Secondary battery electrolyte and secondary battery
By using oxysulfur azaphosphine as a water-removing additive in lithium secondary batteries, a dense interface film is formed, which solves the problem of side reactions between the electrolyte and the positive and negative electrode materials, improves the cycle performance and safety performance of the battery, and reduces the cost of the battery. impedance, improving energy density and cycle life.
Patent Information
- Application Number
- CN202110742394.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-06-30
AI Technical Summary
The side reaction between the cathode material and the electrolyte in lithium secondary batteries causes the electrolyte to oxidize and decompose, producing gas, causing cycle attenuation and safety issues. In addition, trace amounts of water in the electrolyte react with electrolyte salts to produce by-products, reducing battery performance.
Oxythiazine phosphine is used as a water-removing additive. Through the electron-attracting ability of its sulfonyl and phosphoryl groups, a dense interface film is formed on the surface of the positive and negative electrodes of the battery, inhibiting the reaction between the electrolyte and the positive and negative electrode materials, and removing the ions in the electrolyte. moisture and improve battery durability under high temperature conditions.
It effectively suppresses the side reactions between the electrolyte and the positive and negative electrode materials, improves the cycle performance and safety performance of the battery, reduces battery impedance, and improves energy density and cycle life.
Smart Images

Figure CN115548439B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a secondary battery electrolyte and a secondary battery. Background Art
[0002] Lithium secondary batteries have been widely used in terminal products (smart phones, digital cameras, laptops, electric vehicles, etc.) due to their high energy density, high operating voltage, long service life, low self-discharge rate and environmental friendliness. With the rapid development of the industry, higher requirements are placed on the performance of lithium secondary batteries.
[0003] In the use of lithium secondary batteries, direct contact between the positive electrode material and the electrolyte is prone to side reactions, resulting in oxidation and decomposition of the electrolyte, producing a large amount of gas, causing battery cycle decay and even safety issues. In addition, when the electrolyte contains trace amounts of water, the electrolyte salt reacts with water to produce a series of byproducts, which in turn leads to reduced performance of the lithium secondary battery. In order to solve the above problems, it is necessary to develop a new electrolyte system to improve the cycle performance and safety performance of lithium secondary batteries. Summary of the invention
[0004] In view of this, the present application provides a secondary battery electrolyte, in which the dehydrating additive in the secondary battery electrolyte can not only remove moisture from the electrolyte, but also the reaction product of the dehydrating additive and water can form a dense interface film on the surface of the positive and negative electrodes of the battery, and the interface film can inhibit the reaction between the electrolyte and the positive and negative electrode materials, thereby improving the stability of the battery, reducing the battery impedance, and making the battery have good cycle performance and safety performance.
[0005] In a first aspect, the present application provides a secondary battery electrolyte, comprising an electrolyte salt, an organic solvent and a water-removing additive, wherein the water-removing additive comprises a compound having a structural formula as shown in formula (1):
[0006]
[0007] Wherein, R1 and R3 are independently selected from any one of hydrogen, fluorine, alkyl, fluoroalkyl, alkenylalkyl, alkynylalkyl, alkenyl, and alkynyl; R2 and R4 are independently selected from any one of fluorine, alkyl, fluoroalkyl, alkenylalkyl, alkynylalkyl, alkenyl, and alkynyl.
[0008] In the secondary battery electrolyte of the present application, the dehydrating additive includes oxysulfuryl nitrogen phosphine. The sulfonyl group and phosphoryl group in the oxysulfuryl nitrogen phosphine structure have strong electron-withdrawing ability, so that the POC bond in the dehydrating additive is easily hydrolyzed, thereby removing water from the electrolyte, and the hydrolysis product of the dehydrating additive can form a uniform and dense interface film on the surface of the positive and negative electrodes of the battery. The interface film can effectively prevent the side reactions caused by direct contact between the electrolyte and the positive and negative electrode materials, thereby improving the cycle performance and safety performance of the battery.
[0009] Optionally, at least one of R1, R2, R3 and R4 is fluorine or a fluorinated alkyl group.
[0010] Optionally, at least one of R1, R2, R3 and R4 is fluorine.
[0011] Optionally, at least one of R1, R2, R3 and R4 is alkenylalkyl, alkynylalkyl, alkenyl or alkynyl.
[0012] Optionally, the carbon atoms of the alkyl group, the fluoroalkyl group, the alkenylalkyl group, the alkynylalkyl group, the alkenyl group and the alkynyl group have 1-10 carbon atoms.
[0013] Optionally, the aryl group or the fluorinated aryl group has 6-20 carbon atoms.
[0014] Optionally, the mass percentage of the dehydrating additive in the secondary battery electrolyte is 0.1%-3%. Further, the mass percentage of the dehydrating additive in the secondary battery electrolyte is 0.5%-1.5%.
