Method for manufacturing grain-oriented electrical steel sheet
By controlling the composition of the slab and the content of Cu, Mn and other elements in the pickling solution during the manufacturing process of thin-walled oriented electromagnetic steel sheets, a 3d transition metal segregation layer is formed, and rapid heating and multiple soaking treatments are used to solve the problem of thin-walled oriented electrical steel sheets. Solve the problem of improving the magnetic properties of wall electromagnetic steel plates and achieve the optimization of magnetic flux density and iron loss.
Patent Information
- Application Number
- CN202180013282.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-06-24
- Filing Date
- 2021-06-23
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-06-23
AI Technical Summary
It is difficult to effectively improve the magnetic properties of thin-walled grain-oriented electromagnetic steel sheets with existing technology, especially by increasing the temperature rise rate during primary recrystallization annealing.
By controlling the composition of the slab and the content of Cu, Mn and other elements in the pickling solution during the manufacturing process of thin-walled electromagnetic steel plates, a 3d transition metal segregation layer is formed to stabilize the inhibitor, reduce gas permeability, and recrystallize in one step During annealing, a rapid temperature rise treatment is used, combined with multiple soaking treatments and nitriding treatments to ensure the thermal stability and magnetic properties of the inhibitor are optimized.
It achieves excellent magnetic properties of thin-walled oriented electromagnetic steel sheets, increases magnetic flux density and reduces iron loss, ensures the thermal stability of inhibitors, and is suitable for efficient manufacturing of oriented electromagnetic steel sheets with excellent magnetic properties.
Smart Images

Figure BDA0003786289060000191 
Figure BDA0003786289060000201
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a grain-oriented electromagnetic steel sheet. Background Art
[0002] Grain-oriented electrical steel sheets contain about 2 to 5 mass% of Si, and the orientation of the grains of the steel sheet is highly concentrated in the {110} so-called Goss orientation. <001> Oriented steel sheet. Since oriented electromagnetic steel sheets have excellent magnetic properties, they are used, for example, as core materials for stationary inductors such as transformers. In the past, various developments have been made to improve the magnetic properties of electromagnetic steel sheets. In particular, with the demand for energy conservation in recent years, oriented electromagnetic steel sheets are required to have lower iron loss. In order to reduce the iron loss of oriented electromagnetic steel sheets, it is effective to increase the concentration of the grains of the steel sheet in the Gossian orientation to increase the magnetic flux density and reduce the hysteresis loss. In the manufacture of oriented electromagnetic steel sheets, the control of crystal orientation is carried out by utilizing the catastrophic grain growth phenomenon called secondary recrystallization. In order to appropriately control the crystal orientation through secondary recrystallization, it is important to ensure uniform precipitation of fine precipitates in the steel called inhibitors and thermal stability.
[0003] Various technologies for manufacturing low-iron-loss grain-oriented electromagnetic steel sheets by appropriately controlling secondary recrystallization have been proposed in the past. For example, Patent Document 1 describes a technology for manufacturing a grain-oriented electromagnetic steel sheet with low iron loss over the entire length of the coil by controlling the heating pattern during the temperature rise process of primary recrystallization annealing. In addition, Patent Document 2 describes a technology for reducing the iron loss value of a grain-oriented electromagnetic steel sheet by strictly controlling the average grain size of the grains after secondary recrystallization and the deviation angle from the ideal orientation.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2014 / 049770
[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 7-268567 Summary of the invention
[0008] Problems to be solved by the invention
[0009] The success of secondary recrystallization of a grain-oriented electrical steel sheet is determined by the balance between the frequency of Goss orientation in the steel sheet after decarburization and before final annealing and the thermal stability of precipitates (inhibitors) in the steel. Generally speaking, if the heating rate during primary recrystallization annealing is increased, the amount of Goss-oriented grains increases, thereby improving the magnetic properties. However, according to the research of the inventors of the present invention, for thin-walled materials (materials with a plate thickness of 0.23 mm or less in one embodiment), there is a tendency that the magnetic improvement effect brought about by the increase in the heating rate is smaller than that of thick-walled materials. In the past, there has been no method for manufacturing a grain-oriented electrical steel sheet that is thin-walled but exhibits a good magnetic improvement effect brought about by the increase in the heating rate, thereby having excellent magnetic properties.
[0010] An object of the present invention is to solve the above-mentioned problems and to provide a method for producing a grain-oriented electrical steel sheet having excellent magnetic properties despite being thin.
[0011] Means for solving problems
[0012] The present invention includes the following aspects.
[0013] [1] A method for manufacturing a grain-oriented electrical steel sheet, comprising the following steps:
[0014] A hot rolling process for obtaining a hot-rolled steel sheet by heating a slab and performing hot rolling, wherein the slab has the following slab composition: containing, by mass%, C: 0.02% to 0.10%, Si: 2.5% to 4.5%, Mn: 0.01% to 0.30%, a total of one or two of S and Se: 0.001% to 0.050%, acid-soluble Al: 0.01% to 0.05%, N: 0.002% to 0.020%, P: 0.0400% or less, Cu: 0.05% to 0.50%, and the remainder consisting of Fe and impurities;
[0015] A pickling step, wherein the hot-rolled steel sheet is immersed in a pickling solution, or the hot-rolled steel sheet is subjected to hot-rolled annealing to obtain a hot-rolled annealed sheet and then the hot-rolled annealed sheet is immersed in a pickling solution to obtain a pickled sheet;
[0016] A cold rolling step of obtaining a cold-rolled steel sheet by cold rolling the pickled steel sheet;
[0017] A primary recrystallization annealing step of performing primary recrystallization annealing on the cold-rolled steel sheet to obtain a primary recrystallization annealed sheet;
[0018] A finish annealing step of applying an annealing separator containing MgO to the surface of the primary recrystallization annealed sheet and then performing finish annealing to obtain a finish annealed sheet; and
[0019] After coating the insulating film on the finished annealed sheet, a planarization annealing step of planarization annealing is performed.
[0020] The pickling solution contains 0.0001 g / L to 5.00 g / L of Cu.
[0021] The thickness of the cold-rolled steel sheet is 0.15 mm to 0.23 mm.
[0022] The primary recrystallization annealing step includes a heating step and a decarburization annealing step, and an average heating rate in a temperature range of 30° C. to 400° C. in the heating step exceeds 50° C. / sec and is 1000° C. / sec or less.
[0023] [2] The method for producing a grain-oriented electrical steel sheet according to [1] above, wherein the total content of Cu and Mn in the pickling solution is 0.01 g / L to 5.00 g / L.
