A kind of preparation method of zinc foam

By using the electrolyte of zinc ions, sulfate ions, magnesium ions, strontium carbonate and pine alcohol oil in the electrolysis device, and adding gelatin during the electrodeposition process, the problems of high cost and complicated process of zinc foam preparation were solved and achieved Low-cost and efficient preparation of zinc foam with complete structure and uniform pore size.

CN115074782BActive Publication Date: 2024-10-22KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210508958.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-11
Publication Date
2024-10-22
Estimated Expiration
2042-05-11

AI Technical Summary

Technical Problem

The existing zinc foam preparation methods are costly and complex, making it difficult to achieve efficient and low-cost production.

Method used

The electrolyte in the electrolysis device contains zinc ions, sulfate ions, magnesium ions, strontium carbonate and pine alcohol oil. Through electrodeposition and dripping gelatin to the cathode plate, the competitive mechanism of the hydrogen evolution reaction is controlled to prepare a complete structure and uniform pore size. of zinc foam.

Benefits of technology

The low-cost and efficient preparation of zinc foam is achieved, with simple process, reduced production cost, high porosity, and is suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115074782B_ABST
    Figure CN115074782B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing zinc foam, comprising: providing an electrolysis device, wherein the electrolyte in the electrolysis device comprises zinc ions, sulfate ions, magnesium ions, strontium carbonate, and pine oil; applying power to perform electrolysis and dripping gelatin into the electrolyte, and depositing the zinc foam on the cathode plate of the electrolysis device. The present invention adopts a mixed solution of zinc sulfate and sulfuric acid as an electrolyte system, and adopts gelatin, strontium carbonate, magnesium salt, and pine oil as electrolysis additives, and adjusts the competitive mechanism of zinc ion deposition and hydrogen evolution reaction on the cathode plate to prepare a zinc foam with a complete structure, uniform pore size, good brightness, and high porosity. The preparation process is simple and the production cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of foam metal preparation, and in particular to a method for preparing foam zinc. Background Art

[0002] Porous metal materials have emerged in recent decades. Foam metals have excellent cushioning effects, heat insulation, sound insulation, and electromagnetic wave shielding. They can be used in aerospace, automobile, construction and other fields, and can also be used for biological implants.

[0003] At present, the methods used to prepare zinc foam include powder metallurgy, melt foaming, infiltration casting, etc. Among the same type of foam metal products, the price of zinc foam is relatively expensive and the production and processing technology is complicated.

[0004] Therefore, the existing preparation process of zinc foam needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for preparing zinc foam, aiming to solve the problems of high cost and complex process in the existing preparation of zinc foam.

[0006] A method for preparing zinc foam, comprising:

[0007] An electrolysis device is provided, wherein the electrolyte in the electrolysis device comprises zinc ions, sulfate ions, magnesium ions, strontium carbonate and pine oil;

[0008] Electricity is supplied for electrodeposition and gelatin is added dropwise to the electrolyte to deposit on the cathode plate of the electrolytic device to obtain zinc foam.

[0009] Optionally, in the method for preparing zinc foam, the zinc ion concentration in the electrolyte is 30 g / L-50 g / L; and the sulfate ion concentration is 100 g / L-180 g / L.

[0010] Optionally, in the method for preparing zinc foam, the magnesium ion concentration in the electrolyte is 20 g / L-40 g / L; and the pine oil concentration is 0.10 g / L-0.20 g / L.

[0011] Optionally, in the method for preparing zinc foam, the gelatin is added in a ratio of 0.007-0.02 kg per ton of zinc.

[0012] Optionally, the method for preparing the zinc foam, wherein the step of applying electricity for electrodeposition specifically comprises:

[0013] The anode plate of the electrolysis device is connected to the positive electrode of the power supply, and the cathode plate is connected to the negative electrode of the power supply, and direct current is passed for electrolysis; wherein the electrolysis temperature is 35°C-42°C, and the current density of the cathode plate is 480A / m 2 -550A / m 2 .

