Electrochemical device and electronic device

By optimizing the content ratio and doping elements of nickel-cobalt lithium manganate and lithium manganate in the positive electrode active material of lithium ion batteries, combined with the electrolyte components, the problem of performance attenuation of lithium ion batteries at high temperatures is solved, and high-temperature cycle is realized and improve storage performance and reduce production costs.

CN115053379BActive Publication Date: 2024-11-01NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180012182.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-28
Publication Date
2024-11-01
Estimated Expiration
2041-09-28

AI Technical Summary

Technical Problem

Lithium-ion batteries have a large performance attenuation at high temperatures, which is difficult to meet the needs of improving high-temperature circulation and storage performance.

Method used

By controlling the content ratio of nickel-cobalt lithium manganate (NCM) and lithium manganate (LMO) in the positive electrode active material of the electrochemical device, and the addition of doped elements, the peak intensity ratio and 2θ angle offset of the XRD diffraction pattern are optimized. The amount, combined with the appropriate electrolyte components, improve the high-temperature circulation and storage performance of the electrochemical device.

Benefits of technology

It significantly improves the circulation and storage performance of lithium-ion batteries at high temperatures, while controlling production costs, ensuring high cost-effectiveness of electrochemical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115053379B_ABST
    Figure CN115053379B_ABST
Patent Text Reader

Abstract

The present application provides an electrochemical device and an electronic device, which include a positive electrode, a negative electrode and an electrolyte. The positive electrode active material includes a manganese-containing composite material. Under the condition of 30% SOC to 40% SOC, the XRD diffraction spectrum of the positive electrode active material includes a first diffraction peak of lithium manganate characteristic peak (400) and a second diffraction peak of nickel cobalt lithium manganate characteristic peak (104) in the range of 40° to 46°. The 2θ angle of the first diffraction peak is less than the 2θ angle of the second diffraction peak. The peak intensity of the first diffraction peak is A, and the peak intensity of the second diffraction peak is B, which satisfies: 0.01≤B / A≤0.55, thereby improving the high temperature cycle performance and storage performance of the electrochemical device and improving the low temperature cycle performance of the electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to an electrochemical device and an electronic device. Background Art

[0002] Lithium-ion batteries have the characteristics of high specific energy, high operating voltage, low self-discharge rate, small size and light weight. They are widely used in various fields such as energy storage, portable electronic devices and electric vehicles.

[0003] With the rapid development of lithium-ion battery applications in consumer terminals and other fields, people have higher requirements for the charge and discharge cycle performance of lithium-ion batteries. However, the performance of current lithium-ion batteries attenuates significantly at high temperatures. Summary of the invention

[0004] The purpose of this application is to provide an electrochemical device and an electronic device to improve the performance of the electrochemical device at high temperatures. The specific technical solution is as follows:

[0005] The first aspect of the present application provides an electrochemical device, comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises a positive electrode active material, wherein the positive electrode active material comprises a manganese-containing composite material, and under the condition of 30% SOC (State of Charge) to 40% SOC, the XRD (X-ray diffraction) diffraction spectrum of the positive electrode active material comprises a first diffraction peak of lithium manganese oxide LMO characteristic peak (400) and a second diffraction peak of lithium nickel cobalt manganese oxide NCM characteristic peak (104) in the range of 40° to 46°, the 2θ angle of the first diffraction peak is less than the 2θ angle of the second diffraction peak, the peak intensity of the first diffraction peak is A, and the peak intensity of the second diffraction peak is B, satisfying: 0.01≤B / A≤0.55. Controlling the peak intensity of the first diffraction peak to be A and the peak intensity of the second diffraction peak to be B to satisfy 0.01≤B / A≤0.55 can make the electrochemical device of the present application have excellent high temperature performance and make the electrochemical device have high cost competitiveness.

[0006] In one embodiment of the present application, under 60% SOC conditions, in the XRD diffraction pattern of the positive electrode active material, the peak area of ​​the first diffraction peak is I1, and the peak area of ​​the second diffraction peak is I2, satisfying: 0.1≤I2 / I1≤0.5. By controlling I2 / I1 within the above range, the high temperature cycle performance and storage performance of the electrochemical device can be improved.

[0007] In one embodiment of the present application, when the electrochemical device rises from 0% SOC to 100% SOC, the 2θ angle of the first diffraction peak shifts to a high angle by 0.5° to 1°. By controlling the shift of the 2θ angle of the first diffraction peak to a high angle within the above range, the stability of the Mn-O bond in the positive electrode active material can be improved, and the high temperature cycle performance of the electrochemical device can be improved.

[0008] In one embodiment of the present application, the electrochemical device satisfies at least one of the following conditions a) to c): a) based on the mass of the positive electrode active material, the mass content of lithium nickel cobalt manganese oxide NCM is 0.5% to 35%; b) based on the mass of the positive electrode active material, the mass content of lithium manganese oxide LMO is 50% to 92%; c) the positive electrode active material also includes a doping element, the doping element includes at least one of Al, Mg or Nb, and the mass content of the doping element is 0.1% to 2.5% based on the mass of the positive electrode active material. By controlling the content of NCM within the above range, it is beneficial to improve the high temperature performance while controlling the cost of the electrochemical device. By controlling the content of LMO within the above range, it is beneficial to reduce the production cost of the electrochemical device. By controlling the content of the doping element within the above range, the high temperature performance of the electrochemical device, such as high temperature cycle performance and high temperature storage performance, can be improved.