[0024] [3] The method for producing a grain-oriented electrical steel sheet according to [1] or [2], wherein in the pickling step, the pH of the pickling solution is greater than -1.5 and less than 7.0, the liquid temperature is 15°C to 100°C, and the immersion is performed for 5 seconds to 200 seconds.
[0025] [4] The method for producing a grain-oriented electrical steel sheet according to any one of [1] to [3], wherein the pickling solution contains Ni: 0.01 g / L to 5.00 g / L.
[0026] [5] The method for producing a grain-oriented electrical steel sheet according to any one of [1] to [4], wherein in the temperature raising step of the primary recrystallization annealing step, the dew point in the temperature range of 30°C to 800°C is -50°C to 0°C.
[0027] [6] The method for producing a grain-oriented electrical steel sheet according to any one of [1] to [5], wherein an average heating rate in the temperature range of 550°C to 700°C in the heating step is 100°C / sec to 3000°C / sec.
[0028] [7] The method for producing a grain-oriented electrical steel sheet according to any one of [1] to [6], wherein an average heating rate in the temperature range of 700°C to 800°C in the heating step is 400°C / sec to 2500°C / sec.
[0029] [8] The method for producing a grain-oriented electrical steel sheet according to any one of [1] to [7], wherein the decarburization annealing step includes heating the steel sheet at a temperature of 750°C to 900°C and an oxygen potential (P H2O / P H2 The heat treatment is carried out in an atmosphere with a ) of 0.2 to 0.6.
[0030] [9] The method for manufacturing a grain-oriented electrical steel sheet according to [8], wherein the decarburization annealing step includes a first soaking treatment and a second soaking treatment, wherein the first soaking treatment is performed at a temperature of 750°C to 900°C and an oxygen potential (P H2O / P H2 ) is 0.2 to 0.6, the second soaking treatment is performed after the first soaking treatment at a temperature of 900°C to 1000°C and an oxygen potential (P H2O / P H2 ) is implemented in an atmosphere with a pH lower than 0.2.
[0031]
[10] The method for producing a grain-oriented electrical steel sheet according to any one of [1] to [9], wherein a nitriding treatment is performed after the cold rolling step and before the finish annealing step.
[0032]
[11] The method for producing a grain-oriented electrical steel sheet according to any one of [1] to
[10] , wherein the slab composition contains, in terms of mass %, one or more elements selected from the following elements in place of a portion of the Fe:
[0033] Sn: 0.50% or less,
[0034] Cr: 0.500% or less,
[0035] Bi: 0.0200% or less,
[0036] Sb: 0.500% or less,
[0037] Mo: 0.500% or less, and
[0038] Ni: 0.500% or less.
[0039] Effects of the Invention
[0040] According to one aspect of the present invention, there is provided a method for producing a grain-oriented electrical steel sheet having excellent magnetic properties despite being thin. DETAILED DESCRIPTION
[0041] Hereinafter, exemplary embodiments of the present invention will be described, but the present invention is not limited to the following embodiments. In addition, unless otherwise specified, the description of "A to B" regarding numerical values A and B means "A or more and B or less".
[0042] One embodiment of the present invention provides a method for manufacturing a grain-oriented electrical steel sheet, comprising the following steps:
[0043] A hot rolling process for obtaining a hot-rolled steel sheet by heating a slab and performing hot rolling, wherein the slab has the following slab composition: containing, by mass%, C: 0.02% to 0.10%, Si: 2.5% to 4.5%, Mn: 0.01% to 0.30%, a total of one or two of S and Se: 0.001% to 0.050%, acid-soluble Al: 0.01% to 0.05%, N: 0.002% to 0.020%, P: 0.0400% or less, Cu: 0.05% to 0.50%, and the remainder consisting of Fe and impurities;
[0044] A pickling step, wherein the hot-rolled steel sheet is immersed in a pickling solution, or the hot-rolled steel sheet is subjected to hot-rolled annealing to obtain a hot-rolled annealed sheet and then the hot-rolled annealed sheet is immersed in a pickling solution to obtain a pickled sheet;
[0045] A cold rolling step of obtaining a cold-rolled steel sheet by cold rolling the pickled steel sheet;
[0046] A primary recrystallization annealing step of performing primary recrystallization annealing on the cold-rolled steel sheet to obtain a primary recrystallization annealed sheet;
[0047] A finish annealing step of applying an annealing separator containing MgO to the surface of the primary recrystallization annealed sheet and then performing finish annealing to obtain a finish annealed sheet; and
[0048] After the insulating film is applied to the finish annealed sheet, a planarization annealing step of planarization annealing is performed.
[0049] In one embodiment, the pickling solution contains 0.0001 g / L to 5.00 g / L of Cu. In one embodiment, the total content of Cu and Mn in the pickling solution is 0.01 g / L to 5.00 g / L.
[0050] In the case where there are components (representatively MnS, MnSe and AlN) that function as inhibitors during the final annealing in the steel, it is important to keep the inhibitors without decomposing until the specified temperature during the final annealing to obtain the desired secondary recrystallization. However, according to the research of the inventors of the present invention, when the thickness of the steel plate provided for the final annealing is small (i.e., thin-walled material), there is a tendency that the Gaussian orientation increase effect brought about by increasing the heating rate during the primary recrystallization annealing is small. Although it is not expected to be bound by theory, in thin-walled materials, it is likely that the decomposition reaction of the inhibitors will easily occur due to the size of their surface area, and the Gaussian orientation increase effect cannot be fully enjoyed. That is, in thin-walled materials, in order to fully exert the Gaussian orientation increase effect, it is not sufficient to simply increase the heating rate during the primary recrystallization annealing, and a stabilization countermeasure for the inhibitor is required. For example, MnS is decomposed by the reaction of MnS→Mn+S, so that S is released outside the system as a gas, so during the final annealing, it is necessary to reduce the gas permeability.
