A calculation method for fatigue crack growth life of dual-performance powder disks
Through detailed measurement and finite element analysis, the fatigue crack shape factor and stress strength factor model of the dual-performance powder disk was established, which solved the fatigue crack life calculation error caused by material performance differences and structural complexity in traditional calculation methods, and achieved more Accurate fatigue crack growth life prediction.
Patent Information
- Application Number
- CN202210520813.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-12
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-05-12
AI Technical Summary
Traditional fatigue crack proliferation life calculation methods cannot accurately calculate fatigue crack proliferation life of different positions of dual-performance powder disks, mainly due to differences in material performance and complex structural shape factors.
By measuring fatigue crack information, obtaining stress state, establishing the relationship between shape factor and characteristic dimensions, calculating stress strength factor, and constructing crack propagation rate models for different partitions, the specific steps include measuring tensile limits, finite element analysis, obtaining shape factor, Establish stress intensity factor expression and calculate crack propagation life.
The calculation accuracy of fatigue crack stress strength factor and crack propagation life of dual-performance powder disk is improved, and partition characteristics and structural parameters are taken into account, which enhances the prediction accuracy.
Smart Images

Figure CN115019913B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aviation engine fuel system fault diagnosis, and in particular relates to a method for calculating fatigue crack growth life of a dual-performance powder disk. Background Art
[0002] As a turbine disk with different microstructures in the rim and hub, the dual-performance powder disk has characteristics that can meet the use of powder disks in different working environments. However, the material properties of dual-performance powder disks will be different in different tissue areas. Therefore, due to the difference in material properties, the traditional fatigue crack growth life calculation method cannot accurately calculate the fatigue crack growth life of dual-performance powder disks in different positions.
[0003] The commonly used method for calculating fatigue crack growth life is the Paris formula:
[0004]
[0005] Where: C and n are Paris formula parameters;
[0006] ΔK is the stress intensity factor amplitude.
[0007] The crack extends from the initial crack a0 to the critical crack a c The extended life can be calculated by the following formula
[0008]
[0009] The crack growth rate curves (i.e., Paris formula) of dual-performance powder disks in different tissue areas are not the same. If the same crack growth rate is used for cracks at different positions in dual-performance powder disks, a large error will occur in the crack growth life. Therefore, the influence of different grains on the crack growth rate needs to be considered when calculating the crack growth life.
[0010] To calculate the crack growth life, an accurate stress intensity factor must be obtained. The current calculation of fatigue crack stress intensity factor is generally expressed as: Where σ is the nominal stress, a is the crack size, and Y is the shape factor. The dual-performance powder disk has a complex structure, and fatigue cracks are greatly affected by structural factors. Therefore, the shape factor is complex and variable, and the expressions of shape factors for different structures are different. For dual-performance powder disks, the calculation of stress intensity factor cannot be calculated using the above general formula. Summary of the invention
[0011] In order to solve the above problems, the object of the present invention is to provide a method for calculating fatigue crack growth life of a dual-performance powder disk, the method comprising the following steps:
[0012] S1: Measure fatigue crack information of dual performance powder disk;
[0013] S2: Measure the tensile limit of the samples in the fine grain area and the coarse grain area;
[0014] S3: Obtain the stress state at the crack location by using the finite element method;
[0015] S4: measuring the characteristic dimensions of the dual-performance powder disk at the crack location;
[0016] S5: Establish the function of fatigue crack shape factor and characteristic size;
[0017] S6: Get shape factor;
[0018] S7: Establish the relationship between stress intensity factor and crack size, stress and wheel structure size;
[0019] S8: Obtain the stress intensity factor expression for the deepest part of mode I fatigue crack and the part of crack close to the free surface;
[0020] S9: Obtain the crack growth life.
[0021] The dual-performance powder disk fatigue crack growth life calculation method provided by the present invention also has the following characteristics: the crack information includes crack size and crack position, and the crack size includes crack depth and crack surface half-length.
