Electrolyte additive, secondary battery electrolyte and secondary battery

By using nitrogen-based trimethylene thiophosphate to form an electrode interface film in lithium secondary batteries, the problem of side reactions between electrolyte and positive and negative electrode materials in lithium secondary batteries at high temperatures is solved, and the high temperature resistance of the battery is significantly improved. Performance and security.

CN115472909BActive Publication Date: 2024-10-29SHENZHEN BYD LITHIUM BATTERY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202110659018.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-11
Publication Date
2024-10-29
Estimated Expiration
2041-06-11

AI Technical Summary

Technical Problem

In existing lithium secondary batteries, side reactions between the electrolyte and the positive and negative electrode materials under high temperature conditions lead to swelling, cycle attenuation and safety problems, and the high temperature resistance is poor.

Method used

Nitrotrimethylene phosphorothioate is used as an electrolyte additive to form a uniform and dense interface film on the electrode surface, which enhances the lithium ion binding ability, inhibits positive and negative electrode side reactions under high temperature conditions, and improves the high temperature resistance of the battery.

Benefits of technology

Significantly improve the high temperature resistance of lithium secondary batteries, improve the safety factor and cycle life of the battery, and ensure the stability and storage performance under high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115472909B_ABST
    Figure CN115472909B_ABST
Patent Text Reader

Abstract

The present application provides an electrolyte additive, comprising a compound with a structural formula as shown in formula (I): #imgabs0# wherein R1, R2, R3, R4, R5 and R6 are independently selected from any one of an alkyl group, a halogenated alkyl group, an alkenyl alkyl group, an alkynyl alkyl group, an aryl group, a halogenated aryl group, an alkyl aryl group, and a halogenated alkyl aryl group. The electrolyte additive can form a dense interface film on the surface of the positive and negative electrodes of the battery. The interface film has good thermal stability and can also inhibit the reaction of the electrolyte with the positive and negative electrode materials under high temperature conditions, thereby improving the high temperature resistance of the lithium secondary battery and making the battery have a higher safety factor. The present application also provides a secondary battery electrolyte and a secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to an electrolyte additive, a secondary battery electrolyte and a secondary battery. Background Art

[0002] Lithium secondary batteries have been widely used in terminal products (smart phones, digital cameras, laptops, electric vehicles, etc.) due to their high energy density, high operating voltage, long service life, low self-discharge rate and environmental friendliness. With the rapid development of the industry, higher requirements are placed on the performance of lithium secondary batteries, especially the high temperature resistance of lithium secondary batteries.

[0003] In existing lithium secondary batteries, when the ambient temperature reaches above 60°C, a series of side reactions will occur between the electrolyte and the positive and negative electrode materials. As the side reactions intensify, the battery swells, the battery cycle decays, and even causes safety problems. To solve the above problems, it is necessary to develop a high temperature resistant electrolyte system to improve the safety performance of the battery. Summary of the invention

[0004] In view of this, the present application provides an electrolyte additive, which can form a dense interface film on the surface of the positive and negative electrodes of the battery. The interface film has good thermal stability and can inhibit the reaction between the electrolyte and the positive and negative electrode materials under high temperature conditions, thereby improving the high temperature resistance of the lithium secondary battery and giving the battery a higher safety factor.

[0005] In a first aspect, the present application provides an electrolyte additive, wherein the electrolyte additive comprises a compound having a structural formula as shown in formula (I):

[0006]

[0007] Among them, the R 1 , R 2 , R 3 , R 4 , R 5 and R 6 Any one independently selected from the group consisting of alkyl, halogenated alkyl, alkenyl alkyl, alkynyl alkyl, aryl, halogenated aryl, alkylaryl, and halogenated alkylaryl.

[0008] The electrolyte additive of the present application is nitrogen-based trimethylene thiophosphate. The N atom and S atom in the structure both contain lone pairs of electrons and have a certain electron-donating ability, and can form coordination with lithium ions. Moreover, since the spatial positions of the heteroatoms are relatively close, a chelating effect can be formed, thereby enhancing the binding ability with lithium ions. During the charge and discharge process of the battery, the electrolyte additive can approach the positive and negative electrodes as the lithium ions migrate, thereby forming a uniform and dense CEI film or SEI film on the surface of the positive and negative electrodes of the battery. The P, N, and S heteroatoms in the electrolyte additive can greatly improve the thermal stability of the CEI film and the SEI film, thereby inhibiting the occurrence of positive and negative electrode side reactions under high temperature conditions, and ensuring that the lithium secondary battery has good high temperature resistance.