[0009] In one embodiment of the present application, the particle size distribution of the positive electrode active material satisfies: 0.9≤(Dv90-Dv10) / Dv50≤2.0. By controlling (Dv90-Dv10) / Dv50 within the above range, the low temperature kinetic performance of the electrochemical device can be improved. Furthermore, when the particle size distribution of the positive electrode active material satisfies 0.9≤(Dv90-Dv10) / Dv50≤1.24, the low temperature kinetic performance of the electrochemical device is better.

[0010] In one embodiment of the present application, the electrochemical device satisfies at least one of the following conditions d) to e): d) the electrolyte includes a solvent, the solvent includes dimethyl carbonate (DMC), ethylene carbonate (EC) and propylene carbonate (PC), and the mass ratio between dimethyl carbonate and ethylene carbonate is 3.1 to 7; e) the electrolyte also includes at least one of sultone compounds, polynitrile compounds, boron-containing lithium salts, ethylene sulfate, biphenyl or vinylene carbonate. By controlling the mass ratio between dimethyl carbonate and ethylene carbonate within the above range, the high temperature storage performance of the electrochemical device can be improved, and the low temperature kinetic performance of the electrochemical device can be improved; the electrolyte of the present application includes the above compounds, which can improve the high temperature storage performance of the electrochemical device and improve the low temperature kinetic performance of the electrochemical device.

[0011] In one embodiment of the present application, the electrochemical device satisfies at least one of the following conditions f) to g): f) the sultone compound includes at least one of 1,3-propane sultone, 1,3-butane sultone or 2-fluoro-1,3-propane sultone, and the mass content of the sultone compound is 0.01% to 5% based on the mass of the electrolyte; g) the polynitrile compound includes at least one of succinonitrile, adiponitrile, trans-butene dinitrile, glutaronitrile or 1,3,6-hexane trinitrile, and the mass content of the polynitrile compound is 0.01% to 5% based on the mass of the electrolyte. The electrolyte of the present application includes the above-mentioned sultone compound, and controlling the content of the sultone compound within the above range can further improve the high temperature storage performance of the electrochemical device and improve the low temperature kinetic performance of the electrochemical device. The electrolyte of the present application includes the above-mentioned polynitrile compound, and controlling the content of the polynitrile compound within the above range can further improve the high temperature storage performance of the electrochemical device and improve the low temperature kinetic performance of the electrochemical device.

[0012] In one embodiment of the present application, the negative electrode includes a negative electrode active material, and the particle size distribution of the negative electrode active material satisfies: 1.8≤(Dv90-Dv10) / Dv50≤2.8. Controlling the particle size distribution of the negative electrode active material within the above range can improve the high temperature storage performance of the electrochemical device and improve the low temperature kinetic performance of the electrochemical device.

[0013] A second aspect of the present application provides an electronic device, comprising the electrochemical device in any one of the above embodiments.

[0014] The present application provides an electrochemical device and an electronic device. Under the condition of 30% SOC to 40% SOC, the XRD diffraction spectrum of the positive electrode active material of the electrochemical device contains a first diffraction peak of lithium manganese oxide LMO characteristic peak (400) and a second diffraction peak of lithium nickel cobalt manganese oxide NCM characteristic peak (104), wherein the 2θ angle of the first diffraction peak is smaller than the 2θ angle of the second diffraction peak, and the peak intensity A of the first diffraction peak and the peak intensity B of the second diffraction peak satisfy 0.01≤B / A≤0.55, so that the electrochemical device having the positive electrode of the present application has excellent high-temperature cycle performance and storage performance, and improves its low-temperature cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions of the present application and the prior art, the following briefly introduces the drawings required for use in the embodiments and the prior art. Obviously, the drawings described below are only some embodiments of the present application.

[0016] Figure 1 The button cell assembled based on the lithium-ion battery of Example 1 of the present application shows an XRD diffraction pattern of the positive electrode active material after full discharge (0% SOC);

[0017] Figure 2 This is an XRD diffraction pattern of the positive electrode active material of a button cell assembled based on the lithium-ion battery of Example 1 of the present application after full charge (100% SOC). DETAILED DESCRIPTION

[0018] In order to make the purpose, technical scheme, and advantages of the present application more clearly understood, the present application is further described in detail with reference to the accompanying drawings and embodiments. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other technical schemes obtained by ordinary technicians in the field belong to the scope of protection of the present application.

[0019] It should be noted that in the specific embodiments of the present application, a lithium-ion battery is used as an example of an electrochemical device to explain the present application, but the electrochemical device of the present application is not limited to a lithium-ion battery.

[0020] The first aspect of the present application provides an electrochemical device, comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises a positive electrode active material, wherein the positive electrode active material comprises a manganese-containing composite material, and under the condition of 30% SOC (State of Charge) to 40% SOC, the XRD (X-ray diffraction) diffraction spectrum of the positive electrode active material comprises a first diffraction peak of lithium manganate LMO characteristic peak (400) and a second diffraction peak of lithium nickel cobalt manganate NCM characteristic peak (104) in the range of 40° to 46°, the 2θ angle of the first diffraction peak is less than the 2θ angle of the second diffraction peak, the peak intensity of the first diffraction peak is A, and the peak intensity of the second diffraction peak is B, satisfying: 0.01≤B / A≤0.55. For example, B / A can be 0.01, 0.02, 0.05, 0.07, 0.1, 0.3, 0.5, 0.55 or any range therebetween.