[0022] The method for calculating the fatigue crack propagation life of a dual-performance powder disk provided by the present invention also has the following characteristics: S2 also includes sampling along the radial direction of the dual-performance powder disk, with the number of samples being not less than 10, performing crystal phase analysis on the samples taken, determining the grain size, and then determining the partition where the crack is located.
[0023] The method for calculating fatigue crack growth life of a dual-performance powder disk provided by the present invention also has the following characteristics: in S4, the crack position of the dual-performance powder disk includes the center hole position and the throat position.
[0024] When the crack is located at the center hole, the characteristic dimensions include the center hole radius R and the hub thickness 2W;
[0025] When the crack is located at the throat, the characteristic dimensions include the axial thickness H1 of the center of the throat crack along the wheel disc and the distance H2 from the center of the throat crack to the bottom of the wheel disc groove.
[0026] The method for calculating fatigue crack growth life of dual-performance powder disk provided by the present invention also has the following characteristics: in S5,
[0027] The shape factor and characteristic size of the central hole in the fine grain area satisfy the following formula:
[0028]
[0029] Where, l is the crack size;
[0030] m1 is the shape factor structural coefficient, m1∈[1.5,2];
[0031] m2 is the shape factor structure index, m2∈[0.5,0.8];
[0032] Y is the shape factor base value;
[0033] The throat shape factor and characteristic size of the coarse grain region satisfy the following formula:
[0034]
[0035] Where, l is the crack size;
[0036] m3, m4, and m5 are shape factor structural coefficients, m3∈[2,2.5], m4∈[1,1.3], and m5∈[0.5,0.8];
[0037] Y is the shape factor base value.
[0038] The method for calculating fatigue crack growth life of dual-performance powder disk provided by the present invention also has the following characteristics: S6 comprises the following steps:
[0039] S6.1: Introduce a surface crack in the flat specimen and calculate the shape factors for at least 10 sets of crack sizes using the three-dimensional finite element method. The crack sizes are a < 0.005R, a < 0.005H2, c < 0.005W, c < 0.005H1;
[0040] S6.2: Take the average of the shape factors obtained in S6.1 to obtain the shape factor,
[0041] Among them, a is the crack depth, c is the half length of the crack surface, H1 is the axial thickness of the center of the throat crack along the wheel disc, H2 is the distance from the center of the throat crack to the bottom of the wheel disc groove, W is half of the hub thickness, and R is the radius of the center hole.
[0042] The method for calculating fatigue crack growth life of a dual-performance powder disk provided by the present invention also has the following characteristics: in S7, the relationship between the stress intensity factor and the crack size, stress and disk structure size is as follows:
[0043]
[0044] Among them, X is the characteristic size of the dual-performance powder disk obtained by S4, Y is the shape factor, σ is the stress state at the crack location obtained by the finite element method, and l is the crack size.
[0045] The method for calculating fatigue crack growth life of dual-performance powder disk provided by the present invention also has the following characteristics: in S8,
[0046] The stress intensity factor expression of the deepest type I fatigue crack in the center hole of the fine grain zone of the dual-performance powder disk and the crack close to the free surface is:
[0047]
[0048] The stress intensity factor expression of the deepest I-type fatigue crack in the throat of the coarse-grained zone of the dual-performance powder disk and the crack close to the free surface is:
[0049]
[0050] Among them, a is the crack depth, c is the half length of the crack surface, H1 is the axial thickness of the disc along the center of the throat crack, H2 is the distance from the center of the throat crack to the bottom of the disc groove, W is half of the hub thickness, R is the radius of the center hole, and σ is the stress state at the crack location obtained by the finite element method.