[0009] Optionally, the alkyl group, the haloalkyl group, the alkenylalkyl group, and the alkynylalkyl group have 1-10 carbon atoms.

[0010] Optionally, the aryl group, the halogenated aryl group, the alkyl aryl group, and the halogenated alkyl aryl group have 6-20 carbon atoms.

[0011] Optionally, the R 1 , R 2 , R 3 , R 4 , R 5 and R 6 At least one of the groups is alkenylalkyl or alkynylalkyl.

[0012] Optionally, the R 1 , R 2 , R 3 , R 4 , R 5 and R 6 At least one of them is an allyl group.

[0013] Optionally, the halogen in the halogenated alkyl group, the halogenated aryl group and the halogenated alkyl aryl group includes fluorine, chlorine, bromine and iodine, and the halogenation is full halogenation or partial halogenation.

[0014] The electrolyte additive provided in the first aspect of the present application can form an SEI film on the surface of the negative electrode, inhibit the damage of the electrolyte solvent to the negative electrode structure, and play a role in protecting the negative electrode; it can also form a CEI film on the surface of the positive electrode to protect the positive electrode and inhibit the gas production of the electrolyte on the positive electrode side, thereby ensuring that the battery has a high energy density and cycle life; the formed SEI film and CEI film have good thermal stability, and can also well protect the positive and negative electrodes under high temperature conditions, inhibit the occurrence of side reactions, thereby improving the high temperature cycle performance and high temperature storage performance of the battery, and improving the safety factor of the battery.

[0015] In a second aspect, the present application provides a secondary battery electrolyte, comprising an electrolyte salt, an organic solvent and an additive, wherein the additive comprises the electrolyte additive as described in the first aspect of the present application.

[0016] Optionally, the mass percentage of the electrolyte additive in the secondary battery electrolyte is 1%-5%.

[0017] Optionally, the additives further include film-forming additives.

[0018] Optionally, the film-forming additive includes one or more of vinylene carbonate, fluoroethylene carbonate, propylene sulfite, vinyl sulfate, methylene methanedisulfonate, 1,3-propane sultone and tripropylene phosphate.

[0019] Optionally, the mass percentage of the film-forming additive in the secondary battery electrolyte is 0.5%-3%.

[0020] Optionally, the mass ratio of the film-forming additive to the electrolyte additive is 1:(0.1-3)

[0021] Optionally, the electrolyte salt includes at least one of a lithium salt, a sodium salt and a potassium salt.

[0022] Optionally, the organic solvent includes one or more of a carbonate solvent, an ether solvent, and a carboxylate solvent.

[0023] In a third aspect, the present application provides a secondary battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte comprises the secondary battery electrolyte as described in the second aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of the structure of a secondary battery provided in one embodiment of the present application;

[0025] Figure 2 This is a scanning electron microscope image of the negative electrode of the battery provided in Example 3 of the present application;

[0026] Figure 3 This is a scanning electron microscope image of the positive electrode of the battery provided in Example 3 of the present application. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0028] The existing secondary batteries have poor high temperature resistance. Under high temperature conditions, the electrolyte in the secondary battery and the positive and negative electrode materials are prone to a large number of side reactions and produce gas, causing battery swelling, excessive internal pressure of the battery, battery capacity decay and other adverse consequences. The present application provides an electrolyte additive. Adding a small amount of the electrolyte additive to the electrolyte can significantly improve the high temperature resistance of the battery, and the addition of the electrolyte additive has little effect on the battery system.

[0029] The electrolyte additive provided in the present application includes nitrogen-based trimethylene thiophosphate, and the structural formula of nitrogen-based trimethylene thiophosphate is shown in formula (I):

[0030]

[0031] In the embodiment of the present application, there are six substituent groups on the six oxygen atoms in the nitrogen trimethylene thiophosphate, namely, R 1 , R 2 , R 3 , R 4 , R 5 and R 6 , wherein the six substituents are independently selected from any one of an alkyl group, a haloalkyl group, an alkenylalkyl group, an alkynylalkyl group, an aryl group, a haloaryl group, an alkylaryl group, and a haloalkylaryl group. In the embodiment of the present application, when the substituent group is selected from alkyl, the alkyl group may be any one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, cyclopropyl or cyclobutyl; when the substituent group is selected from alkenylalkyl, the alkenylalkyl group may be any one of allyl, allylbutyl, allylisobutyl, allylpentyl and allylisopentyl; when the substituent group is selected from alkynylalkyl, the alkynylalkyl group may be any one of propargyl, alkynylbutyl, isobutyl, alkynylpentyl and isopentyl; when the substituent group is selected from haloalkyl, the haloalkyl group may be any one of trifluoromethyl, trifluoroethyl, trifluoropropyl, pentafluoropropyl, trifluorobutyl and pentafluorobutyl; when the substituent group is selected from haloalkyl, the haloalkyl group may be any one of p-trifluoromethylphenyl, trifluoroethyl, p-fluorophenyl, p-chlorophenyl, o-trifluoromethylphenyl and p-fluorobenzyl. In the embodiment of the present application, the six substituent groups may be the same or different groups.

