Highly tough, conductive PEEK for aircraft fuel systems
By using a combination of high-temperature PEEK polymer matrix and conductive and dielectric fillers in aerospace fuel systems, the tensile strength and elongation at break of the material are improved, and the problem of material deformation during high temperature and bending processing in the existing technology is solved. It solves the problem of brittleness, meets the requirements of aerospace fuel systems for electrostatic discharge and lightning strike protection, and provides high-performance conductive composite materials.
Patent Information
- Application Number
- CN202210362319.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-04-07
AI Technical Summary
It is difficult for existing polymer composites to simultaneously meet electrostatic discharge (ESD) specifications, lightning protection and structural strength requirements in aerospace fuel systems. In particular, they tend to become brittle and hard during high temperatures and bending processes, making them unsuitable for fuel pipes, etc. application.
Using a conductive composite material composed of a high-temperature PEEK polymer matrix, conductive fillers (such as carbon nanotubes), dielectric fillers (such as fumed silica) and dispersed processing aids (such as POSS), by adjusting the filler ratio and composition structure , improve the tensile strength, elongation at break and toughness modulus of the material, and meet the conductivity and lightning protection requirements of the Radio Technical Committee for Aeronautics (RTCA) DO-160 standard.
It achieves high strength, toughness and ductility at room temperature and high temperature, meets the multiple requirements of aerospace fuel delivery systems for conductivity and structural performance, and provides high-performance materials suitable for components such as fuel pipes.
Smart Images

Figure CN115304902B_ABST
Abstract
Description
Background Art
[0001] The need for improved fuel efficiency in the aerospace industry has led to tremendous developments in the field of polymer composites to reduce weight while maintaining the structural integrity of aircraft and aircraft components used in fuselage, wing and cabin applications. In order to further reduce the weight of the aircraft and simplify the architecture of the aircraft, composite materials must also be introduced in the fuel delivery system (e.g., including fuel pipes, reducers, flanges, brackets, etc.). In order to successfully use polymer composites in aerospace fuel systems, the material needs to have customized electrical conductivity to meet electrostatic discharge (ESD) specifications and lightning strike protection that meets the Radio Technical Commission for Aeronautics (RTCA) DO-160 (environmental) standard. In addition, during manufacturing, assembly and use, the material needs to have high strength, ductility and toughness to meet structural load requirements and withstand rigorous post-processing steps such as hot bending and test evaluation.
[0002] Historically, fillers such as carbon black, graphite, and carbon fibers have been used to develop conductive polymers with ESD performance. 5 Up to 10 8 This resistance range typically requires >10 wt% filler. At such high filler loadings, the polymer becomes brittle and stiff, making these polymers unsuitable for applications such as fuel lines, which require post-processing such as bending and thermoforming.
[0003] High temperature polymers such as PEEK have good tensile properties, chemical resistance, thermal stability, and have relatively high ductility and elongation at break typically between 25% and 45%, theoretically making these high temperature polymers suitable for replacing aluminum metal fuel pipes.
[0004] Commercially available PEEK-carbon nanotube (CNT) composite polymers have suitable resistance for ESD discharge, but unfortunately, their elongation at break may only be between 2% and 5%, so these materials may not be suitable for fuel pipe applications.
[0005] US Patent No. 10,435,539 to Mapkar et al. describes solid polymer composites, for example, including polyamide or polyetheretherketone, carbon nanotubes, and spherical nanodiamond additives.
[0006] US 20130206273, Guest et al. describe a downhole composite component comprising a polymer matrix including a thermosetting or thermoplastic polymer, a nanoparticle filler, and reinforcing fibers.
[0007] US 20140091253, Myllymaki et al. describe a nanodiamond-containing thermoplastic thermocomposite material comprising nanodiamonds, a thermoplastic polymer and a filler such as a boron nitride filler.
[0008] Improved and economical electrically conductive composites with improved strength and toughness that include tailored electrical conductivity for ESD and lightning strike protection required for non-metallic fuel delivery systems are desired. Summary of the invention
[0009] The present disclosure provides economical conductive composites prepared from compositions comprising high temperature PEEK polymers having improved strength and toughness as compared to a base PEEK polymer and tailored conductivity for ESD and lightning strike protection to meet or exceed the electrostatic discharge (ESD) specifications and lightning strike protection compliant with the Radio Technical Commission for Aeronautics (RTCA) DO-160 (Environmental) standard.
[0010] The present disclosure provides a solid polymer conductive composite material comprising a polyaryletherketone (PAEK) polymer, a conductive filler, a dispersion processing aid and a dielectric filler. The PAEK polymer may be selected from the group consisting of polyetheretherketone (PEEK) and polyetherketoneketone (PEKK).
[0011] The matrix PEEK polymer may be a medium to high viscosity PEEK polymer.The matrix PEEK polymer may be unreinforced.
[0012] The conductive filler may be selected from the group consisting of carbon nanotubes, graphene, graphene oxide, carbon nanofibers and carbon nanostructures.
[0013] The dispersion processing aid may be selected from cage silsesquioxane (POSS), silane and silanol-POSS. The dielectric filler may be selected from the group consisting of nanoalumina, nanosilica, fumed alumina, fumed silica, ZnO and TiO2. In some embodiments, the conductive composite does not contain nanodiamond fillers.
[0014] The solid polymer composite may include from about 90 wt % to about 99 wt % of a polyetheretherketone (PEEK) matrix polymer.
[0015] The solid polymer composite may include from about 0.25 wt % to about 5 wt % of the conductive filler.
[0016] The solid polymer composite may contain from about 0.25 wt % to about 5 wt % of a dispersion processing aid.
