherein the comfort factor of the foam is greater than 4, determined according to Reference Example 3;
[0121] (ii) processing the foam into a molded article.
[0122] 12. The method of embodiment 11, wherein the foam is a foamed particulate material.
[0123] 13. A method according to embodiment 12, wherein the processing according to step (ii) is carried out by welding, foaming or bonding beads of foamed particulate material.
[0124] 14. The method according to any one of embodiments 11 to 13, wherein the compression hardness of the foam at 10% compression is less than or equal to 22 kPa, determined according to Reference Example 5 after the 4th measurement cycle.
[0125] 15. The method according to any one of embodiments 11 to 14, wherein the compression hardness of the foam at 25% compression is less than or equal to 65 kPa, determined according to Reference Example 5 after the 4th cycle.
[0126] 16. The method according to any one of embodiments 11 to 15, wherein the thermoplastic elastomer (TPE-1) is selected from thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters, thermoplastic olefin-based elastomers, crosslinked thermoplastic olefin-based elastomers, thermoplastic sulfides or thermoplastic styrene-butadiene block copolymers.
[0127] 17. The process according to any one of embodiments 11 to 16, wherein the thermoplastic elastomer (TPE-1) is selected from thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters or thermoplastic styrene-butadiene block copolymers.
[0128] 18. The process according to any one of embodiments 11 to 17, wherein the thermoplastic elastomer (TPE-1) has a G modulus in the densified state in the range of 0.8 to 8.5 MPa, determined according to Reference Example 6.
[0129] 19. A moulding obtained or obtainable by the process according to any one of embodiments 11 to 18.
[0130] 20. The molded article according to embodiment 17, wherein the molded article is a shoe sole, a part of a shoe sole, a bicycle saddle, a cushion, a mattress, a padding, a backrest, an arm pad, a pad, a substrate, a handle, a protective film, a protector, a damping element, an anti-fall pad, an elastic insulating material, a sealing material or a component in the field of automotive interior and exterior.
[0131] 21. Use of the molding according to any of embodiments 1 to 10 or 19 or 20 for producing floor coverings, mattresses, seating furniture, bicycle saddles, car seats, motorcycle seats, parts of shoes, as insoles, packaging, shock absorbers, protectors, fall protection mats, elastic insulating materials or sealing materials.
[0132] 22. A molded article comprising a foam composed of a thermoplastic elastomer (TPE-1), wherein the foam has a storage modulus (G modulus) at 25°C and 1 Hz in the range of 0.01 to 0.5 MPa, determined according to Reference Example 1 (TPE molding), and a molding density in the range of 20 to 400 kg / m 3 The range is determined according to Reference Example 2, wherein the foam is a foamed particle material.
[0133] 23. The molded article according to embodiment 22, wherein the thermoplastic elastomer (TPE-1) is selected from thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters, thermoplastic olefin-based elastomers, crosslinked thermoplastic olefin-based elastomers, thermoplastic sulfides or thermoplastic styrene-butadiene block copolymers.
[0134] 24. The molded article according to embodiment 22 or 23, wherein the thermoplastic elastomer (TPE-1) is selected from thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters or thermoplastic styrene-butadiene block copolymers.
[0135] 25. The molded article according to any one of embodiments 22 to 24, wherein the thermoplastic elastomer (TPE-1) has a G modulus in the densified state in the range of 0.8 to 8.5 MPa, determined according to Reference Example 6.
[0136] 26. The molded article according to any one of embodiments 22 to 25, wherein the molded article comprises a shell and beads of foamed particulate material.
[0137] 27. The molding according to any one of embodiments 22 to 25, wherein the foam consists of fused beads of foamed particulate material.
[0138] 28. The molded article according to any of embodiments 22 to 25, wherein the foam is a hybrid foam comprising a foamed particle material consisting of a thermoplastic elastomer (TPE-1).
[0139] 29. A method for producing a molded article, the method comprising the steps of:
[0140] (i) providing a foam composed of a thermoplastic elastomer (TPE-1), wherein the foam has a storage modulus (G modulus) at 25° C. and 1 Hz in the range of 0.01 to 0.5 MPa, determined according to Reference Example 1 (TPE molding), and a molding density in the range of 20 to 400 kg / m 3 Within the range determined according to Reference Example 2, wherein the foam is a foamed particle material;
[0141] (ii) processing the foam into a molded article.