[0032] In some embodiments of the present application, R 1 , R 2 , R 3 , R 4 , R 5 and R 6At least one of them is a haloalkyl, a haloaryl or a haloalkylaryl, wherein the substituted halogen includes fluorine, chlorine, bromine, and iodine, and the halogen can be fully halogenated or partially halogenated. In the embodiment of the present application, when the substituent group is a haloalkyl, a haloaryl or a haloalkylaryl, the electrolyte additive contains a certain amount of halide (such as LiF) in the interface film formed on the electrode surface, thereby more effectively isolating the electrolyte from the electrode, thereby inhibiting the occurrence of side reactions under high temperature conditions. Further, when R 1 , R 2 , R 3 , R 4 , R 5 When there are multiple substituted groups in R and R are the above-mentioned halogen-containing groups, it is beneficial to increase the content of halides in the interface film and improve the protection performance of the interface film. In some embodiments of the present application, the substituted halogen includes fluorine. When the substituted group is a fluorine-containing group, the interface film can contain a certain content of stable fluoride, which is more conducive to effective protection of the positive electrode.

[0033] In some embodiments of the present application, R 1 , R 2 , R 3 , R 4 , R 5 and R 6 At least one of them is an alkenylalkyl group or an alkynylalkyl group. When the substituent group contains an unsaturated double bond or a triple bond, the electrolyte additive contains a certain amount of organic polymer in the interface film formed on the electrode surface. The organic polymer can improve the structural strength and thermal stability of the interface film, which can reduce the battery impedance on the one hand and improve the high temperature resistance of the battery on the other hand. Further, when R 1 , R 2 , R 3 , R 4 , R 5 and R 6 When there are multiple substituents in which are alkenyl alkyl or alkynyl alkyl, it is beneficial to increase the content of organic polymer in the interface film and improve the protective performance of the interface film. 1 , R 2 , R 3 , R 4 , R 5 and R 6 When one or more of the substituent groups is an allyl group, the intermediate product of the electrolyte additive reaction is Among them, R x Including any one of methyl, ethyl, benzyl or phenethyl, the intermediate product will further react on the electrode surface. The reaction process is as follows:

[0034]

[0035] It can be seen from the above reaction formula that when the substituent group contains an unsaturated double bond or triple bond, the electrolyte additive can generate an organic polymer, and the organic polymer can form a composite film with the inorganic components in the reaction product of the electrolyte additive, thereby making the interface film have good structural stability and high temperature resistance.

[0036] In the embodiment of the present application, the carbon number of the alkyl, haloalkyl, alkenylalkyl and alkynylalkyl is 1-10, and further, the carbon number of the alkyl, haloalkyl, alkenylalkyl and alkynylalkyl is 1-5. The carbon number of the alkyl, haloalkyl, alkenylalkyl and alkynylalkyl can be, but not limited to, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10. When the carbon number is too high, the content of alkyl lithium in the interface film formed by the electrolyte additive is too high, which is not conducive to improving the thermal stability of the interface film.

[0037] In the embodiment of the present application, the carbon number of the aryl group, the halogenated aryl group, the alkyl aryl group and the halogenated alkyl aryl group is 6-20, and further, the carbon number of the aryl group, the halogenated aryl group, the alkyl aryl group and the halogenated alkyl aryl group is 6-10. The carbon number of the aryl group, the halogenated aryl group, the alkyl aryl group and the halogenated alkyl aryl group can be, but not limited to, 6, 7, 8, 9, 10, 13, 17 or 20. A lower carbon number is conducive to controlling the molecular weight of the additive, thereby better controlling the viscosity of the electrolyte.

[0038] In some specific embodiments of the present application, the molecular structure of the electrolyte additive may be as shown in formula (A)-(G):

[0039]

[0040]

[0041] The electrolyte additive provided by the present application is a nitrogen-based trimethylene thiophosphate structure, which has a strong binding ability with lithium ions and can form a uniform and dense CEI film or SEI film. The structure of the electrolyte additive contains three heteroatoms of P, N, and S at the same time. Compared with the additive of a single heteroatom, it has a better film-forming effect and can form a powerful defense barrier on the surface of the positive and negative electrodes, thereby improving the high-temperature cycle performance and high-temperature storage performance of the electrolyte. The electrolyte additive of the present application has good compatibility with the positive and negative electrode materials and has little effect on the battery system.