[0014] Optionally, in the method for preparing zinc foam, the anode plate is an inert anode plate; and the cathode plate is a rolled aluminum plate or a stainless steel plate.

[0015] Optionally, the method for preparing the zinc foam, wherein the step of adding gelatin to the electrolyte comprises:

[0016] Gelatin is dissolved in water to obtain a gelatin solution; the concentration of gelatin in the gelatin solution is 1 mg / L-3 mg / L.

[0017] Optionally, in the method for preparing zinc foam, the method for preparing the electrolyte comprises:

[0018] Dissolving zinc sulfate and sulfuric acid in water to obtain a mixed solution;

[0019] Magnesium salt, strontium carbonate and pine oil are respectively added to the mixed solution to obtain the electrolyte; the strontium carbonate is added in an amount of 5-10 kg per ton of zinc.

[0020] Beneficial effects: Compared with the traditional chemical analysis method, the present invention adopts a mixed solution of zinc sulfate and sulfuric acid as the electrolyte system, gelatin, strontium carbonate, magnesium salt and pine oil as electrolytic additives, and regulates the competitive mechanism of zinc ion deposition and hydrogen evolution reaction on the cathode plate to prepare a zinc foam with a complete structure, uniform pore size, good brightness and high porosity. The preparation process is simple and the production cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The figure is a schematic flow chart of the method for preparing zinc foam in the present invention;

[0022] Figure 2 It is a schematic diagram of the structure of the electrolysis device;

[0023] Figure 3 This is the morphology of the zinc foam prepared in Example 1;

[0024] Figure 4 This is the morphology of the zinc foam prepared in Example 2. DETAILED DESCRIPTION

[0025] The present invention provides a method for preparing zinc foam. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] See also Figure 1 , Figure 1 The present invention is a schematic flow chart of a method for preparing zinc foam. As shown in the figure, the method for preparing zinc foam comprises:

[0027] S10. Provide an electrolysis device, wherein the electrolyte in the electrolysis device contains zinc ions, sulfate ions, magnesium ions, strontium carbonate and pine oil.

[0028] Specifically, the electrolysis device includes an electrolytic cell 10, an anode plate 11 and a cathode plate 12 arranged in the electrolytic cell 10, wherein the anode plate can be an inert anode plate, such as a lead-silver alloy plate, and the cathode plate is a rolled aluminum plate. The anode plate is connected to the positive electrode of an external power source 13, and the cathode plate is connected to the negative electrode of the external power source 13.

[0029] A certain amount of zinc sulfate and sulfuric acid are weighed, added to a certain amount of water, and mixed to obtain a mixed solution. According to a preset ratio, magnesium salt, strontium carbonate and pine oil are added to the mixed solution, and stirred to form an electrolyte 14, which is added to the electrolytic cell.

[0030] Combination Figure 2 In this embodiment, the electrolysis device further includes: an electrolytic cell baffle 15, a pump 16, the pump may be a peristaltic pump, a first pipe 17, a second pipe 18, the first pipe 17 and the second pipe 18 may be silicone tubes, and a voltmeter 19. The electrolytic cell baffle 15 is fixed inside the electrolytic cell 10 and is located on one side of the anode plate 11. A small isolation area is formed between the electrolytic cell and the baffle by setting the electrolytic cell baffle 15. It should be noted that there is a space between the electrolytic cell baffle and the bottom of the electrolytic cell, and the electrolyte can flow from one side of the electrolytic cell baffle 15 to the other side. One end of the first pipe 17 is connected to the liquid inlet of the pump 16, and the other end extends into the isolation area between the electrolytic cell baffle and the electrolytic cell. One end of the second pipe is connected to the liquid outlet of the pump, and the other end extends into the area where the cathode plate is located. Through the operation of the pump 16, the electrolyte in the electrolytic cell circulates. The voltage during the electrolysis process is measured by a voltmeter 19, and the current density passing through the cathode plate is controlled according to the measured voltage value, thereby adjusting the zinc ion deposition rate on the cathode plate. The competitive mechanism between zinc ion deposition and hydrogen evolution reaction on the cathode plate is utilized to prepare a foam zinc plate with uniform pore size and large specific surface area through electrolytic deposition. The technology has a simple process flow, low reagent consumption, low energy consumption and production cost, and is suitable for large-scale applications.