[0142] 30. A method according to embodiment 29, wherein the processing according to step (ii) is carried out by welding, foaming or bonding beads of foamed particulate material.
[0143] 31. The method according to embodiments 29 to 31, wherein the thermoplastic elastomer (TPE-1) is selected from thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters, thermoplastic olefin-based elastomers, cross-linked thermoplastic olefin-based elastomers, thermoplastic sulfides or thermoplastic styrene-butadiene block copolymers.
[0144] 32. The method according to any one of embodiments 29 to 31, wherein the thermoplastic elastomer (TPE-1) is selected from thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters or thermoplastic styrene-butadiene block copolymers.
[0145] 33. The process according to any one of embodiments 29 to 32, wherein the thermoplastic elastomer (TPE-1) has a G modulus in the densified state in the range of 0.8 to 8.5 MPa, determined according to Reference Example 6.
[0146] 34. A moulding obtained or obtainable by the process according to any one of embodiments 29 to 33.
[0147] 35. The molded article according to embodiment 34, wherein the molded article is a shoe sole, a part of a shoe sole, a bicycle saddle, a cushion, a mattress, a padding, a backrest, an arm pad, a pad, a substrate, a handle, a protective film, a protector, a damping element, an anti-fall pad, an elastic insulating material, a sealing material or a component in the field of automotive interior and exterior decoration.
[0148] 36. Use of the molding according to any of embodiments 22 to 28 or 34 or 35 for producing floor coverings, mattresses, seating furniture, bicycle saddles, car seats, motorcycle seats, parts of shoes, as insoles, packaging, shock absorbers, protectors, fall protection mats, elastic insulating materials or sealing materials.
[0149] BRIEF DESCRIPTION OF THE DRAWINGS
[0150] Figure 1 A diagram comparing stress-strain curves of an example according to the invention with stress-strain curves of a comparative example is shown. Here, force (y-axis) is plotted against distance (%, x-axis).
[0151] The following examples serve to illustrate the invention but do not in any way limit the subject matter of the invention. Example
[0152] I. Production Example
[0153] 1. Preparation of Example Materials and Comparative Materials
[0154] The production of the example materials TPU 1 to 4 described below was carried out in a ZSK58 MC twin-screw extruder from Coperion with a processing length of 48D (12 barrels).
[0155] The melt is discharged from the extruder via a gear pump. After melt filtration, the polymer melt is processed into granules by an underwater granulation system, which are continuously dried in a heated fluidized bed at a temperature of 40-90°C.
[0156] Polyols, chain extenders and diisocyanates and optionally catalysts are metered into zone 1. The supply of further additives takes place in zone 8.
[0157] The barrel temperature is in the range of 150 to 230°C. The melt is discharged into the underwater pelletizing system at a melt temperature of 180 to 210°C. The screw speed is between 180 and 240 min -1 The throughput is in the range of 180 to 220 kg / h.
[0158] Table 1 summarizes the amounts of raw materials used to produce the example materials.
[0159] Table 1: Composition of the materials used
[0160]
[0161] This blending and synthesis produced thermoplastic polyurethanes having the properties listed in Table 2. The storage modulus (G modulus) was determined according to Reference Example 1 (compacted granular material). The melt flow rate (MFR) of the granules was measured according to DIN EN ISO 1133-2:2012. The conditions used are listed in Table 2.