[0015] Optionally, the additives further include film-forming additives.
[0016] Optionally, the film-forming additive includes one or more of vinylene carbonate, fluoroethylene carbonate, methylene disulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, propylene sulfite, vinyl sulfate, 1,3-propane sultone and tripropylene phosphate.
[0017] Optionally, the mass percentage of the film-forming additive in the secondary battery electrolyte is 0.1%-5%.
[0018] Optionally, the mass ratio of the water-removing additive to the film-forming additive is 1:(0.1-10).
[0019] Optionally, the organic solvent includes one or more of a carbonate solvent, an ether solvent, and a carboxylate solvent.
[0020] Optionally, the electrolyte salt includes at least one of a lithium salt, a sodium salt and a potassium salt.
[0021] In a second aspect, the present application provides a secondary battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte comprises the secondary battery electrolyte as described in the first aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A schematic diagram of the structure of a secondary battery provided in one embodiment of the present application;
[0023] Figure 2 This is a scanning electron microscope image of the positive electrode sheet of the battery provided in Example 1 of the present application;
[0024] Figure 3 This is a scanning electron microscope image of the positive electrode of the battery provided in Comparative Example 3 of the present application. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0026] When the battery electrolyte contains water, the electrolyte lithium salt reacts with water to produce a series of by-products, such as HF, PF5, HPO2F2, H2PO3F and H3PO4, etc. Such substances will cause irreversible damage to lithium-ion batteries. For example, HF will dissolve the interface film on the surface of the positive and negative electrodes of the battery, causing the electrolyte to decompose on the surface of the positive and negative electrodes, reducing the service life of the battery. Although the existing dehydrating additives can remove water from the electrolyte, they cannot form a complete protective film, causing the electrolyte to be continuously oxidized at the positive electrode, deteriorating the battery performance. The present application provides a dehydrating additive, which can not only remove water and acid from the electrolyte and reduce side reactions in the battery, but also the product of the reaction between the dehydrating additive and water has good film-forming properties, and can form a stable interface film on the surface of the positive and negative electrodes of the battery, thereby protecting the positive and negative electrode materials of the battery, inhibiting the side reactions of the electrolyte on the surface of the positive and negative electrodes of the battery, and improving the battery performance.
[0027] The dewatering additive provided in the present application includes oxathiazophosphorus, and the structural formula of oxathiazophosphorus is shown in formula (1):
[0028]
[0029] In the present application, the oxythioazaphosphine contains a variety of heteroatoms, and the positions of the heteroatoms and the substitution positions of the substituents ensure that the oxythioazaphosphine has high stability and is not easy to decompose. The sulfonyl and phosphoryl groups in the oxythioazaphosphine structure have strong electron-withdrawing ability, so that the POC bond in the water-removing additive is easily hydrolyzed, thereby removing the water in the electrolyte, and the P, N, S heteroatoms in the hydrolysis product can greatly improve the thermal stability of the CEI film and the SEI film, thereby inhibiting the occurrence of positive and negative electrode side reactions under high temperature conditions, and ensuring that the lithium secondary battery has good high temperature resistance.
[0030] In the embodiment of the present application, R1 and R3 are independently selected from any one of hydrogen, fluorine, alkyl, fluoroalkyl, alkenylalkyl, alkynylalkyl, alkenyl, and alkynyl, and R2 and R4 are independently selected from any one of fluorine, alkyl, fluoroalkyl, alkenylalkyl, alkynylalkyl, alkenyl, alkynyl, aryl, and fluoroaryl. In the embodiment of the present application, when the substituent group is selected from alkyl, the alkyl group can be any one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, cyclopropyl, or cyclobutyl; when the substituent group is selected from fluoroalkyl, the fluoroalkyl group can be any one of trifluoromethyl, trifluoroethyl, trifluoropropyl, pentafluoropropyl, trifluorobutyl, and pentafluorobutyl; when the substituent group is selected from alkenylalkyl, the alkenylalkyl group can be any one of allyl, allylbutyl, allylisobutyl, allylpentyl, and allylisopentyl; the substituent group When selected from alkynylalkyl, alkynylalkyl can be any one of propargyl, alkynylbutyl, isobutyl, alkynylpentyl and isopentyl; when the substituent group is selected from alkenyl, the alkenyl can be any one of vinyl, propenyl and butenyl; when the substituent group is selected from alkynyl, the alkynyl can be any one of ethynyl and propynyl; when the substituent group is selected from aryl, the aryl can be any one of phenyl, methylphenyl and dimethylphenyl; when the substituent group is selected from fluoroaryl, the fluoroaryl can be any one of p-fluorophenyl, p-trifluorophenyl and p-trifluoroethylphenyl. In the embodiment of the present application, R1, R2, R3 and R4 can be the same or different groups.