[0031] In this embodiment, the aqueous electrolyte system used has the characteristics of low electrolyte toxicity, environmental friendliness, easy recycling, etc. Finished products of different sizes can be obtained by controlling the electrolysis area, and the addition of pine oil and gelatin can make the hydrogen evolution reaction more uniform, thereby controlling the pore size and structure of the zinc foam to be more uniform and controllable, closer to actual use.

[0032] In this embodiment, the concentration of zinc ions in the electrolyte may be 30 g / L to 35 g / L, 35 g / L to 40 g / L, 40 g / L to 45 g / L, or 45 g / L to 50 g / L.

[0033] The concentration of sulfate ions may be 100 g / L to 120 g / L, 120 g / L to 140 g / L, 140 g / L to 160 g / L, 160 g / L to 180 g / L.

[0034] The concentration of magnesium ions can be 20g / L to 25g / L, 25g / L to 30g / L, 30g / L to 35g / L, 35g / L to 40g / L. The concentration of pine oil is 0.10g / L-0.20g / L; the amount of strontium carbonate added can be 5kg / t zinc-10kg / t zinc according to the mass of cathode zinc deposition.

[0035] After step S10, the method further includes step S20, wherein power is supplied for electrolysis and gelatin is added dropwise to the electrolyte to deposit on the cathode plate of the electrolysis device to obtain foamed zinc.

[0036] Specifically, direct current is supplied to the electrolysis device for electrolysis, the electrolysis temperature is controlled to be 35°C-42°C, and the cathode plate current density is 480A / m 2 Up to 500A / m 2 , 500A / m 2 Up to 520A / m 2 , 520A / m 2 Up to 550A / m 2 The electrolysis cycle is 12 to 48 hours, and the electrolyte circulation adopts the top-in-bottom-out or bottom-in-top-out type. The electrolyte circulation flow rate is controlled to be 1 to 2 hours for the solution in the electrolytic cell to be renewed for one cycle. After a certain period of electrolytic deposition, a porous cathode deposition layer with uniform pore size is deposited on the cathode. After peeling and washing with clean water, a porous zinc foam plate is obtained. Among them, the control of the electrolysis temperature can be controlled by a constant temperature water bath 20 arranged outside the electrolytic cell.

[0037] In this embodiment, gelatin can be first added to a certain amount of cold water for soaking (such as soaking for 4 hours) to obtain a gelatin solution with a concentration of 1 mg / L-3 mg / L. The gelatin solution is added dropwise to the electrolyte during the electrodeposition process, and the amount of gelatin added can be added according to the mass of the cathode zinc deposition, such as adding 0.007-0.02 kg of gelatin per ton of zinc.

[0038] The preparation method of the zinc foam provided by the present invention is further explained below through specific examples.