[0162] Table 2: Properties of the produced densified example materials
[0163]
[0164] 2. General production method according to the examples and comparative examples of the extrusion method
[0165] After the raw materials have been produced, they are further processed into expanded thermoplastic polyurethane particles as follows. For this purpose, the dried thermoplastic polyurethane is mixed in a twin-screw extruder (ZSK 40, Coperion) with a further additive of 0.2% talc (particle size 5.6 μm-D50, volume distribution) as a nucleating agent, optionally TPU mixed with 4,4′-diphenylmethane diisocyanate having an average functionality of 2.05 in a separate extrusion process (additive 1), and optionally triacetin as a plasticizer (additive 2) and optionally with polystyrene (melt flow rate, 200° C. / 5 kg: 3 g / 10 min) (additive 3) and melted in a temperature range of 130 to 220° C. As blowing agents, CO2 and N2 are injected into the melt in the extruder and blended with the thermoplastic polyurethane and other additives to form a homogeneous melt. The compositions of the various examples and comparative examples are listed in Table 3. The material is then pressed into a die plate (130 to 200° C., depending on the material composition) using a gear pump (about 130 to 200° C., depending on the material composition), cut into pellets in the cutting chamber of an underwater pelletizing system (UWP), and transported away with temperature-controlled and pressurized water, expanding in the process. After separating the expanded pellets from the water by a centrifugal dryer, the expanded pellets are dried at 50 to 60° C. for 2 hours. The water temperature and water pressure, the amount of CO2 and N2 used in the examples and comparative examples, as well as the bead mass and the resulting bulk density according to Reference Example 4 are listed in Table 3.
[0166] The expanded particle material is produced by the autoclave method (a standard process known in the art) by the following process:
[0167] (i) providing the TPU composition of the present invention;
[0168] (ii) impregnating the composition with a blowing agent under pressure;
[0169] (iii) expanding the composition by a pressure drop.
[0170] The amount of blowing agent is preferably 0.1 to 40 parts by weight, in particular 0.5 to 35 parts by weight, particularly preferably 1 to 30 parts by weight, based on 100 parts by weight of composition (Z) used.
[0171] The impregnation in step (ii) can be carried out in the presence of water and optionally a suspension aid, or only in the presence of a blowing agent and without water.
[0172] The properties of the suspension process are known to the person skilled in the art and have been extensively described, for example in WO 2007 / 082838.
[0173] 3. General production method of Examples and Comparative Examples according to the autoclave method (tank method)
[0174] 100.0 parts by weight (corresponding to 27.5% by weight, based on the total suspension without blowing agent) of granular material, 257 parts by weight (corresponding to 70.6% by weight, based on the total suspension without blowing agent) of water, 6.7 parts by weight (corresponding to 1.8% by weight, based on the total suspension without blowing agent) of calcium carbonate (suspending agent), 0.13 parts by weight (corresponding to 0.04% by weight, based on the total suspension without blowing agent) of a surface-active substance (Lutensol AT 25, suspension aid) and an appropriate amount of butane as blowing agent (based on the amount of granular material used) are heated while stirring.
[0175] Nitrogen is then additionally injected into the liquid phase at 50°C and the internal pressure is adjusted to a predetermined pressure (800 kPa). Subsequently, when the impregnation temperature (IMT) is reached and optionally after a holding time (HZ) is observed, and at the finally established impregnation pressure (IMP), expansion is carried out by means of an expansion device. The gas space is here adjusted to a fixed discharge pressure (AP) and remains constant during the expansion process. The expansion jet downstream of the expansion device can optionally be cooled with a defined volume flow of water at a defined temperature (water quenching).
[0176] The holding time refers to the time during which the liquid phase temperature is within the temperature range of 5°C lower than the immersion temperature to 2°C higher than the immersion temperature.
[0177] The bulk density (SD) of the obtained foam beads was measured according to Reference Example 4 after removal of the suspending agent / suspension aid system (dispersant / surfactant) and drying.
[0178] The specific production parameters and bulk density of the resulting batches are listed in Table 4.
[0179] Table 3a and 3b: Data of Examples and Comparative Examples (Extrusion Method)
[0180]
[0181]
[0182]
[0183] Table 4: Data of Examples and Comparative Examples (Autoclave Method)
[0184]
[0185] The expanded granules produced by the extrusion and pot process were then welded into square slabs with a side length of 200 mm and a thickness of 20 mm by contact with steam in a molding machine (Energy Foamer K68) from Kurtzersa GmbH. The welding parameters of the examples and comparative examples were selected so that the surface of the final molding exhibited as few collapsed eTPU beads as possible. In each experiment, a cooling time of 120 seconds was always set at the end for the fixed side and the moving side of the mold. The respective steaming conditions are listed in Table 5 in the form of steam pressure and the respective steaming time. The blocks obtained were heated at 70° C. for 4 hours.
