PW 12 @PDADMAC / WMCNT modified polypropylene separator and its application in lithium-sulfur batteries

By using PW12@PDADMAC/WMCNT/PP composite separator in lithium-sulfur batteries, the problems of poor cycleability and low Coulombic efficiency caused by the polysulfide shuttle effect are solved, and higher discharge specific capacity and longer cycle life are achieved.

CN114824648BActive Publication Date: 2024-10-18YANGZHOU UNIV
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
CN202210269822.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-18
Publication Date
2024-10-18
Estimated Expiration
2042-03-18

AI Technical Summary

Technical Problem

The poor cycleability, low Coulombic efficiency, high self-discharge rate and irreversible loss of active materials in lithium-sulfur batteries are mainly caused by the shuttle effect of polysulfides. The existing technology still has shortcomings in improving energy density and cycle life.

Method used

Using PW12@PDADMAC/WMCNT/PP composite separator, PW12@PDADMAC precipitated particles and carbon nanotubes (WMCNT) are evenly coated on the polypropylene separator, and PDADMAC is used to fix PW12 to prevent it from being reduced to heteropoly blue, and pass through WMCNT Improves the electrical conductivity of the separator and physically blocks the shuttle of polysulfides.

Benefits of technology

Significantly improve the specific discharge capacity and cycle stability of lithium-sulfur batteries, extend the service life of the battery, and reduce the self-discharge rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114824648B_ABST
    Figure CN114824648B_ABST
Patent Text Reader

Abstract

The present invention discloses a PW 12 @PDADMAC / WMCNT modified polypropylene separator and its application in lithium sulfur battery. The method firstly reacts phosphotungstic acid and polydimethyldiallylammonium chloride in proportion to produce PW 12 @PDADMAC particles, then PW 12 @PDADMAC particles, carbon nanotubes, and PVDF were added to N-methylpyrrolidone solvent and finally vacuum filtered and loaded onto a polypropylene membrane to obtain PW 12 @PDADMAC / WMCNT / PP composite membrane. The composite membrane of the present invention can physically hinder the shuttling of polysulfides, adsorb and catalyze the conversion of polysulfides, inhibit the passivation of lithium metal and significantly improve the rate performance, coulombic efficiency and cycle life of lithium-sulfur batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium-sulfur batteries and relates to a PW 12 @PDADMAC / WMCNT modified polypropylene separator and its application in lithium-sulfur batteries. Background Art

[0002] Lithium-ion secondary batteries are currently recognized as a new generation of energy storage devices. They have been successfully commercialized and are developing rapidly in the field of portable devices. However, in the fields of electric vehicles, aerospace and defense equipment, the current commercial lithium-ion secondary batteries are limited by energy density and are far from meeting the needs of rapid energy development. Therefore, there is an urgent need to develop new energy storage devices with higher energy density, longer cycle life, low cost and environmental friendliness.

[0003] The theoretical specific capacity and energy density of lithium-sulfur secondary batteries (referred to as lithium-sulfur batteries) with metallic lithium as the negative electrode and elemental sulfur as the positive electrode are 1672 mAh g -1 and 2600Wh / kg. Moreover, elemental sulfur is abundant in nature, has no environmental pollution, and is low in cost. At present, the actual energy density of lithium-sulfur batteries has reached 590Wh / kg, which is much higher than other commercial electrode materials such as LiFeO4 and LiMn2O4.

[0004] The diaphragm is an important component of lithium-sulfur batteries. It is used to isolate the positive and negative electrodes to avoid internal short circuits in the battery and provide a channel for the transfer of lithium ions between the positive and negative electrodes. The separator of lithium-sulfur batteries is usually a non-polar film such as polypropylene / polyethylene (PP / PE). However, during the charging and discharging process of lithium-sulfur batteries, elemental sulfur is reduced to polysulfide Li2Sn (4≤n≤8) and it is easily soluble in organic electrolytes. Under the concentration gradient, it shuttles from the positive electrode to the negative electrode through the diaphragm, causing the shuttle effect. The shuttle effect causes lithium-sulfur batteries to have poor cyclability, low Coulomb efficiency, high self-discharge rate, irreversible loss of active substances, and surface passivation of lithium sheets.

