C-type hollow core optical fiber, preparation method and application thereof
Through laser erosion and heating drawing technology, the problem of side channel processing of hollow core fibers is solved, and the preparation of C-type hollow core fiber structures is realized at a meter-level continuous C-type hollow core fiber structure, simplifying the processing process and improving the practicality and universality of the structure. .
Patent Information
- Application Number
- CN202211223642.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-10-08
AI Technical Summary
The introduction or opening of the side channels of the hollow core fiber in the prior art requires complex micro-machining processing, resulting in difficulty in positioning, structural damage, increased loss and the inability to achieve a meter-level continuous C-type hollow core fiber structure, which is insufficient in practicality and universality. .
The casing cladding of the hollow core fiber prefabricated rod is laterally eroded by laser to form slits, and combined with heating and drawing, the drawing parameters are adjusted to achieve longitudinal continuous side channels, forming a C-type air-space that can be used for gas exchange Core fiber structure.
Simplified the processing process, improved positioning accuracy and structural integrity, realized the preparation of continuous C-type hollow core optical fiber structures with a meter-length length, avoided secondary casing processing and subsequent complex processing, and improved practicality and universality .
Smart Images

Figure CN115572058B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of optical fiber technology, and in particular to a method for preparing a C-type hollow-core optical fiber and the C-type hollow-core optical fiber and its application. Background Art
[0002] Hollow-core fiber is an excellent choice for new low-capacity, low-loss interaction gas cavity in laser gas sensing technology. Using hollow-core fiber as a gas absorption microcavity is not only resistant to electromagnetic interference, stable in operation, lightweight, and easy to integrate, but its natural longitudinal ductility can greatly increase the distance of light-gas interaction and improve the sensitivity of gas detection. In particular, the anti-resonant hollow-core fiber that has emerged in recent years can confine more than 99.99% of the light energy in the air core through a single-layer wavelength-thick negative curvature thin-wall microstructure cladding. The low-loss transmission window covers the ultraviolet to mid-infrared band, and is an ideal platform channel for high-precision, multi-component gas sensing. However, ordinary hollow-core optical fibers can only exchange gas through the end face, and the core hole of only micrometer level will result in a slower response speed when using long-distance hollow-core optical fiber for sensing. In addition, the end-face air intake method requires the input of the laser to rely on spatial coupling, making it difficult to achieve full fiberization of the device.
[0003] To this end, a microchannel is manufactured on the side of the hollow-core fiber to form a C-shaped structure to connect the outside world and the core, so that the outside gas can enter the core through the side microchannel, which is conducive to shortening the gas exchange time and improving the response speed. At the same time, the end face is freed for non-spatial coupling connection to realize the full fiberization of the system. In particular, thanks to the node-free characteristics of the antiresonant cladding, it is expected to introduce side channels into the antiresonant hollow-core fiber without destroying the microstructure cladding, and in theory, it basically does not affect the fiber loss properties [J. Lightwave Technol. 36, 3162–3168 (2018)]. In the prior art, a femtosecond laser [Sensors 21, 7591 (2021)] is usually used to perform micromachining on the side of the hollow-core fiber, thereby forming a number of spaced side through holes along the length of the fiber as a gas exchange channel between the core and the outside world. In addition, there are also reports [Opt. Mater. Express 11, 338–343 (2021)] using a focused ion beam to micro-process and remove the sleeve cladding of the hollow-core fiber to obtain a microchannel. Patent CN113885120A also provides a double-clad antiresonant hollow-core optical fiber and a preparation method thereof. The prepared C-type hollow-core optical fiber structure is wrapped in a secondary casing. After further post-processing of the optical fiber to remove the secondary casing, the side channel can be opened to expose it to the external environment. Summary of the invention
[0004] In the prior art, the introduction or opening of the side channel of the hollow-core optical fiber needs to be achieved through complex processing at the optical fiber scale. Not only is the technical requirement high, but the processing position is difficult to determine. It is easy to cause damage to the optical fiber structure due to inaccurate positioning during the processing, introducing additional losses, and it is time-consuming. Most of them can only process single-point through holes at intervals over a short length, and cannot achieve a meter-level continuous C-type hollow-core optical fiber structure. It lacks practicality and universality, and is difficult to promote.