[0051] The method for calculating fatigue crack growth life of a dual-performance powder disk provided by the present invention also has the following characteristics: S9 comprises: obtaining the material tensile limit σ of the center hole and the throat b1 , σ b2 , at this time, the coefficient of difference in material properties in different tissue regions is k = σ b1 / σ bi (i=1, 2), and the crack growth rate model of different partitions is constructed by this coefficient:
[0052]
[0053] At this time, the fatigue crack growth life of the center hole is
[0054]
[0055] The fatigue crack growth life of the throat is
[0056]
[0057] Where l is the crack size;
[0058] X is the characteristic size of the dual-performance powder disk;
[0059] Y is the shape factor base value;
[0060] m1 is the shape factor structural coefficient, m1∈[1.5,2];
[0061] m2 is the shape factor structure index, m2∈[0.5,0.8];
[0062] m3, m4, m5 are shape factor structural coefficients, m3∈[2,2.5], m4∈[1,1.3], m5∈[0.5,0.8].
[0063] Beneficial Effects
[0064] The dual-performance powder disk fatigue crack growth life calculation method provided by the present invention takes into account the dual-performance powder disk partition characteristics and structural parameters, and uses it for dual-performance powder disk fatigue crack growth life prediction, thereby improving the calculation progress of dual-performance powder disk fatigue crack stress intensity factor and crack growth life. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] Figure 1 A flow chart of a method for calculating fatigue crack growth life of a dual-performance powder disk provided in an embodiment of the present invention.
[0066] Figure 2 Schematic diagram of the partitioning of the dual-performance powder disk in an embodiment of the present invention.
[0067] Figure 3 Schematic diagram of typical location structural parameters of cracks in a dual-performance powder disk in an embodiment of the present invention.
[0068] Figure 4 Schematic diagram of a flat plate sample in an embodiment of the present invention. DETAILED DESCRIPTION
[0069] The present invention is further described in detail below in conjunction with the accompanying drawings and examples, but it should be noted that these implementation modes are not limitations of the present invention, and equivalent changes or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these implementation modes are all within the scope of protection of the present invention.
[0070] In the description of the embodiments of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the invention.
[0071] In addition, the terms "first", "second", "third", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0072] The terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the invention can be understood according to specific circumstances.
[0073] like Figure 1-4 As shown, this embodiment provides a method for calculating fatigue crack growth life of a dual-performance powder disk, the method comprising the following steps:
[0074] S1: Measure fatigue crack information of dual performance powder disk;
[0075] S2: Measure the tensile limit of the samples in the fine grain area and the coarse grain area;
[0076] S3: Obtain the stress state at the crack location by using the finite element method;
[0077] S4: measuring the characteristic dimensions of the dual-performance powder disk at the crack location;
[0078] S5: Establish the function of fatigue crack shape factor and characteristic size;
[0079] S6: Get shape factor;
[0080] S7: Establish the relationship between stress intensity factor and crack size, stress and wheel structure size;
[0081] S8: Obtain the stress intensity factor expression for the deepest part of mode I fatigue crack and the crack close to the free surface;
[0082] S9: Obtain the crack growth life.
[0083] In some embodiments, the crack information includes crack size and crack location, and the crack size includes crack depth and crack surface half length.
[0084] In some embodiments, S2 further includes sampling along the radial direction of the dual-performance powder disk, with the number of samples being no less than 10, performing crystal phase analysis on the samples, determining the grain size, and then determining the partition where the crack is located.
[0085] In some embodiments, in S4, the crack positions of the dual-performance powder disk include the center hole position and the throat position.
[0086] When the crack is located at the center hole, the characteristic dimensions include the center hole radius R and the hub thickness 2W;
[0087] When the crack is located at the throat, the characteristic dimensions include the axial thickness H1 of the center of the throat crack along the wheel disc and the distance H2 from the center of the throat crack to the bottom of the wheel disc groove.
