Lithium ion secondary battery and power-using device
By adding high thermal conductivity ceramic materials to the positive electrode active coating of lithium-ion secondary batteries, the problem of insufficient thermal conductivity in the thickness direction of the battery is solved, significantly improving heat dissipation performance and thermal safety, and ensuring that the battery can be used under fast charging conditions. security.
Patent Information
- Application Number
- CN202210841315.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-07-18
AI Technical Summary
Existing lithium-ion secondary batteries have poor thermal conductivity in the thickness direction, resulting in insufficient heat dissipation performance and prone to thermal runaway.
Adding thermally conductive ceramic materials, such as silicon carbide, silicon nitride, and aluminum nitride, to the positive active coating increases the thermal conductivity of the battery in the thickness direction, thereby improving heat dissipation performance and thermal safety.
By adding thermally conductive ceramic materials, the overall heat dissipation performance and thermal safety of the battery are significantly improved, ensuring the safety of the battery under efficient and fast charging conditions.
Smart Images

Figure BDA0003751187960000091 
Figure BDA0003751187960000101
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of secondary batteries, and in particular relates to a lithium ion secondary battery and an electric device. Background Art
[0002] With the promotion of new energy vehicles, their shortcomings of slow charging speed and long waiting time have been increasingly criticized. In order to make up for this defect, vehicle manufacturers have successively launched models with fast charging capabilities. However, lithium batteries generate a lot of heat under fast charging, and the power battery has poor thermal conductivity in the thickness direction (Y axis), which seriously limits the heat dissipation performance of the power battery. After heat accumulation, thermal runaway is very likely to occur. Therefore, it is particularly important to improve the heat dissipation performance of the power battery in the Y axis direction. Summary of the invention
[0003] The purpose of the present invention is to provide a lithium ion secondary battery in view of the shortcomings of the prior art, wherein a heat-conducting ceramic material is added to the positive electrode active coating, and the heat-conducting ceramic material has a high thermal conductivity, which can improve the thermal conductivity of the battery in the thickness direction, thereby improving the overall heat dissipation performance of the battery and improving the thermal safety of the battery.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] A lithium ion secondary battery comprises a positive electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active coating arranged on at least one surface of the positive electrode current collector, wherein the positive electrode active coating comprises a positive electrode active material and a thermally conductive ceramic material, wherein the thermal conductivity of the thermally conductive ceramic material is 200 to 320 W / m·K.
[0006] Wherein, the thermally conductive ceramic material accounts for 0.1-20% by weight of the positive electrode active coating.
[0007] Wherein, the thermally conductive ceramic material includes one or more of silicon carbide, silicon nitride and aluminum nitride.
[0008] The mass percentage of the thermally conductive ceramic material in the positive electrode active coating is R, and the surface density of the positive electrode active coating is W, and the two satisfy the following relationship: 0.5≤100*R / W≤500, the unit of R is wt%, and the unit of W is mg / 1540.25mm 2 .
[0009] The positive electrode active material includes one or more of a coated or uncoated layered lithium nickel cobalt manganese transition metal oxide or a coated or uncoated lithium nickel cobalt aluminum transition metal oxide, wherein the chemical formula of the coated or uncoated layered lithium nickel cobalt manganese transition metal oxide is Li x1 Ni (1-y1-z1-a1) Co y1 Mn z1M1 a1 O2, 0.90≤x1≤1.05, 0<y1≤0.2, 0<z1≤0.2, 0≤a1≤0.05, M1 is selected from one or more of Ti, Al, Zr, Mg, Zn, Ba, Mo, B; the chemical formula of the coated or uncoated lithium nickel cobalt aluminum transition metal oxide is Li x2 Ni (1-y2-z2-a2) Co y2 Al z2 M2 a2 O2, 0.90≤x2≤1.05, 0<y2≤0.1, 0<z2≤0.1, 0≤a2≤0.05, M2 is selected from one or more of Ti, Mn, Zr, Mg, Zn, Ba, Mo, and B.