[0005] Phosphotungstic acid (H3PW 12 0 40 , PW 12) can adsorb polysulfides and accelerate their kinetic conversion (JCYe, JJChen, RMYuan, et al, Strategies to Explore and Develop ReversibleRedoxReactions of Li-S in Electrode ArchitecturesUsing Silver-PolyoxometalateClusters, J.Am.Chem.Soc.140(2018)3134-3138.). Su et al. mixed phosphotungstic acid and conductive agent (Superp) evenly and applied it on polypropylene separator by scraper, which hindered the diffusion of polysulfides and improved the electrochemical performance of batteries (W.Yao, L.Liu, X.Wu, et al, Polyoxometalates / Active Carbon ThinSeparator for ImprovingCycle Performance of Lithium-Sulfur Batteries, ACSAppl.Mater.Interfaces 10(2018)35911-35918.). Cui et al. used polyoxometalates (K3PW 12 O 40 ) mixed with elemental sulfur (S) to improve the discharge capacity and cycle life of lithium-sulfur batteries (NFYan, WHZhang, JSShi, et al, Nano potassium phosphotungstate spheres / sulfur composites ascathodefor Li-S batteries, Materials Letters 229 (2018) 198–201.). Ni et al. prepared rGO-CNT@PW 12 Composite materials as sulfur carriers, although PW 12 It can promote the conversion of polysulfides, but PW 12It will also be reduced to heteropoly blue (L.Ni, G.Yang, Y.Liu, et al, Self-Assembled Polyoxometalate Nanodots as Bidirectional Cluster Catalysts for Polysulfide / Sulfide Redox Conversion in Lithium-Sulfur Batteries, ACS Nano 15 (2021) 12222-12236.). However, due to the concentration gradient, heteropoly blue will diffuse to the lithium anode and react with the lithium anode, causing corrosion of the lithium metal and loss of active substances, thereby leading to a decrease in the specific capacity of the battery and a reduction in the cycle life. Summary of the invention

[0006] The object of the present invention is to provide a PW having good cycle stability, long service life and high discharge specific capacity. 12 @PDADMAC / WMCNT / PP composite separator and its application in lithium-sulfur batteries.

[0007] The technical solution for achieving the purpose of the present invention is:

[0008] PW 12 The preparation method of @PDADMAC / WMCNT / PP composite diaphragm, the specific steps are as follows:

[0009] At a molar ratio of 1:1, first add PW 12 The powder and polydimethyldiallyl ammonium chloride (PDADMAC) solution were mixed to form PW 12 @PDADMAC precipitate particles; then PW 12 @PDADMAC precipitated particles, carbon nanotubes (WMCNT) and binder polyvinylidene fluoride (PVDF) were added to N-methylpyrrolidone (NMP) solvent, and after uniform dispersion, the mixed solution was filtered onto a polypropylene (PP) diaphragm by vacuum filtration and vacuum dried to obtain PW 12 @PDADMAC / WMCNT / PP composite diaphragm.

[0010] Furthermore, PW 12 The total concentration of PDADMAC particles and WMCNT in NMP was 10 mg / mL.

[0011] Furthermore, the vacuum drying temperature is 80° C., and the drying time is 6 hours.

[0012] The present invention also provides PW prepared by the above preparation method 12 @PDADMAC / WMCNT / PP composite diaphragm.

[0013] Furthermore, the present invention provides the above-mentioned PW 12 @Application of PDADMAC / WMCNT / PP composite separator in lithium-sulfur batteries.

[0014] Specifically, the application method is: PW 12 @PDADMAC / WMCNT / PP composite diaphragm PW 12 One side of @PDADMAC / WMCNT faces the sulfur cathode.