[0005] In order to solve the above technical problems, the present invention provides a method for preparing a C-type hollow-core optical fiber, in which a laser is used to ablate the side of the sleeve cladding of the hollow-core optical fiber preform to form a slit, thereby forming a side channel for gas exchange between the fiber core and the outside world.
[0006] The technical solution of the present invention is as follows:
[0007] A method for preparing a C-type hollow core optical fiber, characterized in that it comprises:
[0008] A laser is used to ablate the side of the sleeve cladding of the hollow core optical fiber preform rod, thereby forming one or more continuous slits in the longitudinal direction thereof;
[0009] The hollow-core optical fiber preform with a slit is heated and drawn, and the structural forming of the C-type hollow-core optical fiber is achieved by adjusting the drawing parameters and maintained continuously at a meter-level length, that is, a side channel that connects the fiber core with the external environment and allows gas exchange is formed, and the side channel extends continuously in the longitudinal direction at a meter-level length.
[0010] In the method for preparing the C-type hollow core optical fiber, the laser is a continuous or pulsed laser, and the selected wavelength can ablate the corresponding optical fiber matrix material. For example, for a silica matrix, preferably, a carbon dioxide laser with a wavelength of 10.6 μm can be selected.
[0011] In the C-type hollow-core optical fiber preparation method, the laser is focused on the side surface of the sleeve cladding of the hollow-core optical fiber preform or its vicinity through a lens, and reciprocates relative displacement with it in the longitudinal or transverse direction. An electric translation stage can be used to control the longitudinal movement of the hollow-core optical fiber preform, and a galvanometer system can be used to control the transverse movement of the laser beam. The inner wall of the sleeve cladding corresponding to the laser processing position is connected to the fiber core, forming one or more continuous slits in the longitudinal direction.
[0012] In the C-type hollow-core optical fiber preparation method, by adjusting the focused spot size, average power, scanning length, width, speed and number of repetitions of the laser, the heat energy accumulated on the side surface of the hollow-core optical fiber preform is made higher than the ablation threshold of the matrix material, and the width control of the side slit is achieved.
[0013] In the method for preparing the C-type hollow-core optical fiber, the width of the slit is within 1 mm, and each slit extends for more than 10 cm along the longitudinal direction of the hollow-core optical fiber preform.
[0014] In the C-type hollow-core optical fiber preparation method, when the laser is performing ablation processing, an inert gas can be introduced into the hollow-core optical fiber preform rod at the same time, and an extraction device can be placed near the laser processing location to remove dust generated during the laser ablation process and prevent it from being deposited on the hollow-core optical fiber preform rod and optomechanical components.
[0015] In the method for preparing the C-type hollow-core optical fiber, when the hollow-core optical fiber preform is drawn into an optical fiber, depending on the type of matrix material, the heating source can optionally be a graphite heating element, a resistance wire or a laser.
[0016] In the C-type hollow-core optical fiber preparation method, when drawing the C-type hollow-core optical fiber, the drawing parameters adjusted are temperature and / or speed and / or air pressure, wherein the core area is connected to the atmosphere, and the pores of the microstructure cladding need to be inflated to prevent it from collapsing, and preferably, the drawing speed is not less than 5m / min.