[0031] In some embodiments of the present application, at least one of R1, R2, R3 and R4 is fluorine or fluoroalkyl. In the embodiments of the present application, when the substituent group includes fluorine or fluoroalkyl, the dehydrating additive contains a certain amount of fluoride (such as LiF) in the interface film formed on the electrode surface, thereby more effectively isolating the electrolyte from the electrode, thereby inhibiting the occurrence of side reactions of the electrolyte on the electrode surface. Further, when multiple substituent groups include fluorine or fluoroalkyl in R1, R2, R3 and R4, it is beneficial to increase the content of fluoride in the interface film and improve the protective performance of the interface film. In some embodiments of the present application, at least one of R1, R2, R3 and R4 is fluorine. When at least one of R1, R2, R3 and R4 is fluorine, since the fluorine atom has a strong electron-withdrawing ability, the reactivity of the POC bond in the oxygen, sulfur, nitrogen and phosphorus can be greatly improved with water, thereby promoting the reaction of the dehydrating additive with water, increasing the reaction rate, and achieving effective removal of water in the electrolyte.
[0032] In the present application, when the substituent group contains an unsaturated double bond or triple bond, that is, at least one of R1, R2, R3 and R4 is an alkenyl alkyl, alkynyl alkyl, alkenyl or alkynyl group, since the unsaturated double bond or triple bond has electron-withdrawing ability, the reactivity of the POC bond in the oxysulfuryl nitrogen phosphine with water can be increased, thereby promoting the reaction of the water removal additive with water, increasing the reaction rate, and achieving effective removal of water from the electrolyte.
[0033] In the embodiment of the present application, the carbon number of the carbon atoms of the alkyl, fluoroalkyl, alkenylalkyl, alkynylalkyl, alkenyl and alkynyl groups is 1-10, and further, the carbon number of the alkyl, fluoroalkyl, alkenylalkyl, alkynylalkyl, alkenyl and alkynyl groups is 1-5. The carbon number of the alkyl, fluoroalkyl, alkenylalkyl, alkynylalkyl, alkenyl and alkynyl groups can be, but not limited to, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10. When the number of carbon atoms is too high, the steric hindrance of the substituent is too large, reducing the stability of the water removal additive, and the excessive chain length of the substituent group will cause the non-polarity of the water removal additive to be too strong, reducing the solubility of the water removal additive in the electrolyte.
[0034] In the embodiment of the present application, the carbon number of the aryl group and the fluoroaryl group is 6-20, and further, the carbon number of the aryl group and the fluoroaryl group is 6-10. The carbon number of the aryl group and the fluoroaryl group can be, but is not limited to, 6, 7, 8, 9, 10, 13, 17 or 20. A lower carbon number is beneficial to control the molecular weight of the water removal additive, thereby better controlling the viscosity of the electrolyte.
[0035] In some specific embodiments of the present application, the water removal additive may be any one or more compounds as shown in Table 1:
[0036] Table 1 Structural formula and name of additives in some embodiments of the present application
[0037]
[0038]
[0039]
[0040] The dewatering additive provided by the present application includes a compound whose main structure is an oxygen-sulfur-nitrogen-phosphine compound. The dewatering additive of this structure can effectively remove water from the electrolyte and reduce the occurrence of side reactions. The hydrolyzed product of the dewatering additive can form an SEI film on the surface of the negative electrode, inhibit the damage of the electrolyte solvent to the negative electrode structure, and protect the negative electrode. It can also form a CEI film on the surface of the positive electrode to prevent the dissolution of positive electrode metal ions, stabilize the positive electrode structure, and inhibit the gas production of the electrolyte on the positive electrode side, ensuring that the battery has a high energy density and cycle life. The formed SEI film and CEI film have low impedance, which is conducive to improving the internal dynamic characteristics of lithium-ion batteries and reducing interface impedance, thereby effectively improving the cycle performance, high temperature storage performance and low temperature performance of lithium secondary batteries. The dewatering additive of the present application has good compatibility with positive and negative electrode materials and has little impact on the battery system.
[0041] The dewatering additive of the present application can be prepared by different methods, and the specific preparation method is not limited. Taking the dewatering additive 2-fluoro-1,5,4,2-oxothioazophosphine-4-fluorosulfonyl-2,5,5-trioxide numbered 1 in Table 1 as an example, the synthesis route of the dewatering additive 1 is as follows:
[0042]
[0043] The dewatering additive numbered 1 in Table 1 can be obtained through the above synthesis route. Correspondingly, other dewatering additives of the present application can be obtained by adjusting the substituent groups of the reactants, which will not be described in detail here.
