Integrated lithium deposition with protective layer tool

By using lithium metal thin films and protective films in lithium ion energy storage devices, the deposition and processing challenges of lithium metal in energy storage systems are solved, improving battery performance and simplifying the manufacturing process.

CN115064654BActive Publication Date: 2024-11-19APPLIED MATERIALS INC
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202210706128.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2016-01-28
Filing Date
2017-01-16
Publication Date
2024-11-19
Estimated Expiration
2037-01-16

AI Technical Summary

Technical Problem

Lithium metals have challenges in deposition and handling in energy storage systems, especially due to their strong reactivity and instability, resulting in traditional protection measures affecting battery performance and increasing manufacturing complexity.

Method used

Lithium metal films are used and covered with protective films, including ion-conducting polymer material or interlayer films, to compensate for capacitance loss of first charge and discharge in the lithium ion energy storage device, and through the roll-to-roll system in the processing tool and The evaporation process deposits lithium metal film and protective film.

Benefits of technology

Effectively compensates for the irreversible loss of lithium metal, improves battery performance, simplifies the manufacturing process, and reduces tool complexity and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115064654B_ABST
    Figure CN115064654B_ABST
Patent Text Reader

Abstract

In one embodiment, an integrated processing tool for the deposition and processing of lithium metal in an energy storage device is disclosed. The integrated processing tool may be a web tool. The integrated processing tool may include a reel-to-reel system for conveying a continuous sheet of material through the following chambers: a chamber for depositing a thin film of lithium metal on the continuous sheet of material and a chamber for depositing a protective film on the surface of the thin film of lithium metal. The chamber for depositing a thin film of lithium metal may include a PVD system such as an electron beam evaporator, a thin film conveying system, or a slot-die deposition system. The chamber for depositing a protective film on a lithium metal film may include a chamber for depositing an interlayer film or a chamber for depositing a lithium ion conductive polymer on a lithium metal film.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application date of January 16, 2017, application number 201780008939.4, and invention name “Integrated lithium deposition with protective layer tool”. Technical Field

[0002] Embodiments described herein generally relate to lithium metal deposition and processing. In particular, embodiments described herein relate to methods and systems for deposition and processing of lithium metal in energy storage devices. Background Art

[0003] Rechargeable electrochemical storage systems are becoming increasingly important for many areas of daily life. Large-capacity electrochemical energy storage devices such as lithium-ion (Li-ion) batteries are used in an increasing number of applications, including portable electronics, medical, transportation, grid-connected large-scale energy storage, renewable energy storage, and uninterruptible power supply (UPS). Conventional lead-acid / sulfuric acid batteries often have insufficient capacity and often do not have enough cycles for these growing applications. However, lithium-ion batteries are considered to have the best opportunity.

[0004] Typically, lithium batteries do not contain any metallic lithium for safety reasons, but instead use graphite materials as anodes. However, the use of graphite can be charged to the limited composition LiC6 when in a charged state, and the use of graphite results in a much smaller capacity than the use of metallic lithium. Currently, the industry is moving from graphite-based anodes to silicon-blended graphite to increase energy cell density. However, silicon-blended graphite anodes have the disadvantage of capacity loss during the first charge and discharge. Therefore, lithium metal deposition is needed to compensate for the capacity loss of silicon-blended graphite anodes during the first charge and discharge. However, lithium metal faces several device integration challenges.

[0005] Lithium is an alkali metal. Similar to its heavy element counterparts in the first main group, lithium is characterized by strong reactivity with a variety of different substances. Lithium reacts violently with water, alcohol, and other substances containing proton hydrogen, often resulting in combustion. Lithium is unstable in air and reacts with oxygen, nitrogen, and carbon dioxide. Lithium is generally transported under an inert gas environment (noble gas, such as argon) and the strong reactivity of lithium requires that other handling operations are also performed in an inert gas environment. Therefore, lithium has several challenges when it comes to handling, storage, and transportation.

[0006] Protective surface treatments have been developed for lithium metal. One method for protective surface treatment of lithium metal includes coating the lithium metal with a wax layer, such as polyethylene wax. However, a large amount of coating agent must be applied, which can affect subsequent treatment of the lithium metal layer.

[0007] Another approach to protective surface treatment proposes the use of continuous carbonate coatings, polymer coatings (e.g., polyurethanes, PTFE, PVC, polystyrene, and others) to produce stabilized lithium metal powders (SLMP). However, these polymer coatings can cause problems when prelithiating electrode materials.

[0008] Thus, there is a need for methods and systems for the deposition and processing of lithium metal in energy storage systems. Summary of the invention

[0009] Embodiments described herein generally relate to lithium metal deposition and processing. In particular, embodiments described herein relate to methods and systems for the deposition and processing of lithium metal in energy storage devices. In one embodiment, a negative electrode is provided. The negative electrode is coated with a thin film of lithium metal. The thin film of lithium metal may have sufficient thickness to compensate for the irreversible loss of lithium metal during the first charge and discharge of the battery, and the thin film of lithium metal may be a lithium metal film having a thickness from about 1 micron to about 20 microns in some embodiments. The lithium metal film may be used as a lithium metal anode. Furthermore, the lithium metal film may be coated with a protective film for protecting the lithium metal film from the influence of surrounding oxidants. In one embodiment, the protective film comprises an ion-conducting polymer material, which is incorporated into the final battery cell. In another embodiment, the protective film comprises an interlayer film, which protects the lithium metal film from the influence of surrounding oxidants. The interlayer film is usually removed before additional processing. In some embodiments, the interlayer film may serve as a separator.

[0010] In another embodiment, a lithium battery is provided. The lithium battery includes: a positive electrode, a negative electrode coated with a thin film of lithium metal. The thin film of lithium metal may have a sufficient thickness to compensate for the irreversible loss of lithium metal during the first charge and discharge of the battery, and the thin film of lithium metal may be a lithium metal film having a thickness from about 1 micron to about 20 microns in some embodiments. Furthermore, the lithium metal film may be coated with an ion conductive polymer for protecting the lithium metal film from the influence of surrounding oxidants.

[0011] In another embodiment, an integrated processing tool for forming a negative electrode coated with lithium is provided. The integrated processing tool may be a coil tool, covering roll-to-roll of vacuum and non-vacuum deposition techniques (e.g., PVD, slot-die, gravure, thermal spraying, lamination, and screen-printing). The integrated processing tool may include: a roll-to-roll system for transmitting a continuous sheet of material via the following chambers: a chamber for depositing a thin film of lithium metal on a continuous sheet of material and a chamber for depositing a protective film on the surface of a thin film of lithium metal. In some embodiments, a chamber for depositing a thin film of lithium metal may include: a PVD system such as an electron beam evaporator, a film delivery system (including a large area pattern printing system such as a gravure system), a lithium film delivery system (e.g., using an optional release layer between lithium and the negative electrode to press lithium to the negative electrode), or a slot deposition system. In some embodiments, the chamber for depositing the protective film on the lithium metal film may include: a chamber for depositing an interlayer film or a chamber for depositing a lithium ion conductive polymer on the lithium metal film. The integrated processing tool may further include: a chamber for removing the interlayer film before additional processing. In some embodiments, the integrated processing tool further includes: a chamber for forming the negative electrode material on a continuous material sheet. In some embodiments, the continuous material sheet is a flexible conductive substrate.

[0012] In another embodiment, a method for forming a negative electrode is provided, the method comprising the following steps: forming a lithium metal film on the negative electrode, forming an interface film on the lithium metal film, and forming a protective film on the interface film, wherein the interface film is a release film, a metal fluoride film, or a metal oxide film. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] The manner in which the above-described detailed features of the disclosure briefly summarized above can be specifically understood, as well as a more particular description of the embodiments, can be obtained by reference to the embodiments, some of which are illustrated in the accompanying drawings. However, it should be noted that the drawings illustrate only typical embodiments of this disclosure and are not to be considered as limiting the scope of the disclosure, as the disclosure may admit to other equally effective embodiments.