[0042] The electrolyte additive of the present application can be prepared by different methods, and the specific preparation method is not limited. Taking the electrolyte additive (A) nitrogen trimethylene thiophosphate hexamethyl ester as an example, the synthesis route of the electrolyte additive (A) is as follows:

[0043]

[0044] When the substituent group R 1 , R 2 , R 3 , R 4 , R 5 and R 6 When all are methyl groups, methanol and nitrogen trimethylene thiophosphoric acid can be used for substitution reaction to prepare the electrolyte additive (A).

[0045] The present application also provides a secondary battery electrolyte, comprising an electrolyte salt, an organic solvent and an additive, wherein the additive comprises the electrolyte additive mentioned above in the present application.

[0046] In the embodiments of the present application, the mass percentage of the electrolyte additive in the electrolyte of the secondary battery is 1%-5%. In some embodiments of the present application, the mass percentage of the electrolyte additive in the electrolyte of the secondary battery is 1.5%-3%. The mass percentage of the electrolyte additive in the electrolyte of the secondary battery can be, but is not limited to, 1%, 1.5%, 2%, 2.5%, 3% or 5%. Within the above mass percentage range, the electrolyte additive can form a complete protective layer on the surface of the positive and negative pole pieces, effectively improving the high temperature resistance of the battery. If the concentration of the electrolyte additive is too high, the thickness of the protective layer formed will be too large, causing a large interface impedance, hindering the transmission of lithium ions, reducing the discharge capacity, and affecting the low temperature performance of the battery.

[0047] In some embodiments of the present application, the additive further comprises a film-forming additive. The film-forming additive can form an organic film on the electrode surface, thereby further improving the density and elastic properties of the interface film. In some embodiments of the present application, the film-forming additive comprises one or more of vinylene carbonate, fluoroethylene carbonate, propylene sulfite, vinyl sulfate, methylene disulfonate, 1,3-propane sultone and tripropylene phosphate.

[0048] In the embodiment of the present application, the mass percentage of the film-forming additive in the secondary battery electrolyte is 0.5%-3%. The mass percentage of the film-forming additive in the secondary battery electrolyte can be, but is not limited to, 0.5%, 1%, 2%, 2.5% or 3%. In the embodiment of the present application, the mass ratio of the electrolyte additive to the film-forming additive is 1:(0.1-3). The mass ratio of the electrolyte additive to the film-forming additive can be, but is not limited to, 1:0.1, 1:0.5, 1:1, 1:2 or 1:3. Within the above mass ratio range, the electrolyte additive can cooperate well with the film-forming additive to form an organic-inorganic composite film, so that the interface film has good mechanical properties and high temperature resistance.

[0049] In the embodiments of the present application, the electrolyte salt in the secondary battery electrolyte may be a lithium salt, a sodium salt, a potassium salt, etc., depending on the different secondary battery systems. In some embodiments of the present application, the lithium salt includes lithium hexafluorophosphate (LiPF 6 ), lithium bis(trifluoromethanesulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium tetrafluoroborate (LiBF 4 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium hexafluoroantimonate (LiSbF 6 ), lithium perchlorate (LiClO 4 ), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium dioxalatoborate (LiBOB), lithium difluorooxalatoborate (LiDFOB), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), lithium perfluorobutanesulfonate (LiC 4 F 9 SO 3 ), lithium bis(trifluoromethylsulfonyl)imide (Li(CF 3 SO 2 ) 2 N), lithium bis(perfluoroethylsulfonyl)imide (Li(C 2 F 5 SO 2 ) 2 N) one or more. In some embodiments of the present application, the electrolyte salt includes lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide and lithium bis(trifluorosulfonyl)imide. In the present application, there is no special requirement for the content of electrolyte salt in the secondary battery electrolyte, and its content can refer to the conventional amount in the art. In some embodiments of the present application, the concentration of electrolyte salt in the secondary battery electrolyte is 0.1mol / L-5mol / L, and further, the concentration of electrolyte salt in the secondary battery electrolyte is 1mol / L-1.5mol / L.

[0050] In the embodiments of the present application, the organic solvent includes one or more of carbonate solvents, ether solvents, and carboxylate solvents. Wherein, carbonate solvents can be cyclic and / or chain-shaped, and carboxylate solvents can be linear and / or branched. In some embodiments of the present application, the organic solvent includes ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate, ethyl acetate, propyl acetate, ethyl propionate, ethyl butyrate, etc. One or more, but not limited to this. In some embodiments of the present application, the organic solvent includes ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC), wherein the volume ratio of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) is 1: (1-1.5): (0.5-1).