[0051] The inventors of the present invention have achieved the object of the present invention, namely, to improve the magnetic properties (magnetic flux density and iron loss) of thin-walled materials by making the slab contain more than 0.05% Cu and controlling the pickling conditions of the hot-rolled steel sheet or the hot-rolled annealed sheet. The inventors of the present invention analyzed the steel slab after hot-rolled sheet annealing and pickling, and found the possibility of forming a surface segregation layer of Cu or Mn, and a surface segregation layer of Ni (hereinafter sometimes referred to as a 3d transition metal segregation layer) on the surface of the sample. More specifically, the inventors of the present invention analyzed the above-mentioned steel slab by glow discharge luminescence spectroscopy (GDS), and the luminescence intensity derived from the above-mentioned 3d transition metal was observed in the form of a peak on the surface of the sample, and thus the existence of the above-mentioned surface segregation layer was inferred. It should be noted that in this analysis, since the luminescence peaks of light elements such as oxygen or nitrogen that are believed to be combined with the above-mentioned 3d transition metal cannot be confirmed on the surface of the sample, it is inferred that the above-mentioned 3d transition metal is not segregated as a compound but as a metal single substance. It is believed that the 3d transition metal segregation layer is a layer obtained by dissolving 3d transition metals such as Cu and Mn contained in the steel into the acid solution during pickling, and re-precipitating them for some reason. It is believed that in the presence of a 3d transition metal segregation layer on the surface of the steel plate, the gas permeability to the steel plate is significantly reduced. Conversely, the release of gas from the steel is also suppressed. For example, MnS, which serves as an inhibitor, decomposes in the form of MnS→Mn+S, and S is converted into gas and released to the outside of the steel. Here, in the presence of a 3d transition metal segregation layer on the surface of the steel plate that reduces the gas permeability, the gasification of S is suppressed (that is, the activity of the solid solution S in the steel increases). While the gasification of S is suppressed, the above-mentioned decomposition reaction of MnS→Mn+S is also suppressed, which leads to the thermal stabilization of MnS.
[0052] As a metal component contained in the pickling solution, 3d transition metals (Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn) are advantageous from the viewpoint of being easily precipitated on the surface of the steel plate and having little load on the environment. 3d transition metals are particularly preferably Cu, Mn and / or Ni, but if they are 3d transition metals, the thermal stabilization effect of MnS can be shown, so Sc, Ti, V, Co, Cr and Zn are also preferred as 3d transition metals. Therefore, in one embodiment, the pickling solution contains one or more metals selected from Sc, Ti, V, Cu, Mn, Ni, Co, Cr and Zn, more advantageously, one or more metals selected from Cu, Mn and Ni, further advantageously, one or more metals selected from Cu and Mn, particularly advantageously, Cu and optional Mn. The 3d transition metal in the pickling solution is not limited to its source. That is, it can be a 3d transition metal that is dissolved into the pickling solution by a component in the steel, or it can be intentionally contained in the pickling solution.
[0053] In one embodiment, from the viewpoint of good precipitation on the surface of the steel sheet and good effect of suppressing the decomposition of the inhibitor, the Cu content in the pickling solution is 0.0001 g / L or more. In addition, from the viewpoint of preventing the unfavorable conditions (insufficient decarburization, insufficient oxide film formation, etc.) during the primary recrystallization caused by excessive precipitation of the metal component, in one embodiment, it is 5.00 g / L or less. That is, the Cu content in the pickling solution is 0.0001 g / L to 5.00 g / L, preferably 0.005 g / L to 5.00 g / L, more preferably 0.01 g / L to 5.00 g / L, further preferably 0.02 g / L to 4.00 g / L, and further preferably 0.03 g / L to 2.00 g / L in one embodiment.
[0054] In one embodiment, from the viewpoint of good precipitation on the steel plate surface and good effect of suppressing the decomposition of the inhibitor, the total content of Cu and Mn in the pickling solution is preferably 0.01 g / L or more, and from the viewpoint of preventing the unfavorable conditions (insufficient decarburization, insufficient oxide film formation, etc.) during primary recrystallization caused by excessive precipitation of metal components, it is preferably 5.00 g / L or less. The total content of Cu and Mn in the pickling solution is preferably 0.01 g / L to 5.00 g / L, more preferably 0.02 g / L to 4.00 g / L, and further preferably 0.03 g / L to 2.00 g / L.
[0055] The Ni content in the pickling solution is preferably 0.01 g / L to 5.00 g / L, more preferably 0.02 g / L to 4.00 g / L, and further preferably 0.03 g / L to 2.00 g / L.
[0056] The amount of metal components in the pickling solution can be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry).
[0057] According to the method of this embodiment, the thermal stability of the inhibitor can be improved not only in thick-walled materials but also in thin-walled materials, so the advantage of the method of this embodiment is particularly significant in the manufacture of directional electromagnetic steel sheets using thin-walled materials. In one embodiment, the thickness of the cold-rolled steel sheet in the method of this embodiment is 0.23 mm or less, less than 0.23 mm, or less than 0.22 mm. The thickness of the cold-rolled steel sheet can be 0.15 mm or more, 0.16 mm or more, 0.17 mm or more, or 0.18 mm or more, depending on the desired use of the directional electromagnetic steel sheet.
[0058] Hereinafter, a method for producing a grain-oriented electrical steel sheet according to the present embodiment will be described in detail.
[0059] [Slab composition]
[0060] First, the component composition of the slab used in the grain-oriented electrical steel sheet of the present embodiment is described. It should be noted that, unless otherwise specified, "%" means "mass %". In addition, the remainder of the slab other than the elements described below is Fe and impurities.
[0061] The content of C (carbon) is 0.02% to 0.10%. C has various effects, but when the content of C is less than 0.02%, the crystal grain size becomes excessively large when the slab is heated, thereby increasing the iron loss value of the final directional electromagnetic steel sheet, which is not preferred. When the content of C exceeds 0.10%, the decarburization time becomes long during decarburization after cold rolling, and the manufacturing cost increases, which is not preferred. In addition, when the content of C exceeds 0.10%, decarburization tends to become incomplete, and magnetic aging may be caused in the final directional electromagnetic steel sheet, which is not preferred. Therefore, the content of C is 0.02% to 0.10%, preferably 0.04% to 0.09%, and more preferably 0.05% to 0.09%.
[0062] The content of Si (silicon) is 2.5% to 4.5%. Si reduces eddy current loss, one of the causes of iron loss, by increasing the electrical resistance of the steel sheet. When the content of Si is less than 2.5%, it becomes difficult to fully suppress the eddy current loss of the final directional electromagnetic steel sheet, so it is not preferred. When the content of Si exceeds 4.5%, the workability of the directional electromagnetic steel sheet decreases, so it is not preferred. Therefore, the content of Si is 2.5% to 4.5%, preferably 2.7% to 4.0%, and more preferably 3.2% to 3.7%.
[0063] The content of Mn (manganese) is 0.01% to 0.30%. Mn forms inhibitors that affect secondary recrystallization, such as MnS and MnSe. When the content of Mn is less than 0.01%, the absolute amount of MnS and MnSe that produce secondary recrystallization is insufficient, so it is not preferred. When the content of Mn exceeds 0.30%, the solid solution of Mn becomes difficult when the slab is heated, so it is not preferred. In addition, when the content of Mn exceeds 0.30%, the precipitation size of MnS and MnSe as inhibitors tends to coarsen, and the optimal size distribution as inhibitors is damaged, so it is not preferred. Therefore, the content of Mn is 0.01% to 0.30%, preferably 0.03% to 0.20%, and more preferably 0.05% to 0.15%.