[0088] In some embodiments, when the crack is infinitely small (l / X<0.005, X represents the characteristic size parameter in step 4), the shape factor approaches a constant value Y, and in S5,
[0089] The shape factor and characteristic size of the central hole in the fine grain area satisfy the following formula:
[0090]
[0091] Where, l is the crack size;
[0092] m1 is the shape factor structural coefficient, m1∈[1.5,2];
[0093] m2 is the shape factor structure index, m2∈[0.5,0.8];
[0094] Y is the shape factor base value;
[0095] The throat shape factor and characteristic size of the coarse grain region satisfy the following formula:
[0096]
[0097] Where, l is the crack size;
[0098] m3, m4, and m5 are shape factor structural coefficients, m3∈[2,2.5], m4∈[1,1.3], and m5∈[0.5,0.8];
[0099] Y is the shape factor base value.
[0100] In some embodiments, the shape factor base value is obtained by a flat plate sample, such as Figure 4 As shown, the relationship between the crack size and the structural parameters of the flat specimen is: a / H<0.005, c / W<0.005. When the crack size changes within this range, the shape factor is a constant value, and this value is used as the shape factor base value. S6 includes the following steps:
[0101] S6.1: Introduce a surface crack in the flat specimen and calculate the shape factors for at least 10 sets of crack sizes using the three-dimensional finite element method. The crack sizes are a < 0.005R, a < 0.005H2, c < 0.005W, c < 0.005H1;
[0102] S6.2: Take the average of the shape factors obtained in S6.1 to obtain the shape factor,
[0103] Among them, a is the crack depth, c is the half length of the crack surface, H1 is the axial thickness of the center of the throat crack along the wheel disc, H2 is the distance from the center of the throat crack to the bottom of the wheel disc groove, W is half of the hub thickness, and R is the radius of the center hole.
[0104] In some embodiments, in S7, the relationship between the stress intensity factor and the crack size, stress and wheel disc structure size is as follows:
[0105]
[0106] Among them, X is the characteristic size of the dual-performance powder disk obtained by S4, Y is the shape factor, σ is the stress state at the crack location obtained by the finite element method, and l is the crack size.
[0107] In some embodiments, in S8,
[0108] The stress intensity factor expression of the deepest type I fatigue crack in the center hole of the fine grain zone of the dual-performance powder disk and the crack close to the free surface is:
[0109]
[0110] The stress intensity factor expression of the deepest I-type fatigue crack in the throat of the coarse-grained zone of the dual-performance powder disk and the crack close to the free surface is:
[0111]
[0112] Among them, a is the crack depth, c is the half length of the crack surface, H1 is the axial thickness of the disc along the center of the throat crack, H2 is the distance from the center of the throat crack to the bottom of the disc groove, W is half of the hub thickness, R is the radius of the center hole, and σ is the stress state at the crack location obtained by the finite element method.
[0113] In some embodiments, S9 includes: obtaining the material tensile limit σ of the center hole and the throat b1 , σ b2 , at this time, the coefficient of difference in material properties in different tissue regions is k = σ b1 / σ bi (i=1, 2), and the crack growth rate model of different partitions is constructed by this coefficient:
[0114]
[0115] At this time, the fatigue crack growth life of the center hole is
[0116]
[0117] The fatigue crack growth life of the throat is
[0118]
[0119] Where l is the crack size;
[0120] X is the characteristic size of the dual-performance powder disk;
[0121] Y is the shape factor base value;
[0122] m1 is the shape factor structural coefficient, m1∈[1.5,2];
[0123] m2 is the shape factor structure index, m2∈[0.5,0.8];
[0124] m3, m4, m5 are shape factor structural coefficients, m3∈[2,2.5], m4∈[1,1.3], m5∈[0.5,0.8].
[0125] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.