[0014] Figure 1A Illustrated is a cross-sectional view of one embodiment of an electrode structure formed according to embodiments described herein.

[0015] Figure 1B A cross-sectional view of a bi-sided negative electrode structure formed according to embodiments described herein is shown.

[0016] Figure 2A schematic diagram illustrating an integrated processing tool according to embodiments described herein.

[0017] Figure 3 The illustration is a flow chart outlining one embodiment of a method for forming an electrode structure according to embodiments described herein.

[0018] Figure 4A A schematic diagram illustrates another integrated processing tool according to embodiments described herein.

[0019] Figure 4B A schematic diagram illustrates another integrated processing tool according to embodiments described herein.

[0020] Figure 5 The illustration is a flow chart outlining one embodiment of a method for forming an electrode structure according to embodiments described herein.

[0021] Figure 6 a schematic diagram illustrating another integrated processing tool according to embodiments described herein; and

[0022] Figure 7 A schematic diagram illustrates yet another integrated processing tool according to embodiments described herein.

[0023] To facilitate understanding, identical reference numerals have been used, where possible, to designate identical elements that are common to the figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further description. DETAILED DESCRIPTION

[0024] The following disclosure describes the negative electrode, the high performance electrochemical cell and battery including the aforementioned negative electrode, and the method for making the aforementioned negative electrode and the high performance electrochemical cell and battery including the aforementioned negative electrode. Figure 7 Certain details are set forth in order to provide a thorough understanding of the various embodiments of the present disclosure. Other details describing well-known structures and systems often associated with electrochemical cells and batteries are not set forth in the subsequent disclosure to avoid unnecessarily obscuring the description of the various embodiments.

[0025] Many of the details, dimensions, angles, and other features shown in the drawings are merely examples of specific embodiments. Therefore, other embodiments may have other details, components, dimensions, angles, and features without departing from the spirit or scope of the present disclosure. In addition, further embodiments of the present disclosure may be implemented without certain details described below.

[0026] The embodiments described herein will be referred to later in the text as roll-to-roll coating systems (e.g., TopMet TM、SmartWeb TM 、TopBeam TM ), all of which are available from Applied Materials, Inc. of Santa Clara, California. Other tools capable of performing high rate evaporation processes may also be adapted to benefit from the embodiments described herein. In addition, any system that facilitates the high rate evaporation procedures described herein may be advantageously used. The apparatus described herein is exemplary and should not be understood or construed as limiting the scope of the embodiments described herein. It should also be understood that although described as a roll-to-roll process, the embodiments described herein may also be performed on separate substrates.

[0027] Energy storage devices (e.g., batteries) typically include a positive electrode, a negative electrode separated by a porous separator and an electrolyte, which is used as an ion-conducting matrix. Graphite anodes are the latest technology, but the industry is moving away from graphite-based anodes toward hybrid silicon graphite anodes to increase battery energy density. However, hybrid silicon graphite anodes often have the disadvantage of irreversible capacitance loss that occurs during the first charge and discharge. Therefore, a method for compensating for this first charge and discharge capacitance loss is needed.

[0028] Deposition of lithium metal is one such method for compensating for the capacity loss of this first charge and discharge of the hybrid silicon graphite anode. Although there are many methods for lithium metal deposition (e.g., thermal evaporation, lamination, printing, etc.), the problem of handling lithium metal deposited on a roll before device stacking needs to be solved (especially in a high-volume manufacturing environment). In one embodiment, a method and system for forming an interleaf on a lithium metal film is provided. In another embodiment, a method and system for lithium polymer deposition is provided. In yet another embodiment, an integrated tool for both lithium metal deposition and ion conductive polymer deposition is provided.

[0029] Using the embodiments described herein, the deposited lithium metal (single or double sided) can be protected during winding and unwinding of downstream reels. Depositing a thin film of Li ion conductive polymer, ion conductive ceramic, or ion conductive glass is helpful in several aspects. First, a reel containing an electrode of lithium metal can be wound / unwound without the lithium metal contacting the adjacent electrode. Second, a stable solid electrolyte interface (SEI) is established to achieve better battery performance and high electrochemical utilization of lithium metal. In addition, the use of a protective film reduces the complexity of the manufacturing system and is compatible with current manufacturing systems.

[0030] Figure 1A An example lithium ion energy storage device 100 having a lithium metal film formed according to an embodiment of the present disclosure is illustrated. The lithium ion energy storage device 100 has a positive current collector 110, a positive electrode 120, a separator 130, a negative electrode 140, a lithium metal film 145, an optional interface film 147 (with an optional protective film 170 formed thereon), and a negative current collector 150. Note that in FIG. 1 , the current collector is shown as extending beyond the stack, although it is not necessary for the current collector to extend beyond the stack, and the portion extending beyond the stack may serve as tabs.

[0031] The current collectors 110, 150, respectively located on the positive electrode 120 and the negative electrode 140, may be the same or different electrical conductors. Examples of metals that the current collectors 110, 150 may include include aluminum (Al), copper (Cu), zinc (Zn), nickel (Ni), cobalt (Co), tin (Sn), silicon (Si), manganese (Mn), magnesium (Mg), alloys thereof, and combinations thereof. In one embodiment, at least one of the current collectors 110, 150 is perforated. In addition, the current collectors may have any outer dimensions (e.g., metal foil, sheet, or plate), shape, and microstructure / macrostructure. Generally speaking, in prismatic batteries, the tabs are formed of the same material as the current collectors and may be formed during the manufacture of the stack (or added later). All components except the current collectors 110 and 150 contain an electrolyte of lithium ions.

[0032] The negative electrode 140 or anode can be any material that is compatible with the positive electrode 120. The negative electrode 140 can have an energy capacity greater than or equal to 372 mAh / g, preferably an energy capacity of ≥700 mAh / g, and most preferably an energy capacity of ≥1000 mAh / g. The negative electrode 140 can be constructed from graphite, graphite containing silicon, lithium metal, lithium metal foil or lithium alloy foil (e.g., aluminum-lithium alloy), or a mixture of lithium metal and / or lithium alloy and materials such as carbon (e.g., coke, graphite), nickel, copper, tin, indium, silicon, oxides of the above, or combinations thereof. The negative electrode 140 typically comprises: intercalation compounds containing lithium or insertion compounds containing lithium. In some embodiments, where the negative electrode 140 comprises lithium metal, the lithium metal can be deposited using the methods described herein.

[0033] In some embodiments, a lithium metal film 145 is formed on the negative electrode 140. The lithium metal film 145 may be formed according to the embodiments described herein. In some embodiments, the negative electrode 140 is a silicon graphite anode having a lithium metal film 145, which is formed on the silicon graphite anode. The lithium metal film 145 compensates for the lithium loss (lithium lost) of the capacity loss from the first charge and discharge of the negative electrode 140. The lithium metal film may be a thin lithium metal film (e.g., 20 microns or less, from about 1 micron to about 20 microns, from about 2 microns to about 10 microns). In some embodiments where the lithium metal film 145 acts as a negative electrode, the lithium metal film 145 replaces the negative electrode 140. In some embodiments where the lithium metal film 145 acts as a negative electrode, the lithium metal film 145 is formed on the current collector 150.