[0021] The inventors of the present application have found that the peak intensity of the first diffraction peak is A and the peak intensity of the second diffraction peak is B, which satisfies 0.01≤B / A≤0.55, which can make the electrochemical device of the present application have excellent high-temperature storage performance and make the electrochemical device have high cost competitiveness. Without being limited to any theory, the inventors of the present application believe that when B / A is too small (for example, less than 0.01), it indicates that the peak intensity of the first diffraction peak is too large, indicating that the LMO content is too high and the high temperature performance is poor; when B / A is too large (for example, greater than 0.55), it indicates that the peak intensity of the first diffraction peak is too small, indicating that the number of LMO (110) faces is too small, the LMO content is too small, and the cost of the electrochemical device is high. By controlling B / A within the above range, the Li in the LMO of the positive electrode active material can be increased. + The number of de-embedding surfaces (110), Li +The easier it is to deintercalate, the better the low-temperature performance of the electrochemical device. A certain amount of nickel cobalt manganese oxide (NCM) is compounded to improve the high-temperature cycle performance and storage performance of the electrochemical device, improve the low-temperature performance of the electrochemical device, and help control the production cost of the electrochemical device, making the electrochemical device cost-effective.

[0022] In one embodiment of the present application, under 60% SOC conditions, in the XRD diffraction pattern of the positive electrode active material, the peak area of ​​the first diffraction peak is I1, and the peak area of ​​the second diffraction peak is I2, satisfying: 0.1≤I2 / I1≤0.5. For example, I2 / I1 can be 0.1, 0.2, 0.3, 0.4, 0.5 or any range therebetween. Without being limited to any theory, the inventors of the present application believe that when the electrochemical device is under 60% SOC conditions, when I2 / I1 is too small (for example, less than 0.1), it indicates that the peak area of ​​the first diffraction peak is too small and the NCM content is too low, which is not conducive to the improvement of the high temperature cycle and storage performance of the electrochemical device; when I2 / I1 is too large (for example, greater than 0.5), Li in LMO + The number of the deintercalation surfaces (110) is too small, and the low temperature performance is poor; by controlling I2 / I1 within the above range, the high temperature cycle performance and storage performance of the electrochemical device can be improved.

[0023] In one embodiment of the present application, when the electrochemical device rises from 0% SOC to 100% SOC, the 2θ angle of the first diffraction peak shifts to a high angle by 0.5° to 1°. By controlling the shift of the 2θ angle of the first diffraction peak to a high angle within the above range, the stability of the Mn-O bond in the positive electrode active material can be improved, and the high temperature cycle performance of the electrochemical device can be improved.

[0024] In one embodiment of the present application, the electrochemical device satisfies at least one of the following conditions a) to c):

[0025] a) based on the mass of the positive electrode active material, the mass content of NCM is 0.5% to 35%;

[0026] For example, the mass content of NCM is 0.5%, 1%, 5%, 10%, 20%, 25%, 35% or any range therebetween. Without being limited to any theory, when the content of NCM is too low (e.g., less than 0.5%), it is not conducive to improving the high temperature cycle and storage performance of the electrochemical device; when the content of NCM is too high (e.g., greater than 35%), it affects the production cost of the electrochemical device. By controlling the content of NCM within the above range, it is beneficial to improve the high temperature performance of the electrochemical device and reduce its production cost.

[0027] The present application has no particular limitation on the type of NCM, as long as the purpose of the present application can be achieved, for example, it may include at least one of NCM811, NCM622, NCM523 or NCM111.

[0028] b) based on the mass of the positive electrode active material, the mass content of LMO is 50% to 92%;

[0029] For example, the mass content of LMO is 50%, 60%, 70%, 80%, 90%, 92% or any range therebetween. Without being limited to any theory, when the content of LMO is too low (for example, less than 50%), the content of other types of positive electrode active materials (such as NCM) increases, affecting the production cost of the electrochemical device; when the content of LMO is too high (for example, higher than 92%), the content of other types of positive electrode active materials (such as NCM) decreases, which is not conducive to improving the high temperature performance of the electrochemical device. By controlling the content of LMO within the above range, it is beneficial to reduce the production cost of the electrochemical device. In the present application, in addition to NCM and LMO, the positive electrode active material may also contain lithium iron phosphate LFP.

[0030] c) The positive electrode active material further includes a doping element, the doping element includes at least one of Al, Mg or Nb, and the mass content of the doping element is 0.1% to 2.5% based on the mass of the positive electrode active material.

[0031] For example, the content of the doping element is 0.1%, 0.2%, 0.5%, 1%, 1.2%, 1.5, 2%, 2.5% or any range therebetween. Without being limited to any theory, when the content of the doping element is too low (e.g., less than 0.1%), the high temperature performance of the electrochemical device deteriorates; when the content of the doping element is too high (e.g., greater than 2.5%), the degree of improvement in the high temperature performance of the electrochemical device is limited, and the specific capacity of the electrochemical device decreases. By controlling the content of the doping element within the above range, the high temperature performance and specific capacity of the electrochemical device, such as high temperature cycle performance and high temperature storage performance, can be improved.

[0032] In one embodiment of the present application, the particle size distribution of the positive electrode active material satisfies: 0.9≤(Dv90-Dv10) / Dv50≤2.0. For example, (Dv90-Dv10) / Dv50 is 0.9, 1, 1.5, 1.8, 2.0 or any range therebetween. Without being limited to any theory, when (Dv90-Dv10) / Dv50 is too large (for example, greater than 2.0), it is not conducive to the improvement of the low-temperature kinetic performance of the electrochemical device; when (Dv90-Dv10) / Dv50 is too small (for example, less than 0.9), the processing is difficult and the manufacturing cost of the electrochemical device is increased. By controlling (Dv90-Dv10) / Dv50 within the above range, the low-temperature kinetic performance of the electrochemical device can be improved and the manufacturing cost of the electrochemical device can be reduced.