[0010] Wherein, the positive electrode active material also includes olivine-type lithium phosphate LiFe 1-x3-y3 Mn x3 M3 y3 PO4, wherein 0≤x3≤1, 0≤y3≤0.1, 0≤x3+y3≤1, and M3 is selected from one or more of transition metal elements and non-transition metal elements except Fe and Mn.
[0011] Wherein, the lithium-ion secondary battery further comprises a negative electrode sheet, the negative electrode sheet comprises a negative electrode active material, and the negative electrode active material comprises one or more of graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microspheres, and silicon-based materials.
[0012] The lithium-ion secondary battery further comprises a separator, which is one of a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite membrane.
[0013] Wherein, the lithium-ion secondary battery further comprises a shell, and the material of the shell is stainless steel or aluminum-plastic film.
[0014] The second purpose of the present invention is to provide an electrical device with good heat resistance and thermal safety performance in view of the deficiencies in the prior art.
[0015] In order to achieve the above object, the present invention adopts the following technical solutions:
[0016] An electrical device comprises the above-mentioned lithium-ion secondary battery.
[0017] The electrical devices of the present invention include any one of a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini CD, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, and a large household battery.
[0018] Compared with the prior art, the beneficial effect of the present invention is that: in a lithium-ion secondary battery of the present invention, a thermally conductive ceramic material is added to the positive electrode active coating, and the thermally conductive ceramic material has a high thermal conductivity, which can improve the thermal conductivity of the battery in the thickness direction, thereby improving the overall heat dissipation performance of the battery and improving the thermal safety of the battery. DETAILED DESCRIPTION
[0019] The present invention will be described in further detail below in conjunction with specific implementation modes, but the implementation modes of the present invention are not limited thereto.
[0020] A lithium ion secondary battery comprises a positive electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active coating arranged on at least one surface of the positive electrode current collector, wherein the positive electrode active coating comprises a positive electrode active material and a thermally conductive ceramic material, wherein the thermal conductivity of the thermally conductive ceramic material is 200 to 320 W / m·K.
[0021] Traditional lithium-ion secondary batteries have metal pole pieces in the height direction, and the metal pole pieces have good thermal conductivity, which can quickly dissipate heat in the height direction. In the thickness direction, they have multiple layers of pole pieces and diaphragms, and the surfaces of the pole pieces and diaphragms are also coated. The multi-layer arrangement causes the heat dissipation rate of the battery in the thickness direction to be slow, thereby affecting the overall heat dissipation effect of the battery. A lithium-ion secondary battery of the present invention adds a thermally conductive ceramic material to the positive electrode active coating to increase the thermal conductivity in the thickness direction, so that the heat in the battery can be conducted and dissipated through layers of pole pieces and diaphragms, thereby improving the overall heat dissipation performance of the battery and improving the thermal safety of the battery.
[0022] In some embodiments, the thermally conductive ceramic material accounts for 0.1-20% of the weight of the positive electrode active coating. Preferably, the thermally conductive ceramic material accounts for 0.1-5%, 6-10%, 11-15%, 16-20% of the weight of the positive electrode active coating. Specifically, the thermally conductive ceramic material accounts for 0.1%, 0.5%, 6%, 12%, 16%, 20% of the weight of the positive electrode active coating. Preferably, the thermally conductive ceramic material accounts for 8% of the weight of the positive electrode active coating.