[0017] The method for preparing a C-type hollow-core optical fiber also includes preparing a hollow-core optical fiber preform rod before the laser ablation operation, which may include the following contents and combinations thereof:
[0018] (a) drawing the thick tube into a capillary tube with a desired outer diameter or a hollow core optical fiber preform containing only a sleeve cladding;
[0019] (b) drawing the rod-shaped object into a small thin rod with a desired outer diameter;
[0020] (c) forming a plurality of capillaries into a unit body and bonding them by heating;
[0021] (d) inserting the capillary tube, small thin rod or unit body into a sleeve with a large diameter and stacking them to form a stacked body;
[0022] (e) heating and stretching the stacked body described in (d) as a whole to obtain a hollow core optical fiber preform having a microstructure cladding.
[0023] In the method for preparing the C-type hollow core optical fiber, the stacking refers to fixing the position of the capillary tube, the small thin rod or the unit body in the sleeve by using local heating or an auxiliary tube.
[0024] In the method for preparing a C-type hollow-core optical fiber, the outer diameter of the hollow-core optical fiber preform is between 1 and 10 mm, and preferably, the thickness of the sleeve cladding is not higher than 3 mm.
[0025] A C-type hollow-core optical fiber prepared by the above preparation method is characterized in that it includes: an optical fiber core and an optical fiber casing cladding; the optical fiber casing cladding is unclosed, and there is a side channel on the optical fiber casing cladding that extends in the length direction by meters and penetrates the outside and the optical fiber core.
[0026] The C-type hollow-core optical fiber is characterized in that it may also include an optical fiber microstructure cladding, which is unclosed and attached to the inner surface of the optical fiber sleeve cladding, and together with the optical fiber sleeve cladding, defines an optical fiber core with an effective radius, such as a node-free antiresonant hollow-core optical fiber.
[0027] In the C-type hollow-core optical fiber, the optical fiber core is filled with a non-solid medium, such as gas or liquid. The matrix material of the C-type hollow-core optical fiber can be glass or plastic, preferably silica glass. The transmission band is in the ultraviolet to terahertz band range, preferably the gas molecule fingerprint zone in the infrared band.
[0028] Preferably, the side channel of the C-type hollow-core optical fiber can be exposed by stripping off the optical fiber coating at any position, so as to facilitate the entry of external environmental gas molecules into the fiber core.
[0029] The C-type hollow core optical fiber is used as a microcavity for interaction between light and matter, and is mainly used in the field of gas sensing, and can also be used in the field of microfluid sensing or gas / liquid lasers.
[0030] Compared with the prior art, the present invention introduces laser to perform side ablation processing at the hollow core optical fiber preform stage, which brings the following beneficial effects:
[0031] 1. Compared with micro-machining of micron-scale optical fibers, the processing positioning at the preform stage is more convenient and easier, and there is no need to use a microscopic imaging system for observation and prediction. It also avoids the risk of optical fiber structure damage or even disconnection due to inaccurate positioning during optical fiber micro-machining;
[0032] 2. Compared with the conventional side corrosion, polishing or cutting treatment of the preform rod, the laser processing accuracy is higher and the controllability is better. It can form a side slit of appropriate width on the hollow-core optical fiber preform rod. Further combined with the adjustment of the drawing parameters, it is easy to achieve the shape preservation of the side slit channel and prepare a continuous C-type hollow-core optical fiber structure with a length of meters. Therefore, there is no need to use a secondary casing to restrict the C-type structure, and at the same time simplifies the difficulty of preform assembly.
[0033] 3. The present invention does not introduce a secondary casing, but ensures the mechanical properties of the optical fiber through the casing cladding and coating layer of the hollow-core optical fiber preform rod itself. Therefore, there is no need for complex optical fiber post-processing. The side channel can be exposed by stripping the coating to obtain a C-type hollow-core optical fiber structure, and the coating can be stripped at any position. The operation is simple and convenient, the practicability is strong, and it is easy to promote and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 : Schematic diagram of the laser processed hollow core optical fiber preform of the present invention;
[0036] Figure 2 : Schematic diagram of drawing a C-type hollow core optical fiber of the present invention;
[0037] Figure 3 : Schematic diagram of the cross section of a C-type hollow-core optical fiber containing a microstructure cladding in the present invention;
[0038] Figure 4 : A schematic diagram of the structure of a C-type hollow-core optical fiber obtained by the preparation method of the present invention provided in Example 1 of the present invention;
[0039] Figure 5 : A schematic diagram of the structure of a C-type hollow-core optical fiber obtained by the preparation method of the present invention provided in Example 2 of the present invention;
[0040] Figure 6 : Schematic diagram of the structure of a C-type hollow-core optical fiber obtained by the preparation method of the present invention provided in Example 3 of the present invention.