[0064] The total content of S (sulfur) and Se (selenium) is 0.001% to 0.050%. S and Se form inhibitors together with the above-mentioned Mn. S and Se may both be contained in the slab, but at least one of them is sufficient as long as it is contained in the slab. When the total content of S and Se deviates from the above range, a sufficient inhibitor effect cannot be obtained, so it is not preferred. Therefore, the total content of S and Se is 0.001% to 0.050%, preferably 0.001% to 0.040%, and more preferably 0.005% to 0.030%.
[0065] The content of acid-soluble Al (acid-soluble aluminum) is 0.01% to 0.05%. Acid-soluble Al constitutes an inhibitor required for manufacturing a directional electromagnetic steel sheet with a high magnetic flux density. When the content of acid-soluble Al is less than 0.01%, the inhibitor strength is low, so it is not preferred. When the content of acid-soluble Al exceeds 0.05%, AlN precipitated as an inhibitor coarsens, which reduces the inhibitor strength, so it is not preferred. Therefore, the content of acid-soluble Al is 0.01% to 0.05%, preferably 0.01% to 0.04%, and more preferably 0.01% to 0.03%.
[0066] The content of N (nitrogen) is 0.002% to 0.020%. N forms AlN as an inhibitor together with the above-mentioned acid-soluble Al. When the content of N deviates from the above range, a sufficient inhibitor effect cannot be obtained, so it is not preferred. Therefore, the content of N is 0.002% to 0.020%, preferably 0.004% to 0.015%, and more preferably 0.005% to 0.010%.
[0067] The content of P (phosphorus) is less than 0.0400%. The lower limit includes 0%, but since the detection limit is 0.0001%, the substantial lower limit is 0.0001%. P makes the texture after the primary recrystallization annealing preferred for the magnetic flux density. That is, it is an element that improves the magnetic properties. When P is less than 0.0001%, the effect of P addition will not be exerted. On the other hand, if more than 0.0400% of P is added, the risk of fracture in cold rolling increases and the passability of the plate is significantly deteriorated. The P content is preferably 0.0030% to 0.0300%, and more preferably 0.0060% to 0.0200%.
[0068] The content of Cu (copper) is 0.05% to 0.50%. Cu is an important element in the present invention because it forms a Cu segregation layer and plays a role in the thermal stabilization of the inhibitor. The Cu content used to enhance the thermal stability of the inhibitor brought about by the Cu segregation layer needs to be 0.05% or more. However, when the Cu content exceeds 0.50%, it will become a cause of deterioration of hot brittleness, so the sheet passability is significantly deteriorated. Therefore, the Cu content is 0.05% to 0.50%, preferably 0.07% to 0.40%, and more preferably 0.09% to 0.30%.
[0069] In addition, the slab used in the manufacture of the grain-oriented electrical steel sheet of the present embodiment may contain, in addition to the above-mentioned elements, one or more selected from Sn: 0.50% or less, Cr: 0.500% or less, Bi: 0.0200% or less, Sb: 0.500% or less, Mo: 0.500% or less, and Ni: 0.500% or less, in order to improve the magnetic properties, in order to replace a part of the remaining Fe.
[0070] In one embodiment, the Sn content may preferably be 0.02% to 0.40%, and more preferably 0.04% to 0.20%.
[0071] In one embodiment, the Cr content may preferably be 0.020% to 0.400%, and more preferably 0.040% to 0.200%.
[0072] In one embodiment, the Bi content may be 0.0005% or more, preferably 0.0005% to 0.0150%, and more preferably 0.0010% to 0.0100%.
[0073] In one embodiment, the Sb content may be 0.005% or more, preferably 0.005% to 0.300%, and more preferably 0.005% to 0.200%.
[0074] In one embodiment, the Mo content may be 0.005% or more, preferably 0.005% to 0.400%, and more preferably 0.005% to 0.300%.
[0075] In one embodiment, the Ni content may preferably be 0.010% to 0.200%, and more preferably 0.020% to 0.100%.
[0076] The slab is formed by casting the molten steel adjusted to the above-described component composition. It should be noted that the casting method of the slab is not particularly limited. In addition, during research and development, even if the steel ingot is formed by a vacuum melting furnace, the same effect as that of the case of forming the slab can be confirmed with respect to the above-described components. The preferred scheme for each process for manufacturing a grain-oriented electromagnetic steel sheet from a slab is further described below.
[0077] [Hot rolling process]
[0078] In this process, the hot-rolled steel sheet is obtained by heating the slab and performing hot rolling. In one embodiment, from the viewpoint of dissolving the inhibitor components (e.g., MnS, MnSe, AlN, etc.) in the slab and obtaining a good inhibitor effect, the heating temperature of the slab may be preferably 1280°C or more or 1300°C or more. In this case, the upper limit of the heating temperature of the slab is not particularly specified, but is preferably 1450°C from the viewpoint of equipment protection. In one embodiment, from the viewpoint of reducing the burden of the heating furnace during hot rolling, reducing the amount of scale generated, and downstream process control of the inhibitor, the heating temperature of the slab may be preferably lower than 1280°C or lower than 1250°C.
[0079] The heated slab is hot rolled to be processed into a hot-rolled steel sheet. From the viewpoint of being able to stably control the precipitation of inhibitors in the steel by making it difficult to reduce the temperature of the steel sheet, the thickness of the hot-rolled steel sheet after processing is preferably, for example, 1.8 mm or more, and from the viewpoint of being able to reduce the rolling load in the cold rolling process, for example, 3.5 mm or less.
[0080] [Pickling process]
[0081] In this process, the hot rolled steel sheet is immersed in a pickling solution, or the hot rolled steel sheet is subjected to hot rolled sheet annealing to obtain a hot rolled annealed sheet, and then the hot rolled annealed sheet is immersed in a pickling solution to obtain a pickled sheet. Pickling is performed at least once after hot rolling and before primary recrystallization annealing. In one embodiment, pickling is performed before the cold rolling process from the viewpoint of reducing roll wear during cold rolling.
[0082] The pH of the pickling solution is lower than 7.0 in one embodiment. When the pH is lower than 7.0, the scale removal effect is good, which is preferred. On the other hand, the solution that can be prepared in reality has a pH of -1.5 or more. The pH is preferably lower than 2, and more preferably lower than 1.
[0083] Examples of the acid component contained in the pickling solution include sulfuric acid, hydrochloric acid, and nitric acid.