[0034] In some embodiments, the protective film 170 is formed on the lithium metal film 145. The protective film 170 may be an ion conductive polymer. The protective film 170 may be porous. In some embodiments, the protective film 170 has nanopores. In one embodiment, the protective film 170 has a plurality of nanopores whose sizes are adjusted to have an average pore size or diameter of less than about 10 nanometers (e.g., from about 1 nanometer to about 10 nanometers; from about 3 nanometers to about 5 nanometers). In another embodiment, the protective film 170 has a plurality of nanopores whose sizes are adjusted to have an average pore size or diameter of less than about 5 nanometers. In one embodiment, the protective film 170 has a plurality of nanopores whose diameters range from about 1 nanometer to about 20 nanometers (e.g., from about 2 nanometers to about 15 nanometers; or from about 5 nanometers to about 10 nanometers).

[0035] The protective film 170 may be a coating or a separation layer, either of which has a thickness in the range of 1 nm to 2,000 nm (e.g., in the range of 10 nm to 600 nm; in the range of 50 nm to 200 nm; in the range of 100 nm to 150 nm). The protective film 170 may be a separation membrane having a thickness in the range of 5 μm to 50 μm (e.g., in the range of 6 μm to 25 μm). In some embodiments where the protective film 170 is an interlayer film, the protective film 170 acts as a separator and replaces the separator 130.

[0036] Examples of polymers that can be used to form the protective film 170 include, but are not limited to, polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), poly-acrylonitrile (PAN), carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), ionic liquids, and combinations thereof. Without being bound by theory, it is believed that the protective film 170 can form a colloid with the Li-conductive electrolyte during device manufacturing, which is beneficial for forming a good solid electrolyte interface (SEI) and also helps to reduce resistance. The protective film 170 can be formed by dipping coating, slit coating, gravure coating, or printing. The protective film 170 can also be deposited using a Metacoat device.

[0037] The protective film 170 may be a lithium ion conductive material. The lithium ion conductive material may be a lithium ion conductive ceramic or a lithium ion conductive glass. The lithium ion conductive material may be composed of one or more of the following: LiPON, crystalline or amorphous Li7La3Zr2O 12 doped variants, doped anti-perovskite compositions, Li2S-P2S5, Li 10 GeP2S 12 , and Li3PS4, lithium phosphate glasses, (1-x)LiI-(x)Li4SnS4, xLiI-(1-x)Li4SnS4, mixed sulfide and oxide electrolytes (crystalline LLZO, amorphous (1-x)LiI-(x)Li4SnS4 mixtures, and amorphous xLiI-(1-x)Li4SnS4). In one embodiment, x is between 0 and 1 (e.g., 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, and 0.9). The lithium ion conductive metal can be deposited directly on the lithium metal film using (or by) physical vapor deposition (PVD), chemical vapor deposition (CVD), spraying, doctor blade, printing, or any number of coating methods. A suitable method for some embodiments is PVD. In some embodiments, the protective membrane 170 need not be ionically conductive, however, once filled with an electrolyte (liquid, gel, solid, combination, etc.), the porous substrate and electrolyte combination may be ionically conductive.

[0038] In one embodiment, the protective film is a lithium-ion conductive material and the lithium-ion conductive material is selected from the group consisting of: LiPON, crystalline or amorphous garnet-type Li7La3Zr2O 12 , LISICON (e.g., Li 2+ 2x Zn 1-x GeO4, where 0 < x < 1), NASICON (e.g., Na 1+x Zr2Si x P3-xO 12 , where 0 < x < 3), lithium borohydride (LiBH4), doped anti-perovskite compositions, lithium-containing sulfides (e.g., Li2S, Li2S-P2S5, Li 10 GeP2S 12 , and Li3PS4), and lithium argyrodites (e.g., LiPS5X, where x is Cl, Br, or I).

[0039] The protective film 170 may be an interlayer film. The interlayer film may include thermoplastics (e.g., polyethylene, polypropylene, poly(ethyleneterephthalate), poly(butylene terephthalate), polyester, polyamide, polyaramid, polyacrylate, polycarbonate, poly(ester carbonate), polybenzimidazole, polyimide, polyether imide, polyamide imide, and the like). In some embodiments, the interlayer film is selected from the group consisting of polyethylene, polypropylene, poly(ethylene terephthalate), poly(butylene terephthalate), polyester, polyamide, polyaramid, polyacrylate, polycarbonate, poly(ester carbonate), polybenzimidazole, polyimide, polyether imide, polyamide imide, and combinations thereof.

[0040] In some embodiments, the interface film 147 is formed between the protective film 170 and the lithium metal film 145. In some embodiments, the interface film 147 has a thickness from about 0.1 micrometers to about 5.0 micrometers (e.g., in a range of about 1 micrometer to about 4 micrometers; or in a range of about 2 micrometers to about 3 micrometers). The interface film 147 is generally thin enough to conduct ions.

[0041] In some embodiments where the protective film 170 is an interlayer film, the interface film 147 includes a release agent. The release agent helps to improve the removal of the protective film 170 from the lithium metal film 145. The release agent can be a silicon-containing compound, polyolefin, polyfluorocarbon, polyamide, polyester, polycarbonate, polyurethane, polystyrene, polycaprolactone, and mixtures and copolymers thereof. The interface film 147 including the release agent is formed by roll coating, spray coating, gravure coating, slot coating, or other similar methods. In some embodiments, the interface film 147 is selected from the group consisting of polyolefin, polyfluorocarbon, polyamide, polyester, polycarbonate, polyurethane, polystyrene, polycaprolactone, and mixtures and copolymers thereof. In some embodiments, the interface film 147 including a release agent is formed on the protective film 170 before forming the lithium ion energy storage device 100.

[0042] In some embodiments where the protective film 170 is a lithium ion conductive film, the interface film 147 improves the stability of the lithium metal film 145 for the protective film 170. In some embodiments, the interface film 147 is a metal oxide film. The metal oxide film may be: Al2O3, LiAlO2, LiAl5O8, ZrO2, Li2ZrO3, Li2O, Li2S, and mixtures thereof. In some embodiments, the interface film 147 is a lithium-containing metal fluoride film (e.g., LiF). In some embodiments, the interface film is selected from the group consisting of: LiF, Al2O3, LiAlO2, LiAl5O8, ZrO2, Li2ZrO3, Li2O, and mixtures thereof. The interface film 147 (comprising a metal oxide film or a lithium fluoride film) may be formed by evaporation, roll coating, spray coating, gravure coating, slot coating, or other similar methods. In some embodiments, before forming the lithium ion energy storage device 100 , the interface film 147 including a metal oxide film is formed on the protective film 170 .

[0043] The positive electrode 120 or cathode may be any material that is compatible with the anode and may include: an intercalation compound, an insertion compound, or an electrochemically active polymer. Suitable intercalation materials include, for example, lithium-containing metal oxides, MoS2, FeS2, MnO2, TiS2, NbSe3, LiCoO2, LiNiO2, LiMnO2, LiMn2O4, V6O 13 , and V2O5. Suitable polymers include, for example, polyacetylene, polypyrrole, polyaniline, and polythiopene. The positive electrode 120 or cathode may be made of a layered oxide, for example, lithium cobalt oxide, olivine (e.g., lithium iron phosphate), or spinel (e.g., lithium manganese oxide). Exemplary lithium-containing oxides may be layered, such as lithium cobalt oxide (LiCoO2), or mixed metal oxides, such as LiNi x Co 1-2x MnO2, LiNiMnCoO2 (“NMC”), LiNi 0.5 Mn 1.5 O4、Li(Ni 0.8 Co 0.15 Al 0.05 )O2, LiMn2O4, and doped lithium-rich layered-layered materials, wherein x is 0 or a non-zero number. Exemplary phosphates may be iron olivine (LiFePO4) and its variants (e.g., LiFe (1-x) Mg x PO4), LiMoPO4, LiCoPO4, LiNiPO4, Li3V2(PO4)3, LiVOPO4, LiMP2O7, or LiFe 1.5 P2O7, wherein x is zero or a non-zero number. Exemplary fluorophosphates may be: LiVPO4F, LiAlPO4F, Li5V(PO4)2F2, Li5Cr(PO4)2F2, Li2CoPO4F, or Li2NiPO4F. Exemplary silicates may be: Li2FeSiO4, Li2MnSiO4, or Li2VOSiO4. An exemplary non-lithium compound is Na5V2(PO4)2F3.