[0017] The solid polymer composite may include from about 0.05 wt % to about 3 wt % of the dielectric filler.
[0018] The solid polymer composite material according to the present disclosure may exhibit one or more of a tensile strength of at least 80 MPa at room temperature (73°F); an elongation at break of at least 20%; and a tensile strength of at least 10 MPa. 5 Ω and 10 8 Ω resistance; at least 95MPa or greater maximum tensile strength; at least 15MPa or greater toughness modulus; and at least 60KJ / m2 or greater Izod notched impact strength.
[0019] Non-metallic fuel delivery system components for aircraft can be prepared from the conductive composite materials according to the present disclosure. The aircraft components can be fuel pipes, hoses, couplings, clamps, conduits, reducers, flanges, ferrules, brackets and housings.
[0020] A non-metallic fuel hose is provided, comprising at least one layer prepared from a conductive composite composition according to the present disclosure. A non-metallic fuel hose is provided, comprising a single layer prepared from a conductive composite composition according to the present disclosure. The fuel hose may exhibit a resistance between 100 KΩ and 100 MΩ / 15"; a maximum operating pressure of at least 120 psi; a continuous operating temperature from -65°F or less to at least 275°F; an excursion operating temperature of at least 325°F; and comply with RTCA DO-160 environmental standards.
[0021] A solid polymer conductive composite is provided, which is prepared from a composition comprising: 90 wt%-99 wt% PEEK polymer; 0.25 wt%-5.0 wt% conductive filler; 0 wt%-3 wt% dielectric filler; and 0.25 wt%-5.0 wt% dispersion processing aid. The solid polymer conductive composite can be prepared from a composition comprising: 95 wt%-98.5 wt% PEEK polymer; 0.5 wt%-3.0 wt% conductive filler; 0.5 wt%-2 wt% dielectric filler; and 0.5 wt%-3.0 wt% dispersion processing aid. The solid polymer conductive composite can be prepared from a composition comprising: 95 wt%-98.5 wt% PEEK polymer; 0.5 wt%-3.0 wt% carbon nanotubes; 0.5 wt%-2 wt% fumed silica; and 0.5 wt%-3.0 wt% POSS. A solid polymer conductive composite is provided, which is prepared from a composition comprising: 96 wt%-98.5 wt% of a PEEK polymer; 0.5 wt%-2.0 wt% of a conductive filler; 0.5 wt%-1.5 wt% of a dielectric filler; and 0.5 wt%-2.0 wt% of a dispersed processing aid. In some embodiments, the solid polymer conductive composite includes a total of no more than 5 wt% of the combined fillers.
[0022] According to ASTM D638, the conductive composite material may exhibit a tensile strength of 100 MPa or more at room temperature. When measured at room temperature according to ASTM D638, the elongation at break may be 20% or more, 30% or more, 60% or more, 70% or more, 80% or more, or 90% or more. The modulus of toughness measured according to the area under the tensile stress-strain curve may be 18 MPa or more. The maximum tensile strength may be 100 MPa or more. The tensile strength at -65°F may be 140 MPa or more. The tensile strength at 73°F may be 90 MPa or more. The tensile strength at 275°F may be 50 MPa or more. The tensile modulus at -65°F may be 4.5 GPa or more. The tensile modulus at 73°F may be 4.0 GPa or more. The tensile modulus at 275°F may be 3.5 GPa or more. The notched Izod impact strength at -65°F may be 15 KJ / m2 or more. The Izod notched impact strength at 73°F may be 16KJ / m2 or higher. The Izod notched impact strength at 275°F may be 100KJ / m2 or higher.
[0023] The composite polymer may be a conductive composite polymer. The conductive composite polymer may be prepared from a conductive composite composition.
[0024] In some embodiments, the conductive composite composition may include a matrix PEEK polymer in an amount between 90 wt % and 99 wt %, 95 wt % and 99 wt %, or 96 wt % and 98.5 wt %. In some embodiments, the conductive composite composition may include a conductive filler in an amount between 0.5 wt % and 5.0 wt %, 0.5 wt % and 3 wt %, or 0.5 wt % and 2 wt %. In some embodiments, the conductive composite composition may include a dielectric filler in an amount between 0 wt % and 3 wt %, 0 wt % and 2 wt %, 0.5 wt % and 2 wt %, or 0.5 wt % and 1.5 wt %. In some embodiments, the conductive composite composition may include a dispersing processing aid in an amount between 0.3 wt % and 5.0 wt %, 0.5 wt % and 3 wt %, or 0.5 wt % and 2.0 wt %.
[0025] In some embodiments, the conductive composite composition may include 90 wt% to 99 wt% of a matrix PEEK polymer, 0.5 wt% to 5.0 wt% of a conductive filler, 0 wt% to 3 wt% of a dielectric filler, and 0.3 wt% to 5.0 wt% of a dispersed processing aid.
[0026] In some embodiments, the conductive composite composition may include 95 wt % to 99 wt % of a matrix PEEK polymer, 0.5 wt % to 3 wt % of a conductive filler, 0.5 wt % to 2 wt % of a dielectric filler, and 0.5 wt % to 3 wt % of a dispersed processing aid.
[0027] In some embodiments, the conductive composite composition may include 96 wt % to 98.5 wt % of a matrix PEEK polymer, 0.5 wt % to 2 wt % of a conductive filler, 0.5 wt % to 1.5 wt % of a dielectric filler, and 0.5 wt % to 2.0 wt % of a dispersed processing aid.
[0028] The composite polymer may exhibit a tensile strength of at least 80 MPa, at least 90 MPa, or at least 100 MPa at room temperature (73°F).