[0084] The liquid temperature of the pickling solution is 15°C to 100°C in one embodiment. When the liquid temperature of the pickling solution is lower than 15°C, the scale removal effect obtained by pickling becomes insufficient, which is not preferred. When the liquid temperature of the pickling solution exceeds 100°C, the handling of the pickling solution becomes difficult, which is not preferred. The fact that the liquid temperature of the pickling solution is 15°C to 100°C is also advantageous from the perspective of precipitating the metal component on the surface of the steel plate to the desired degree. The liquid temperature can be preferably 50°C to 90°C, and more preferably 60°C to 90°C.
[0085] The time for immersing the steel plate in the pickling solution is 5 seconds to 200 seconds in one embodiment. When the time for immersing the steel plate in the pickling solution is less than 5 seconds, the scale removal effect obtained by pickling becomes insufficient, which is not preferred. When the time for immersing the steel plate in the pickling solution exceeds 200 seconds, the equipment becomes large, which is not preferred. The immersion time may be preferably 10 seconds to 150 seconds, and more preferably 20 seconds to 150 seconds.
[0086] [Cold rolling process]
[0087] In this process, a cold-rolled steel sheet is obtained by cold rolling the pickled sheet for one or more passes, or by inserting intermediate annealing between the passes. For example, in the case of cold rolling by reversible rolling such as a Sendzimir mill, the number of passes in the cold rolling is not particularly limited, but from the viewpoint of manufacturing cost, it is preferably 9 or less. Between the passes of cold rolling, between the roll stands, or during rolling, the steel sheet may also be heated at a temperature below about 300°C. Such heating is preferred from the perspective of being able to improve the magnetic properties of the final directional electromagnetic steel sheet.
[0088] Intermediate annealing may be performed one or more times between multiple passes. The temperature of the intermediate annealing may also be set to 900°C to 1200°C. The holding time of the intermediate annealing is not particularly limited, but is preferably 200 seconds or less from the perspective of manufacturing cost. Pickling is preferably performed after the intermediate annealing.
[0089] The cumulative reduction ratio (%) of the steel plate in the cold rolling process can be appropriately designed in a manner to obtain a cold-rolled steel plate of the desired thickness, for example, it can be 80% to 95%. It should be noted that the cumulative reduction ratio (%) of the steel plate in the cold rolling process is defined by [(hot-rolled plate thickness - steel plate thickness after the final cold rolling pass) / hot-rolled plate thickness] × 100 when the above-mentioned intermediate annealing is not included; when the intermediate annealing is performed n times (n≥1), it is defined by [(steel plate thickness after the nth intermediate annealing - steel plate thickness after the final cold rolling pass) / steel plate thickness after the nth intermediate annealing] × 100.
[0090] [Primary recrystallization annealing step]
[0091] Next, in this process, a primary recrystallization annealing is performed on the cold-rolled steel sheet. The primary recrystallization annealing process includes a heating process and a decarburization annealing process. After the heating process, the cold-rolled steel sheet is decarburized in the decarburization annealing process. It is preferred to continuously perform the heating process from the heating process to the decarburization annealing process. When the heating process is set to a rapid heating process, the amount of Gaussian oriented grains of the cold-rolled steel sheet before the final annealing can be increased, thereby, in the final annealing, the secondary recrystallization of oriented grains close to the Gaussian orientation can be well formed.
[0092] (Heating process)
[0093] In the heating step, the cold rolled steel sheet is heated to a desired decarburization annealing temperature. The heating rate is preferably appropriately controlled according to the temperature range. An example of the heating rate is described below.
[0094] The average heating rate in the temperature range of 30°C to 400°C in the heating process exceeds 50°C / second and is less than 1000°C / second in one embodiment. When the residence time of the metal segregation layer formed by Cu precipitated by pickling and optionally Mn in 30°C to 400°C is long, the above-mentioned inhibitor stabilization effect is reduced. The metal component precipitated from the pickling solution may have a crystal structure different from that of the metal component precipitated by, for example, electrodeposition. It is believed that the crystal structure is a dense structure that prevents gas permeability. However, this dense crystal structure changes into a crystal structure with high gas permeability in a relatively low temperature range. Such a tendency is significant in the temperature range of 30°C to 400°C. Although the cause of the change in the crystal structure is not clear, for example, the change in the lattice constant caused by the oxidation of the metal can be cited. In any case, in order to stabilize the inhibitor, it is necessary to control the above-mentioned metal segregation layer so that it does not change to a state with high gas permeability, that is, to shorten the residence time in the temperature range of 30°C to 400°C. By setting the average heating rate in the above temperature range to more than 50°C / second, the oxidation of the metal components precipitated on the surface of the steel plate can be suppressed, and the decomposition inhibition effect of the inhibitor brought by the metal components can be well obtained. The average heating rate in the temperature range of 30°C to 400°C is preferably more than 50°C / second, more preferably more than 60°C / second, more preferably more than 100°C / second, more preferably more than 200°C / second, and more preferably more than 300°C / second. The upper limit is not particularly set, but if the steel plate is rapidly heated in a relatively low temperature range (here 30°C to 400°C) including room temperature, the shape of the steel plate deteriorates and it becomes difficult to pass the plate. The upper limit of the heating rate that can pass the plate is typically 1000°C / second. Therefore, the average heating rate in the temperature range of 30°C to 400°C is less than 1000°C / second in one embodiment, preferably less than 800°C / second, and more preferably less than 600°C / second.
[0095] In the heating process, the average heating rate between 400°C and 550°C does not need to be specially controlled, and may be the same as the average heating rate exemplified above as the average heating rate between 30°C and 400°C. For example, the temperature may be kept at 400±50°C for more than 1 second before the next heating to 550°C or more. For example, keeping the temperature at 400±50°C for more than 1 second may be preferable from the viewpoint of magnetic properties.
[0096] In the heating process, it is preferred to set the average heating rate in the temperature range of 550°C to 700°C to 100°C / second to 3000°C / second. In this way, the amount of Gauss-oriented grains before the finished annealing of the cold-rolled steel sheet can be increased, and the magnetic flux density of the final directional electromagnetic steel sheet can be improved. As mentioned above, thin-walled materials are less likely to exert the effect of increasing the heating rate than thick-walled materials. Therefore, in order to enjoy the above-mentioned effect well, the average heating rate in the temperature range of 550°C to 700°C is preferably above 400°C / second, above 500°C / second, above 600°C / second or above 700°C / second. The higher the heating rate, the better. However, when the heating rate becomes too large, the Gauss orientation increases. On the other hand, the oriented grains {111} eroded by the Gauss orientation are eroded. <112> The average heating rate in the temperature range of 550°C to 700°C is preferably set to the above range at least in the range of 550°C to 700°C, so that the recovery of dislocations in the steel plate (i.e., the reduction of dislocation density in the steel plate) will not be excessive, and the start of primary recrystallization of oriented grains other than Goss-oriented grains can be avoided, and the completion of primary recrystallization of other oriented grains before the completion of primary recrystallization of Goss-oriented grains can be avoided.