[0023] In some embodiments, the thermally conductive ceramic material includes one or more of silicon carbide, silicon nitride, and aluminum nitride. Silicon carbide is an inorganic substance with the chemical formula SiC. It is made of raw materials such as quartz sand, petroleum coke (or coal coke), and sawdust (salt needs to be added when producing green silicon carbide) through high-temperature smelting in a resistance furnace. Silicon nitride is an inorganic substance with the chemical formula Si3N4. It is an important structural ceramic material with high hardness, inherent lubricity, and wear resistance. It is an atomic crystal; it is resistant to oxidation at high temperatures. It can also resist thermal shocks. It will not break even if it is heated to more than 1000°C in air, cooled rapidly, and then heated rapidly. Aluminum nitride, a covalent bond compound with the chemical formula AIN, is an atomic crystal, belongs to diamond-like nitride, hexagonal system, and has a wurtzite-type crystal structure. It is non-toxic and white or grayish white. AlN can be stabilized up to 2200°C. It has high strength at room temperature, and its strength decreases slowly with increasing temperature. It has good thermal conductivity and a small thermal expansion coefficient, and is a good heat shock-resistant material. It has a strong ability to resist corrosion by molten metals and is an ideal crucible material for melting and casting pure iron, aluminum or aluminum alloys. Aluminum nitride is also an electrical insulator with good dielectric properties, and is also promising for use as an electrical component. The aluminum nitride coating on the surface of gallium arsenide can protect it from ion injection during annealing. Aluminum nitride is also a catalyst for the transformation of hexagonal boron nitride to cubic boron nitride. It reacts slowly with water at room temperature. It can be synthesized from aluminum powder at 800-1000°C in an ammonia or nitrogen atmosphere, and the product is a white to gray-blue powder. Or it can be synthesized by reacting the Al2O3-C-N2 system at 1600-1750°C, and the product is an off-white powder. Or it can be obtained by gas phase reaction of aluminum chloride and ammonia. The coating can be synthesized by vapor deposition from the AlCl3-NH3 system.
[0024] AlN+3H2O==catalyst===Al(OH)3↓+NH3↑.
[0025] The thermally conductive ceramic material of the present invention has stable performance and good thermal conductivity. When added to the positive electrode active coating of the battery, it can improve the heat dissipation performance of the battery in the thickness direction, thereby improving the overall heat dissipation performance of the battery.
[0026] In some embodiments, the mass percentage of the thermally conductive ceramic material in the positive electrode active coating is R, and the surface density of the positive electrode active coating is W, and the two satisfy the following relationship: 0.5≤100*R / W≤500, the unit of R is wt%, and the unit of W is mg / 1540.25mm 2 When there is a certain relationship between the mass percentage R of the thermally conductive ceramic material in the positive electrode active coating and the surface density W of the positive electrode active coating, the thermal conductivity of the positive electrode sheet is better. The thicker the surface density of the positive electrode active coating, the worse the heat dissipation performance of the battery in the thickness direction, and more thermally conductive ceramic material needs to be added to offset the increase in the thickness direction of the thermally conductive ceramic material.
[0027] In some embodiments, the positive electrode active material includes one or more of a coated or uncoated layered lithium nickel cobalt manganese transition metal oxide or a coated or uncoated lithium nickel cobalt aluminum transition metal oxide, wherein the chemical formula of the coated or uncoated layered lithium nickel cobalt manganese transition metal oxide is Li x1 Ni (1-y1-z1-a1) Co y1 Mn z1 M1 a1 O2, 0.90≤x1≤1.05, 0<y1≤0.2, 0<z1≤0.2, 0≤a1≤0.05, M1 is selected from one or more of Ti, Al, Zr, Mg, Zn, Ba, Mo, B; the chemical formula of the coated or uncoated lithium nickel cobalt aluminum transition metal oxide is Li x2 Ni (1-y2-z2-a2) Co y2 Al z2 M2 a2 O2, 0.90≤x2≤1.05, 0<y2≤0.1, 0<z2≤0.1, 0≤a2≤0.05, M2 is selected from one or more of Ti, Mn, Zr, Mg, Zn, Ba, Mo, and B.
[0028] In some embodiments, the positive electrode active material further comprises an olivine-type lithium phosphate such as LiFe 1-x3- y3 Mn x3 M3 y3 PO4, wherein 0≤x3≤1, 0≤y3≤0.1, 0≤x3+y3≤1, and M3 is selected from one or more of transition metal elements and non-transition metal elements except Fe and Mn.