[0044] In some embodiments of lithium-ion batteries according to the present disclosure, lithium is contained in atomic layers of a crystal structure of, for example, carbon graphite (LiC6) at the negative electrode and lithium manganese oxide (LiMnO4) or lithium cobalt oxide (LiCoO2) at the positive electrode, although in some embodiments, the negative electrode may also contain lithium absorbing materials, such as silicon, tin, etc. Even though the wound layer stack is shown as a planar structure, the battery can be formed into a cylinder from the wound layer stack; in addition, other battery configurations (e.g., square batteries, button cells) can be formed.

[0045] The electrolyte impregnated in the battery elements 120, 130, 140, 147, 145, and 170 may be composed of a liquid / gel or a solid polymer, and may be different in each battery element 120, 130, 140, 147, 145, and 170. In some embodiments, the electrolyte mainly includes: a salt and a medium (e.g.: in a liquid electrolyte, the medium may be called a solvent; in a gel electrolyte, the medium may be: a polymer matrix). The salt may be a lithium salt. The lithium salt may include, for example, LiPF6, LiAsF6, LiCF3SO3, LiN(CF3SO3)3, LiBF6, and LiClO4, BETTE electrolyte (commercially available from 3M Corp. of Minneapolis, MN) and combinations thereof. The solvent may include, for example, ethylene carbonate (EC), propylene carbonate (PC), EC / PC 2-MeTHF (2-methyltetrahydrofuran) / EC / PC, EC / DMC (dimethylcarbonate), EC / DME (dimethyl ethane), EC / DEC (diethylcarbonate), EC / EMC (ethyl methyl carbonate), EC / EMC / DMC / DEC, EC / EMC / DMC / DEC / PE, PC / DME, and DME / PC. The polymer matrix may include, for example, PVDF (polyvinylidene fluoride), PVDF:THF (PVDF: tetrahydrofuran), PVDF:CTFE (PVDF: chlorotrifluoroethylene), PAN (polyacrylonitrile), and PEO (polyethylene oxide).

[0046] Figure 1B An example of a negative electrode unit 160 is shown, which can be combined with a positive electrode unit to form a lithium ion energy storage device. The negative electrode unit 160 has a lithium metal film 145a, a lithium metal film 145b, and the lithium metal film 145a has a protective film 170a formed thereon according to an embodiment of the present disclosure, and the lithium metal film 145b has a protective film 170b formed thereon according to an embodiment of the present disclosure. In some embodiments, an interface film 147a is formed between the lithium metal film 145a and the protective film 170a, and an interface film 147b is formed between the lithium metal film 145b and the protective film 170b. The lithium metal films 145a, 145b can be thin lithium metal films (e.g., 20 microns or less, from about 1 micron to about 20 microns, from about 2 microns to about 10 microns). The protective films 170a, 170b can be interlayer films or ion-conductive polymer films described herein. The interface film 147a, 147b may include a release agent or a metal oxide as previously described herein. In some embodiments where the protective film 170a, 170b is an interlayer film, the interlayer film is typically removed before the negative electrode unit 160 is combined with the positive electrode unit to form a lithium ion storage device. In some embodiments where the protective film 170a, 170b is an ion-conducting polymer film, the ion-conducting polymer film is incorporated into the final battery structure.

[0047] The negative electrode unit 160 has a negative current collector 150, negative electrodes 140a, 140b formed on the negative current collector 150, lithium metal films 145a, 145b formed on the negative electrodes 140a, 140b, and protective films 170a, 170b formed on the lithium metal films 145a, 145b. Although the negative electrode unit 160 is depicted as a double-sided unit, it should be understood that the embodiments described herein also apply to single-sided units.

[0048] The negative electrode unit can be manufactured using the tools of the present disclosure described herein. According to some embodiments, the coil tool for forming the negative electrode coated with lithium may include: a roll-to-roll system for conveying a substrate or a current collector through the following chambers: a chamber for depositing the negative electrode on the current collector, a chamber for depositing a thin film of lithium on the negative electrode, and a chamber for depositing a protective film on the thin film of lithium. The chamber for depositing the thin film of lithium may include: an evaporation system such as an electron beam evaporator, a thermal evaporator, or a thin film conveying system (including a large area pattern printing system such as a gravure printing system).

[0049] In some embodiments, the tool may further include: a chamber for surface modification of the continuous material sheet prior to deposition of the lithium thin film and protective film (e.g., a plasma pre-treatment chamber). Furthermore, in some embodiments, the tool may further include: a chamber for depositing a binder soluble in the liquid electrolyte or lithium ion conductive dielectric material.

[0050] According to some embodiments, Figure 1B The negative electrode unit 160 can be manufactured using the processes and equipment described below. Some configurations of the coil tool for manufacturing the negative electrode unit 160 according to the present disclosure are schematically shown in Figure 2 , Figure 4A , Figure 4B , Figure 6 ,and Figure 7 It should be noted that these figures are schematic representations and it should be understood that the configuration of the web system and chamber may be varied as desired to control different manufacturing processes.

[0051] Figure 2 A schematic diagram of an integrated processing tool 200 according to embodiments described herein is illustrated. In certain embodiments, the integrated processing tool 200 includes: a plurality of processing modules or chambers 220 and 230 arranged in a line, each of which is configured to perform processing operations on a continuous material sheet 210. In one embodiment, the processing chamber 220 and the processing chamber 230 are independent modular processing chambers, wherein each modular processing chamber is structurally separated from the other modular processing chambers. Thus, each modular processing chamber in the independent modular processing chambers can be independently arranged, rearranged, replaced, or maintained without affecting each other. In certain embodiments, the processing chamber 220 and the processing chamber 230 are configured to process two sides of the continuous material sheet 210. Although the integrated processing tool 200 is configured to process a vertically oriented continuous material sheet 210, the integrated processing tool 200 can be configured to process substrates arranged in different orientations (e.g., a horizontally oriented continuous material sheet 210). In certain embodiments, the continuous material sheet 210 is a flexible conductive substrate.

[0052] In certain embodiments, the integrated processing tool 200 includes: a conveyor mechanism 205. The conveyor mechanism 205 may include: any conveyor mechanism capable of moving a continuous material sheet 210 through the processing areas of the processing chamber 220 and the processing chamber 230. The conveyor mechanism 205 may include a common conveyor architecture. The common conveyor architecture may include a roll-to-roll system having a common take-up reel 214 and a feed reel 212 for the system. The take-up reel 214 and the feed reel 212 may be heated separately. The take-up reel 214 and the feed reel 212 may be heated separately using an external heat source or an internal heat source disposed within each reel. The common conveyor architecture may further include one or more intermediate conveyor reels (213a & 213b, 216a & 216b, 218a & 218b) disposed between the take-up reel 214 and the feed reel 212. Although the integrated processing tool 200 is depicted as having a single processing area, in certain embodiments, it may be advantageous to have independent or separate processing areas, modules, or chambers for each processing step. For embodiments having separate processing areas, modules, or chambers, a common transport architecture may be a roll-to-roll system in which each chamber or processing area has a separate take-up reel and supply reel, and one or more optional intermediate transport reels disposed between the take-up reel and the supply reel. The common transport architecture may include a track system. The track system extends through the processing area or the separate processing areas. The track system is configured to transport a web substrate or a separate substrate.