[0051] The present application also provides a secondary battery, including a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte includes the secondary battery electrolyte provided in the present application. Figure 1 , Figure 1 A schematic diagram of the structure of a secondary battery provided in one embodiment of the present application. The secondary battery includes a positive electrode 10, a negative electrode 20, a separator 30, and an electrolyte 40. When the secondary battery is charged, lithium ions are released from the positive electrode 10, and are deposited on the negative electrode 20 after passing through the electrolyte 40; when the secondary battery is discharged, lithium ions are released from the negative electrode 20, and are embedded in the positive electrode 10 after passing through the electrolyte 40. Since the secondary battery provided in the present application adopts the above-mentioned secondary battery electrolyte, it still has good cycle performance and safety performance in a high temperature environment. In the embodiment of the present application, the secondary battery can be a lithium secondary battery, a potassium secondary battery, a sodium secondary battery, a magnesium secondary battery, a zinc secondary battery, an aluminum secondary battery, etc.

[0052] In the present application, the negative electrode of the secondary battery may be any negative electrode known in the art. In the embodiment of the present application, the negative electrode may include one or more of a carbon-based negative electrode, a silicon-based negative electrode, a tin-based negative electrode, a lithium negative electrode, a sodium negative electrode, a potassium negative electrode, a magnesium negative electrode, a zinc negative electrode and an aluminum negative electrode. Among them, the carbon-based negative electrode may include graphite, hard carbon, soft carbon, graphene, etc.; the silicon-based negative electrode may include silicon, silicon carbon, silicon oxygen, silicon metal compounds, etc.; the tin-based negative electrode may include tin, tin carbon, tin oxygen, tin metal compounds; the lithium negative electrode may include metallic lithium or a lithium alloy. The lithium alloy may specifically be at least one of a lithium silicon alloy, a lithium sodium alloy, a lithium potassium alloy, a lithium aluminum alloy, a lithium tin alloy and a lithium indium alloy. In some embodiments of the present application, the current collector of the negative electrode is copper foil, and the negative electrode active material includes one or more of natural graphite, artificial graphite, hard carbon, soft carbon, lithium titanate, iron oxide, lithium titanium phosphate, titanium dioxide, silicon, silicon oxide, aluminum, tin and antimony; the binder includes one or more of polyacrylic acid (PAA), polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC) and styrene butadiene latex (SBR); the conductive agent includes one or more of acetylene black, Ketjen black, Super-P, carbon nanotubes, carbon nanofibers, activated carbon and graphene. In the present application, the preparation method of the negative electrode can adopt any method known in the art.

[0053] In the embodiment of the present application, the positive electrode of the secondary battery includes a positive electrode active material that can reversibly embed / de-embed metal ions (lithium ions, sodium ions, potassium ions, magnesium ions, zinc ions, aluminum ions, etc.). The positive electrode of the secondary battery in the present application can be any positive electrode known in the art. Taking a lithium secondary battery as an example, the positive electrode active material can be, but is not limited to, lithium cobalt oxide (LiCoO 2 ), lithium iron phosphate (LiFePO 4 )、LiNi 0.33 Co 0.33 Mn 0.33 O 2 (NCM111), LiNi 0.4 Co 0.2 Mn 0.4 O 2 (NCM424), LiNi 0.5 Co 0.2 Mn 0.3 O 2 (NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O 2 (NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O 2 (NCM811) or more.

[0054] In the embodiment of the present application, the separator of the secondary battery can be any separator known to those skilled in the art, for example, the separator can be one or more of polyolefin microporous membrane, polyethylene terephthalate, polyethylene felt, glass fiber felt or ultrafine glass fiber paper.

[0055] In the embodiments of the present application, the battery can be prepared by using either a lamination process or a winding process. In some embodiments of the present application, the battery is prepared by using a lamination process.

[0056] The present application also provides a power vehicle, which includes the secondary battery provided by the present application, and the secondary battery supplies power to the power vehicle.

[0057] The technical solution of the present application is further described below with reference to a number of embodiments.