[0029] The composite polymer may exhibit an elongation at break of at least 20%, at least 30%, at least 40%, at least 50%, at least 60%, or at least 70%.
[0030] The composite polymer may be an ESD composite polymer having a resistance between 100 KΩ and 100 MΩ / 15".
[0031] The composite polymer may have a 5 Ω and 10 8 Ω of resistance between the ESD polymer composites.
[0032] The composite polymer may exhibit a maximum tensile strength of 95 MPa or greater, or 100 MPa or greater.
[0033] The composite polymer may exhibit a toughness modulus of at least 15 MPa or at least 18 MPa.
[0034] The composite polymer may exhibit a notched Izod impact strength at 275°F of at least 60 KJ / m2, at least 80 KJ / m2, or at least 100 KJ / m2. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 A schematic diagram of an exemplary non-metallic fuel delivery system is shown.
[0036] Figure 2A A pie chart showing the weight reduction ratio and associated fuel savings (20% overall) of aluminum components including fuel pipes, flanges, couplings, accessories and brackets replaced with components made of the conductive composite material of the present invention based on a single-aisle aircraft fuel delivery system.
[0037] Figure 2B An aircraft tube process diagram is shown, including mixing PAEK composite polymer with carbon nanotube filler, tube extrusion, overmolding of sleeve, thermoforming / tube bending and assembly. High strength and toughness are important for the bending and assembly steps.
[0038] Figure 3From left to right, a bar graph of the tensile strength (MPa) at room temperature of comparative matrix PEEK 1, comparative matrix PEEK 2, PEEK 1 composite polymer sample of the present invention, PEEK 2 composite polymer sample of the present invention, and four comparative commercial PEEK CNT samples is shown. According to ASTM D638, both the sample of the present invention and a commercial PEEK with conductive CNT sample exhibited a tensile strength of >100 MPa at room temperature.
[0039] Figure 4 From left to right, a bar graph of the elongation at break (%) of the comparative matrix PEEK 1, the comparative matrix PEEK 2, the PEEK 1 composite polymer sample of the present invention, the PEEK 2 composite polymer sample of the present invention, and four comparative commercial PEEK CNT samples at room temperature is shown. The elongation at break of each of the matrix PEEK 1 and matrix PEEK 2 samples is >20%. The elongation at break of the PEEK 1 composite polymer sample of the present invention is >30%, and the elongation at break of the PEEK 2 composite polymer sample of the present invention is >80%. However, all four commercial PEEK samples with conductive CNT fillers exhibit an elongation at break of <4%.
[0040] Figure 5 Stress-strain data plots are shown for two different formulations of PEEK 2 composite polymer samples of the present invention and a comparative PEEK 2 sample. The tensile stress (MPa) was plotted against the tensile strain (mm / mm) to obtain the stress-strain curves.
[0041] The PEEK 2 composite polymer formulation 2 sample of the present invention exhibited a stress-strain curve indicating that the sample was hard and ductile, and the PEEK 2 composite polymer formulation 1 sample of the present invention exhibited a stress-strain curve indicating that the sample was hard and tough, while the comparative matrix PEEK 2 sample exhibited a stress-strain curve indicating that the sample was hard and brittle.
[0042] Figure 6 A bar graph of mechanical properties including maximum tensile strength (MPa) and elongation at break (%) of a comparative matrix PEEK 1 sample, a comparative matrix PEEK 2 sample, a PEEK 1 composite polymer sample of the present invention, and a PEEK 2 composite polymer sample of the present invention is shown. The sample of the present invention exhibits a maximum tensile strength similar to or slightly greater than that of the comparative matrix PEEK 1 (98.7MPa) sample and the comparative matrix PEEK 2 (93.6MPa) sample (101.5MPa, 104.1MPa, respectively). The composite polymer sample of the present invention exhibits a significantly higher elongation at break (%) than the comparative matrix PEEK 1 sample and the comparative matrix PEEK 2 sample, which is 2 times or 3 times greater.
[0043] Figure 7 A bar graph showing the toughness modulus (MPa) of the comparative matrix PEEK 1 sample and the comparative matrix PEEK 2 sample, the inventive PEEK 1 composite polymer sample and the inventive PEEK 2 composite polymer sample. The inventive composite polymer sample exhibits increased toughness compared to the PEEK 1 comparative sample and the PEEK 2 comparative sample.
[0044] Figure 8 A bar graph of the tensile strength (MPa) of the comparative matrix PEEK 1 sample and the comparative matrix PEEK 2 sample, the PEEK 1 composite polymer sample of the present invention, and the PEEK 2 composite polymer sample of the present invention at three temperatures (-65°F, 73°F, 275°F) is shown. At each of the three temperatures, the comparative polymer, the PEEK 1 composite polymer of the present invention, and the PEEK 2 composite polymer of the present invention exhibit comparable tensile strength.
[0045] Fig. 9 A bar graph of the tensile modulus (GPa) of the comparative matrix PEEK 1 sample and the comparative matrix PEEK 2 sample, the PEEK 1 composite polymer sample of the present invention, and the PEEK 2 composite polymer sample of the present invention at three temperatures (-65°F, 73°F, 275°F) is shown. At each of the three temperatures, the comparative polymer, the PEEK 1 composite polymer of the present invention, and the PEEK 2 composite polymer of the present invention exhibit comparable tensile moduli.
[0046] Fig.10 A bar graph showing the Izod notched impact strength of a comparative matrix PEEK 2 sample and the inventive PEEK 2+CNT-2 sample at three temperatures of -65°F, 73°F, and 275°F is shown. The inventive sample exhibits significantly improved impact strength of at least about 2 times or more than the comparative sample at each of the three temperatures.