[0186] Table 5a and 5b: Steam overpressure and time for welding example and comparative example materials
[0187]
[0188]
[0189] The G modulus of the welded molded article was determined according to Reference Example 1 (TPE molding).
[0190] The G modulus of the individual loose foam beads (Examples 1 to 8) was determined according to Reference Example 1 (foamed particulate material) and is summarized in Table 6.
[0191] Table 6: G modulus (storage modulus) measured at 25°C and 1 Hz
[0192]
[0193] The comfort of seating furniture and mattresses is usually evaluated by the SAG factor (determined according to DIN EN ISO 2439: 2009-05). The SAG factor is calculated from the ratio of the indentation hardness at a depth of 65% to the indentation hardness at a depth of 25% using a punch with a smaller area than the test specimen. As a modification of the standard, the examples and comparative examples were evaluated using the method for determining the compression hardness to determine the comfort factor according to Reference Example 3.
[0194] The density of the molded article was determined according to Reference Example 2.
[0195] The compression hardness was measured according to Reference Example 5.
[0196] Tables 7 and 8 summarize the results of the compression hardness tests for the examples and comparative examples. Table 7 shows the compression hardness for the 1st cycle, Table 8 shows the values for different cycles. The specification of the cycles is important, because the first compression leads to changes in the eTPU. Therefore, the compression hardness measured in the next cycle is significantly lower. From no later than the 4th cycle onwards, this change is less pronounced, which can be illustrated, for example, by an example in Table 8. The 4 cycles were measured on a part produced from the eTPU of Comparative Example 1.
[0197] Table 7: Results of compression hardness test (1st cycle) of welded blocks of Examples and Comparative Examples
[0198]
[0199] Table 8: Results of compression hardness test (different cycles) of the welded blocks of the examples and comparative examples
[0200]
[0201] According to Reference Example 6 (production of injection-molded pieces) and Reference Example 1 (determination of the G modulus (compact material)), the G modulus of a recompacted TPU consisting of an expanded TPU was determined.
[0202] 4. Examples of producing hybrid materials from block foam (adhesive) and eTPU (Examples 17 to 22)
[0203] The beads produced above are used to produce molded articles using a PU foam system as an adhesive. To this end, the liquid formulation components are first formulated according to the formulation of component A (Table 10) and then mixed with component B (Table 11) in a mixing ratio of 100:104 using a laboratory stirrer (EWTHV-05 type from Vollrath GmbH) for 10 seconds. The reacted PU system is then immediately weighed onto the beads in a ratio of 20% by weight of the PU system: 80% by weight of the beads and mixed thoroughly for 30 seconds in a plastic container made of polyethylene with the aid of a laboratory stirrer and then discharged into the mold. The mold used is an open wooden frame treated with a release agent with an internal dimension of 20x20x1.4 cm. After smoothing the surface with a Teflon film, the system is left to harden in the mold for at least 30 minutes. Before the test blocks are tested, they are stored at room temperature for at least 2 days to ensure that the PU system has reacted completely. Table 12 lists the compression hardness of the test blocks obtained. The method for determining the compression hardness and density is the same as for the eTPU blocks.
[0204] 5. Comparative Examples of Producing Hybrid Materials from Slabstock Foam (Binder) and eTPU (Comparative Examples 8 to 10)
[0205] 5.1 Comparative Example 8
[0206] The moldings from Example 7 were produced using the PU foam system. For this purpose, the liquid formulation components were first compounded according to the formulation (Table 10) and then mixed with component B (Table 11) in a mixing ratio of 100:104 using a laboratory stirrer (model EWTHV-05 from Vollrath GmbH) for 10 seconds. The residual NCO content of component B was 18%. The residual NCO content was determined by potentiometric titration using chloroaniline solution.
[0207] The reacted PU system was then immediately weighed onto the beads in a ratio of 61.5 wt. % PU system: 38.5 wt. % beads and mixed thoroughly for 30 seconds in a plastic container made of polyethylene with the aid of a laboratory stirrer and then poured into the mold. The mold used was a wooden mold coated with a Teflon film with internal dimensions of 20x20x2 cm. After filling, the mold was tightly closed with a lid. To ensure that the PU foam system was fully hardened, the molding was left in the mold for 120 minutes. Before the test blocks were tested, they were stored at room temperature for at least 2 days to ensure that the PU system had reacted completely.