[0044] The present application also provides a secondary battery electrolyte, comprising an electrolyte salt, an organic solvent and an additive, wherein the additive comprises the water-removing additive mentioned above in the present application.
[0045] In the embodiments of the present application, the mass percentage of the dehydrating additive in the secondary battery electrolyte is 0.1%-3%. In some embodiments of the present application, the mass percentage of the dehydrating additive in the secondary battery electrolyte is 0.5%-1.5%. The mass percentage of the dehydrating additive in the secondary battery electrolyte can be, but is not limited to, 0.1%, 0.5%, 1%, 1.5%, 2% or 3%. Within the above mass percentage range, the dehydrating additive can fully remove the water in the battery electrolyte, and the hydrolysis product can form a complete protective layer on the surface of the positive and negative pole pieces, effectively improving the stability of the battery pole pieces. Considering that the thickness of the protective layer formed by the hydrolysis product is too large, it will cause a large interfacial impedance, hinder the transmission of lithium ions, and reduce the discharge capacity. Therefore, the concentration of the dehydrating additive should not be too high.
[0046] In some embodiments of the present application, the additive also includes a film-forming additive. The film-forming additive can form an organic film on the surface of the electrode. In the formation stage of the battery, the hydrolyzate of the water-removing additive can work together with the film-forming additive to form an interface film with high density and good elastic properties. In some embodiments of the present application, the film-forming additive includes one or more of vinylene carbonate (VC), fluoroethylene carbonate (FEC), methylene disulfonate (MMDS), lithium difluorophosphate (LiDFP), lithium difluorooxalatoborate (LiDFOB), vinyl sulfate (DTD), 1,3-propane sultone (PS), propylene sulfite and tripropylene phosphate.
[0047] In the implementation manner of the present application, the mass percentage of the film-forming additive in the secondary battery electrolyte is 0.1%-5%. The mass percentage of the film-forming additive in the secondary battery electrolyte can be, but is not limited to, 0.1%, 0.5%, 1%, 2%, 3% or 5%. In the implementation manner of the present application, the mass ratio of the water-removing additive to the film-forming additive is 1:(0.1-10). In some implementation manners of the present application, the mass ratio of the water-removing additive to the film-forming additive is 1:(0.7-1.5). Within the above mass ratio range, the water-removing additive can play a good cooperative role with the film-forming additive, which is conducive to the formation of a dense and elastic interface film. In the present application, the mass ratio of the water-removing additive to the film-forming additive can be, but is not limited to, 1:0.1, 1:0.5, 1:0.7, 1:1, 1:1.5, 1:2, 1:5 or 1:10.
[0048] In the embodiment of the present application, according to different secondary battery systems, the electrolyte salt in the secondary battery electrolyte can be a lithium salt, a sodium salt, a potassium salt, etc. In some embodiments of the present application, the lithium salt includes lithium hexafluorophosphate (LiPF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethylsulfonyl imide (LiTFSI), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium hexafluoroantimonate (LiSbF6), lithium perchlorate (LiClO4), lithium bistrifluoromethylsulfonyl imide (LiTFSI), lithium bisoxalate borate (LiBOB), lithium difluorooxalate borate (LiDFOB), lithium trifluoromethylsulfonate (LiCF3SO3), lithium perfluorobutylsulfonate (LiC4F9SO3), lithium bis(trifluoromethylsulfonyl) imide (Li(CF3SO2)2N), lithium bis(perfluoroethylsulfonyl) imide (Li(C2F5SO2)2N) One or more. In this application, there is no special requirement for the electrolyte salt content in the secondary battery electrolyte, and its content can refer to the conventional amount in the art. In some embodiments of this application, the concentration of the electrolyte salt in the secondary battery electrolyte is 0.1mol / L-5mol / L, and further, the concentration of the electrolyte salt in the secondary battery electrolyte is 0.5mol / L-1.5mol / L.
[0049] In the embodiments of the present application, the organic solvent includes one or more of carbonate solvents, ether solvents, and carboxylate solvents. Wherein, carbonate solvents can be cyclic and / or chain-shaped, and carboxylate solvents can be linear and / or branched. In some embodiments of the present application, the organic solvent includes ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate, ethyl acetate, propyl acetate, ethyl propionate, ethyl butyrate, etc. One or more, but not limited to this. In some embodiments of the present application, the organic solvent includes ethylene carbonate (EC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC) and dimethyl carbonate (DMC), wherein the mass ratio of ethylene carbonate (EC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC) and dimethyl carbonate (DMC) is 1:(0.5-1.5):(0.5-1.5):(0.1-1).