[0033] In this application, Dv90 refers to the particle size at which the volume accumulation reaches 90% from the small particle size side in the volume-based particle size distribution, Dv50 refers to the particle size at which the volume accumulation reaches 50% from the small particle size side in the volume-based particle size distribution, and Dv10 refers to the particle size at which the volume accumulation reaches 10% from the small particle size side in the volume-based particle size distribution.

[0034] In one embodiment of the present application, the electrochemical device satisfies at least one of the following conditions d) to e):

[0035] d) The electrolyte includes a solvent, and the solvent includes dimethyl carbonate DMC, ethylene carbonate EC and propylene carbonate PC, wherein the mass ratio between DMC and EC is 3.1 to 7. For example, the mass ratio between dimethyl carbonate and ethylene carbonate is 3.1, 4, 4.5, 5, 6, 7 or any range therebetween. By controlling the mass ratio between dimethyl carbonate and ethylene carbonate within the above range, the high temperature storage performance of the electrochemical device can be improved, and the low temperature kinetic performance of the electrochemical device can be improved.

[0036] e) The electrolyte further comprises at least one of a sultone compound, a polynitrile compound, a boron-containing lithium salt, ethylene sulfate, biphenyl or vinylene carbonate. The electrolyte of the present application comprises the above compounds, which can improve the high-temperature storage performance of the electrochemical device and improve the low-temperature kinetic performance of the electrochemical device.

[0037] In one embodiment of the present application, the electrochemical device satisfies at least one of the following conditions f) to g):

[0038] f) The sultone compound includes at least one of 1,3-propane sultone, 1,3-butane sultone or 2-fluoro-1,3-propane sultone, and the mass content of the sultone compound is 0.01% to 5% based on the mass of the electrolyte. For example, the mass content of the sultone compound is 0.01%, 0.1%, 1%, 5% or any range therebetween. The electrolyte of the present application includes the above-mentioned sultone compound, and controlling the content of the sultone compound within the above-mentioned range can further improve the high temperature storage performance of the electrochemical device and improve the low temperature kinetic performance of the electrochemical device.

[0039] g) The polynitrile compound includes at least one of succinonitrile, adiponitrile, trans-butene dinitrile, glutaronitrile or 1,3,6-hexane trinitrile, and the mass content of the polynitrile compound is 0.01% to 5% based on the mass of the electrolyte, for example, the mass content of the polynitrile compound is 0.01%, 0.1%, 1%, 5% or any range therebetween. The electrolyte of the present application includes the above-mentioned polynitrile compound, and controlling the content of the polynitrile compound within the above-mentioned range can further improve the high temperature storage performance of the electrochemical device and improve the low temperature kinetic performance of the electrochemical device.

[0040] In one embodiment of the present application, the negative electrode includes a negative electrode active material, and the particle size distribution of the negative electrode active material satisfies: 1.8≤(Dv90-Dv10) / Dv50≤2.8. For example, (Dv90-Dv10) / Dv50 is 1.8, 2.0, 2.2, 2.5, 2.8 or any range therebetween. Controlling the particle size distribution of the negative electrode active material within the above range can improve the high temperature storage performance of the electrochemical device and improve the low temperature kinetic performance of the electrochemical device.

[0041] The present application does not particularly limit the preparation method of the manganese-containing composite material with doping elements, and the preparation method of those skilled in the art can be adopted. For example, in the process of synthesizing the manganese-containing composite material, an aluminum-containing compound (such as Al2O3, Al(OH)3, AlF3), a magnesium-containing compound (such as MgO) or a niobium-containing compound (such as Nb2O5, NbF5) can be added to LiMn2O4 to obtain the above-mentioned lithium manganese-containing composite material. In addition, the present application can achieve the change of the doping element in the positive electrode active material by adjusting the content of the doping element in the manganese-containing composite material, such as controlling the addition amount of the doping element compound. The present application does not specifically limit its adjustment process, as long as the purpose of the present application can be achieved.

[0042] The positive electrode current collector in the present application is not particularly limited and can be any positive electrode current collector in the art, such as aluminum foil, aluminum alloy foil or composite current collector.

[0043] There is no particular limitation on the negative electrode current collector in the present application, and materials such as metal foil or porous metal plate can be used, such as foil or porous plate of metals such as copper, nickel, titanium or iron or their alloys, such as copper foil. The negative electrode active material layer includes a negative electrode active material, a conductive agent, a binder and a thickener. There is no particular limitation on the negative electrode active material, and any negative electrode active material in the art can be used. For example, it can include artificial graphite, natural graphite, mesophase carbon microbeads (MCMB), soft carbon, hard carbon, silicon, silicon carbon, SiO, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structured lithium titanate Li4Ti5O 12 , Li-Al alloy or metallic lithium; the conductive agent may be at least one of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene or carbon nanofibers; the binder may be at least one of styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin or carboxymethyl cellulose (CMC); the thickener may be carboxymethyl cellulose (CMC).

[0044] The substrate of the isolation film of the present application includes, but is not limited to, at least one selected from polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyimide (PI) or aramid. For example, polyethylene includes at least one component selected from high-density polyethylene, low-density polyethylene and ultra-high molecular weight polyethylene. In particular, polyethylene and polypropylene have excellent effects on preventing short circuits and can improve the stability of electrochemical devices through the shutdown effect. The substrate can be a single-layer structure or a multi-layer composite structure of a plurality of mixtures, with a thickness of 3μm to 20μm.