[0208] 5.2 Comparative Example 9
[0209] A molding was produced from Example 6 in a manner analogous to Comparative Example 9 using a PU system.
[0210] 5.3 Comparative Example 10
[0211] A molding was produced from Comparative Example 1 in a manner similar to Comparative Example 9 using a PU system.
[0212] Table 9: Composition of Component A
[0213]
[0214]
[0215] Table 10: Composition of component B with 18% residual NCO
[0216]
[0217] Table 11: Results of the compression hardness test (1st cycle) of the mixed materials consisting of adhesive and eTPU in Examples and Comparative Examples (block thickness 20 mm).
[0218]
[0219]
[0220] Table 11: Results of compression hardness test (4th cycle) of mixed materials composed of adhesive and eTPU in Examples and Comparative Examples (block thickness 20 mm)
[0221]
[0222] II. Measurement method
[0223] 1. Reference Example 1: Determination of G modulus (storage modulus)
[0224] 1.1 Dense materials
[0225] The G modulus of the dense thermoplastic elastomer is determined in accordance with DIN EN ISO 6721-1-7: 2018-03 by dynamic mechanical analysis (DMA) on test specimens, more specifically injection-molded pieces, which have been previously heated at 100° C. for 20 h, but are measured in a similar manner from −80 to 120° C. with a step heating program of 5° C. at a continuous heating rate of 2° C. / min, under torsion, at 1 Hz, and from this the storage modulus (G modulus) at 25° C.
[0226] 1.2 Foamed particle material
[0227] To determine the G modulus of individual loose foam beads, these are first poured into a cylinder and compacted by repeated compression to achieve the highest possible packing density. Subsequently, the compression modulus is determined under quasi-static compression, from which the storage modulus (G modulus) is calculated.
[0228] 1.3 eTPE Molding Products
[0229] The G modulus of the welded examples and welded comparative examples was determined according to DIN EN ISO 6721-1-7: 2018-03 by dynamic mechanical analysis (DMA) on eTPE moldings which had been previously heated at 70°C for 4 hours, but were measured in a similar manner at a continuous heating rate of 2°C / min, under torsion, at 1 Hz with a step heating program of 5°C from -80 to 120°C, and the G modulus at 25°C was determined from this. In order to produce test specimens with a size of 50x12x5 mm for this purpose, an eTPU block (200x200x10 or 20 mm) was first cut in half longitudinally. The skin was then removed at the top and bottom with a slitter to obtain a sheet with a thickness of 5 mm. Care was taken to ensure that the sheet was cut out from the middle of the block. The test specimen was then punched out from this sheet.
[0230] 2. Reference Example 2: Determination of molding density
[0231] Prior to the actual test, the length and width of the specimen are determined with callipers (accuracy: ±0.01 mm, measured in each case at a point in the center of the component), and the weight of the specimen is determined with a precision balance (accuracy: ±0.001 g). The thickness of the specimen is determined by a compression hardness tester using a "crosshead" displacement measuring system (accuracy: ±0.25 mm). The measured values can then be used to calculate the volume and density.
[0232] 3. Reference Example 3: Determination of Comfort Factor
[0233] By analogy with the SAG factor, the comfort factor is considered to be the ratio of the compression hardness (StH) at 65% compression to the compression hardness at 25% compression. Comparative measurements on eTPU blocks and flexible foam blocks have shown that both measurement methods (SAG value determination and compression hardness test) show the same trend when comparing different materials. For eTPU, the absolute values of the determined ratios may differ from each other, because, unlike the compression hardness determination, the measurement in the SAG factor determination is influenced by the presence of a skin on the test specimen or the condition of the skin. However, since the influence of the skin on the performance can also vary greatly depending on the purpose of the component, the compression hardness can also be used to compare different materials.