[0050] The present application also provides a secondary battery, including a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte includes the secondary battery electrolyte provided in the present application. Figure 1 , Figure 1A schematic diagram of the structure of a secondary battery provided in one embodiment of the present application. The secondary battery includes a positive electrode 10, a negative electrode 20, a separator 30, and an electrolyte 40. When the secondary battery is charged, lithium ions are released from the positive electrode 10 and deposited on the negative electrode 20 after passing through the electrolyte 40; when discharged, lithium ions are released from the negative electrode 20 and embedded in the positive electrode 10 after passing through the electrolyte 40. The secondary battery provided in the present application has good cycle performance and safety performance because it adopts the above-mentioned secondary battery electrolyte. In the embodiment of the present application, the secondary battery can be a lithium secondary battery, a potassium secondary battery, a sodium secondary battery, etc.
[0051] In the present application, the negative electrode of the secondary battery may be any negative electrode known in the art. In the embodiment of the present application, the negative electrode may include one or more of a carbon-based negative electrode, a silicon-based negative electrode, a tin-based negative electrode, a lithium negative electrode, a sodium negative electrode and a potassium negative electrode. Among them, the carbon-based negative electrode may include graphite, hard carbon, soft carbon, graphene, etc.; the silicon-based negative electrode may include silicon, silicon carbon, silicon oxygen, silicon metal compounds, etc.; the tin-based negative electrode may include tin, tin carbon, tin oxygen, tin metal compounds; the lithium negative electrode may include metallic lithium or a lithium alloy. The lithium alloy may specifically be at least one of a lithium silicon alloy, a lithium sodium alloy, a lithium potassium alloy, a lithium aluminum alloy, a lithium tin alloy and a lithium indium alloy. In some embodiments of the present application, the current collector of the negative electrode is copper foil, and the negative electrode active material includes one or more of natural graphite, artificial graphite, hard carbon, soft carbon, lithium titanate, iron oxide, lithium titanium phosphate, titanium dioxide, silicon, silicon oxide, tin and antimony; the binder includes one or more of polyacrylic acid (PAA), polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC) and styrene butadiene latex (SBR); the conductive agent includes one or more of acetylene black, ketjen black, Super-P, carbon nanotubes, carbon nanofibers, activated carbon and graphene. In the present application, the preparation method of the negative electrode can adopt any method known in the art.
[0052] In the embodiment of the present application, the positive electrode of the secondary battery includes a positive electrode active material that can reversibly embed / de-embed metal ions (lithium ions, sodium ions, potassium ions, etc.). The positive electrode of the secondary battery in the present application can be any positive electrode known in the art. Taking lithium secondary batteries as an example, the positive electrode active material can be but is not limited to lithium cobalt oxide (LiCoO2), lithium iron phosphate (LiFePO4), LiNi 0.33 Co 0.33 Mn 0.33 O2(NCM111), LiNi 0.4 Co 0.2 Mn 0.4 O2(NCM424),LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523),LiNi 0.6 Co 0.2 Mn 0.2O2(NCM622),LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811) or more.
[0053] In the embodiment of the present application, the separator of the secondary battery can be any separator known to those skilled in the art, for example, the separator can be one or more of polyolefin microporous membrane, polyethylene terephthalate, polyethylene felt, glass fiber felt or ultrafine glass fiber paper.
[0054] In the embodiments of the present application, the battery can be prepared by using either a lamination process or a winding process. In some embodiments of the present application, the battery is prepared by using a lamination process.
[0055] The technical solution of the present application is further described below with reference to a number of embodiments.
[0056] Example 1
[0057] 1) Preparation of secondary battery electrolyte
[0058] 30g of ethylene carbonate (EC), 30g of ethyl methyl carbonate (EMC), 30g of diethyl carbonate (DEC) and 10g of dimethyl carbonate (DMC) are mixed to obtain an organic solvent, and then 14g of lithium hexafluorophosphate (LiPF6) and 1g of vinylene carbonate (VC) are dissolved in the above solvent, stirred and mixed to form a uniform solution, and then a dehydrating additive having a molecular structure shown in formula (A) is added to the above solution to obtain a secondary battery electrolyte. The mass of the dehydrating additive is 1g.
[0059]
[0060] 2) Preparation of lithium secondary batteries
[0061] Graphite, sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) were mixed in a weight ratio of 100:3:2, and water was added to stir into a uniform slurry. The slurry was coated on a copper foil current collector with a thickness of 10 μm, and after drying in an oven at 100°C for 24 hours, the negative electrode sheet was obtained after rolling and slitting.
[0062] LiFePO4, acetylene black and polyvinylidene fluoride (PVDF) are mixed in a weight ratio of 95:3:2, and N-methylpyrrolidone is added and stirred into a uniform slurry. The slurry is coated on an aluminum foil with a thickness of 12 μm, dried at 120°C for 24 hours, and rolled and cut to obtain positive electrode sheets. The water content of the positive electrode sheets is 50ppm-400ppm.