[0097] If the metal component is precipitated on the surface of the steel sheet, the decarburization reaction in the decarburization annealing process becomes difficult to proceed. In order to make the decarburization proceed to the desired degree and also obtain the inhibitor decomposition inhibition effect, it is preferred to control the heating rate at 700°C to 800°C in the heating process. In one embodiment, from the viewpoint of suppressing the formation of SiO2 that hinders decarburization during decarburization annealing, the average heating rate in the temperature range of 700°C to 800°C is preferably 400°C / second or more, more preferably 600°C / second or more, and further preferably 800°C / second or more. The upper limit of the average heating rate in the temperature range of 700°C to 800°C is not particularly limited, but from the viewpoint of equipment cost and manufacturing cost, it can be, for example, 2500°C / second or less, preferably 2000°C / second or less, and more preferably 1800°C / second or less. Such rapid heating can be implemented, for example, by using an electric heating method or an induction heating method.
[0098] The temperature raising step may be performed by a plurality of devices.
[0099] The heating rate can be measured by measuring the temperature of the steel plate using a radiation thermometer or the like. In addition, the method for measuring the temperature of the steel plate is not particularly limited. However, it is difficult to measure the temperature of the steel plate. When it is difficult to estimate the accurate temperature of the heating start point and the heating end point that should control the heating rate, these temperatures can also be estimated by analogy with the heating modes of heating and cooling. In addition, the inlet side temperature and the outlet side temperature of the steel plate to the heating device in the heating process can be further set as the heating start point and the heating end point.
[0100] (Decarburization annealing process)
[0101] After the heating process, a decarburization annealing process is performed. In a common scheme, the decarburization annealing process includes a soaking treatment. The soaking treatment can be performed in a moist atmosphere containing hydrogen and / or nitrogen, for example, at a temperature below 900°C or at 750°C to 900°C. The decarburization annealing temperature can be the same as the heating end temperature of the above-mentioned heating process or a higher temperature or a lower temperature than it. In the case where the heating end temperature of the heating process is a lower temperature than the decarburization annealing temperature, the steel plate can be further heated before the decarburization annealing. On the other hand, in the case where the heating end temperature of the heating process is a higher temperature than the decarburization annealing temperature, the steel plate can be cooled by heat dissipation treatment, gas cooling treatment, etc. before the decarburization annealing. Furthermore, after the heating process, the steel plate can be cooled to a temperature lower than the decarburization annealing temperature and then reheated in the decarburization annealing process.
[0102] The soaking treatment can be performed once or twice or more. For example, in the case where the soaking treatment is performed twice, namely the first soaking treatment and the second soaking treatment, after the first soaking treatment is completed, the steel plate can be temporarily cooled (for example, cooled to room temperature) and then reheated, or the second soaking treatment can be performed without cooling. From the viewpoint of improving the film adhesion of the directional electromagnetic steel sheet, it is expected that a forsterite film (Mg2SiO4) is well formed on the surface of the steel plate after the finished annealing. However, during the soaking treatment, Fe2Si4O that hinders the formation of the forsterite film may be generated. In the case of performing the first soaking treatment and the second soaking treatment, even if Fe2Si4O is generated in the first soaking treatment, SiO2 is generated by reducing it in the second soaking treatment, thereby improving the film adhesion by forming a forsterite film in the subsequent finished annealing process. The improvement of the film adhesion is beneficial to the improvement of the film tension and therefore the improvement of the magnetic properties. It should be noted that even if SiO 2 is generated in the second soaking treatment, since decarburization has been sufficiently performed in the first soaking treatment, there will be no adverse effect on decarburization due to the SiO 2 .
[0103] From the viewpoint of achieving good internal oxidation and forming a uniform oxide film on the surface of the steel sheet, the oxygen potential of the soaking treatment atmosphere, that is, the partial pressure P of water vapor in the atmosphere, is H2O With hydrogen partial pressure P H2 The ratio (P H2O / P H2 The ratio is preferably 0.2 or more, 0.3 or more, or 0.4 or more, and is preferably 0.6 or less or 0.55 or less from the viewpoint of obtaining good magnetic properties. In addition, for example, when the first soaking treatment and the second soaking treatment are performed, it is preferred that the P ratio of the first soaking treatment be H2O / P H2 The ratio is set to the above range, and the P H2O / P H2 The ratio is set to be less than 0.2, less than 0.1, or less than 0.08, for example. H2O / P H2 The lower limit of the ratio is not particularly limited, but from the viewpoint of ease of process control, it may be, for example, 0.01 or more or 0.02 or more.
[0104] In one embodiment, the decarburization annealing process may include a first soaking treatment at 750°C to 900°C and a second soaking treatment at 900°C to 1000°C. In one embodiment, the decarburization annealing process may include the following first soaking treatment and the following second soaking treatment, wherein the first soaking treatment is performed at a temperature of 750°C to 900°C and an oxygen potential (P H2O / P H2 ) is 0.2 to 0.6, and the second soaking treatment is performed after the first soaking treatment at a temperature of 900°C to 1000°C and an oxygen potential (P H2O / P H2 ) is implemented in an atmosphere with a pH of less than 0.2.
[0105] In the temperature raising step of the primary recrystallization annealing step, the dew point temperature of the atmosphere between 30°C and 800°C is preferably -50°C to 0°C. From the viewpoint of suppressing metal oxidation in the steel sheet and suppressing the generation of SiO2 caused by external oxidation so as to perform decarburization well, the dew point temperature is preferably 0°C or less, -5°C or less, or -10°C or less. From the viewpoint of performing internal oxidation well, the dew point temperature may be, for example, -50°C or more or -40°C or more.
[0106] [Nitriding treatment]
[0107] After the cold rolling process and before the final product annealing, a nitriding treatment may be further performed for the purpose of inhibitor strengthening. In one embodiment, the nitriding treatment may be performed after the soaking treatment and before the final product annealing, for example, the sequence of soaking treatment-nitriding treatment-final product annealing, the sequence of first soaking treatment-second soaking treatment-nitriding treatment-final product annealing, or the sequence of first soaking treatment-nitriding treatment-second soaking treatment-final product annealing. The nitriding treatment may be performed in a nitriding gas (e.g., ammonia-containing gas) atmosphere.