[0047] Fig.11 Shown are photographs of comparative matrix PEEK 2 samples that fractured or hinged during notched Izod impact strength testing at an elevated temperature of 275°F.
[0048] Fig. 12A A photograph of a PEEK1 composite polymer tube sample of the present invention having a 2" OD and a 0.05" wall thickness after impact testing is shown. The tube sample showed no signs of failure after a 35J impact. After impact testing, the tube sample was subjected to both proof pressure and burst pressure. The tube burst at approximately 410 psi and did not fail at the point of impact.
[0049] Fig. 12BA photograph of a PEEK2 composite polymer tube sample of the present invention having a 2" OD and a 0.05" wall thickness after impact testing is shown. The tube sample withstood 35J and 50J impacts and ultimately failed in a 65J impact. After the impact test, the tube sample was subjected to both a withstand pressure and a burst pressure. Similar to the PEEK 1 composite polymer sample tube of the present invention, the PEEK2 composite polymer sample tube of the present invention burst at approximately 410psi and did not fail at the impact point.
[0050] Fig.13 A bar graph of tensile fatigue is shown showing that at room temperature, 5 Hz, 73 MPa, ESD PEEK with high toughness according to the present disclosure exhibits greater than 2,250,000 fatigue cycles relative to fatigue cycles of a comparative base PEEK, ESD PEEK with lower toughness. DETAILED DESCRIPTION
[0051] The present disclosure provides composite compositions and polymer materials with tailored conductivity for electrostatic discharge (ESD) while increasing the strength and toughness of the base PEEK (polyetheretherketone) polymer to about 2 times that of the base PEEK polymer, and achieving an improved elongation at break of up to 60% to 120%, which may be about 2 times to about 3 times that of the base PEEK. This allows the design of strong, high impact strength, improved fatigue resistance and more resilient fuel pipes and other fuel system components compared to commercially available ESD PEEK.
[0052] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the concepts of the present disclosure.
[0053] Unless the context clearly indicates otherwise, as used herein, the singular forms "a", "an" and "the" are intended to include the plural forms as well. The term "and / or" refers to and encompasses any and all possible combinations of one or more of the associated listed items.
[0054] When referring to an amount of a measurable value such as a mixture, dosage, time, temperature, etc., the term "about" is meant to encompass variations of 10%, 5%, 1%, 0.5% or even 0.1% of the specified amount.
[0055] The terms “include” and / or “comprises” used in this specification indicate the presence of the described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0056] Unless otherwise defined, all terms (including technical and scientific terms) used in this specification have the same meaning as commonly understood by ordinary technicians in the field to which the present disclosure belongs. In the event of a conflict in terms, the present specification shall prevail.
[0057] All patents, patent applications, and publications mentioned herein are incorporated by reference in their entirety.
[0058] The embodiments described in one aspect of the present disclosure are not limited to the described aspects. As long as these embodiments do not hinder these aspects of the present disclosure from being applied to the intended purposes of the present disclosure, these embodiments may also be applied to different aspects of the present disclosure.
[0059] Unless otherwise indicated, the term "room temperature" means approximately 73°F (23°C).
[0060] The disclosure provides customizable nanocomposite polymers, which have higher ductility and toughness than independent matrix polymers, and impart functional properties such as electrical conductivity and thermal conductivity. When adopting different chemical compositions, the size and shape of nanofillers and appropriate ratios to enhance the performance of nanocomposite materials, synergistic behavior has been found, which may not be obvious when adding independent nanofillers. Every kind of filler material can impart unique performance to composite materials and enhance the performance of this composite material, so that these materials can be used for metal substitutes in aerospace and automotive applications.
[0061] The present invention provides a lightweight non-metallic fuel delivery system that is compatible with static electricity and lightning and exhibits increased strength and toughness compared to the matrix polymer alone or compared to commercially available PEEK-carbon nanotube materials. Figure 1 As shown, the fuel delivery system may include tubes, flanges, joints, couplings, accessories, brackets, ferrules, sleeves and gaskets. The tube may be a fuel tube. The tube may include a rotary bend. The tube may be an extruded tube. The accessories may include mounting accessories. The flanges may include overmolded flanges. The gaskets may include conductive gaskets. The lightweight non-metallic fuel delivery system will result in weight reduction (approximately 20%) and fuel savings, as well as system-level cost reduction, and maintain the installation strategy of curved tubes and flexible couplings. As shown Figure 2A As shown, based on a single-channel aircraft fuel delivery system, the aluminum components including pipes, flanges, couplings, accessories and brackets are replaced with parts made of the conductive composite material of the present invention, thereby predicting weight reduction and related fuel savings (overall 20%). Replacement of the aircraft fuel delivery system fuel pipe is expected to contribute to the largest proportion of weight reduction. Figure 2BAn aircraft tube process diagram is shown, including mixing PAEK composite polymer with carbon nanotube filler, tube extrusion, overmolding of sleeve, thermoforming / tube bending and assembly. High strength and toughness are important for the bending and assembly steps.
[0062] Generally, the polymer composite can be prepared by providing a polyaryletherketone polymer, adding a conductive filler (such as carbon nanotubes), one or more dispersed processing fillers, and optionally a dielectric filler. The combination described herein produces a synergistic enhancement effect in the structural properties of the non-metallic composite polymer.
[0063] The present disclosure provides a conductive composite polymer comprising a matrix polymer, a conductive filler, a dielectric filler, and one or more dispersed processing fillers. In some embodiments, the conductive composite polymer does not contain a polyamide (such as a nylon material).