[0063] Take a PE separator with a thickness of 12 μm and cut it into the required size to obtain a battery separator. The positive electrode sheet, negative electrode sheet and battery separator prepared above are wound into a battery cell, and the above secondary battery electrolyte is poured into it. After the formation process, a soft-pack lithium secondary battery S1 is made.
[0064] Example 2
[0065] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 2 is the same as that in Example 1, except that the dehydrating additive in Example 2 has a different component. The molecular structure of the dehydrating additive in Example 2 is shown in Formula (B):
[0066]
[0067] The soft-pack lithium secondary battery prepared in Example 2 is named S2.
[0068] Example 3
[0069] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 3 is the same as that in Example 1, except that the dehydrating additive in Example 3 has a different component. The molecular structure of the dehydrating additive in Example 3 is shown in Formula (C):
[0070]
[0071] The soft-pack lithium secondary battery prepared in Example 3 is named S3.
[0072] Example 4
[0073] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 4 is the same as that in Example 1, except that the dehydrating additive in Example 4 has a different component. The molecular structure of the dehydrating additive in Example 4 is shown in Formula (D):
[0074]
[0075] The soft-pack lithium secondary battery prepared in Example 4 is named S4.
[0076] Example 5
[0077] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 5 is the same as that in Example 1, except that the dehydrating additive in Example 5 has a different component. The molecular structure of the dehydrating additive in Example 5 is shown in Formula (E):
[0078]
[0079] The soft-pack lithium secondary battery prepared in Example 5 is named S5.
[0080] Example 6
[0081] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 6 is the same as that in Example 1, except that the dehydrating additive in Example 6 has a different component. The molecular structure of the dehydrating additive in Example 6 is shown in Formula (F):
[0082]
[0083] The soft-pack lithium secondary battery prepared in Example 6 is named S6.
[0084] Example 7
[0085] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 7 is the same as that in Example 1, except that the dehydrating additive in Example 7 has a different component. The molecular structure of the dehydrating additive in Example 7 is shown in Formula (G):
[0086]
[0087] The soft-pack lithium secondary battery prepared in Example 7 is named S7.
[0088] Example 8
[0089] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 8 is the same as that in Example 1, except that the dehydrating additive in Example 8 has a different component. The molecular structure of the dehydrating additive in Example 8 is shown in Formula (H):
[0090]
[0091] The soft-pack lithium secondary battery prepared in Example 8 is named S8.
[0092] Example 9
[0093] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 9 is the same as that in Example 1, except that the dehydrating additive in Example 9 has a different component. The molecular structure of the dehydrating additive in Example 9 is shown in Formula (I):
[0094]
[0095] The soft-pack lithium secondary battery prepared in Example 9 is named S9.
[0096] Example 10
[0097] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 10 is the same as that in Example 1, except that the dehydrating additive in Example 10 has a different component. The molecular structure of the dehydrating additive in Example 10 is shown in Formula (J):
[0098]
[0099] The soft-pack lithium secondary battery prepared in Example 10 is named S10.
[0100] Embodiment 11
[0101] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 11 is the same as that in Example 1, except that the dehydrating additive in Example 11 has a different component. The molecular structure of the dehydrating additive in Example 11 is shown in Formula (K):
[0102]
[0103] The soft-pack lithium secondary battery prepared in Example 11 is named S11.
[0104] Example 12
[0105] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 12 is the same as that in Example 1, except that the dehydrating additive in Example 12 has a different component. The molecular structure of the dehydrating additive in Example 12 is shown in Formula (L):
[0106]
[0107] The soft-pack lithium secondary battery prepared in Example 12 is named S12.
[0108] Example 13
[0109] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 13 is the same as that in Example 1, except that the dehydrating additive in Example 13 has a different component. The molecular structure of the dehydrating additive in Example 13 is shown in Formula (M):
[0110]
[0111] The soft-pack lithium secondary battery prepared in Example 13 is named S13.
[0112] Embodiment 14
[0113] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 14 is the same as that in Example 1, except that the mass of the water removal additive in Example 14 is 0.1 g. The soft-pack lithium secondary battery prepared in Example 14 is named S14.
[0114] Embodiment 15
[0115] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 15 is the same as that in Example 1, except that the mass of the water removal additive in Example 15 is 4 g. The soft-pack lithium secondary battery prepared in Example 15 is named S15.
[0116] Example 16
[0117] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Example 16 is the same as that in Example 1, except that vinylene carbonate is not added in Example 16. The soft-pack lithium secondary battery prepared in Example 16 is named S16.
[0118] In order to highlight the beneficial effects of the present application, the following comparative examples are set.