[0041] 1——hollow-core optical fiber preform; 1-1——preform core region; 1-2——preform sleeve cladding region; 1-4——preform side slit; 2——C-type hollow-core optical fiber; 2-1——optical fiber core region; 2-2——optical fiber sleeve cladding region; 2-3——optical fiber microstructure cladding region; 2-4——optical fiber side channel; 3——laser; 4——lens; 5——transverse and longitudinal reciprocating relative displacement; 6——introduction of inert gas; 7——extraction device; 8——heat source for heating. DETAILED DESCRIPTION
[0042] The following is a detailed description of an embodiment of the present invention. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiment.
[0043] Example 1: Please refer to Figure 4 , Figure 4A schematic diagram of the structure of a C-type hollow-core optical fiber obtained by the preparation method of the present invention provided in this embodiment: the optical fiber core region 2-1 is an air core, the optical fiber sleeve cladding region 2-2 is composed of quartz glass, the optical fiber microstructure cladding region 2-3 is composed of 7 discrete thin-walled quartz glass capillaries, and the optical fiber side channel 2-4 is in the gap between the thin-walled quartz glass capillaries.
[0044] 1) Obtain a quartz glass thin tube, heat and draw it to obtain a plurality of glass thin tubes with an outer diameter of 2 mm;
[0045] 2) inserting 7 glass tubes into a quartz glass sleeve with an outer diameter of 20 mm and a wall thickness of 4 mm for stacking, and using several short tubes at both ends for structural auxiliary support to form a stack;
[0046] 3) The stack is heated and stretched as a whole to obtain a hollow-core optical fiber preform 1 with an outer diameter of 6 mm and a wall thickness of the sleeve cladding 1-2 of 1.2 mm;
[0047] 4) One end of the hollow-core optical fiber preform 1 is fixed on an electric translation stage, and a carbon dioxide continuous laser 3 with an emission wavelength of 10.6 μm and an average power of 40 W is converged on the side of the hollow-core optical fiber preform 1 through a lens 4. The converged light spot has a diameter of about 0.5 mm, and the inner wall of the sleeve cladding 1-2 corresponding to the convergence point is connected to the core area 1-1 through the gap of 7 thin-walled glass capillaries.
[0048] 5) Control the electric translation stage to move the hollow-core optical fiber preform 1 back and forth in the length direction, and control the galvanometer to move the laser 3 back and forth in the lateral direction. By adjusting the moving length, speed and number of back and forth movements, the laser 3 ablates the quartz glass on the side of the hollow-core optical fiber preform 1 and obtains a slit with a length of 25 cm and a width of about 400 μm.
[0049] 6) The hollow-core optical fiber preform 1 after the laser 3 ablation operation is placed in a graphite furnace 8 for drawing, and at the same time, the 7 thin-walled capillaries in the optical fiber microstructure cladding area 2-3 are inflated to prevent their collapse. By adjusting the drawing temperature and speed, a C-type hollow-core optical fiber structure with a node-free anti-resonant microstructure cladding is obtained and maintained continuously at a meter-level length, wherein the optical fiber outer diameter is 300 μm and the side channel 2-4 width is about 20 μm.