[0053] The integrated processing tool 200 may include a supply reel 212 and a take-up reel 214 for moving a continuous material sheet 210 through different processing chambers; a first processing chamber 220 for depositing a lithium metal film and a second processing chamber 230 for forming a protective coating over the lithium metal film to protect the lithium metal film from the surrounding oxidants. In some embodiments, the finished negative electrode will not be collected on the take-up reel 214, as shown in the figure, but directly integrated with a separator and a positive electrode, etc. to form a battery cell.

[0054] The first processing chamber 220 is configured to deposit a thin film of lithium metal on the continuous material sheet 210. Any suitable lithium deposition process for depositing a thin film of lithium metal can be used to deposit the thin film of lithium metal. The thin film of lithium metal can be deposited by a PVD process (e.g., evaporation, slot process, conveyor process, lamination process, or three-dimensional lithium printing process). The chamber for depositing a thin film of lithium metal can include a PVD system such as an electron beam evaporator, a thin film conveyor system (including a large area pattern printing system such as a gravure printing system), a lamination system, or a slot deposition system.

[0055] In one embodiment, the first processing chamber 220 is an evaporation chamber. The evaporation chamber has a processing area 242, which is shown as including evaporation sources 244a, 244b (collectively 244) that can be placed in a crucible, wherein the evaporation sources 244a, 244b can be thermal evaporators or electron beam evaporators (cold) in a vacuum environment.

[0056] The second processing chamber 230 is configured to form a protective film on the lithium metal film. The protective film may be an ion conductive material as described herein. The protective film may be formed by dip coating, slot coating, gravure coating, lamination, or printing.

[0057] In one embodiment, the second processing chamber 230 is a three-dimensional printing chamber. The printing chamber has a processing area 252, which is shown as including printing sources 254a, 254b (collectively 254) for printing polymer ink.

[0058] In one embodiment, the processing region 242 and the processing region 252 are maintained under vacuum conditions and / or at a pressure below atmospheric pressure during processing. The vacuum level of the processing region 242 can be adjusted to match the vacuum level of the processing region 252. In one embodiment, the processing region 242 and the processing region 252 are maintained at atmospheric pressure during processing. In one embodiment, the processing region 242 and the processing region 252 are maintained under an inert gas environment during processing. In one embodiment, the inert gas environment is an argon environment. In one embodiment, the inert gas environment is a nitrogen (N2) environment.

[0059] Figure 3The diagram summarizes a flow chart of one embodiment of a method 300 for forming an electrode structure according to embodiments described herein. At operation 310, a substrate is provided. The substrate may be a continuous sheet of material 210. The substrate may have a negative electrode material formed thereon. The negative electrode material may be a negative electrode 140. At operation 320, a lithium metal film is formed. The lithium metal film may be a lithium metal film 145. If a negative electrode material is present, the lithium metal film is formed on the negative electrode. If the negative electrode 140 is not present, the lithium metal film may be formed directly on the substrate. The lithium metal film may be formed in the first processing chamber 220. Optionally, at operation 325, an interface film 147 is formed on the lithium metal film 145. At operation 330, a protective film is formed on the lithium metal film 145 or on the interface film 147. The protective film may be a protective film 170. The protective film may be an ion conductive polymer. The protective film may be formed in the second processing chamber 230. At operation 340, the substrate with the lithium metal film and the protective film may be optionally stored, transferred to another tool, or stored and transferred to another tool at the same time. At operation 350, the substrate with the lithium metal film and the protective film formed on the substrate is subjected to additional processing.

[0060] FIG. 4 illustrates a schematic diagram of another integrated processing tool 400 according to embodiments described herein. The integrated processing tool 400 is similar to the integrated processing tool 200 except that the integrated processing tool 400 is configured to deposit an interlayer film 430 on a lithium metal film. In certain embodiments, the integrated processing tool 400 includes a first processing chamber 420 configured to perform processing operations on a continuous material sheet 210. The first processing chamber 420 is configured to deposit a thin film of lithium metal on a continuous material sheet 210. The first processing chamber 420 is further configured to deposit an interlayer film 430a, 430b (collectively 430) on the lithium metal film for protecting the lithium metal film from the surrounding oxidants. Although the first processing chamber 420 includes both the lithium metal film deposition equipment and the interlayer film, it should be understood that the lithium metal film and the interlayer film can be deposited in separate independent modular processing chambers.

[0061] In some embodiments, the first processing chamber 420 is configured to process both sides of the continuous material sheet 210. Although the integrated processing tool 400 is configured to process a vertically oriented continuous material sheet 210, the integrated processing tool 400 can be configured to process substrates arranged in different orientations (e.g., a horizontally oriented continuous material sheet 210). In some embodiments, the continuous material sheet 210 is a flexible conductive substrate.

[0062] In certain embodiments, the integrated processing tool 400 includes a conveyor mechanism 205. The conveyor mechanism 205 may include any conveyor mechanism capable of moving a continuous sheet of material 210 through a processing area of ​​the first processing chamber 420. The conveyor mechanism 205 may include a common conveyor architecture. The common conveyor architecture may include a roll-to-roll system having a common take-up reel 214 and a supply reel 212 for the system. The take-up reel 214 and the supply reel 212 may be heated separately. The take-up reel 214 and the supply reel 212 may be heated separately using an external heat source or an internal heat source disposed within each reel. The conveyor mechanism 205 may further include one or more intermediate conveyor reels (413a and 413b, 416a and 416b, 418a and 418b) disposed between the take-up reel 214 and the supply reel 212. In some embodiments, the intermediate conveyor reels 418a, 418b laminate the interlayer film to the lithium metal film. In some embodiments, the intermediate transfer reels 418a, 418b laminate the interlayer film to the lithium metal film. In some embodiments, the intermediate transfer reels 418a, 418b are heated.

[0063] Although the integrated processing tool 400 is depicted as having a single processing area, in certain embodiments, it may be advantageous to have independent or separate processing areas, modules, or chambers for each processing operation. For embodiments with separate processing areas, modules, or chambers, the common transport architecture may be a roll-to-roll system in which each chamber or processing area has a separate take-up reel and supply reel, and one or more optional intermediate transport reels disposed between the take-up reel and the supply reel. The common transport architecture may include a track system. The track system extends through the processing area or the separate processing area. The track system is configured to transport the coiled substrate or the separate substrate.

[0064] The first processing chamber 420 is configured to deposit a thin film of lithium metal on the continuous material sheet 210. Any suitable lithium deposition process for depositing a thin film of lithium metal can be used to deposit the thin film of lithium metal. The thin film of lithium metal can be deposited by a PVD process (e.g., evaporation, a slot process, a conveyor process, or a three-dimensional lithium printing process). The chamber for depositing a thin film of lithium metal may include a PVD system such as an electron beam evaporator, a thin film conveyor system (including a large area pattern printing system such as a gravure printing system), or a slot deposition system.

[0065] In one embodiment, the first processing chamber 420 is an evaporation chamber. The evaporation chamber has a processing area 442, which is shown to include evaporation sources 444a and 444b (collectively 444) that can be placed in a crucible. For example, the evaporation sources 444a and 444b can be thermal evaporators or electron beam evaporators (cold type) in a vacuum environment.

[0066] The first processing chamber 420 is further configured to deposit an interlayer film 430 on the lithium metal film.

[0067] In one embodiment, the processing region 442 is maintained under vacuum conditions and / or at a pressure below atmospheric pressure during processing. In one embodiment, the processing region 442 is maintained under an inert gas environment during processing. In one embodiment, the inert gas environment is an argon environment. In one embodiment, the inert gas environment is a nitrogen (N2) environment.