[0058] Example 1

[0059] 1) Preparation of secondary battery electrolyte

[0060] 40 mL of ethylene carbonate (EC) and 60 mL of ethyl methyl carbonate (EMC) were mixed to obtain an organic solvent, and then 7.6 g of lithium hexafluorophosphate (LiPF 6 ) and 9.35 g of lithium bis(fluorosulfonyl)imide (LiFSI) were dissolved in the above solvent, stirred and mixed to form a uniform solution, and then the electrolyte additive (A) (nitrothrymethylene hexamethyl thiophosphate) was added to the above solution to obtain a secondary battery electrolyte. Among them, LiPF 6 The molar concentrations of LiFSI and LiFSI are 0.5 mol / L respectively, the mass percentage of the electrolyte additive (A) is 2%, and the structural formula of the electrolyte additive (A) is as follows:

[0061]

[0062] 2) Preparation of lithium secondary batteries

[0063] Graphite, sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) are mixed in a weight ratio of 95:2:3, and water is added to stir into a uniform slurry. The slurry is coated on a copper foil current collector, and the negative electrode sheet is obtained after drying, rolling and slitting.

[0064] Will Li(Ni 0.6 Co 0.2 Mn 0.2 ) 2 (NCM622), carbon nanotubes (CNT), and polyvinylidene fluoride (PVDF) are mixed and stirred in a weight ratio of 100:2:2 to form a uniform slurry, the slurry is coated on an aluminum foil, dried at 80°C for 24 hours, and rolled and cut to obtain a positive electrode sheet.

[0065] The positive electrode sheet, negative electrode sheet and separator prepared above are wound into a battery cell, and the above secondary battery electrolyte is poured into the battery cell. After the formation process, a soft-pack lithium secondary battery S1 is manufactured.

[0066] Example 2

[0067] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 2 is the same as that in Example 1, except that the electrolyte additive in Example 2 is electrolyte additive (B) (nitrilotrimethylene hexaethyl thiophosphate), and the structural formula of the electrolyte additive (B) is as follows:

[0068]

[0069] The soft-pack lithium secondary battery prepared in Example 2 is named S2.

[0070] Example 3

[0071] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 3 is the same as that in Example 1, except that the electrolyte additive in Example 3 is electrolyte additive (C) (nitrilotrimethylenethiophosphate hexa(trifluoroethyl) ester), and the structural formula of the electrolyte additive (C) is as follows:

[0072]

[0073] The soft-pack lithium secondary battery prepared in Example 3 is named S3.

[0074] Example 4

[0075] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 4 is the same as that in Example 1, except that the electrolyte additive in Example 4 is an electrolyte additive (D) (nitrilotrimethylene hexa(allyl) thiophosphate), and the structural formula of the electrolyte additive (D) is as follows:

[0076]

[0077] The soft-pack lithium secondary battery prepared in Example 4 is named S4.

[0078] Example 5

[0079] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 5 is the same as that in Example 1, except that the electrolyte additive in Example 5 is electrolyte additive (E) (nitrothrimethylene hexaphenyl thiophosphate), and the structural formula of the electrolyte additive (E) is as follows:

[0080]

[0081] The soft-pack lithium secondary battery prepared in Example 5 is named S5.

[0082] Example 6

[0083] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 6 is the same as that in Example 1, except that the electrolyte additive in Example 6 is an electrolyte additive (F) (nitrilotrimethylenethiophosphate hexa(p-fluorophenyl) ester), and the structural formula of the electrolyte additive (F) is as follows:

[0084]

[0085] The soft-pack lithium secondary battery prepared in Example 6 is named S6.

[0086] Example 7

[0087] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 7 is the same as that in Example 1, except that the electrolyte additive in Example 7 is electrolyte additive (G) (nitrilotrimethylenethiophosphate hexa(p-trifluoromethylphenyl) ester), and the structural formula of the electrolyte additive (G) is as follows:

[0088]

[0089] The soft-pack lithium secondary battery prepared in Example 7 is named S7.

[0090] Example 8

[0091] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 8 is the same as that in Example 1, except that the mass percentage of the electrolyte additive (A) in Example 8 is 4%. The soft-pack lithium secondary battery prepared in Example 8 is named S8.

[0092] Example 9

[0093] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 9 is the same as that in Example 1, except that the mass percentage of the electrolyte additive (A) in Example 9 is 1%. The soft-pack lithium secondary battery prepared in Example 9 is named S9.

[0094] Example 10

[0095] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 10 is the same as that in Example 4, except that difluoroethylene carbonate (DFEC, a film-forming additive) is further added during the preparation of the secondary battery electrolyte in Example 10, and the mass ratio of difluoroethylene carbonate to the electrolyte additive (D) is 1:1.

[0096] The soft-pack lithium secondary battery prepared in Example 10 is named S10.

[0097] In order to highlight the beneficial effects of the present application, the following comparative examples are set.