[0050] Example 2: Please refer to Figure 5 , Figure 5 The schematic diagram of the structure of a C-type hollow-core optical fiber obtained by the preparation method of the present invention is provided in this embodiment: the optical fiber core region 2-1 is an air core, the optical fiber sleeve cladding region 2-2 is composed of quartz glass, the optical fiber microstructure cladding region 2-3 is composed of 5 discrete nested unit bodies, and the optical fiber side channel 2-4 is in the gap between the nested unit bodies.
[0051] 1) obtaining two quartz glass thin tubes with different outer diameters for nesting, and then heating and drawing them to obtain a plurality of nested unit bodies with an outer diameter of 6 mm;
[0052] 2) inserting five nested unit bodies into a quartz glass sleeve with an outer diameter of 30 mm and a wall thickness of 6 mm for stacking, and using several short tubes at both ends for structural auxiliary support to form a stacked body;
[0053] 3) The stack is heated and stretched as a whole to obtain a hollow-core optical fiber preform 1 with an outer diameter of 5 mm and a wall thickness of the sleeve cladding 1-2 of 1 mm;
[0054] 4) One end of the hollow-core optical fiber preform 1 is fixed on an electric translation stage, and a carbon dioxide continuous laser 3 with an emission wavelength of 10.6 μm and an average power of 30 W is converged on the side of the hollow-core optical fiber preform 1 through a lens 4. The converged light spot has a diameter of about 0.5 mm, and the inner wall of the sleeve cladding 1-2 corresponding to the convergence point is connected to the core area 1-1 through the gap of the five nested unit bodies.
[0055] 5) Control the electric translation stage to move the hollow-core optical fiber preform 1 back and forth in the length direction, and control the galvanometer to move the laser 3 back and forth in the lateral direction. By adjusting the moving length, speed and number of back and forth movements, the laser 3 ablates the quartz glass on the side of the hollow-core optical fiber preform 1 and obtains a slit with a length of 30 cm and a width of about 300 μm.
[0056] 6) The hollow-core optical fiber preform rod 1 after the laser 3 ablation operation is placed in a graphite furnace 8 for drawing, and at the same time, the five nested unit body pores in the optical fiber microstructure cladding area 2-3 are inflated to prevent their collapse. By adjusting the drawing temperature and speed, a C-type hollow-core optical fiber structure with a node-free nested anti-resonant microstructure cladding is obtained and maintained continuously at a meter-level length, wherein the optical fiber outer diameter is 200 μm and the side channel 2-4 width is about 12 μm.
[0057] Example 3: Please refer to Figure 6 , Figure 6 The schematic diagram of the structure of a C-type hollow-core optical fiber obtained by the preparation method of the present invention is provided in this embodiment: the optical fiber core region 2-1 is an air core, the optical fiber sleeve cladding region 2-2 is composed of quartz glass, the optical fiber microstructure cladding region 2-3 is composed of 6 discrete three-hole unit bodies, and the optical fiber side channel 2-4 is in the gap between the three-hole unit bodies.
[0058] 1) Obtain a quartz glass thin tube, heat and draw it to obtain a plurality of glass thin tubes with an outer diameter of 1 mm;
[0059] 2) Every three glass tubes are welded by femtosecond laser to form a three-hole unit body, and the six unit bodies are inserted into a quartz glass sleeve with an outer diameter of 28 mm and a wall thickness of 5.6 mm for stacking, and a plurality of short tubes are used at both ends for structural auxiliary support to form a stacked body;
[0060] 3) The stack is heated and stretched as a whole to obtain a hollow-core optical fiber preform 1 with an outer diameter of 5 mm and a wall thickness of the sleeve cladding 1-2 of 1 mm;
[0061] 4) One end of the hollow-core optical fiber preform 1 is fixed on an electric translation stage, and a carbon dioxide continuous laser 3 with an emission wavelength of 10.6 μm and an average power of 30 W is converged on the side of the hollow-core optical fiber preform 1 through a lens 4. The converged light spot has a diameter of about 0.5 mm, and the inner wall of the sleeve cladding 1-2 corresponding to the convergence point is connected to the core area 1-1 through the gaps of the six three-hole unit bodies.