[0029] In some embodiments, the lithium-ion secondary battery further comprises a negative electrode sheet, the negative electrode sheet comprises a negative electrode active material, the negative electrode active material comprises one or more of graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microspheres, and silicon-based materials. The silicon-based material may be selected from one or more of elemental silicon, silicon-oxygen compounds, silicon-carbon composites, and silicon alloys.
[0030] In some embodiments, the thermal conductivity of the thermally conductive ceramic material is 200 to 320 W / m·K. The thermally conductive ceramic material of the present invention has a relatively high thermal conductivity, and can be added to the positive electrode active coating to improve the thermal conductivity of the positive electrode active coating, thereby allowing the battery to have fast and effective thermal conductivity in the thickness direction, allowing the heat inside the battery to be dissipated in the horizontal and vertical directions, greatly improving the thermal conductivity and heat dissipation performance, thereby improving the thermal safety performance of the secondary battery.
[0031] In some embodiments, the lithium ion secondary battery further comprises a separator, which is one of a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite membrane. Preferably, the lithium ion secondary battery uses a polyethylene porous membrane.
[0032] In some embodiments, the lithium-ion secondary battery further comprises a shell, and the shell is made of stainless steel or aluminum-plastic film. Stainless steel has high hardness, and the aluminum-plastic film has certain hardness and plasticity, and can be shaped according to the shape of the battery core, and is easy to process.
[0033] In some embodiments, the lithium-ion secondary battery further includes a separator, an electrolyte, and a shell. The separator is used to separate the positive electrode sheet and the negative electrode sheet, and the shell is used to package and install the positive electrode sheet, the separator, the negative electrode sheet, and the electrolyte.
[0034] In some embodiments, the positive electrode current collector is generally a structure or part that collects current. The positive electrode current collector can be any material in the art that is suitable for use as a positive electrode current collector for lithium-ion batteries. For example, the positive electrode current collector can include but is not limited to metal foil, and more specifically can include but is not limited to aluminum foil.
[0035] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active coating disposed on at least one surface of the negative electrode current collector, the negative electrode active coating includes the above-mentioned negative electrode active material, the negative electrode current collector can be various materials in the art suitable for use as a negative electrode current collector for lithium-ion batteries, for example, the negative electrode current collector can be including but not limited to metal foil, more specifically can be including but not limited to copper foil, etc.
[0036] The lithium-ion battery also includes an electrolyte, which includes an organic solvent, an electrolyte lithium salt and an additive. Among them, the electrolyte lithium salt can be LiPF6 and / or LiBOB used in high-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, and LiPF6 used in low-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, LiPF6, and LiTFSI used in anti-overcharge electrolytes; it can also be at least one of LiClO4, LiAsF6, LiCF3SO3, and LiN(CF3SO2)2. The organic solvent can be a cyclic carbonate, including PC and EC; it can also be a chain carbonate, including DFC, DMC, or EMC; it can also be a carboxylic acid ester, including MF, MA, EA, MP, etc. The additives include but are not limited to at least one of film-forming additives, conductive additives, flame retardant additives, anti-overcharge additives, additives for controlling the content of H2O and HF in the electrolyte, additives for improving low-temperature performance, and multifunctional additives.
[0037] Example 1
[0038] A lithium ion secondary battery comprises a positive electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active coating arranged on at least one surface of the positive electrode current collector, wherein the positive electrode active coating comprises a positive electrode active material and a thermally conductive ceramic material, wherein the thermal conductivity of the thermally conductive ceramic material is 300 to 320 W / m·K.
[0039] (1) Preparation of positive electrode
[0040] LiNi 1.5 Co 0.1 Mn 0.12 Ti 0.02 The positive electrode active material of O2, the conductive agent superconducting carbon and carbon tube, the binder polyvinylidene fluoride and the silicon nitride thermal conductive ceramic material are mixed uniformly in a mass ratio of 88:2.0:0.5:1.5:8 to form a positive electrode slurry, and the positive electrode slurry is coated on one surface of the current collector aluminum foil and dried at 85°C to form a positive electrode coating. The surface density of the positive electrode active coating is 120mg / 1540.25mm 2 After the pole piece is rolled up, the positive electrode slurry is coated and dried on the other side of the aluminum foil according to the above method, and then the pole piece with the positive electrode active material layer coated on both sides of the aluminum foil is cold pressed; trimming, cutting and stripping are performed, and after stripping, the positive pole piece of the lithium-ion battery is made.