[0068] Figure 4B A schematic diagram of another integrated processing tool 450 according to embodiments described herein is illustrated. In certain embodiments, the integrated processing tool 450 includes a plurality of processing modules or processing chambers 460 and 470 arranged in a line, each of which is configured to perform processing operations on a continuous material sheet 210. In one embodiment, the processing chamber 460 and the processing chamber 470 are independent modular processing chambers, wherein each modular processing chamber is structurally separated from the other modular processing chambers. Therefore, each modular processing chamber of the independent modular processing chambers can be independently arranged, rearranged, replaced, or maintained without affecting each other. In certain embodiments, the processing chamber 460 and the processing chamber 470 are configured to process two sides of the continuous material sheet 210. Although the integrated processing tool 450 is configured to process a horizontally oriented continuous material sheet 210, the integrated processing tool 450 can be configured to process substrates arranged in different orientations (e.g., a horizontally oriented continuous material sheet 210). In certain embodiments, the continuous material sheet 210 is a flexible conductive substrate.

[0069] In certain embodiments, the integrated processing tool 450 includes a conveyor mechanism 205. The conveyor mechanism 205 may include any conveyor mechanism capable of moving a continuous sheet of material 210 through the processing areas of the processing chamber 460 and the processing chamber 470. The conveyor mechanism 205 may include a common conveyor architecture. The common conveyor architecture may include a roll-to-roll system having a common take-up reel 214 and a supply reel 212 for the system. The take-up reel 214 and the supply reel 212 may be heated separately. The take-up reel 214 and the supply reel 212 may be heated separately using an external heat source or an internal heat source disposed within each reel. The common conveyor architecture may further include one or more intermediate conveyor reels (473a and 473b, 476a and 476b, 478a and 478b) disposed between the take-up reel 214 and the supply reel 212.

[0070] Although the integrated processing tool 200 is depicted as having two separate processing areas, in certain embodiments, it may be advantageous to have a common processing area. For embodiments having separate processing areas, modules, or chambers, a common transport architecture may be a roll-to-roll system in which each chamber or processing area has a separate take-up reel and supply reel, and one or more optional intermediate transport reels disposed between the take-up reel and the supply reel. The common transport architecture may include a track system. The track system extends through the processing areas or the separate processing areas. The track system is configured to transport the web substrate or the separate substrate.

[0071] The integrated processing tool 200 may include: a supply reel 212 and a take-up reel 214 for moving a continuous material sheet 210 through different processing chambers; a first processing chamber 460, which is used to remove the interlayer film from the negative electrode; and a second processing chamber 470, which is used to perform additional processing on the negative electrode. In one embodiment, the intermediate conveying reels 473a and 473b are configured to remove the interlayer film from the continuous material sheet 210. In some embodiments, the completed negative electrode will not be collected on the take-up reel 214, as shown in the figure, but directly integrated with the separator and positive electrode, etc. to form a battery cell.

[0072] The first processing chamber 460 is configured to remove the interlayer film 430 from the continuous material sheet 210. The first processing chamber includes a processing area 462 and at least one set of intermediate transfer reels 473a, 473b for removing the interlayer film prior to additional processing.

[0073] The second processing chamber 470 is configured for additional processing of the continuous material sheet 210. The second processing chamber includes a processing area 472.

[0074] In one embodiment, the processing region 462 and the processing region 472 are maintained under vacuum conditions and / or at a pressure below atmospheric pressure during processing. The vacuum level of the processing region 462 can be adjusted to match the vacuum level of the processing region 472. In one embodiment, the processing region 462 and the processing region 472 are maintained at atmospheric pressure during processing. In one embodiment, the processing region 462 and the processing region 472 are maintained under an inert gas environment during processing. In one embodiment, the inert gas environment is an argon environment. In one embodiment, the inert gas environment is a nitrogen (N2) environment. In one embodiment, at least one of the processing region 462 and the processing region 472 is maintained under vacuum conditions and / or at a pressure below atmospheric pressure during processing, while the other processing region is maintained at atmospheric pressure or maintained under an inert gas atmosphere.

[0075] Figure 5 The diagram summarizes a flow chart of one embodiment of a method 500 for forming an electrode structure according to an embodiment described herein. At operation 510, a substrate is provided. The substrate may be a continuous sheet of material 210. The substrate may have a negative electrode material formed thereon. The negative electrode material may be: a negative electrode 140. At operation 520, a lithium metal film is formed. If a negative electrode material is present, the lithium metal film is formed on the negative electrode material. If no negative electrode material is present, the lithium metal film may be formed directly on the substrate. The lithium metal film may be formed in a first processing chamber 420. The lithium metal film may be a lithium metal film 145. If a negative electrode material is present, the lithium metal film is formed on the negative electrode. At operation 530, an interlayer film is formed on the lithium metal film. The interlayer film may be formed on the lithium metal film in the first processing chamber 420. In some embodiments, the interlayer film may be formed on the lithium metal film in a separate processing chamber. At operation 540, the substrate with the lithium metal film and the interlayer film may be optionally stored, transferred to another tool, or both stored and transferred to another tool. At operation 550, the interlayer film is removed. At operation 560, the substrate with the lithium metal film is subjected to additional processing.

[0076] Figure 6A schematic diagram of another integrated processing tool 600 is illustrated according to an embodiment described herein. The integrated processing tool 600, for example, can be used to form a lithium-ion energy storage device 100 or a negative electrode unit 160. The integrated processing tool 600 is similar to the integrated processing tool 200, except that the integrated processing tool 600 is constructed to deposit a lithium metal film by a lamination process. The first processing chamber 220 of the integrated processing tool 200 is replaced by a lamination-processing chamber 620. The lamination-processing chamber 620 is constructed to deposit a thin film of lithium metal formed on the interlayer film. In one embodiment, an interface film (e.g., a release film) is formed between the lithium metal film and the interlayer film, as described herein. In addition, after the lithium metal film is laminated to the continuous material sheet 210, the lamination-processing chamber 620 is constructed to remove the interlayer film from the laminated metal film. If a release film is present, the release film generally helps to remove the interlayer film from the lithium metal film and can be removed together with the interlayer film. If the negative electrode is patterned, the continuous lamination layer is moved in a segmented semi-continuous manner to match the lamination of the patterned electrode.

[0077] In some embodiments, the lamination-processing chamber 620 is configured to process both sides of the continuous material sheet 210. Although the integrated processing tool 600 is configured to process a vertically oriented continuous material sheet 210, the integrated processing tool 600 can be configured to process substrates arranged in different orientations (e.g., a horizontally oriented continuous material sheet 210). In some embodiments, the continuous material sheet 210 is a flexible conductive substrate.

[0078] In certain embodiments, the integrated processing tool 600 includes a conveyor mechanism 205. The conveyor mechanism 205 may include any conveyor mechanism capable of moving a continuous sheet of material 210 through the processing area of ​​the lamination-processing chamber 620. The conveyor mechanism 205 may include a common conveying architecture. The common conveying architecture may include a roll-to-roll system having a common take-up reel 214 and a supply reel 212 for the system. The take-up reel 214 and the supply reel 212 may be heated separately. The take-up reel 214 and the supply reel 212 may be heated separately using an external heat source or an internal heat source disposed in each reel. The conveyor mechanism 205 may further include one or more intermediate conveying reels (613a and 613b, 616a and 616b, 618a and 618b) disposed between the take-up reel 214 and the supply reel 212.