[0015] Compared with the prior art, the present invention has the following advantages:

[0016] (1) The method of the present invention is simple, PW 12 @The WMCNT in the PDADMAC / WMCNT / PP composite membrane has high conductivity, which increases the conductivity of the overall composite membrane.

[0017] (2) PW of the present invention 12 @PDADMAC / WMCNT / PP composite diaphragm has unique properties, PW 12 @PDADMAC is loaded on a conventional PP film. 12 It can effectively adsorb polysulfides and accelerate their kinetic conversion, but it will be reduced to heteropoly blue, shuttle to the lithium anode and react with it. 12 After the reaction, PW can be effectively fixed 12 , so that while it catalyzes the conversion of polysulfides, it will not be reduced to heteropoly blue, thereby not causing a negative impact on the lithium anode.

[0018] (3) The present invention converts PW 12 @pDADMAC / WMCNT loaded on the PP separator can physically hinder the shuttling of polysulfides, effectively inhibit the shuttle effect, and further improve the discharge capacity and cycle stability of lithium-sulfur batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 For PW 12 SEM image of @PDADMAC.

[0020] Figure 2 PW prepared in Example 1 12 @Scanning electron microscope image of PDADMAC / WMCNT / PP composite membrane.

[0021] Figure 3 For PW 12 and PW 12 @X-ray diffraction pattern of PDADMAC powder.

[0022] Figure 4 The PP diaphragm and the PW prepared in Example 1 12 @CV comparison chart of PDADMAC / WMCNT / PP diaphragm.

[0023] Figure 5 PW prepared in Example 1 12 @Battery rate cycle diagram of PDADMAC / WMCNT / PP composite membrane assembly.

[0024] Figure 6 PW prepared in Example 1 12 @1.0C long cycle diagram of battery assembled with PDADMAC / WMCNT / PP composite diaphragm. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with the embodiments and drawings.

[0026] Example 1

[0027] 1. Preparation of PW 12 @PDADMAC precipitated particles:

[0028] According to PW 12 The molar ratio of powder to PDADMAC solution is 1:1. Weigh 1.846 g PW 12 Powder and 1g PDADMAC solution, the two are mixed and reacted to produce PW 12 @PDADMAC precipitated particles.

[0029] 2. Preparation of PW 12 @PDADMAC / WMCNT / PP composite diaphragm:

[0030] PW 12 @PDADMAC precipitated particles, WMCNT and PVDF are in a mass ratio of 6:2:2, and 0.06gPW 12 @PDADMAC precipitate, 0.02g WMCNT and 0.02g PVDF were added to 8mL NMP solvent and stirred thoroughly to make PW 12 @PDADMAC precipitated particles and WMCNT are fully dispersed and PVDF is fully dissolved. 0.5mL of the mixed solution is extracted and filtered on a PP diaphragm. After the filtration is completed, it is dried to obtain PW 12 @PDADMAC / WMCNT / PP composite diaphragm, and cut the diaphragm with a diameter of 19mm.

[0031] 3. Preparation of lithium-sulfur batteries:

[0032] Sulfur is used as the positive electrode material and lithium sheet is used as the negative electrode material.12 @PDADMAC / WMCNT / PP composite diaphragm replaces the traditional polypropylene diaphragm, PW 12 @PDADMAC / WMCNT / PP composite diaphragm contains PW 12 One side of @PDADMAC / WMCNT faces the sulfur cathode, and the battery is assembled in the glove box to further measure its performance.

[0033] Comparative Example 1

[0034] 1. Preparation of PW 12 @PDADMAC precipitated particles:

[0035] According to PW 12 The molar ratio of powder to PDADMAC solution is 1:1. Weigh 1.846 g PW 12 Powder and 1g PDADMAC solution, the two are mixed and reacted to produce PW 12 @PDADMAC precipitated particles.