[0064] The matrix polymer may be a thermoplastic polyaryletherketone polymer (PAEK). PAEK is a linear aromatic polyetherketone polymer. The PAEK polymer may be selected from the group consisting of polyetheretherketone (PEEK) and polyetherketoneketone (PEKK). The structures of PEEK and PEKK have aromatic rings with different ratios of ether and ketone groups. PEKK has a second ketone group in its repeating structure.
[0065] PEEK polymers can be obtained by dialkylation step-growth polymerization of bisphenolates. This involves reacting 4,4'-difluorobenzophenone or 1,4-bis(4-fluorobenzoyl)benzene with hydroquinone in the presence of an alkali metal carbonate. The polymer is then isolated by removing the alkali metal fluoride and the polymerization solvent.
[0066] The PEEK polymer may be a commercially available PEEK polymer. The PEEK polymer may be selected from: for example, Victrex PEEK, such as VICTREX TM PEEK TM (Victrex); Dow DuPont PEEK (polyimide); Quadrant PEEK (Ketron); SABIC PEEK, such as LNP TM THERMOCOMP TM 、LNP TM LUBRICOMP TM 、LNP TM STAT-KON TM ; Lehman&Voss PEEK, such as RTP Company PEEK, such as RTP 2200 series; Solvay PEEK, such as and Evonik PEEK, such as PEEK. The PEEK polymer may be an unreinforced PEEK polymer. The PEEK may be semi-crystalline. The PEEK may be in granular form. The PEEK polymer may have a melt viscosity of between about 130 Pa.s and about 500 Pa.s at 400°C. According to ISO 11443, the PEEK polymer may have a medium to high melt viscosity of between about 300 Pa.s and about 500 Pa.s. The melt viscosity may be measured as [1000s -1 ] / Pa.s. In some embodiments, the matrix PEEK is not blended with a polyamide (such as a nylon material). In some embodiments, the matrix PEEK polymer is unreinforced. In some embodiments, the matrix PEEK polymer may be semi-crystalline.
[0067] PEEK can be processed by conventional methods such as injection molding, extrusion, compression molding, etc. However, the processing conditions used to mold PEEK can affect the crystallinity and thus the mechanical properties. As a linear thermoplastic, polyetheretherketone can be melt processed in a temperature range of about 370°C to about 420°C. When polyetheretherketone is processed, no corrosive gases are released. The matrix polymer can be present in the composition in an amount ranging from about 90% by weight to about 99% by weight, from about 95% by weight to about 99% by weight, or from about 96% by weight to about 98.5% by weight.
[0068] The conductive filler may be an electrically conductive filler. The conductive filler may be an electrically conductive and thermally conductive filler. The conductive filler may be selected from the group consisting of carbon nanotubes, graphene, graphene oxide, carbon nanofibers and other carbon nanostructures. The graphene oxide may be reduced graphene oxide. Carbon nanotubes can increase mechanical properties (such as stiffness and strength), electrical conductivity and thermal conductivity. Flake nano additives such as graphene may affect stiffness and strength, barrier properties, and may impart electrical conductivity and thermal conductivity. In a specific embodiment, the conductive filler is a carbon nanotube.
[0069] The conductive filler can be present in the composition in an amount ranging from about 0.25 wt % to about 5 wt %, from about 0.5 wt % to about 4 wt %, from about 0.5 wt % to about 3 wt %, or from about 0.5 wt % to about 2 wt %, or from about 1 wt % to about 2 wt %, or <5 wt %, <4 wt %, <3 wt %, or <2 wt %. Lower loadings may help maintain the properties of the base polymer.
[0070] The dielectric filler can be selected from the group consisting of: fumed silica, fumed alumina, nano-alumina, nano-silicon dioxide, boron nitride flakes, boron nitride nano-flakes, boron nitride nano-tubes, ZnO and TiO2. In a specific embodiment, the dielectric filler is fumed silica. Nano-alumina fillers can be used to increase the dielectric constant, direct current (DC) volume resistivity and DC breakdown strength of the composite polymer. The dielectric filler can be present in the conductive composite composition in an amount between about 0 wt% and about 3 wt%, 0.05 wt% and about 3 wt%, 0.1 wt% and 2 wt%, or about 0.5 wt% to about 1.5 wt% of the composition.
[0071] Dispersion processing aid can be selected from the group consisting of: cage silsesquioxane (POSS), silane and silanol-POSS. Dispersion aid can be used to improve the dispersion of additives in the whole polymer matrix. For example, cage silsesquioxane (POSS) can be used alone as an auxiliary agent, such as OctaIsobutyl POSS, TriSilanolPhenyl POSS, TriSilanolIsobutyl POSS, or as a flow or dispersion aid (such as silanol-POSS). POSS compounds can be purchased commercially, such as from Hybrid Plastics. In a specific composition, the dispersion processing aid is POSS. The dispersion processing aid can be present in the composition in an amount in the range of about 0.1 % by weight to about 5 % by weight, about 0.3 % by weight to about 5.0 % by weight, about 0.5 % by weight to about 3 % by weight, and about 0.5 % by weight to about 2.0 % by weight.
[0072] In some embodiments, the above combined conductive fillers and dielectric fillers may be used in combination in the range of 0.1 wt % to 5 wt % while keeping the total weight percentage of fillers < 5 wt %, < 4 wt % or 3 wt % to achieve enhanced performance.