[0098] Comparative Example 1

[0099] 1) Preparation of secondary battery electrolyte

[0100] 40 mL of ethylene carbonate (EC) and 60 mL of ethyl methyl carbonate (EMC) were mixed to obtain an organic solvent, and then 7.6 g of lithium hexafluorophosphate (LiPF 6 ) and 9.35g of lithium bis(fluorosulfonyl)imide (LiFSI) were dissolved in the above solvent, stirred and mixed into a uniform solution, and then 3g of vinyl sulfate was added to the above solution to obtain a secondary battery electrolyte. Among them, LiPF 6 The molar concentrations of LiFSI and LiFSI are 0.5 mol / L respectively, and the mass percentage of vinyl sulfate is 2%.

[0101] 2) Preparation of lithium secondary batteries

[0102] The positive electrode sheet and the negative electrode sheet are prepared in the same manner as in Example 1, and the positive electrode sheet, the negative electrode sheet and the separator are wound into a battery cell, which is then filled with the above-mentioned secondary battery electrolyte, and the soft-pack lithium secondary battery S11 is manufactured after processes such as formation.

[0103] Comparative Example 2

[0104] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Comparative Example 2 is the same as that in Comparative Example 1, and the difference from Comparative Example 1 is that the additive in Comparative Example 2 is lithium difluorophosphate. The soft-pack lithium secondary battery prepared in Comparative Example 2 is named S12.

[0105] Comparative Example 3

[0106] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Comparative Example 3 is the same as that in Comparative Example 1, and the difference from Comparative Example 1 is that the additive in Comparative Example 3 is bisfluoroethylene carbonate (DFEC). The soft-pack lithium secondary battery prepared in Comparative Example 3 is named S13.

[0107] Effect Example

[0108] In order to strongly support the beneficial effects brought by the technical solutions of the embodiments of this application, the following tests are provided:

[0109] 1) The soft-pack lithium secondary battery S3 of Example 3 was disassembled and the battery electrode was taken out for morphological characterization. Figure 2 and Figure 3 , Figure 2 This is a scanning electron microscope image of the negative electrode of the battery provided in Example 3 of the present application. Figure 3 This is a scanning electron microscope image of the positive electrode of the battery provided in Example 3 of the present application. Figure 2It can be seen that there is a waxy deposition layer on the surface of the negative electrode, which is the SEI film on the surface of the negative electrode of the battery. Figure 3 It can be seen that there is a dense accumulation of particles on the surface of the battery's positive electrode, and this accumulation layer is the CEI film on the surface of the battery's positive electrode.

[0110] 2) The battery electrode of Example 3 was subjected to elemental analysis by using scanning electron microscope energy spectrum analysis. The test process includes: the soft-pack lithium secondary battery S3 of Example 3 was disassembled and the negative electrode of the battery was taken out for elemental analysis. Please refer to Table 1. Table 1 is a table of elemental composition of the SEI film on the negative electrode surface of the soft-pack lithium secondary battery S3, wherein Wt% is weight percentage and At% is atomic percentage.

[0111] Table 1 Element composition of SEI film on negative electrode surface in soft-pack lithium secondary battery S3

[0112] element Wt% At% C 53.84 64.83 O 32.31 29.21 F 2.18 1.66 N 0.31 0.19 P 4.71 2.42 S 0.79 0.35 Cu 5.87 1.34

[0113] It can be seen from Table 1 that the SEI film on the surface of the negative electrode of the battery contains N, P, and S elements in the electrolyte additive, which indicates that the electrolyte additive of the present application can participate in the formation of the interface film on the surface of the battery electrode.

[0114] 3) The soft-pack batteries of Examples 1-10 and Comparative Examples 1-3 were subjected to a high-temperature cycle performance test. The specific test conditions were as follows: a domestic blue-electric model CT2001C test cabinet was used for the test, and the soft-pack batteries were cycled 500 times at 60°C between 2.75V and 4.35V at a current of 1000mA (1C); the initial discharge capacity was recorded, and after 500 repeated charge and discharge cycles, the discharge capacity of the 500th cycle was recorded, and the capacity retention rate of the battery after high-temperature cycling was calculated. The calculation formula was: capacity retention rate (%) = discharge capacity after 500 cycles / initial discharge capacity × 100%. Ten groups of batteries were set for each group of Examples and Comparative Examples, and the test results were averaged. The test results of the high-temperature cycle performance of the soft-pack batteries of Examples 1-10 and Comparative Examples 1-3 are shown in Table 2.