[0041] (2) Preparation of negative electrode sheet
[0042] The silicon-carbon negative electrode active material, the conductive agent superconducting carbon, the thickener sodium carboxymethyl cellulose, and the binder styrene-butadiene rubber are prepared into a negative electrode slurry in a mass ratio of 96.5:1.0:1.0:1.5, coated on the current collector copper foil and dried and rolled at 85°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with a negative electrode active material layer on both sides is cold pressed; trimming, cutting, and stripping are performed, and after stripping, a lithium-ion battery negative electrode sheet is made.
[0043] (3) Diaphragm: A polyethylene porous film with a thickness of 7 μm was selected as the diaphragm.
[0044] (4) Preparation of electrolyte:
[0045] Lithium hexafluorophosphate (LiPF6) is dissolved in a mixed solvent of dimethyl carbonate (DEC), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) (the mass ratio of the three is 3:5:2) to obtain an electrolyte.
[0046] (5) Preparation of batteries:
[0047] The positive electrode sheet, separator and negative electrode sheet are wound into a battery cell with a capacity of about 5Ah. The separator is located between adjacent positive and negative electrode sheets, the positive electrode is spot welded out with an aluminum tab, and the negative electrode is spot welded out with a nickel tab; the battery cell is then placed in an aluminum-plastic packaging bag, baked, and injected with the above electrolyte, and finally made into a lithium-ion battery through packaging, formation, capacity division and other processes.
[0048] Example 2
[0049] The difference from Example 1 is that the thermally conductive ceramic material accounts for 0.5% of the weight of the positive electrode active coating.
[0050] The rest is the same as Example 1 and will not be described again here.
[0051] Example 3
[0052] The difference from Example 1 is that the thermally conductive ceramic material accounts for 3% of the weight of the positive electrode active coating.
[0053] The rest is the same as Example 1 and will not be described again here.
[0054] Example 4
[0055] The difference from Example 1 is that the thermally conductive ceramic material accounts for 12% of the weight of the positive electrode active coating.
[0056] The rest is the same as Example 1 and will not be described again here.
[0057] Example 5
[0058] The difference from Example 1 is that the thermally conductive ceramic material accounts for 18% of the weight of the positive electrode active coating.
[0059] The rest is the same as Example 1 and will not be described again here.
[0060] Example 6
[0061] The difference from Example 1 is that the positive electrode active material is Li 0.92 Ni 0.77 Co 0.1 Mn 0.1 Mg 0.03 O2.
[0062] The rest is the same as Example 1 and will not be described again here.
[0063] Example 7
[0064] The difference from Example 1 is that the positive electrode active material is Li 0.95 Ni 0.9 Co 0.01 Mn 0.08 B 0.01O2.
[0065] The rest is the same as Example 1 and will not be described again here.
[0066] Example 8
[0067] The difference from Example 1 is that the positive electrode active material is carbon-coated Li 0.93 Ni 0.89 Co 0.05 Al 0.02 M2 0.0 4O2.
[0068] The rest is the same as Example 1 and will not be described again here.
[0069] Example 9
[0070] The difference from Example 1 is that the positive electrode active material is carbon-coated Li 0.94 Ni 0.91 Co 0.03 Al 0.01 M2 0.0 2O2.
[0071] The rest is the same as Example 1 and will not be described again here.
[0072] Example 10
[0073] The difference from Example 1 is that the positive electrode active material is olivine-type lithium phosphate, and its chemical formula is LiFe 0.24 Mn 0.8 V 0.06 PO4.