[0036] 2. Preparation of PW 12 @PDADMAC / WMCNT / PP composite diaphragm:

[0037] PW 12 @PDADMAC precipitated particles, WMCNT and PVDF are in a mass ratio of 5:3:2, and 0.05gPW 12 @PDADMAC precipitate, 0.03g WMCNT and 0.02g PVDF were added to 8mL NMP solvent and stirred thoroughly to make PW 12 @PDADMAC precipitated particles and WMCNT are fully dispersed and PVDF is fully dissolved. 0.5mL of the mixed solution is extracted and filtered on a PP diaphragm. After the filtration is completed, it is dried to obtain PW 12 @PDADMAC / WMCNT / PP composite diaphragm, and cut the diaphragm with a diameter of 19mm.

[0038] 3. Preparation of lithium-sulfur batteries:

[0039] Sulfur is used as the positive electrode material and lithium sheet is used as the negative electrode material. 12 @PDADMAC / WMCNT / PP composite diaphragm replaces the traditional polypropylene diaphragm, PW 12 @PDADMAC / WMCNT / PP composite diaphragm contains PW 12 One side of @PDADMAC / WMCNT faces the sulfur cathode, and the battery is assembled in the glove box to further measure its performance.

[0040] In this comparative example, the content of the conductive material WMCNT is increased, which can more effectively improve the overall conductivity of the composite diaphragm. 12 @The reduction in the content of PDADMAC will weaken the adsorption and conversion capabilities of polysulfides, and the performance of the battery will decrease.

[0041] Comparative Example 2

[0042] 1. Preparation of PW 12 @PDADMAC precipitated particles:

[0043] According to PW 12 The molar ratio of powder to PDADMAC solution is 1:1. Weigh 1.846 g PW 12 Powder and 1g PDADMAC solution, the two are mixed and reacted to produce PW 12 @PDADMAC precipitated particles.

[0044] 2. Preparation of PW 12 @PDADMAC / WMCNT / PP composite diaphragm:

[0045] PW 12 @PDADMAC precipitated particles, WMCNT and PVDF are in a mass ratio of 7:1:2, and 0.07gPW 12 @PDADMAC precipitate, 0.07g WMCNT and 0.02g PVDF were added to 8mL NMP solvent and stirred thoroughly to make PW 12 @PDADMAC precipitated particles and WMCNT are fully dispersed and PVDF is fully dissolved. 0.5mL of the mixed solution is extracted and filtered on a PP diaphragm. After the filtration is completed, it is dried to obtain PW 12 @PDADMAC / WMCNT / PP composite diaphragm, and cut the diaphragm with a diameter of 19mm.

[0046] 3. Preparation of lithium-sulfur batteries:

[0047] Sulfur is used as the positive electrode material and lithium sheet is used as the negative electrode material. 12 @PDADMAC / WMCNT / PP composite diaphragm replaces the traditional polypropylene diaphragm, PW 12 @PDADMAC / WMCNT / PP composite diaphragm contains PW 12 One side of @PDADMAC / WMCNT faces the sulfur cathode, and the battery is assembled in a glove box to further measure its performance.

[0048] In this comparative example, PW 12With the increase of @PDADMAC content, the adsorption and conversion capacity of polysulfides increases, but the decrease of WMCNT content will lead to the decrease of conductivity of the composite membrane, increase the impedance of the battery, and reduce the specific capacity and cycle stability of the battery.

[0049] Figure 1 For PW 12 @PDADMAC Scanning electron microscope image of precipitated particles. From the image, it can be seen that the surface of the precipitate is composed of small nano-scale spheres, which increase the adsorption sites for polysulfide.

[0050] Figure 2 PW prepared in Example 1 12 @SEM image of PDADMAC / WMCNT / PP composite membrane. It can be seen from the image that WMCNT is evenly dispersed on the PP membrane, which is beneficial to improve the overall conductivity of the composite membrane. 12 @PDADMAC is scattered among WMCNT, indicating that PW 12 @PDADMAC and WMCNT are evenly dispersed in the solvent, which improves the conductivity while enhancing the adsorption and conversion capabilities of polysulfides.