[0108] [Finished product annealing process]
[0109] Next, the steel sheet after the primary recrystallization annealing process (primary recrystallization annealed sheet) is subjected to finish annealing for the purpose of primary film formation and secondary recrystallization. In a typical scheme, an annealing separator containing MgO as the main component is applied to the primary recrystallization annealed sheet before the finish annealing for the purpose of preventing the steel sheets from sticking, forming a primary film, controlling the secondary recrystallization behavior, etc. The annealing separator is generally applied to the steel sheet surface in the form of a water slurry and dried, but an electrostatic coating method or the like may also be used.
[0110] Finished annealing can be performed, for example, by heat treating the coiled steel sheet using an intermittent heating furnace or the like. Furthermore, for the purpose of further reducing the iron loss of the final directional electromagnetic steel sheet, a purification treatment can be performed by heating the coiled steel sheet to a temperature of about 1200°C and then maintaining the temperature. Finished annealing generally starts heating from about room temperature, and the heating rate of finished annealing varies. The conditions for finished annealing are not particularly limited. For example, from the perspective of productivity and general equipment constraints, the heating rate can be set to 5°C / hour to 100°C / hour, or other known heating modes can be used. The mode of the cooling process is also not particularly limited.
[0111] The composition of the atmosphere gas in the finish annealing is not particularly limited. During the secondary recrystallization process, it can also be a mixed gas of nitrogen and hydrogen. The atmosphere can be a dry atmosphere or a wet atmosphere. The atmosphere of the purification annealing can be, for example, dry hydrogen.
[0112] [Planarization Annealing Process]
[0113] After the finish annealing, an insulating film (for example, an insulating film mainly composed of aluminum phosphate or colloidal silica) may be applied to the surface of the steel sheet for the purpose of imparting insulation and tension to the steel sheet. The composition of the insulating film may be appropriately selected in order to impart the desired insulation and tension to the steel sheet. Next, a flattening annealing may be performed for the purpose of baking the insulating film and flattening the shape of the steel sheet due to the finish annealing.
[0114] The obtained grain-oriented electrical steel sheet may be further subjected to a magnetic domain control treatment depending on the application of the steel sheet and the like.
[0115] The grain-oriented electromagnetic steel sheet having excellent magnetic properties can be manufactured by the above-described steps. The grain-oriented electromagnetic steel sheet manufactured by the method of this embodiment can be processed into a wound core or a laminated core when manufacturing a transformer and can be applied to a desired application.
[0116] [Magnetic properties of grain-oriented electrical steel sheets]
[0117] The directional electromagnetic steel sheet manufactured by the method of the present embodiment has excellent magnetic properties. Specifically, even with thin-walled materials, a good secondary recrystallization structure can be obtained, and the magnetic flux density is improved. Here, the evaluation items of the directional electromagnetic steel sheet manufactured by the method of the present embodiment, namely the magnetic flux density B8 value and the iron loss W17 / 50, are described. The magnetic flux density is an indicator of the concentration of the Gaussian orientation. Here, the magnetic flux density B8 value is the magnetic flux density when a magnetic field of 800A / m is applied to the directional electromagnetic steel sheet at 50Hz. B8 is an indicator of the orientation concentration of the Gaussian orientation. If B8 is low, good iron loss cannot be obtained. When B8 is 1.88T or more, good iron loss can be obtained, which is preferred. In addition, the so-called iron loss W17 / 50 (W / kg) refers to the iron loss of the sample when the frequency is set to 50Hz and the maximum magnetic flux density is set to 1.7T. The above-mentioned magnetic flux density B8 value and W17 / 50 are values obtained according to the single sheet magnetic property test method (Single Sheet Tester: SST) specified in JIS C2556. It should be noted that in research and development, when a steel ingot is formed by a vacuum melting furnace, etc., it becomes difficult to collect test pieces of the same size as those manufactured by an actual machine. In this case, for example, a test piece is collected in a manner of 60 mm in width × 300 mm in length, and the test piece is measured according to the above-mentioned single sheet magnetic property test method. At this time, the obtained result can also be corrected by a correction factor in a manner that obtains a measured value equivalent to the method based on the Epstein test specified in JIS C2550.
[0118] Furthermore, in the above-described embodiment, the case where the method for producing a grain-oriented electrical steel sheet according to one aspect of the present invention is applied to a thin-walled material (0.15 mm to 0.23 mm) is exemplified, but the method of the present invention can also be applied to a plate thickness other than the above.
[0119] Example
[0120] Hereinafter, although the illustrative aspects of the present invention are further described with reference to Examples, the present invention is not limited to the following Examples.
[0121] <Manufacturing of Grain-Oriented Electrical Steel Sheet>
[0122] [Examples 1 to 14, Comparative Examples 1 to 6]
[0123] A slab having the slab composition shown in Table 1 was obtained. The slab was heated at 1100°C to 1400°C and then hot rolled to obtain a hot-rolled steel strip having a thickness of 2.0 mm to 3.0 mm. Next, the hot-rolled steel strip was heated to 1120°C to recrystallize it and then annealed at 900°C to obtain a hot-rolled annealed steel strip. The hot-rolled annealed steel strip was pickled under the pickling conditions shown in Table 2 and then cold rolled to a final product thickness of 0.19 mm to 0.22 mm.
[0124] Next, a primary recrystallization annealing is performed at 800°C to 850°C for about 100 seconds to 200 seconds. It should be noted that the primary recrystallization annealing consists of a heating process and a decarburization annealing process, and the annealing atmosphere is set to a mixed atmosphere of hydrogen and nitrogen or a nitrogen atmosphere. In the heating process, the dew point in the temperature range of 30°C to 800°C is set to -30°C to 0°C. The heating rate at 30°C to 400°C is as shown in Table 2. In the decarburization annealing process, the atmosphere is controlled to 800°C to 850°C, and the oxygen potential is controlled to 0.3 to 0.6. As the heating rate of the heating process, it is controlled in a manner such that the average heating rate is 500°C / second to 2000°C / second in the range of 550°C to 700°C and 800°C / second to 2000°C / second in the range of 700°C to 800°C. After decarburization annealing, slabs No. 1, 4 to 6 were subjected to a second soaking treatment, that is, a second soaking treatment at 900°C to 1000°C for about 10 seconds to 50 seconds. The annealing atmosphere of the second soaking treatment was also set to a mixed atmosphere of hydrogen and nitrogen, and the oxygen potential was controlled to be less than 0.1. On the other hand, slabs No. 2 to 3 were subjected to nitriding treatment without the second soaking treatment.