[0045] A second aspect of the present application provides an electronic device comprising the electrochemical device described in the above embodiments of the present application.

[0046] The electronic device of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.

[0047] The preparation process of the electrochemical device is well known to those skilled in the art and is not particularly limited in this application. For example, a lithium-ion battery can be manufactured by overlapping the positive electrode and the negative electrode via a separator, and placing them in a housing after winding, folding, etc. as required, injecting an electrolyte into the housing and sealing it. In addition, an overcurrent protection element, a guide plate, etc. can also be placed in the housing as required to prevent the pressure inside the lithium-ion battery from rising and overcharging and discharging.

[0048] like Figure 1 As shown, the lithium-ion battery of Example 1 is disassembled to remove the positive electrode sheet and assembled into a button battery. After full discharge (0% SOC), the XRD diffraction pattern of the positive electrode active material thereof has a 2θ angle of 44.09° at the first diffraction peak; Figure 2 As shown, the lithium-ion battery of Example 1 was disassembled to remove the positive electrode plate and assembled into a button battery. After full charge (100% SOC), in the XRD diffraction pattern of its positive electrode active material, the 2θ angle of the first diffraction peak was 44.82°. It can be seen that in the process of the lithium-ion battery rising from 0% SOC to 100% SOC, the 2θ angle shifted to a high angle by 0.73°.

[0049] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0050] Test methods and equipment:

[0051] Test of the ratio of the peak intensity of the second diffraction peak (B) to the peak intensity of the first diffraction peak (A):

[0052] The lithium-ion battery is charged to 4.2V, and then discharged to 2.8V, and the cycle is repeated twice, and then the lithium-ion battery is recharged to different SOCs (for example, any value between 30% SOC and 40% SOC). After completion, the lithium-ion battery is disassembled, the positive electrode plate is taken out, and the positive electrode plate is immersed in DMC (dimethyl carbonate) for 30 minutes to remove the electrolyte and byproducts on the surface of the positive electrode plate, and then dried in a fume hood for 4 hours. The positive electrode active material layer is scraped off with a scraper to obtain the positive electrode active material layer powder, and then the positive electrode active material layer powder is placed on the sample stage of an XRD test instrument (model Bruker, D8), and a scanning rate of 2° / min is used, and the scanning angle range is 10° to 90° to obtain an XRD diffraction pattern. In the XRD diffraction pattern, the peak intensities corresponding to the characteristic peaks (104) of the positive electrode active material and the characteristic peaks (400) of the lithium manganate are taken to obtain the ratio of B to A.

[0053] Test of 2θ angle shift of the first diffraction peak:

[0054] The lithium-ion battery is charged to 4.2V, and then discharged to 2.8V, and the cycle is repeated twice. Then the positive electrode plate is taken out, and the active material on one side of the positive electrode plate is wiped off with NMP. The remaining single-sided plate is punched into a small disc with a diameter of 14mm, assembled into a button battery, and then the lithium-ion battery is charged to 4.3V, and then discharged to 3V, and the cycle is repeated twice. Then the battery is fully charged, and the fully charged and fully discharged button batteries are disassembled to obtain pole plates in different states. The positive electrode active material layer is scraped off with a scraper, and then the positive electrode active material layer powder is placed in the sample stage of the XRD test instrument (model Bruker, D8), and the scanning rate of 2° / min is used, and the scanning angle range is 10° to 90° to obtain the XRD diffraction pattern. The 2θ angle offset of the first diffraction peak (400) of the positive electrode active material in the fully discharged and fully charged states is compared.

[0055] Positive electrode active material element content test:

[0056] The active material of the positive electrode sheet after washing with DMC is scraped off with a scraper, dissolved with a mixed solvent (for example, 0.4 g of positive electrode active material uses 10 mL (nitric acid and hydrochloric acid mixed in a volume ratio of 1:1) aqua regia and 2 mL HF mixed solvent), the volume is fixed to 100 mL, and then an ICP (Inductively coupled plasma) analyzer is used to test the content of elements such as Ni, Co, Mn, Al, Mg, and Nb in the solution.

[0057] The dried positive electrode sheet is sliced, and then a scanning electron microscope (SEM) is used to observe the slice cross section to find the particles in the cross section. Then, the content of each element measured by an energy dispersive spectrometer (EDS) and ICP is used to determine the composition of a single particle. For example, the chemical formula of the particle is determined to be LiNi a Co b Mn (1-a-b) O2, and then infer the content of the substance represented by the chemical formula in the positive electrode active material based on the chemical formula, EDS data and ICP data.

[0058] Particle size test in the positive electrode active material layer:

[0059] After the disassembled positive electrode sheet or negative electrode sheet is sintered into powder at 400°C in vacuum, the particle size is tested using a particle size analyzer to obtain the values ​​of Dv10, Dv50, and Dv90.

[0060] -10℃ discharge capacity / 25℃ discharge capacity test:

[0061] In an environment of 25°C, constant current and constant voltage charging is performed at a charging current of 0.5C until the upper limit voltage is 4.2V, then the environment is adjusted to -10°C, and after standing for 2 hours, constant current discharge is performed at a discharge current of 0.2C until the final voltage is 2.8V, and the first discharge capacity of 0.2C is calculated as the capacity of the battery, which is recorded as the first capacity;

[0062] In an environment of 25°C, constant current and constant voltage charging is performed at a charging current of 0.5C until the upper limit voltage is 4.2V, and then constant current discharge is performed at a discharge current of 0.2C until the final voltage is 2.8V. The first discharge capacity of 0.2C is calculated as the capacity of the battery, which is recorded as the second capacity;

[0063] Then -10°C discharge capacity / 25°C discharge capacity=(first capacity / second capacity)×100%.