Claims
1. A method for calculating fatigue crack growth life of dual-performance powder disks, characterized in that: The method comprises the following steps: S1: Measure fatigue crack information of dual performance powder disk; S2: Measure the tensile limit of the samples in the fine grain area and the coarse grain area; S3: Obtain the stress state at the crack location by using the finite element method; S4: measuring the characteristic dimensions of the dual-performance powder disk at the crack location; S5: Establish the function of fatigue crack shape factor and characteristic size; S6: Get shape factor; S7: Establish the relationship between stress intensity factor and crack size, stress and wheel structure size; S8: Obtain the stress intensity factor expression for the deepest part of mode I fatigue crack and the part of crack close to the free surface; S9: Get the crack growth life, In S4, the crack positions of the dual-performance powder disk include the center hole position and the throat position. In S5, The shape factor and characteristic size of the central hole in the fine grain area satisfy the following formula: Where, l is the crack size; X is the characteristic size of the dual-performance powder disk; m1 is the shape factor structural coefficient, m1∈[1.5,2]; m2 is the shape factor structure index, m2∈[0.5,0.8]; Y is the shape factor base value; The throat shape factor and characteristic size of the coarse grain region satisfy the following formula: Where, l is the crack size; m3, m4, and m5 are shape factor structural coefficients, m3∈[2,2.5], m4∈[1,1.3], and m5∈[0.5,0.8]; Y is the base value of the shape factor, In S7, the relationship between the stress intensity factor and the crack size, stress and wheel disc structure size is as follows: Where σ is the stress at the crack location obtained by the finite element method, In S8, The stress intensity factor expression of the deepest type I fatigue crack in the center hole of the fine grain zone of the dual-performance powder disk and the crack close to the free surface is: The stress intensity factor expression of the deepest I-type fatigue crack in the throat of the coarse-grained zone of the dual-performance powder disk and the crack close to the free surface is: Among them, a is the crack depth, c is the half length of the crack surface, H1 is the axial thickness of the disc along the center of the throat crack, H2 is the distance from the center of the throat crack to the bottom of the disc groove, W is half of the hub thickness, and R is the radius of the center hole. The S9 includes: obtaining the material tensile limit σ of the center hole and the throat b1 , σ b2 , at this time, the coefficient of difference in material properties in different tissue regions is k = σ b1 / σ bi (i=1, 2), and the crack growth rate model of different partitions is constructed by this coefficient: At this time, the fatigue crack growth life of the center hole is The fatigue crack growth life of the throat is In the formula, C and n are Paris formula parameters, ΔK is the stress intensity factor amplitude, l0 represents the initial crack size, l c It refers to the critical crack size and k is the coefficient of difference in material properties in different tissue areas.
2. The method for calculating fatigue crack growth life of dual-performance powder disks according to claim 1, characterized in that: The crack information includes crack size and crack position, and the crack size includes crack depth and crack surface half length.
3. The method for calculating fatigue crack growth life of dual-performance powder disk according to claim 1, characterized in that: The S2 also includes sampling along the radial direction of the dual-performance powder disk, with the number of samples being no less than 10, performing crystal phase analysis on the samples, determining the grain size, and then determining the partition where the crack is located.
4. The method for calculating fatigue crack growth life of a dual-performance powder disk according to claim 1, characterized in that: In S4, When the crack is located at the center hole, the characteristic dimensions include the center hole radius R and the hub thickness 2W; When the crack is located at the throat, the characteristic dimensions include the axial thickness H1 of the center of the throat crack along the wheel disc and the distance H2 from the center of the throat crack to the bottom of the wheel disc groove.
5. The method for calculating fatigue crack growth life of dual-performance powder disk according to claim 1, characterized in that: The S6 comprises the following steps: S6.1: Introduce a surface crack in the flat specimen and calculate the shape factors for at least 10 sets of crack sizes using the three-dimensional finite element method. The crack sizes are a < 0.005R, a < 0.005H2, c < 0.005W, c < 0.005H1; S6.2: Take the average of the shape factors obtained in S6.1 to obtain the shape factor, Among them, a is the crack depth, c is the half length of the crack surface, H1 is the axial thickness of the center of the throat crack along the wheel disc, H2 is the distance from the center of the throat crack to the bottom of the wheel disc groove, W is half of the hub thickness, and R is the radius of the center hole.