[0234] 4. Reference Example 4: Determination of bulk density
[0235] The bulk density of the bead foam is determined gravimetrically from the volume and mass of the particle bed in a container (10 L). This is done by filling a funnel with about 11 to 12 L of beads, which is closed at the lower outlet. During filling, the 10 L container is centrally located below the funnel. The lid of the funnel is then opened and the beads are allowed to flow evenly into the container of defined volume (10 L). The surface of the container is leveled with a flat edge at an angle of 45°. The mass is then determined gravimetrically using a balance. This must be deducted from the empty weight of the container beforehand, or the empty weight must be subtracted afterwards to obtain the weight of the bed. The weight divided by the volume then corresponds to the bulk density of the bead foam. Both when filling the sample container with beads and when transporting it to the balance, care must be taken to ensure that the container is not subjected to any vibrations or shocks.
[0236] 5. Reference Example 5: Determination of compression hardness
[0237] The test specimens for the measurements (50 mm × 50 mm × original thickness of the test block (usually 20 mm, thickness may vary slightly due to shrinkage, the outer skin is not removed)) are cut from the test block (200 × 200 × 20 mm, dimensions may vary slightly due to shrinkage) using a band saw. The block is previously conditioned for 16 hours under standard climatic conditions (23 ± 2 ° C and 50 ± 5% humidity). The compression hardness test is also carried out under these climatic conditions.
[0238] Prior to the actual test, the length and width of the test specimens were determined with callipers (accuracy: ±0.01 mm, measurement in each case at a point in the center of the component), and the weight of the test specimens was determined with a precision balance (accuracy: ±0.001 g).
[0239] The test was carried out using a 50 kN force sensor (class 1 according to DIN EN ISO 7500-1:2018-06), a crosshead displacement sensor (class 1 according to DIN EN ISO 9513:2013) and two parallel unperforated pressure plates (200 mm diameter, maximum permissible force 250 kN, maximum permissible surface pressure 300 N / mm 2 ) testing machine to determine the compression hardness. In order to determine the density of the specimen, the length, width and weight are loaded into the Zwick test method. The thickness of the specimen is determined by a universal testing machine using a "crosshead" displacement measuring system (accuracy: ± 0.25 mm). The measurement itself is carried out at a test speed of 50 mm / min and an initial force of 1 N. The stress values for 10, 25, 50, 65 and 75% compression are recorded respectively. The evaluation is based on the values of the 1st and 4th compressions. The compression hardness is calculated according to formula (4). The compression hardness σ here is the compressive stress (kPa) determined for a certain deformation (e.g. 50%) during loading.
[0240] σ=(F x / A0)x1000 (4)
[0241] F x = Force at x% deformation [N]
[0242] A0 = initial cross section of the specimen [mm 2 ]
[0243] 6. Reference Example 6: Determination of G modulus of compacted foam
[0244] The test specimens for determining the G modulus of the eTPU material were produced by injection molding. To this end, the eTPU material was removed from the component and then ground in a grinder (8 mm screen on a Dreher S26 / 26 GFX-Spez-L). The resulting eTPU chips were then dried at 110°C for 3 hours and processed into 2 mm thick test specimens in an injection molding machine at a maximum barrel temperature of 210 to 215°C, a die temperature of 210 to 220°C, and a mold temperature of 35°C (cycle time 75 seconds). The test specimens thus obtained were immediately heated at 100°C for 20 hours, and the storage modulus (G modulus) was then determined according to Reference Example 1 (compact material).
[0245] Citations
[0246] Ullmann's der technischen Chemie″ [Encyclopedia of Industrial Chemistry], 4th edition, volume 20, pages 416 et seq.