[0064] Lithium-ion battery cycle performance test:

[0065] The lithium-ion battery is repeatedly charged and discharged through the following steps, and the discharge capacity retention rate of the lithium-ion battery is calculated:

[0066] 10℃ cycle test:

[0067] In an environment of 10°C, the first charge and discharge were carried out. Charging was carried out at a charging current of 0.5C until the voltage was 4.2V, and then constant current discharge was carried out at a discharge current of 1C until the final voltage was 2.8V. The discharge capacity was recorded as the discharge capacity of the first cycle. The above steps were then repeated for 500 charge and discharge cycles, and the discharge capacity of the 500th cycle was recorded.

[0068] 10° C. cycle capacity retention rate=(discharge capacity at the 500th cycle / discharge capacity at the first cycle)×100%.

[0069] 50℃ cycle test:

[0070] In an environment of 50°C, the first charge and discharge were carried out. Charging was carried out at a charging current of 0.5C until the voltage was 4.2V, and then constant current discharge was carried out at a discharge current of 1C until the final voltage was 2.8V. The discharge capacity was recorded as the discharge capacity of the first cycle. The above steps were then repeated for 500 charge and discharge cycles, and the discharge capacity of the 500th cycle was recorded.

[0071] 50° C. cycle capacity retention rate=(discharge capacity at the 500th cycle / discharge capacity at the first cycle)×100%.

[0072] Lithium-ion battery high temperature storage performance test:

[0073] In an environment of 25°C, charge at a charging current of 0.5C until the upper limit voltage is 4.2V, then discharge at a constant current of 0.5C until the final voltage is 2.8V, and record the discharge capacity as the capacity before storage;

[0074] Charge at a constant current of 0.5C rate to a voltage of 3.85V, charge at a constant voltage of 4.2V until the current is less than 0.05C, store the battery in a 60°C oven for 7 days, and then discharge at a constant current of 0.5C until the final voltage is 2.8V; then charge at a charging current of 0.5C until the voltage is 4.2V, and then discharge at a constant current of 0.5C until the voltage is 2.8V. Cycle three times, record the third discharge capacity, and record it as the capacity after storage.

[0075] Capacity retention rate of lithium-ion battery = capacity after storage / capacity before storage × 100%.

[0076] 0.1C discharge specific capacity test:

[0077] The lithium-ion batteries in each embodiment and each comparative example were subjected to charge and discharge tests using a LAND series battery test system to test their charge and discharge performance. They were charged at a constant current of 0.1C at room temperature until the voltage reached 4.2V, and further charged at a constant voltage of 4.2V until the current was less than 0.05C, so that they were in a 4.2V fully charged state. Subsequently, they were discharged at a constant current of 0.1C until the voltage reached 2.8V. The electrochemical device was charged and discharged twice using the above operation, and the second capacity obtained was the 0.1C discharge capacity.

[0078] 0.1C discharge specific capacity = 0.1C discharge capacity / mass of active material of the electrode.

[0079] Example 1

[0080] <Preparation of lithium manganate>

[0081] Weigh 203.3 kg of lithium carbonate, 780.6 kg of manganese tetraoxide, 29.68 kg of aluminum oxide, and 5.65 kg of niobium pentoxide, mix them in a high-speed mixer at 300 r / min for 20 min, place the mixture in an air kiln, heat it to 790°C at 5°C / min, keep it for 24 h, take it out after natural cooling, and pass it through a 300-mesh sieve to obtain lithium manganate (LMO).

[0082] <Preparation of mixed positive electrode active material>

[0083] Weigh 180kg of synthesized LMO and commercially available polycrystalline LiNi 0.55 Co 0.15 Mn 0.320kg of O2 (NCM) was added with 15kg of anhydrous ethanol and 2kg of glucose. After mixing evenly and drying, the mixture was placed in an air kiln and heated to 400℃ at 5℃ / min for 4h. After cooling naturally, the mixture was taken out and passed through a 300-mesh sieve to obtain a mixed positive electrode active material, i.e., a manganese-containing composite material.

[0084] <Preparation of positive electrode sheet>

[0085] The mixed positive electrode active material manganese-containing composite material, binder polyvinylidene fluoride (PVDF), conductive carbon black, and carbon nanotubes (CNT) are mixed in a mass ratio of 95:2:1.8:1.2, and then NMP (N-methylpyrrolidone) is added as a solvent, and a uniform positive electrode slurry with a solid content of 75% is prepared under vacuum stirring. The positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 13μm, dried at 90°C, and cold pressed to obtain a positive electrode sheet with a total thickness of 95μm for the positive electrode active material layer, and then the above steps are repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet with a positive electrode active material layer coated on both sides. The positive electrode sheet is cut into a specification of (74mm×867mm) and welded to the pole ear for standby use.

[0086] <Preparation of negative electrode sheet>

[0087] The negative electrode active material artificial graphite, styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) are mixed in a mass ratio of 98:1:1, and then deionized water is added as a solvent to prepare a slurry with a solid content of 70%, and stirred evenly. The slurry is evenly coated on one surface of a copper foil with a thickness of 8μm, dried at 110°C, and cold pressed to obtain a negative electrode sheet with a negative electrode active material layer coated on one side with a thickness of 65μm, and then the above coating steps are repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet with a negative electrode active material layer coated on both sides. The negative electrode sheet is cut into specifications of (74mm×867mm) and welded to the pole ears for standby use.