[0039] Example 1

[0040] A mixed solution of zinc sulfate and sulfuric acid is used as the electrolyte, wherein the zinc ion concentration is 35g / L and the sulfuric acid concentration is 146g / L. Gelatin, strontium carbonate, magnesium salt and pine oil are used as additives, wherein the magnesium ion concentration is 33g / L, the gelatin concentration is 1.5mg / L, the amount of gelatin added is controlled to be 0.007kg / t zinc according to the quality control of cathode zinc deposition, the pine oil concentration is 0.10g / L, and the amount of strontium carbonate added is controlled to be 5.00kg / t zinc according to the quality control of cathode zinc deposition. The cathode is a rolled aluminum plate, the anode is a lead-silver alloy plate containing 2.5% silver, and the cathode current density is 518.86A / m 2 , the electrolysis temperature is 38℃; the electrolyte adopts bottom-in-top-out circulation, and the circulation flow rate is 1 hour for the electrolyte in the electrolytic cell to be renewed once. After 24 hours of electrolysis, the cathode plate is stripped and washed to obtain porous foamed zinc, the cathode current efficiency is 62.30%, and the DC power consumption is 3947kW·h / t·Zn. The morphology of the obtained foamed zinc is as follows Figure 2 shown.

[0041] Example 2

[0042] A mixed solution of zinc sulfate and sulfuric acid is used as the electrolyte, wherein the zinc ion concentration is 45g / L and the sulfuric acid concentration is 160g / L. Gelatin, strontium carbonate, magnesium salt and pine oil are used as additives, wherein the magnesium ion concentration is 25g / L, the gelatin concentration is 1.5mg / L, the amount of gelatin added is controlled to be 0.02kg / t zinc according to the quality of cathode zinc deposition, the pine oil concentration is 0.20g / L, and the amount of strontium carbonate added is controlled to be 5.76kg / t zinc according to the quality of cathode zinc deposition. The cathode is a rolled aluminum plate, the anode is a lead-silver alloy plate containing 2.5% silver, and the cathode current density is 530A / m 2 , the electrolysis temperature is 40℃; the electrolyte adopts bottom-in-top-out circulation, and the circulation flow rate is 1 hour for the electrolyte in the electrolytic cell to be renewed once. After 24 hours of electrolysis, the cathode plate is stripped and washed to obtain porous foamed zinc, the cathode current efficiency is 71.93%, and the DC power consumption is 3373kW·h / t·Zn. The morphology of the obtained foamed zinc is as follows Figure 3 shown.

[0043] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for preparing zinc foam, characterized in that: include: An electrolysis device is provided, wherein the electrolyte in the electrolysis device comprises zinc ions, sulfate ions, magnesium ions, strontium carbonate and pine oil; Power is supplied for electrodeposition and gelatin is dripped into the electrolyte to deposit on the cathode plate of the electrolysis device to obtain zinc foam; The magnesium ion concentration in the electrolyte is 20g / L-40g / L; the pine oil concentration is 0.10g / L-0.20g / L; The electro-deposition by applying electricity specifically comprises: The anode plate of the electrolysis device is connected to the positive electrode of the power supply, and the cathode plate is connected to the negative electrode of the power supply, and direct current is passed for electrolysis; wherein the electrolysis temperature is 35°C-42°C, and the current density of the cathode plate is 480A / m 2 -550 A / m 2 .

2. The method for preparing zinc foam according to claim 1, characterized in that: The zinc ion concentration in the electrolyte is 30 g / L-50 g / L; the sulfate ion concentration is 100 g / L-180 g / L.

3. The method for preparing zinc foam according to claim 1, characterized in that: The gelatin is added in a ratio of 0.007-0.02 kg per ton of zinc.

4. The method for preparing zinc foam according to claim 1, characterized in that: The anode plate is an inert anode plate; the cathode plate is a rolled aluminum plate or a stainless steel plate.

5. The method for preparing zinc foam according to claim 1, characterized in that: The step of adding gelatin dropwise to the electrolyte comprises: Gelatin is dissolved in water to obtain a gelatin solution; the concentration of gelatin in the gelatin solution is 1 mg / L-3 mg / L.

6. The method for preparing zinc foam according to claim 1, characterized in that: The preparation method of the electrolyte comprises: Dissolving zinc sulfate and sulfuric acid in water to obtain a mixed solution; Magnesium salt, strontium carbonate and pine oil are respectively added to the mixed solution to obtain the electrolyte; the strontium carbonate is added in an amount of 5-10 kg per ton of zinc.