[0247] WO 94 / 20568
[0248] WO 2007 / 082838 A1
[0249] WO2017 / 030835
[0250] WO 2013 / 153190 A1
[0251] WO2010 / 010010
[0252] "Handbook of Thermoplastic Elastomers", 2nd edition, June 2014
[0253] "Polymer Chemistry", Interscience Publishers, New York, 1961, pp. 111-127
[0254] "Kunststoffhandbuch" [Plastics Handbook], Volume 8, C. Hanser Verlag, Munich 1973
[0255] Journal of Polymer Science, Part A1, 4, pp. 1851-1859 (1966)
[0256] "Kunststoffhandbuch" [Plastics Handbook], Volume VII, Carl Hanser Verlag, Munich 1966 (pp. 103-113)
[0257] "Kunststoffhandbuch" [Plastics Handbook], Volume VII, "Polyurethane" [Polyurethane], Karl-Hansel Verlag, 3rd edition, 1993, Chapter 3
[0258] "Integralschaumstoff" [Integral foam], Carl-Hanser-Verlag, Munich, Vienna, 1975
[0259] "Kunststoff-Handbuch" [Plastics Handbook], Volume 7, "Polyurethane" [Polyurethane], 3rd edition 1993, Chapter 7
[0260] EP 1979401 B1
[0261] EP 3053732 A1
[0262] WO 2016 / 146537 A1
Claims
1. A molded article comprising a foam composed of a thermoplastic elastomer, wherein the foam has a storage modulus (G modulus) at 25° C. and 1 Hz in the range of 0.01 to 0.5 MPa, excluding 0.5 MPa, determined according to Reference Example 1, and a molding density in the range of 20 to 400 kg / m 3 within the range determined according to Reference Example 2, wherein the foam is a foamed particulate material, wherein the thermoplastic elastomer is selected from thermoplastic polyurethane, thermoplastic polyetheramide, polyetherester, polyesterester, thermoplastic olefin-based elastomer, cross-linked thermoplastic olefin-based elastomer, thermoplastic sulfide or thermoplastic styrene-butadiene block copolymer and, The G modulus of the thermoplastic elastomer in a densified state is in the range of 0.8 to 8.5 MPa, determined according to Reference Example 6.
2. The molded article according to claim 1, wherein the comfort factor of the foam is greater than 4, determined according to Reference Example 3.
3. The molded article of claim 1, wherein the molded article comprises a shell and beads of foamed particulate material.
4. The molded article of claim 1 wherein the foam consists of fused beads of foamed particulate material.
5. The molded article according to claim 1, wherein the foam is a hybrid foam comprising a foamed particle material composed of a thermoplastic elastomer.
6. A method for producing a molded article, comprising the steps of: (i) providing a foam composed of a thermoplastic elastomer, wherein the foam has a storage modulus (G modulus) at 25° C. and 1 Hz in the range of 0.01 to 0.5 MPa, excluding 0.5 MPa, determined according to Reference Example 1, and a molded density in the range of 20 to 400 kg / m 3 within the range determined according to Reference Example 2, wherein the foam is a foamed particle material, wherein the thermoplastic elastomer is selected from thermoplastic polyurethane, thermoplastic polyetheramide, polyetherester, polyesterester, thermoplastic olefin-based elastomer, cross-linked thermoplastic olefin-based elastomer, thermoplastic sulfide or thermoplastic styrene-butadiene block copolymer and, wherein the G modulus of the thermoplastic elastomer in a dense state is in the range of 0.8 to 8.5 MPa, determined according to Reference Example 6; (ii) processing the foam into a molded article.
7. A method according to claim 6, wherein the processing according to step (ii) is carried out by welding, foaming or bonding beads of foamed particulate material.
8. A moulding obtained or obtainable by the process according to claim 6 or 7.
9. The molded article according to claim 8, wherein the molded article is a shoe sole, a part of a shoe sole, a bicycle saddle, a cushion, a mattress, a padding, a backrest, an arm pad, a pad, a substrate, a handle, a protective film, a protector, a damping element, an anti-fall pad, an elastic insulating material, a sealing material or a component in the field of automotive interior and exterior.
10. Use of the molding according to any one of claims 1 to 5 or 9 for producing floor coverings, mattresses, seating furniture, bicycle saddles, car seats, motorcycle seats, shoe parts, as insoles, packaging, shock absorbers, protectors, fall arrest mats, elastic insulating materials or sealing materials.
Citation Information
Patent Citations
Foams based on thermoplastic polyurethanes
EP1979401A1
Thermoplastic polyurethane-based foamed materials
WO1994020568A1
Foams based on thermoplastic polyurethanes
WO2007082838A1
Thermoplastic polymer blends based on thermoplastic polyurethane and styrene polymer, foams produced therefrom and associated manufacturing methods
WO2010010010A1
Method for producing expanded granules
WO2013153190A1