[0079] Although the integrated processing tool 600 is depicted as having separate processing areas, in certain embodiments, it may be advantageous to have a common processing area. For embodiments having separate processing areas, modules, or chambers, a common transport architecture may be a roll-to-roll system in which each chamber or processing area has a separate take-up reel and supply reel, and one or more optional intermediate transport reels disposed between the take-up reel and the supply reel. The common transport architecture may include a track system. The track system extends through the processing area or the separate processing area. The track system is configured to transport the web substrate or the separate substrate.

[0080] The lamination-processing chamber 620 is configured to deposit a thin film of lithium metal on a continuous material sheet 210 via a lamination process. The lamination-processing chamber 620 includes lithium metal film / interlayer film supply rollers 630a, 630b for supplying lithium metal film / interlayer film 632a, 632b to the continuous material sheet 210. The lamination-processing chamber 620 further includes interlayer take-up reels 640a, 640b for collecting the removed interlayer film 634a, 634b. In some embodiments, the lamination-processing chamber 620 further includes optional pressure rollers 650a, 650b for applying pressure to the lithium metal film / interlayer film 632a, 632b to laminate the lithium metal film to the continuous material sheet 210. In some embodiments, the lithium metal film / interlayer film 632a, 632b further includes a release film formed between the lithium metal film 632a and the interlayer film 632b, as described herein. In some embodiments, the pressure rollers 650a, 650b are heated. In some embodiments where the pressure rollers 650a, 650b are not present, the intermediate transfer reels 616a, 616b laminate the lithium metal film / interlayer film 632a, 632b to the continuous material sheet 210. In some embodiments, the intermediate transfer reels 616a, 616b laminate the lithium metal film / interlayer film 632a, 632b to the continuous material sheet 210. In some embodiments, the intermediate transfer reels 616a, 616b are heated.

[0081] In one embodiment, the lamination-processing chamber 620 has a processing region 642. In some embodiments, the processing region 642 is maintained under vacuum conditions and / or at a pressure below atmospheric pressure during processing. In one embodiment, the processing region 642 is maintained under an inert gas environment during processing. In one embodiment, the inert gas environment is an argon environment. In one embodiment, the inert gas environment is a nitrogen (N2) environment.

[0082] In operation, when the continuous material sheet 210 moves between the supply reel 212 and the take-up reel 214, the lithium metal film / interlayer film supply rollers 630a, 630b supply lithium metal film / interlayer film 632a, 632b to the continuous material sheet 210. The lithium metal film / interlayer film supply rollers 630a, 630b supply lithium metal film / interlayer film 632a, 632b, and release film (if present) so that the lithium metal film contacts the continuous material sheet 210. Then, the lithium metal film is pressed by the pressure rollers 650a, 650b to laminate the lithium metal film to the continuous material sheet 210. After lamination, the interlayer film 634a, 634b is removed from the surface of the laminated lithium metal film by the conveying reels 616a, 616b. The removed interlayer film 634a, 634b is collected by the interlayer take-up reels 640a, 640b.

[0083] After laminating the lithium metal film to the continuous material sheet 210, the continuous material sheet moves to a second processing chamber 230 for optional additional processing.

[0084] Figure 7 A schematic diagram of yet another integrated processing tool 700 is illustrated according to some embodiments described herein. The integrated processing tool 700 can be used to form, for example, a lithium-ion energy storage device 100 or a negative electrode cell 160. The integrated processing tool 700 is similar to the integrated processing tool 600, except that the integrated processing tool 700 is configured to deposit a lithium metal film by a closed-loop lamination process. The lamination-processing chamber 620 of the integrated processing tool 600 is replaced by a closed-loop lamination-processing chamber 720. The closed-loop lamination-processing chamber 720 is configured to form a thin film of lithium metal on a continuous loop of interlayer films 734a, 734b, and then form a combined lithium metal film / interlayer film 732a, 732b. The continuous loop of interlayer films may also include a release film formed on the continuous loop of interlayer films. Furthermore, after laminating the lithium metal film to the continuous material sheet 210, the closed-loop lamination-processing chamber 720 is configured to remove the interlayer films 734a, 734b from the laminated metal layers.

[0085] In certain embodiments, the closed-loop lamination-processing chamber 720 is configured to process both sides of the continuous material sheet 210. Although the integrated processing tool 700 is configured to process a vertically oriented continuous material sheet 210, the integrated processing tool 700 can be configured to process substrates disposed in different orientations (e.g., a horizontally oriented continuous material sheet 210). In certain embodiments, the continuous material sheet 210 is a flexible conductive substrate.

[0086] In certain embodiments, the integrated processing tool 700 includes a conveyor mechanism 205. The conveyor mechanism 205 may include any conveyor mechanism capable of moving a continuous sheet of material 210 through a processing area of ​​a closed-loop lamination-processing chamber 720. The conveyor mechanism 205 may include a common conveyor architecture. The common conveyor architecture may include a roll-to-roll system having a common take-up reel 214 and a supply reel 212 for the system. The take-up reel 214 and the supply reel 212 may be heated individually. The take-up reel 214 and the supply reel 212 may be heated individually using an external heat source or an internal heat source disposed within each reel. The conveyor mechanism 205 may further include one or more intermediate conveyor reels (713a and 713b, 714a and 714b, 715a and 715b, 716a and 716b, 718a and 718b) disposed between the take-up reel 214 and the supply reel 212. The transport reels 713a and 713b, 714a and 714b, 715a and 715b, 716a and 716b form a closed loop along which the interlayer films 734a, 734b move.

[0087] The closed-loop lamination-processing chamber 720 further includes optional pressure rollers 750a, 750b for applying pressure to the lithium metal film / interlayer film 732a, 732b to laminate the lithium metal film to the continuous material sheet 210. In some embodiments, the pressure rollers 750a, 750b are heated. In some embodiments where the pressure rollers 750a, 750b are not present, the intermediate transfer reels 716a, 716b press the lithium metal film / interlayer film 732a, 732b onto the continuous material sheet 210. In some embodiments, the intermediate transfer reels 716a, 716b laminate the lithium metal film / interlayer film 732a, 732b onto the continuous material sheet 210. In some embodiments, the intermediate transfer reels 716a, 716b are heated.

[0088] In one embodiment, the closed loop lamination-processing chamber 720 defines a processing region 742. In some embodiments, the processing region 742 is maintained under vacuum conditions and / or at a pressure below atmospheric pressure during processing. In one embodiment, the processing region 742 is maintained under an inert gas environment during processing. In one embodiment, the inert gas environment is an argon environment. In one embodiment, the inert gas environment is a nitrogen (N2) environment.

[0089] The closed loop lamination-processing chamber 720 is further configured to deposit a thin film of lithium metal on the continuous material sheet 210. Any suitable lithium deposition process for depositing a thin film of lithium metal can be used to deposit the thin film of lithium metal. The thin film of lithium metal can be deposited by a PVD process (e.g., evaporation, slot process, transfer process, lamination process, or three-dimensional lithium printing process). The chamber for depositing a thin film of lithium metal can include a PVD system such as an electron beam evaporator, a thin film transfer system (including a large area pattern printing system such as a gravure printing system), a lamination system, or a slot deposition system.

[0090] In one embodiment, the closed-loop lamination-processing chamber 720 includes evaporation sources 744a and 744b (collectively 744) that can be placed in a crucible, for example, the evaporation sources 744a and 744b can be thermal evaporators or electron beam evaporators (cold type) in a vacuum environment. The evaporation source 744 deposits the lithium metal film on the interlayer films 734a and 734b to form the lithium metal film / interlayer films 732a and 732b.