[0051] Figure 3 For PW 12 and PW 12 @PDADMAC powder X-ray diffraction pattern. From the figure, we can see PW 12 and PW 12 The diffraction peaks of @PDADMAC are almost completely consistent.

[0052] Figure 4 The PP diaphragm and the PW prepared in Example 1 12 @PDADMAC / WMCNT / PP diaphragm CV comparison chart. From the figure, it can be seen that the oxidation peaks of the PP diaphragm assembled battery are 2.353 and 2.404V, while the PW 12 @PDADMAC / WMCNT / PP membrane assembled battery's oxidation peaks (2.338 and 2.400) are both smaller than that of PP membrane assembled battery. The reduction peaks of PP membrane assembled battery are 2.029 and 2.289V, which are smaller than PW 12 @PDADMAC / WMCNT / PP membrane reduction peaks (2.050 and 2.300 V), indicating that PW 12 @PDADMAC can promote the conversion kinetics of polysulfides.

[0053] Figure 5 PW prepared in Example 1 12 @Battery rate cycle diagram of PDADMAC / WMCNT / PP composite membrane assembly. PW 12@The different rate performance of the battery assembled with PDADMAC / WMCNT / PP composite diaphragm is much higher than that of the battery assembled with PP diaphragm. 12 @PDADMAC / WMCNT / PP composite separator can improve the discharge capacity and reversibility of the battery.

[0054] Figure 6 PW prepared in Example 1 12 @1.0C long cycle diagram of battery assembled with PDADMAC / WMCNT / PP composite diaphragm. PW 12 The initial discharge capacity of the battery assembled with PDADMAC / WMCNT / PP composite diaphragm is 1100 mAh g -1 Higher than the capacity of PP diaphragm assembled battery (700mAhg -1 ). And PW 12 The cycle life of the battery assembled with @PDADMAC / WMCNT / PP composite diaphragm is 400 cycles, which is higher than the cycle life of the battery assembled with PP diaphragm (150 cycles), indicating that PW 12 @PDADMAC / WMCNT / PP composite diaphragm can improve discharge capacity and cycle life.

Claims

1. PW 12 @PDADMAC / WMCNT / PP composite diaphragm preparation method, It is characterized in that The specific steps are as follows: At a molar ratio of 1:1, first add PW 12 The powder and PDADMAC solution were mixed to form PW 12 @PDADMAC precipitate particles; then PW 12 The precipitated particles, carbon nanotubes and binder polyvinylidene fluoride were added to N-methylpyrrolidone solvent, and after being evenly dispersed, the mixed solution was filtered onto a polypropylene diaphragm by vacuum filtration and vacuum dried to obtain PW 12 @PDADMAC / WMCNT / PP composite diaphragm.

2. The preparation method according to claim 1, It is characterized in that PW 12 The total concentration of PDADMAC particles and WMCNT in NMP was 10 mg / mL.

3. The preparation method according to claim 1, It is characterized in that The vacuum drying temperature was 80°C and the drying time was 6 hours.

4. PW prepared according to any one of the preparation methods described in claims 1 to 3 12 @PDADMAC / WMCNT / PP composite diaphragm.

5. The PW according to claim 4 12 @Application of PDADMAC / WMCNT / PP composite separator in lithium-sulfur batteries.

6. The use according to claim 5, It is characterized in that Application method: PW 12 @PDADMAC / WMCNT / PP composite diaphragm PW 12 One side of @PDADMAC / WMCNT faces the sulfur cathode.

Citation Information

Patent Citations

  • Preparation method of supported hexadecyl trimethyl phosphotungstic acid quaternary ammonium hybrid microgel

    CN101816910A

  • Method for regenerating heteropoly acid quaternary ammonium salt catalyst

    CN101992125A

  • Lithium-sulfur battery separator material, preparation method thereof and application thereof

    CN110010823A

  • Method for synthesizing arbordinone

    CN111499502A

  • Magnesium oxide / iron composite material modified diaphragm and preparation method thereof

    CN111599970A