[0073] The property enhancements achieved with the nanocomposite polymers of the present invention, as compared to the matrix polymer, may include: an increase in tensile strength by at least about 1.1 times, or between about 1.1 times and about 1.25 times; an increase in toughness by at least about 1.5 times, or between about 1.5 times and about 3 times; an increase in impact strength by at least about 1.5 times, or between about 1.5 times and about 3 times; and an increase in elongation at break by at least about 1.5 times, or between about 1.5 times and about 3.5 times.
[0074] The conductive composite polymer can be processed by, for example, injection molding or extrusion processes. The composite polymer material of the present invention exhibits comparable or higher strength and higher toughness than the tested comparative matrix PEEK material or the comparative commercially available PEEK carbon nanotube composite material. The composite polymer of the present invention maintains the ductility of the matrix PEEK polymer and does not become brittle like the commercially available PEEK CNT polymer. The composite polymer of the present invention is easy to post-process, such as by tube bending, machining, etc., without the fracture problem caused by the brittleness that is usually seen in several commercially available PEEK-CNT composite materials.
[0075] A lightweight non-metallic fuel hose is provided, comprising at least one layer made from the composition of the present disclosure. The non-metallic hose can exhibit a controlled electrical resistance between 100 KΩ and 100 MΩ / 15", an excursion at 120 psi working pressure in a continuous temperature range of -65°F to 275°F and a temperature up to 325°F. The non-metallic hose complies with the Radio Technical Commission for Aeronautics (RTCA) DO-160 (Environmental) standard. The electrical resistance can be measured as a surface resistance.
[0076] In the present disclosure, tensile strength, tensile modulus and elongation at break are measured using ASTM D638 standard or ISO 527, for example, using Instron 3369. Toughness is measured according to the area under the stress-strain curve. Impact strength is determined according to ASTM D256, and Izod notch impact is measured using Ceast 9000. Thermal conductivity can be measured using TPS 2500 instrument. Surface resistivity and volume resistivity can be measured according to ASTM D257, IEC 62631-3-1, electrical conductivity can be measured according to ASTM D257 and D4496, and thermal conductivity can be measured using hot plate transient source method and ThermTest TPS2500. Tensile fatigue can be measured according to ASTM D3479 "Standard Test Method for Tension: Tensile Fatigue of Polymer Matrix Materials".
[0077] Composition
[0078] The conductive composite polymer of the present invention can be prepared from the composition according to Table 1.
[0079] Table 1. Compositions of the present invention
[0080]
[0081] Example
[0082] Example 1
[0083] Six comparative samples and three samples of the present invention were prepared. The first comparative matrix PEEK 1 sample was prepared using commercially available Victrex PEEK 450G. The second comparative matrix PEEK 2 sample was prepared using commercially available Evonik PEEK 5000G. Four comparative PEEK composite CNT samples were prepared by: RTP 2299X 115090L PEEK (RTP Plastics, Winona, Minnesota), which is a PEEK containing carbon nanotubes with ESD protection; RTP 2299X 115090M, which is a PEEK containing carbon nanotubes with ESD protection; RTP 2299X 115092A, which is a PEEK containing carbon nanotubes with ESD protection; and TECAPEEK ELS nano black (Ensinger), which contains VICTREX PEEK 450G polymer and carbon nanotubes. The sample compositions of the present invention are shown in Table 2.
[0084] Table 2. Conductive composite polymer composition of the present invention
[0085]
[0086] The samples were prepared by first drying the additives and polymer to remove residual moisture and dry blending the components to form a homogenous mixture. The mixture was fed into the feed hopper of a twin screw extruder at a temperature of about 380°C to about 425°C and a screw speed of about between 100 rpm and 800 rpm.
[0087] The molten strands of the polymer composite were then quenched in water and pelletized into 1 mm to 3 mm composite pellets. To make test specimens and tubes for testing, these pellets were dried and then injection molded or extruded into various shapes and sizes. The tensile properties of the resulting samples were measured according to ASTM D638, the impact properties were measured according to ASTM D256, the electrical conductivity was measured according to ASTM D257 and D4496, and the thermal conductivity was measured using the hot plate transient source method and the ThermTest TPS2500.
[0088] Tensile Strength
[0089] The tensile strength was measured using the ASTM D638 standard using an Instron 3369. The following samples were prepared: comparative matrix PEEK 1 (Victrex PEEK 450G), comparative matrix PEEK 2 (Evonik PEEK 5000G), the PEEK 1 composite polymer sample of the present invention, the PEEK 2 composite polymer sample of the present invention, and four comparative commercial PEEK CNT samples, and the tensile strength (MPa) was tested at room temperature according to ASTM D638. Figure 3A bar graph of the tensile strength (MPa) data of the comparative matrix PEEK 1, the comparative matrix PEEK 2, the PEEK 1 composite polymer sample of the present invention, the PEEK 2 composite polymer sample of the present invention, and four comparative commercial PEEK CNT samples at room temperature is shown. The composite polymer sample of the present invention exhibits a slightly higher tensile strength than the comparative matrix PEEK sample. The composite polymer sample of the present invention exhibits a tensile strength comparable to or slightly higher than the comparative commercial PEEK CNT sample. According to ASTM D638, both the sample of the present invention and a commercial PEEK with a conductive CNT sample exhibit a tensile strength of> 100MPa at room temperature. The tensile strength may be 100MPa or higher.