[0091] In operation, when the interlayer films 734a, 734b move along the closed loop formed by the conveying reels 713a and 713b, 714a and 714b, 715a and 715b, 716a and 716b, the lithium metal film is deposited on the interlayer films 734a, 734b to form the lithium metal film / interlayer films 732a, 732b. When the continuous material sheet 210 moves between the supply reel 212 and the take-up reel 214, the lithium metal film / interlayer films 732a, 732b contact the continuous material sheet 210. Then, the lithium metal film is pressed by the pressing rollers 750a, 750b to laminate the lithium metal film to the continuous material sheet 210. After lamination, the interlayer films 734a, 734b are detached from the surface of the laminated lithium metal film and continue to move along the closed loop. The interlayer films 734a, 734b continue to move along the closed loop, wherein additional lithium metal films are formed on the interlayer films 734a, 734b.

[0092] After laminating the lithium metal film to the continuous material sheet 210, the continuous material sheet moves to a second processing chamber 230 for additional processing.

[0093] Additional chambers may be included in the integrated processing tool 200, the integrated processing tool 400, the integrated processing tool 600, or the integrated processing tool 700. In some embodiments, the additional chambers may provide for the deposition of separators, electrolyte soluble binders, or in some embodiments, the additional chambers may provide for the formation of positive electrodes. In some embodiments, the additional chambers provide for the cutting of negative electrodes. After the cutting of the negative electrodes is performed, the interlayer may be removed.

[0094] Although embodiments of the present disclosure have been described with specific reference to lithium-ion batteries with graphite negative electrodes, the teachings and principles of the present disclosure can be applied to other lithium-based batteries, such as Li-polymer, Li-S, Li-FeS2, Li metal-based batteries, etc. For Li metal-based batteries (e.g., Li-S and Li-FeS2), thicker Li metal electrodes may be required and the thickness of the Li metal depends on the loading of the positive electrode. In some embodiments, for Li-S, the Li metal electrode may have a thickness between 3 and 30 microns, and for Li-FeS2, the Li metal electrode may have a thickness of approximately 190 to 200 microns, and the Li metal electrode may be deposited on one or both sides of a compatible substrate (e.g., Cu or stainless steel foil) - the methods and tools described herein can be used to manufacture these Li metal electrodes.

[0095] In summary, some benefits of the present disclosure include: effectively integrating lithium metal deposition into currently available processing systems. Currently, lithium metal deposition is performed in a dry chamber or an argon environment. Due to the volatility of lithium metal, subsequent processing steps must also be performed in an argon environment. The execution of subsequent processing steps in an argon environment will require improvements to current manufacturing tools. The inventors have discovered that: coating the lithium metal with a protective film before subsequent processing allows subsequent processing to be performed under vacuum conditions or at atmospheric pressure. The protective film eliminates the need to perform additional processing operations in an inert gas environment, while reducing the complexity of the tool. The protective film also allows: the transport, storage, or both transport and storage of the negative electrode having a lithium metal film formed on the negative electrode. In addition, in an embodiment where the protective film is an ion conductive membrane, the ion conductive membrane can be incorporated into the final battery structure to reduce the complexity of the battery formation process. This will reduce the complexity of the tool and subsequently reduce the cost of ownership.

[0096] When introducing elements of the present disclosure, or exemplary aspects or embodiments of the disclosure, the articles “a,” “an,” “the,” and “said” are intended to mean that there are one or more of the elements.

[0097] The terms “comprising,” “including,” and “having” are intended to be inclusive and mean that there may be additional elements other than the listed elements.

[0098] While the foregoing is directed to embodiments of the present disclosure, other and further embodiments of the present disclosure may be devised without departing from the basic scope of the present disclosure, and the scope of the present disclosure is determined by the claims that follow.

Claims

1. A negative electrode, include: an anode made of graphite; a lithium metal film formed on the anode; A protective film formed on the lithium metal film; and an interface film formed between the lithium metal film and the protective film, wherein the protective film is a lithium ion conductive material or an interlayer film, the interlayer film comprises a thermoplastic, and When the protective film is the interlayer film, the interface film is a release film containing a release agent that helps improve the removal of the protective film from the lithium metal film, or when the protective film is the lithium ion conductive material, the interface film is a lithium-containing metal fluoride film or a metal oxide film.

2. The negative electrode according to claim 1, wherein When the protective film is the lithium ion conductive material, the interface film is selected from the group consisting of: LiF, Al 2 O 3 、LiAlO 2 、LiAl 5 O 8 、ZrO 2 , Li 2 ZrO 3 , Li 2 O, and mixtures thereof and When the protective film is the interlayer film, the interface film is selected from the group consisting of: silicon-containing compounds, polyolefins, polyfluorocarbons, polyamides, polyesters, polycarbonates, polyurethanes, polystyrene, polycaprolactone, and mixtures thereof. 3 . The negative electrode of claim 1 , wherein the interface film has a thickness of from 0.1 μm to 5 μm.

4. The negative electrode of claim 1, wherein the interface film is selected from the group consisting of: ZrO 2 , Li 2 ZrO 3 , and mixtures thereof.

5. The negative electrode of claim 1, wherein the interface film is selected from the group consisting of polyolefin, polyfluorocarbon, polyamide, polyester, polycarbonate, polyurethane, polystyrene, polycaprolactone, and mixtures and copolymers thereof. 6 . The negative electrode of claim 1 , wherein the lithium metal film has a thickness of from 1 micrometer to 20 micrometers.

7. The negative electrode according to claim 1, wherein the protective film is the lithium ion conductive material and the lithium ion conductive material is selected from the group consisting of: LiPON; crystalline or amorphous garnet-type Li 7 La 3 Zr 2 O 12 ; Li 2+2x Zn 1-x GeO 4 , where 0 < x < 1; Na 1+x Zr 2 SixP 3 -xO 12 , where 0 < x < 3; lithium borohydride (LiBH 4 ); doped anti-perovskite compositions; and LiPS 5 X, where x is Cl, Br, or I.

8. The negative electrode as claimed in claim 1, wherein the interlayer film is polypropylene.

9. A lithium ion battery incorporating the negative electrode of claim 1.

10. A method for forming a negative electrode, comprising the following steps: providing a substrate having a negative electrode material formed thereon, forming a lithium metal film on the negative electrode; forming an interface film on the lithium metal film; and forming a protective film on the interface film, wherein the protective film is a lithium ion conductive material or an interlayer film, and the interlayer film includes a thermoplastic plastic, When the protective film is the interlayer film, the interface film is a release film containing a release agent that helps improve the removal of the protective film from the lithium metal film, or when the protective film is the lithium ion conductive material, the interface film is a lithium-containing metal fluoride film or a metal oxide film.

11. The method of claim 10, further comprising the step of removing the interface film and the protective film from the lithium metal film.

12. The method according to claim 10 or 11, wherein the lithium metal film is stacked on the negative electrode.

13. The method of claim 10, wherein When the protective film is the lithium ion conductive material, the interface film is selected from the group consisting of: LiF, Al 2 O 3 、LiAlO 2 、LiAl 5 O 8 、ZrO 2 , Li 2 ZrO 3 , Li 2 O, and mixtures thereof, and When the protective film is the interlayer film, the interface film is selected from the group consisting of: silicon-containing compounds, polyolefins, polyfluorocarbons, polyamides, polyesters, polycarbonates, polyurethanes, polystyrene, polycaprolactone, and mixtures thereof.

Citation Information

Patent Citations

  • High-capacity metal lithium powder composite cathode and preparation method thereof, and multi-layer composite electrode

    CN102201565A

  • Passivation film for solid electrolyte interface of three dimensional copper containing electrode in energy storage device

    CN102449841A

  • Lithium battery protected from instrusion by pointed elements

    CN102906901A

  • Lithium ion battery film in situ preparation method, lithium ion battery film, and lithium ion battery

    CN103094513A

  • Rapidly charged flexible lithium ion battery and preparation method of electrodes of rapidly charged flexible lithium ion battery

    CN103682368A