[0119] Comparative Example 1
[0120] 1) Preparation of secondary battery electrolyte
[0121] In an argon glove box with a water content of <2ppm, 30g of ethylene carbonate (EC), 30g of ethyl methyl carbonate (EMC), 30g of diethyl carbonate (DEC) and 10g of dimethyl carbonate (DMC) were mixed to obtain an organic solvent, and then 14g of lithium hexafluorophosphate (LiPF6) and 1g of vinylene carbonate (VC) were dissolved in the above solvent, stirred and mixed into a uniform solution, and then 1g of hexamethyldisilazane was added to the above solution to obtain a secondary battery electrolyte.
[0122] Preparation of lithium secondary batteries
[0123] The positive electrode sheet and the negative electrode sheet were prepared in the same manner as in Example 1, and the positive electrode sheet, the negative electrode sheet and the separator were wound into a battery cell, which was infused with the above-mentioned secondary battery electrolyte, and the soft-pack lithium secondary battery C1 was manufactured after processes such as formation.
[0124] Comparative Example 2
[0125] The preparation method of the secondary battery electrolyte and the lithium secondary battery in Comparative Example 2 is the same as that in Comparative Example 1, except that the mass of hexamethyldisilazane in Comparative Example 2 is 0.1 g. The soft-pack lithium secondary battery prepared in Comparative Example 2 is named C2.
[0126] Comparative Example 3
[0127] 1) Preparation of secondary battery electrolyte
[0128] In an argon glove box with a water content of <2ppm, 30g of ethylene carbonate (EC), 30g of ethyl methyl carbonate (EMC), 30g of diethyl carbonate (DEC) and 10g of dimethyl carbonate (DMC) were mixed to obtain an organic solvent, and then 14g of lithium hexafluorophosphate (LiPF6) and 1g of vinylene carbonate (VC) were dissolved in the above solvent, and the mixture was stirred to form a uniform solution to obtain a secondary battery electrolyte.
[0129] 2) Preparation of lithium secondary batteries
[0130] The positive electrode sheet and the negative electrode sheet were prepared in the same manner as in Comparative Example 1, and the positive electrode sheet, the negative electrode sheet and the separator were wound into a battery cell, which was infused with the above-mentioned secondary battery electrolyte, and the soft-pack lithium secondary battery C3 was prepared after processes such as formation.
[0131] Effect Example
[0132] In order to strongly support the beneficial effects brought by the technical solutions of the embodiments of this application, the following tests are provided:
[0133] 1) The soft-pack lithium secondary battery S1 of Example 1 and the soft-pack lithium secondary battery C3 of Comparative Example 3 were disassembled and the battery electrodes were taken out for morphological characterization. Figure 2 and Figure 3 , Figure 2 This is a scanning electron microscope image of the positive electrode of the battery provided in Example 1 of the present application. Figure 3 This is a scanning electron microscope image of the positive electrode of the battery provided in Comparative Example 3 of this application. Figure 2 It can be seen that when the secondary electrolyte contains the water removal additive of the present application, a granular deposition layer is formed on the surface of the positive electrode of the battery. The deposition layer is the CEI film on the surface of the positive electrode of the battery, which can well protect the positive electrode. Figure 3 It can be seen that when the electrolyte does not contain the water-removing additive, the surface of the positive electrode of the battery is relatively smooth, that is, the positive electrode surface of the soft-pack lithium secondary battery C3 of Comparative Example 3 does not have a protective layer.
[0134] 2) The soft-pack lithium secondary batteries of Examples 1-16 and Comparative Examples 1-3 were subjected to cycle performance tests. The specific test conditions were as follows: the soft-pack lithium secondary batteries were charged to 15% SOC at a constant current of 0.05C at a temperature of 25°C, then charged to 3.8V at 0.25C, constant voltage to 0.02C, and then discharged to 2.5V at 0.33C, and the first charge and discharge capacity was recorded and the coulomb efficiency was calculated. Then the batteries were charged to 3.8V at a current of 1C, constant voltage to a current of 0.02C, and then discharged to 2.5V at 200mA, which was taken as the first cycle; after repeated charge and discharge cycles for 200 times, the discharge capacity of the 200th cycle was recorded, and the capacity retention rate after 200 cycles was calculated. The calculation formula was: Capacity retention rate after 200 cycles (%) = discharge capacity of 200 cycles / discharge capacity of the first cycle × 100%. The test results of the high temperature cycle performance of the soft-pack batteries of Examples 1-16 and Comparative Examples 1-3 are shown in Table 2.