[0090] Elongation at break
[0091] The elongation was measured using the ASTM D638 standard using an Instron 3369. The following samples were prepared: comparative matrix PEEK 1 (Victrex PEEK), comparative matrix PEEK 2 (Evonik PEEK), the PEEK 1 composite polymer sample of the present invention, the PEEK 2 composite polymer sample of the present invention, and four comparative commercial PEEK CNT samples, and the elongation at break (%) was tested at room temperature according to ASTM D638. Figure 4 A bar graph of elongation at break (%) at room temperature is shown. Each of the comparative matrix PEEK 1 sample and the comparative matrix PEEK 2 sample has an elongation at break of >20%. The elongation at break of the PEEK 1 composite polymer sample of the present invention is >30%, and the elongation at break of the PEEK 2 composite polymer sample of the present invention is >80%. However, all four commercial PEEK samples with conductive CNT fillers exhibited an elongation at break of <4%.
[0092] toughness
[0093] Toughness was calculated from the area under the tensile stress-tensile strain curve. Figure 5 Stress-strain data plots for two different formulations of the PEEK 2 composite polymer formulation samples of the present invention and a comparative PEEK 2 sample are shown. The tensile stress (MPa) was plotted against the tensile strain (mm / mm) to obtain the stress-strain curve.
[0094] The PEEK 2 composite polymer formulation 2 sample of the present invention exhibited a stress-strain curve indicating that the sample was hard and ductile, and the PEEK 2 composite polymer formulation 1 sample of the present invention exhibited a stress-strain curve indicating that the sample was hard and tough, while the comparative matrix PEEK 2 sample exhibited a stress-strain curve indicating that the sample was hard and brittle.
[0095] Figure 7 A bar graph of toughness modulus (MPa) of a comparative matrix PEEK 1 sample and a comparative matrix PEEK 2 sample, a PEEK 1 formulation sample of the present invention, and a PEEK 2 formulation sample of the present invention is shown. Compared to the matrix PEEK 1 comparative sample and the matrix PEEK 2 comparative sample, the samples of the present invention exhibit increased toughness. Figure 7 As shown, the toughness modulus can be 18 MPa or higher.
[0096] Mechanical properties
[0097] The tensile strength was measured using an Instron 3369 using the ASTM D638 standard. Figure 6 A bar graph of mechanical properties including maximum tensile strength (MPa) and elongation at break (%) of comparative matrix PEEK1, comparative matrix PEEK 2, PEEK 1 formulation sample of the present invention, and PEEK 2 formulation sample of the present invention is shown. The samples of the present invention exhibited similar or slightly greater maximum tensile strength (101.5 MPa, 104.1 MPa, respectively) than the comparative matrix PEEK 1 (98.7 MPa) sample and the comparative matrix PEEK 2 (93.6 MPa) sample. Figure 6 As shown, the maximum tensile strength can be 100 MPa or higher. The samples of the present invention show significantly higher elongation at break (%) than the comparative matrix PEEK 1 sample and the comparative matrix PEEK 2 sample, which is 2 or 3 times higher.
[0098] Tensile Strength
[0099] The tensile strength was measured using an Instron 3369 using the ASTM D638 standard. Figure 8 A bar graph showing the tensile strength (MPa) of the comparative matrix PEEK1 sample and the comparative matrix PEEK 2 sample, the PEEK 1 composite polymer sample of the present invention, and the PEEK 2 composite polymer sample of the present invention at three temperatures (-65°F, 73°F, 275°F). At each of the three temperatures, the comparative polymer, the PEEK 1 composite polymer of the present invention, and the PEEK 2 composite polymer of the present invention all exhibit comparable tensile strength. The tensile strength at -65°F can be 140 MPa or higher. The tensile strength at 73°F can be 90 MPa or higher. Figure 8 As shown, the tensile strength at 275°F can be 50 MPa or higher.
[0100] Tensile modulus
[0101] The tensile modulus was measured using an Instron 3369 using the ASTM D638 standard. Fig. 9 The tensile modulus (GPa) of the comparative matrix PEEK1 sample and the comparative matrix PEEK 2 sample, the PEEK 1 composite polymer sample of the present invention, and the PEEK 2 composite polymer sample of the present invention at three temperatures (-65°F, 73°F, 275°F) are shown in a bar graph. At each of the three temperatures, the comparative polymer, the PEEK 1 composite polymer of the present invention, and the PEEK 2 composite polymer of the present invention all exhibit comparable tensile moduli. The tensile modulus at -65°F may be 4.5 GPa or higher. The tensile modulus at 73°F may be 4.0 GPa or higher. Fig. 9 As shown, the tensile modulus at 275°F can be 3.5 GPa or higher.
[0102] Impact strength-test
[0103] Notched impact strength was measured using Ceast 9000 and ASTM D266. Fig.10 A bar graph of the Izod notched impact strength of a comparative matrix PEEK 2 sample and the inventive PEEK 2+CNT-2 sample at three temperatures of -65°F, 73°F, and 275°F is shown. The inventive sample exhibits significantly improved impact strength of at least about 2 times or more than the comparative matrix PEEK sample at each of the three temperatures. The matrix PEEK sample partially breaks or articulates at high temperatures. Fig.11 For comparison, here are photos of base PEEK 2 samples that broke or hinged in an Izod notched impact strength test at an elevated temperature of 275°F. The Izod notched impact strength at -65°F can be 15KJ / m2 or higher. The Izod notched impact strength at 73°F can be 16KJ / m2 or higher. The Izod notched impact strength at 275°F can be 100KJ / m2 or higher.