[0088] <Preparation of Separator Film>

[0089] A polyethylene (PE) porous polymer film with a thickness of 15 μm was used as the isolation membrane.

[0090] <Preparation of Electrolyte>

[0091] In an environment with a water content of less than 10 ppm, non-aqueous organic solvents dimethyl carbonate (DMC), ethylene carbonate (EC), and propylene carbonate (PC) are mixed in a mass ratio of 6.2:1:1, and then lithium hexafluorophosphate (LiPF6) is added to the non-aqueous organic solvent to dissolve and mix evenly. Among them, the mass fraction of LiPF6 in the electrolyte is 12.5%.

[0092] <Preparation of lithium-ion batteries>

[0093] The positive electrode sheet, separator, and negative electrode sheet of Preparation Example 1 are stacked in order, with the separator placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then wound to obtain an electrode assembly. The electrode assembly is placed in an aluminum-plastic film packaging bag, and the moisture is removed at 80°C, and the prepared electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, forming, shaping, and other processes.

[0094] <Charging of lithium-ion batteries>

[0095] The prepared lithium ion battery was charged to a SOC of 30%. The first diffraction peak, the second diffraction peak, the value of B / A and the performance parameters are shown in Table 1.

[0096] Example 2 to Example 4

[0097] The process was the same as Example 1 except that in <Preparation of Mixed Positive Electrode Active Material>, the content of NCM in the positive electrode active material was adjusted as shown in Table 1 to adjust the value of B / A.

[0098] Example 5 to Example 7

[0099] Except that the content of the doping element is adjusted as shown in Table 2 in <Preparation of lithium manganate>, the rest is the same as Example 2.

[0100] Example 8 to Example 9

[0101] The process is the same as in Example 2 except that in <Preparation of lithium manganese oxide>, a magnesium compound MgO is added to LMO and the type and content of the doping element are adjusted as shown in Table 2.

[0102] Example 10 to Example 11

[0103] Except that the type and content of the doping element are adjusted as shown in Table 2 in <Preparation of lithium manganate>, the rest is the same as Example 2.

[0104] Example 12 to Example 17

[0105] Except that Dv50 and (Dv90-Dv10) / Dv50 of the positive electrode active material were adjusted as shown in Table 3 in <Preparation of Positive Electrode Sheet>, the rest was the same as Example 2.

[0106] Example 18 to Example 23

[0107] Except that in <Preparation of Electrolyte>, the mass ratio of DMC to EC in the non-aqueous organic solvent was adjusted as shown in Table 4 while maintaining the same content of PC and LiPF6 in the electrolyte as in Example 2, the rest was the same as in Example 2.

[0108] Example 24 to Example 32

[0109] The electrolyte prepared in Example 2 was used as a base electrolyte, and a sultone compound, a polynitrile compound, and biphenyl as shown in Table 5 were further added thereto so that the contents of the above additives were as shown in Table 5. Other aspects were the same as in Example 2.

[0110] Example 33 to Example 38

[0111] Except that in <Preparation of Negative Electrode Sheet>, Dv50 and (Dv90-Dv10) / Dv50 of the negative electrode active material are as shown in Table 6, the rest is the same as Example 2.

[0112] Comparative Example 1 to Comparative Example 2

[0113] The process was the same as Example 1 except that in <Preparation of Mixed Positive Electrode Active Material>, the content of NCM in the positive electrode active material was adjusted as shown in Table 1 to adjust the value of B / A.

[0114] Comparative Example 3

[0115] <Preparation of lithium manganate>

[0116] Weigh 203.3 kg of lithium carbonate and 780.6 kg of manganese tetraoxide, mix them in a high-speed mixer at 300 r / min for 20 min, place the mixture in an air kiln, heat it to 790°C at 5°C / min, keep it for 24 h, take it out after natural cooling, and pass it through a 300-mesh sieve to obtain lithium manganate (LMO).

[0117] <Preparation of mixed positive electrode active material>

[0118] Weigh 140 kg of the synthesized LMO and commercially available polycrystalline LiNi 0.55 Co 0.15 Mn 0.3 60kg of O2 (NCM), 15kg of anhydrous ethanol and 2kg of glucose were added. After mixing evenly and drying, the mixture was placed in an air kiln and heated to 400℃ at 5℃ / min, maintained for 4h, taken out after natural cooling, and passed through a 300-mesh sieve to obtain a mixed positive electrode active material.

[0119] Table 1 Test results of lithium-ion batteries at 30% SOC:

[0120]

[0121] Table 2

[0122]

[0123] Table 3

[0124]

[0125] Table 4

[0126] DMC to EC mass ratio 10℃ cycle capacity retention rate Capacity recovery rate after 7-day storage at 60℃ Example 2 6.2 89.3% 93.5% Embodiment 18 3.1 87.7% 94.2% Embodiment 19 4 88.7% 94.1% Embodiment 20 6.5 90.2% 93.0% Embodiment 21 7 89.6% 91.8% Embodiment 22 3 85.2% 94.1% Embodiment 23 7.2 86.9% 90.2%

[0127] Table 5

[0128]

[0129] In Table 5, “ / ” means not contained or not measured.

[0130] Table 6

[0131]

[0132] It can be seen from Examples 1 to 4 and Comparative Examples 1 to 2 that, in the positive electrode active material, the peak intensity B of the second diffraction peak and the peak intensity A of the first diffraction peak are within the scope of the present application, and the capacity recovery rate of the lithium-ion battery stored at 60°C for 7 days is significantly improved, indicating that the lithium-ion battery of the present application has good high-temperature storage performance.