[0074] The rest is the same as Example 1 and will not be described again here.
[0075] Comparative Example 1
[0076] The difference from Example 1 is that the positive electrode active coating includes NCM811 positive electrode active material, conductive agent superconducting carbon and carbon tube, and binder polyvinylidene fluoride, which are mixed uniformly in a mass ratio of 96:2.0:0.5:1.5 to form a positive electrode slurry.
[0077] The rest is the same as Example 1 and will not be described again here.
[0078] The electrodes of the above-mentioned embodiments 1-10 and comparative example 1 were tested for thermal conductivity in the thickness direction, and the test results are recorded in Table 1.
[0079] Thermal conductivity test in thickness direction: The thermal conductivity of the pole piece in thickness direction is tested using the TCA 3DP method. The instrument used is a 3D thermal property analyzer based on infrared thermal imager temperature measurement and three-dimensional data inversion technology. The equipment applies pulse excitation to the bottom of the soft-pack lithium battery through a flexible electric heater, uses an infrared thermal imager for non-contact temperature measurement on one side of the battery, and calculates the longitudinal and lateral thermal conductivity of the battery through data inversion.
[0080] (i) Sample preparation
[0081] The batteries of Examples 1-10 and Comparative Example 1 were all charged to 100% SOC and numbered respectively.
[0082] (ii) Testing process
[0083] The thermal conductivity of the samples was measured using TCA 3DP-1603D thermal property analyzer (hereinafter referred to as TCA 3DP method), and each sample was measured 6 times. In order to compare and verify the accuracy of the results measured by TCA 3DP method and Hot Disk method, the longitudinal thermal conductivity of the samples was measured using the steady-state method, and each sample was tested 2 times, and the average value was calculated and recorded in Table 1.
[0084] Table 1
[0085]
[0086]
[0087] It can be concluded from Table 1 that the electrode of the present invention has better thermal conductivity in the thickness direction than that of the comparative example 1. Specifically, the thermal conductivity of the present embodiment 1 in the thickness direction is improved by 24.05% compared with that of the comparative example 1, which is a significant improvement.
[0088] From the comparison of Examples 1-5, it can be concluded that when the thermally conductive ceramic material accounts for 8 parts by weight of the positive electrode active coating, the thermal conductivity of the prepared electrode sheet is higher and the performance is better.
[0089] By comparing Examples 1, 6-10, it is found that when the positive electrode active material is LiNi 1.5 Co 0.1 Mn 0.12 Ti 0.02 When O2 is used, the prepared electrode has better performance.
[0090] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A lithium ion secondary battery, It is characterized in that The positive electrode sheet comprises a positive electrode current collector and a positive electrode active coating disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active coating comprises a positive electrode active material and a thermally conductive ceramic material, wherein the thermal conductivity of the thermally conductive ceramic material is 200 to 320 W / m·K; The positive electrode active material is LiNi 1 .5 Co 0 .1 Mn 0 .12 Ti 0 .02 O 2 .
2. The lithium ion secondary battery according to claim 1, It is characterized in that The thermally conductive ceramic material accounts for 0.1-20% of the weight of the positive electrode active coating.
3. The lithium ion secondary battery according to claim 1, It is characterized in that The thermally conductive ceramic material includes one or more of silicon carbide, silicon nitride and aluminum nitride.
4. The lithium ion secondary battery according to claim 1, It is characterized in that The lithium-ion secondary battery further comprises a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, wherein the negative electrode active material comprises one or more of graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microspheres, and silicon-based materials.
5. The lithium ion secondary battery according to claim 1, It is characterized in that The lithium ion secondary battery further comprises a separator, which is one of a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite membrane.
6. The lithium ion secondary battery according to claim 1, It is characterized in that The lithium-ion secondary battery further comprises a shell, and the shell is made of stainless steel or aluminum-plastic film.
7. An electrical device, It is characterized in that A lithium ion secondary battery comprising the lithium ion secondary battery according to any one of claims 1 to 6.