[0104] Impact Test - Tube Horizontal
[0105] Sample tubes having an outer diameter of 2 inches and a wall thickness of 0.05 inches were prepared from the PEEK 1 (including Victrex PEEK) composite polymer material of the present invention and the PEEK 2 (including Evonik PEEK) composite polymer material of the present invention. The impact strength was determined according to ASTM D256, and the Izod notched impact was measured using a Ceast 9000. Photos of the PEEK 1 composite polymer tube sample of the present invention and the PEEK 2 composite polymer tube sample of the present invention after impact testing are shown in FIG. Fig. 12A and Fig. 12B. Both the PEEK 1 composite polymer tube of the present invention and the PEEK 2 composite polymer tube of the present invention showed no signs of failure after the 35J impact. The PEEK 2 composite polymer sample tube of the present invention withstood the 35J and 50J impacts and ultimately failed in the 65J impact. After the impact test, the tubes were subjected to the proof pressure and the burst pressure. Both groups of tubes burst at about 410psi, but they did not fail at the impact point.
[0106] Stretching fatigue
[0107] Comparison of the matrix PEEK material sample, the ESD PEEK composite polymer sample with lower toughness and the ESD PEEK composite polymer with higher toughness was carried out in a tensile fatigue test at room temperature, 5Hz and 73MPa. Fig.13 The ESD PEEK composite polymer with high toughness exhibits comparable tensile fatigue compared to the comparative matrix PEEK sample shown. The conductive composite polymer can exhibit tensile fatigue at room temperature, 5 Hz, 73 MPa, 2,200,000 or more fatigue cycles.
Claims
1. A solid polymer conductive composite material, the solid polymer conductive composite material is prepared from a composition comprising: 90 to 99 weight percent of a polyetheretherketone (PEEK) polymer, wherein the PEEK polymer is not blended with a polyamide; 0.25 wt % to 5 wt % of a conductive filler, wherein the conductive filler is carbon nanotubes; and 0.25 wt % to 5 wt % of a dispersing processing aid, wherein the dispersing processing aid is selected from cage-type silsesquioxane POSS and silanol POSS, The conductive composite material does not contain nano-diamond filler.
2. The solid polymer conductive composite material according to claim 1, further comprising 0.05 wt% to 3 wt% of a dielectric filler.
3. The solid polymer conductive composite material according to claim 1, wherein the PEEK polymer is a PEEK polymer with medium to high melt viscosity.
4. The solid polymer conductive composite according to claim 1, wherein the POSS is selected from the group consisting of octaisobutyl POSS, trisilanolphenyl POSS and trisilanolisobutyl POSS.
5. The solid polymer conductive composite material according to claim 2, wherein the dielectric filler is selected from the group consisting of nano-alumina, nano-silicon dioxide, ZnO, boron nitride nanotubes, boron nitride flakes and TiO2. The solid polymer conductive composite material according to claim 5 , wherein the nano-aluminum oxide is fumed aluminum oxide. The solid polymer conductive composite material according to claim 5 , wherein the nano-silica is fumed silica.
8. The solid polymer conductive composite material according to claim 5, wherein the boron nitride flakes are boron nitride nanoflakes.
9. The solid polymer conductive composite of claim 1 comprising 95 to 99 weight percent of a polyetheretherketone (PEEK) matrix polymer.
10. The solid polymer conductive composite of claim 1, comprising 0.25 wt% to 3 wt% of the conductive filler.
11. The solid polymer conductive composite of claim 1, comprising 0.3 wt% to 5 wt% of the dispersion processing aid.
12. The solid polymer conductive composite of claim 2, comprising 0.1 wt% to 2 wt% of the dielectric filler.
13. The solid polymer conductive composite material according to claim 2, wherein the solid polymer conductive composite material is prepared from a composition comprising: 95 wt% - 98.5 wt% PEEK polymer; 0.5 wt% to 3.0 wt% of a conductive filler; 0.25 wt% to 2 wt% dielectric filler; and 0.5 wt% - 3.0 wt% of a dispersing processing aid.
14. The solid polymer conductive composite material of claim 2, wherein the total amount of combined fillers does not exceed 5 weight percent.
15. The solid polymer conductive composite material according to any one of claims 1 to 14, which exhibits one or more properties selected from the group consisting of: A tensile strength of at least 80 MPa at 73°F; Elongation at break of at least 20%; Between 10 5 Ω and 10 8 The resistance between Ω; Maximum tensile strength of at least 95 MPa; A modulus of toughness of at least 15 MPa; and At least 60KJ / m 2 Izod notched impact strength.
16. A non-metallic fuel delivery system component for an aircraft, the non-metallic fuel delivery system component being prepared from the solid polymer conductive composite material according to claim 1.
17. The component of claim 16, the component being selected from the group consisting of: a fuel line, a hose, a coupling, a clamp, a conduit, a reducer, a flange, a ferrule, a bracket, and a housing.
18. A non-metallic fuel pipe comprising at least one layer made from the solid polymer conductive composite material according to claim 1.
19. The fuel hose of claim 18, wherein the polyetheretherketone (PEEK) polymer is a medium to high melt viscosity PEEK polymer.
20. The fuel pipe of claim 18, wherein the fuel pipe exhibits: Resistors between 100KΩ and 100MΩ / 15"; A maximum operating pressure of at least 120 psi; Continuous operating temperatures from -65°F or below to at least 275°F; An excursion operating temperature of at least 325°F; and Meets RTCA DO-160 environmental standards.
Citation Information
Patent Citations
Multi additive multifunctional composite for use in a non-metallic fuel conveyance system
US10435539B2
Fiber Reinforced Polymer Matrix Nanocomposite Downhole Member
US20130206273A1
Nanodiamonds containing thermoplastic thermal composites
US20140091253A1
Polyetheretherketone-base composite electromagnetic shielding material and preparation method thereof
CN102321338A
High-conductivity polyetheretherketone composite material and preparation method thereof
CN109627679A