[0115] 4) The soft-pack batteries of Examples 1-10 and Comparative Examples 1-3 were tested for high-temperature storage performance. The specific conditions of the test were: the battery was charged to a full charge state at 1000 mA (1C), constant voltage 4.35 V to 50 mA (0.05C), and the battery was placed in a 60°C constant temperature box for 28 days of storage. The capacity retention rate of the battery after high-temperature storage was calculated using the following formula: Capacity retention rate (%) = discharge capacity after 28 days of storage / first discharge capacity × 100%. Ten groups of batteries were set for each group of Examples and Comparative Examples, and the test results were averaged. The test results of the high-temperature storage performance of the soft-pack batteries of Examples 1-10 and Comparative Examples 1-3 are shown in Table 2.

[0116] Table 2 Performance parameters of soft pack batteries of Examples 1-10 and Comparative Examples 1-3

[0117] Battery ID 500 cycles capacity retention rate (%) 28-day storage capacity retention rate (%) S1 83.8% 86.5% S2 85.4% 86.3% S3 87.5% 89.3% S4 90.4% 94.3% S5 85.0% 88.6% S6 87.7% 91.2% S7 87.5% 90.4% S8 89.5% 91.7% S9 83.5% 87.0% S10 92.1% 95.2% S11 76.4% 83.5% S12 79.3% 84.2% S13 82.8% 85.8%

[0118] It can be seen from the test results in Table 1 that the high temperature cycle performance of the battery can be significantly improved when the electrolyte additive provided by the present application is added to the battery electrolyte. It can be seen from the examples that nitrogen trimethylene thiophosphate hexa(allyl) ester has better battery high temperature cycle performance than other nitrogen trimethylene thiophosphates (Example 4), and when it is used in conjunction with the film-forming additive bisfluoroethylene carbonate (DFEC), the battery has the best high temperature cycle performance (Example 10), while when the comparative example uses conventional additives, the battery capacity decays faster under high temperature conditions (Comparative Examples 1-3). The capacity retention rate of the battery after 28 days of high temperature storage is basically consistent with the result of the high temperature cycle capacity retention rate, which shows that the electrolyte additive of the present application can effectively improve the high temperature resistance of the battery.

[0119] The above is a preferred embodiment of the present application, but it should not be understood as limiting the scope of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.

Claims

1. An electrolyte additive, characterized in that: The electrolyte additive includes a compound having a structural formula as shown in formula (I): Wherein, R1, R2, R3, R4, R5 and R6 are independently selected from any one of alkyl, halogenated alkyl, alkenyl alkyl, alkynyl alkyl, aryl, halogenated aryl, alkyl aryl and halogenated alkyl aryl.

2. The electrolyte additive according to claim 1, characterized in that At least one of R1, R2, R3, R4, R5 and R6 is an alkenylalkyl group or an alkynylalkyl group.

3. The electrolyte additive according to claim 1 or 2, characterized in that: The alkyl group, the halogenated alkyl group, the alkenyl alkyl group and the alkynyl alkyl group have 1 to 10 carbon atoms; the aryl group, the halogenated aryl group, the alkyl aryl group and the halogenated alkyl aryl group have 6 to 20 carbon atoms.

4. The electrolyte additive according to claim 1, characterized in that The halogen in the halogenated alkyl group, the halogenated aryl group and the halogenated alkyl aryl group includes fluorine, chlorine, bromine and iodine, and the halogenation is full halogenation or partial halogenation.

5. A secondary battery electrolyte comprising an electrolyte salt, an organic solvent and an additive, wherein the additive comprises the electrolyte additive according to any one of claims 1 to 4.

6. The secondary battery electrolyte according to claim 5, characterized in that: The mass percentage of the electrolyte additive in the secondary battery electrolyte is 1%-5%.

7. The secondary battery electrolyte according to claim 5, characterized in that: The additives also include film-forming additives. 8 . The secondary battery electrolyte according to claim 7 , wherein the mass ratio of the electrolyte additive to the film-forming additive is 1:(0.1-3). 9 . The secondary battery electrolyte according to claim 5 , wherein the organic solvent comprises one or more of a carbonate solvent, an ether solvent, and a carboxylate solvent. 10 . The secondary battery electrolyte according to claim 5 , wherein the electrolyte salt comprises at least one of a lithium salt, a sodium salt and a potassium salt.

11. A secondary battery, characterized in that: The invention comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte comprises the secondary battery electrolyte as claimed in any one of claims 5 to 10.

Citation Information

Patent Citations

  • Electrolyte additive, electrolyte containing additive and lithium metal battery

    CN112103562A

  • Secondary battery electrolyte and secondary battery

    CN115548439A

  • Lithium ion secondary battery

    JP2022126004A