[0133] The cost of NCM material is about 4.2 times that of LMO material. It can be seen from Examples 1 to 4 and Comparative Example 1 that, compared with lithium-ion batteries without NCM (such as Comparative Example 1), the present application can significantly improve the high-temperature storage performance of lithium-ion batteries, but the cost of positive electrode manufacturing is not as much as the cost of NCM materials. It can be seen from Examples 1 to 4 and Comparative Example 2 that further increasing the content of NCM in the positive electrode active material has limited improvement in the high-temperature cycle performance of the lithium-ion battery, but the cost of positive electrode manufacturing is greatly increased. It can be seen that by controlling the NCM content in the positive electrode active material within the scope of this application, a lithium-ion battery with good high-temperature storage performance can be obtained, and it is beneficial to the cost control of lithium-ion batteries.

[0134] It can be seen from Example 3 and Comparative Example 3 that by optimizing the preparation process of the positive electrode active material so that B / A is within the scope of this application, a lithium-ion battery with good high-temperature storage performance can be obtained.

[0135] Parameters such as the type of doping element in the positive electrode active material, the content of the doping element, I2 / I1, and the 2θ angle offset of the first diffraction peak may also affect the performance of the lithium-ion battery. It can be seen from Examples 5 to 11 that by controlling the above parameters, a lithium-ion battery with good high-temperature cycle performance, high-temperature storage performance and specific capacity can be obtained.

[0136] It can be seen from Examples 12 to 17 that by controlling the (Dv90-Dv10) / Dv50 of the positive electrode active material, its -10°C discharge capacity / 25°C discharge capacity is improved, further improving the low temperature kinetics of the lithium-ion battery.

[0137] It can be seen from Examples 18 to 23 that by controlling the mass ratio of DMC to EC in the electrolyte, the high temperature storage performance of the lithium ion battery can be further improved and the low temperature kinetic performance of the lithium ion battery can be improved.

[0138] It can be seen from Example 2 and Examples 24 to 32 that when the electrolyte contains additives such as sultone compounds, polynitrile compounds, biphenyl, etc., the high-temperature storage performance of the lithium-ion battery can be further improved, and the low-temperature dynamics performance of the lithium-ion battery can be improved.

[0139] It can be seen from Examples 33 to 38 that by controlling the (Dv90-Dv10) / Dv50 of the negative electrode active material, the high temperature storage performance and low temperature kinetic performance of the lithium-ion battery can be further improved.

[0140] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. An electrochemical device comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises a positive electrode active material, in, The positive electrode active material comprises a manganese-containing composite material. Under the condition of 30% SOC to 40% SOC, the XRD diffraction spectrum of the positive electrode active material comprises a first diffraction peak of lithium manganate characteristic peak (400) and a second diffraction peak of nickel cobalt lithium manganate characteristic peak (104) in the range of 40° to 46°, and the 2θ angle of the first diffraction peak is smaller than the 2θ angle of the second diffraction peak. The peak intensity of the first diffraction peak is A, and the peak intensity of the second diffraction peak is B, satisfying: 0.01≤B / A≤0.

55.

2. The electrochemical device according to claim 1, wherein: Under the condition of 60% SOC, in the XRD diffraction spectrum of the positive electrode active material, the peak area of ​​the first diffraction peak is I1, and the peak area of ​​the second diffraction peak is I2, satisfying: 0.1≤I2 / I1≤0.

5.

3. The electrochemical device according to claim 1, wherein When the electrochemical device increases from 0% SOC to 100% SOC, the 2θ angle of the first diffraction peak shifts to a higher angle by 0.5° to 1°.

4. The electrochemical device according to claim 1, wherein The electrochemical device satisfies at least one of the following conditions a) to c): a) based on the mass of the positive electrode active material, the mass content of lithium nickel cobalt manganese oxide is 0.5% to 35%; b) based on the mass of the positive electrode active material, the mass content of lithium manganate is 50% to 92%; c) The positive electrode active material further includes a doping element, the doping element includes at least one of Al, Mg or Nb, and the mass content of the doping element is 0.1% to 2.5% based on the mass of the positive electrode active material.

5. The electrochemical device according to claim 1, wherein The particle size distribution of the positive electrode active material satisfies: 0.9≤(Dv90-Dv10) / Dv50≤2.

0.

6. The electrochemical device according to claim 1, wherein Satisfy at least one of the following conditions d) to e): d) the electrolyte comprises a solvent, the solvent comprises dimethyl carbonate, ethylene carbonate and propylene carbonate, and the mass ratio between the dimethyl carbonate and the ethylene carbonate is 3.1 to 7; e) The electrolyte further comprises at least one of a sultone compound, a polynitrile compound, a boron-containing lithium salt, ethylene sulfate, biphenyl or vinylene carbonate.

7. The electrochemical device according to claim 6, wherein: Satisfy at least one of the following conditions f) to g): f) the sultone compound includes at least one of 1,3-propane sultone, 1,3-butane sultone or 2-fluoro-1,3-propane sultone, and the mass content of the sultone compound is 0.01% to 5% based on the mass of the electrolyte; g) the polynitrile compound comprises at least one of succinonitrile, adiponitrile, fumaronitrile, glutaronitrile or 1,3,6-hexanetrinitrile, and the mass content of the polynitrile compound is 0.01% to 5% based on the mass of the electrolyte.

8. The electrochemical device according to claim 1, wherein The negative electrode includes a negative electrode active material, and the particle size distribution of the negative electrode active material satisfies: 1.8≤(Dv90-Dv10) / Dv50≤2.

8.

9. An electronic device comprising the electrochemical device according to any one of claims 1 to 8.