[0135] Table 2 Performance parameters of soft pack batteries of Examples 1-16 and Comparative Examples 1-3
[0136]
[0137]
[0138] As can be seen from Table 2, compared with Comparative Examples 1-3, the soft-pack lithium secondary batteries of Examples 1-16 of the present application have better cycle performance, and the batteries show a higher capacity retention rate after 200 cycles, which is due to the addition of the dehydrating additive of the present application to the electrolyte of Examples 1-16. The dehydrating additive of the present application can effectively remove water from the electrolyte, and the hydrolysis product of the dehydrating additive can form a stable interface film on the surface of the positive and negative electrodes of the battery, preventing the side reactions of the electrolyte on the surface of the positive and negative electrodes, thereby improving the cycle performance of the battery.
[0139] 3) After the soft-pack lithium secondary batteries of Examples 1-16 and Comparative Examples 1-3 were cycled 200 times, an AC impedance test was performed at 80% SOC, and the test frequency range was 0.1-105HZ to obtain the impedance of the battery. The tested battery was disassembled, and the content of iron in the negative electrode plate was tested by an inductively coupled plasma (ICP) instrument. The average value of the test was taken for 200 times to obtain the amount of dissolved iron in the negative electrode plate, and the water content in the battery electrolyte was tested at the same time. The results of the impedance, dissolved iron content and water content of the soft-pack batteries of Examples 1-16 and Comparative Examples 1-3 are shown in Table 3.
[0140] Table 3 Parameters of soft pack batteries of Examples 1-16 and Comparative Examples 1-3
[0141]
[0142]
[0143] It can be seen from Table 3 that compared with comparative examples 1-3, the soft-pack lithium secondary batteries of embodiments 1-16 of the present application have lower impedance, and when the electrolyte contains the dehydrating additive of the present application, the water content in the electrolyte is greatly reduced, and the amount of dissolved iron in the electrode is also greatly reduced, thereby ensuring that the battery has a higher capacity retention rate.
[0144] The above is a preferred embodiment of the present application, but it should not be understood as limiting the scope of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. A secondary battery electrolyte, characterized in that: It includes an electrolyte salt, an organic solvent and a water-removing additive, wherein the water-removing additive includes a compound with a structural formula as shown in formula (1): Wherein, R1 and R3 are independently selected from any one of hydrogen, fluorine, alkyl, fluoroalkyl, alkenylalkyl, alkynylalkyl, alkenyl, and alkynyl; R2 and R4 are independently selected from any one of fluorine, alkyl, fluoroalkyl, alkenylalkyl, alkynylalkyl, alkenyl, and alkynyl.
2. The secondary battery electrolyte according to claim 1, characterized in that At least one of R1, R2, R3 and R4 is fluorine or a fluorinated alkyl group.
3. The secondary battery electrolyte according to claim 2, characterized in that: At least one of R1, R2, R3 and R4 is fluorine.
4. The secondary battery electrolyte according to claim 1, characterized in that At least one of R1, R2, R3 and R4 is alkenylalkyl, alkynylalkyl, alkenyl or alkynyl.
5. The secondary battery electrolyte according to claim 1, characterized in that: The alkyl group, the fluoroalkyl group, the alkenylalkyl group, the alkynylalkyl group, the alkenyl group and the alkynyl group have 1 to 10 carbon atoms; the aryl group and the fluoroaryl group have 6 to 20 carbon atoms.
6. The secondary battery electrolyte according to claim 1, characterized in that: The mass percentage of the water removal additive in the secondary battery electrolyte is 0.1%-3%.
7. The secondary battery electrolyte according to any one of claims 1 to 6, characterized in that: The secondary battery electrolyte also includes a film-forming additive; the film-forming additive includes one or more of vinylene carbonate, fluoroethylene carbonate, methylene disulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, propylene sulfite, vinyl sulfate, 1,3-propane sultone and tripropylene phosphate.
8. The secondary battery electrolyte according to claim 7, characterized in that: The mass ratio of the water removal additive to the film-forming additive is 1:(0.1-10).
9. The secondary battery electrolyte according to claim 1, characterized in that: The organic solvent includes one or more of carbonate solvents, ether solvents, and carboxylate solvents.
10. The secondary battery electrolyte according to claim 1, characterized in that: The electrolyte salt includes at least one of a lithium salt, a sodium salt, and a potassium salt.
11. A secondary battery, characterized in that: The invention comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte comprises the secondary battery electrolyte as claimed in any one of claims 1 to 10.
Citation Information
Patent Citations
Lithium ion power battery non-water electrolyte
CN106025359A
Method for producing lithium fluorosulfonate, lithium fluorosulfonate, nonaqueous electrolyte solution, and nonaqueous electrolyte secondary battery
CN106882820A
High-temperature lithium ion battery electrolyte and preparation method thereof and high-temperature lithium ion battery
CN107331893A
Non-aqueous electrolyte and lithium-ion battery containing non-aqueous electrolyte
CN110299561A
Non-aqueous electrolyte, battery containing non-aqueous electrolyte and electric vehicle
CN110635167A