[0125] Next, the finish annealing is performed. Specifically, an annealing separator having magnesium oxide (MgO) as the main component is applied to the surface of the steel sheet after the primary recrystallization annealing. Next, the primary recrystallization annealing steel sheet coated with the annealing separator is heated to 1200°C to produce a finish annealed steel sheet. The annealing atmosphere of the finish annealing is set to a mixed atmosphere of hydrogen and nitrogen.
[0126] Next, the finish annealed steel sheet was subjected to an insulating film forming step. Specifically, an insulating film forming liquid mainly composed of colloidal silica and phosphate was applied to the surface of the finish annealed steel sheet, and the film was baked.
[0127] Through the above steps, a grain-oriented electrical steel sheet is obtained.
[0128] Evaluation samples of 60 mm in width and 300 mm in length were collected from the produced grain-oriented electrical steel sheets. The samples thus obtained were evaluated for B8 and W17 / 50 in accordance with JIS C2556.
[0129] Samples with B8 lower than 1.88 are set as NG (poor) as they have not obtained a secondary recrystallization structure that is preferred for magnetic properties. In addition, for samples with a W17 / 50 value of 0.890 W / kg or more, it is judged that iron loss deterioration has occurred due to the failure to obtain a good secondary recrystallization structure, and the magnetic properties are set to NG. On the other hand, the magnetic properties of samples with a W17 / 50 value of 0.840 W / kg or more and less than 0.890 W / kg are set to F (Fine), the magnetic properties of samples with a W17 / 50 value of 0.790 W / kg or more and less than 0.840 W / kg are set to G (Good), and the magnetic properties of samples with a W17 / 50 value of less than 0.790 W / kg are set to VG (Very Good).
[0130] The results are shown in Table 2.
[0131]
[0132]
[0133] Industrial Applicability
[0134] The grain-oriented electrical steel sheet obtained by the method disclosed herein can be suitably used in various applications requiring excellent magnetic properties.
Claims
1. A method for manufacturing a grain-oriented electromagnetic steel sheet, comprising the following steps: A hot rolling process for obtaining a hot-rolled steel sheet by heating a slab and performing hot rolling, wherein the slab has the following slab composition: containing, by mass%, C: 0.02% to 0.10%, Si: 2.5% to 4.5%, Mn: 0.01% to 0.30%, a total of one or two of S and Se: 0.001% to 0.050%, acid-soluble Al: 0.01% to 0.05%, N: 0.002% to 0.020%, P: 0.0400% or less, Cu: 0.05% to 0.50%, and the remainder consisting of Fe and impurities; A pickling step, which comprises immersing the hot-rolled steel sheet in a pickling solution, or immersing the hot-rolled steel sheet in a pickling solution to obtain a pickled sheet after annealing the hot-rolled steel sheet to obtain a hot-rolled annealed sheet; A cold rolling step of obtaining a cold-rolled steel sheet by cold rolling the pickled sheet; A primary recrystallization annealing step of performing primary recrystallization annealing on the cold-rolled steel sheet to obtain a primary recrystallization annealed sheet; A finish annealing step of coating the surface of the primary recrystallization annealed sheet with an annealing separator containing MgO and then performing finish annealing to obtain a finish annealed sheet; and After the insulating film is applied to the finished annealed sheet, a planarization annealing step of planarization annealing is performed. The pickling solution contains 0.0001 g / L to 5.00 g / L of Cu, The cold-rolled steel sheet has a thickness of 0.15 mm to 0.23 mm. The primary recrystallization annealing step includes a heating step and a decarburization annealing step, and an average heating rate in a temperature range of 30° C. to 400° C. in the heating step exceeds 50° C. / sec and is 1000° C. / sec or less.
2. The method for producing a grain-oriented electrical steel sheet according to claim 1, in, The total content of Cu and Mn in the pickling solution is 0.01 g / L to 5.00 g / L.
3. The method for producing a grain-oriented electrical steel sheet according to claim 1 or 2, in, In the pickling step, the pH of the pickling solution is not less than -1.5 and less than 7.0, the liquid temperature is 15° C. to 100° C., and the immersion is performed for 5 seconds to 200 seconds.
4. The method for producing a grain-oriented electrical steel sheet according to claim 1 or 2, in, The pickling solution contains Ni: 0.01 g / L to 5.00 g / L.
5. The method for producing a grain-oriented electrical steel sheet according to claim 1 or 2, in, In the temperature raising step of the primary recrystallization annealing step, the dew point in the temperature range of 30°C to 800°C is -50°C to 0°C.
6. The method for producing a grain-oriented electrical steel sheet according to claim 1 or 2, in, The average heating rate in the temperature range of 550° C. to 700° C. in the heating step is 100° C. / sec to 3000° C. / sec.
7. The method for producing a grain-oriented electrical steel sheet according to claim 1 or 2, in, The average heating rate in the temperature range of 700° C. to 800° C. in the heating step is 400° C. / sec to 2500° C. / sec.
8. The method for producing a grain-oriented electrical steel sheet according to claim 1 or 2, in, The decarburization annealing process includes a temperature of 750°C to 900°C and an oxygen potential P H2O / P H2 The soaking treatment is performed in an atmosphere of 0.2 to 0.
6.
9. The method for producing a grain-oriented electrical steel sheet according to claim 8, in, The decarburization annealing process includes a first soaking treatment and a second soaking treatment, wherein the first soaking treatment is performed at a temperature of 750°C to 900°C and an oxygen potential P H2O / P H2 The second soaking treatment is performed after the first soaking treatment at a temperature of 900°C to 1000°C and an oxygen potential P of 0.2 to 0.
6. H2O / P H2 The method is implemented in an atmosphere with a pH lower than 0.
2. 10 . The method for producing a grain-oriented electrical steel sheet according to claim 1 , wherein a nitriding treatment is performed after the cold rolling step and before the finish annealing step.
11. The method for producing a grain-oriented electrical steel sheet according to claim 1 or 2, in, The slab composition contains, by mass%, one or more selected from the following elements to replace a portion of the Fe: Sn: 0.50% or less, Cr: 0.500% or less, Bi: 0.0200% or less, Sb: 0.500% or less, Mo: 0.500% or less, and Ni: 0.500% or less.
Citation Information
Patent Citations
Grain oriented silicon steel sheet having extremely low iron loss
JP1995268567A
Process for producing grain-oriented electromagnetic steel sheet
WO2014049770A1
Method for producing oriented electromagnetic steel sheet
CN103687967A
High-magnetic strength oriented silicon steel and production method thereof
CN103695791A
Process for producing grain-oriented electromagnetic steel sheet with excellent core loss characteristics
CN103781920A