[0062] 5) Control the electric translation stage to move the hollow-core optical fiber preform 1 back and forth in the length direction, and control the galvanometer to move the laser 3 back and forth in the lateral direction. By adjusting the moving length, speed and number of back and forth movements, the laser 3 ablates the quartz glass on the side of the hollow-core optical fiber preform 1 and obtains a slit with a length of 30 cm and a width of about 350 μm.
[0063] 6) The hollow-core optical fiber preform rod 1 after the laser 3 ablation operation is placed in a graphite furnace 8 for drawing, and at the same time, the six three-hole unit body pores in the optical fiber microstructure cladding area 2-3 are inflated to prevent their collapse. By adjusting the drawing temperature and speed, a C-type hollow-core optical fiber structure with a nodeless double-loop anti-resonant microstructure cladding is obtained and maintained continuously at a meter-level length, wherein the optical fiber outer diameter is 260μm and the side channel 2-4 width is about 18μm.
[0064] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as reference individually. In addition, it should be understood that after reading the above teachings of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.
Claims
1. A method for preparing a C-type hollow core optical fiber, characterized in that: include: The sleeve cladding (1-2) of the hollow-core optical fiber preform is eroded sideways by using a laser (3), thereby forming one or more continuous slits (1-4) in the longitudinal direction thereof, wherein the inner wall of the sleeve cladding (1-2) corresponding to the laser processed part is connected with the fiber core (1-1), and the connection means that the path from the inner wall to the fiber core (1-1) is naturally unobstructed; A hollow-core optical fiber preform rod (1) with a slit is directly heated and drawn without introducing a secondary sleeve and destroying the microstructure cladding. The structural forming of a C-type hollow-core optical fiber (2) is achieved by adjusting the drawing parameters and is continuously maintained at a meter-level length, that is, a side channel (2-4) that is connected between the fiber core (2-1) and the external environment and can exchange gas is formed, and the side channel continuously extends in the longitudinal direction at a meter-level length.
2. The method for preparing a C-type hollow core optical fiber according to claim 1, characterized in that: The laser (3) is a continuous or pulsed laser, and the wavelength is selected so as to be able to ablate the corresponding optical fiber matrix material.
3. The method for preparing a C-type hollow core optical fiber according to claim 1 or 2, characterized in that: The laser (3) is focused on the side surface of the sleeve cladding (1-2) of the hollow core optical fiber preform or its vicinity through a lens (4), and undergoes a reciprocating relative displacement (5) with the sleeve cladding (1-2) in the longitudinal or transverse direction, thereby forming one or more continuous slits (1-4) in the longitudinal direction.
4. The method for preparing a C-type hollow core optical fiber according to claim 3, characterized in that: By adjusting the focus spot size, average power, scanning length, width, speed and number of repetitions of the laser (3), the heat energy accumulated on the side surface of the hollow-core optical fiber preform (1) is higher than the ablation threshold of the matrix material, thereby achieving width control of the slits (1-4).
5. The method for preparing a C-type hollow core optical fiber according to claim 4, characterized in that: The width of the slits (1-4) is within 1 mm, and each slit extends for more than 10 cm along the longitudinal direction of the hollow core optical fiber preform (1).
6. The method for preparing a C-type hollow core optical fiber according to claim 1, characterized in that: When the laser (3) performs side ablation, an inert gas (6) can be introduced into the hollow-core optical fiber preform (1) at the same time, and an extraction device (7) is placed near the laser processing location to remove dust generated during the laser ablation process.
7. The method for preparing a C-type hollow core optical fiber according to claim 1, characterized in that: In the heating drawing, the heating source (8) is a graphite heating element, a resistance wire or a laser, and the drawing parameters are temperature and / or speed and / or air pressure.
8. The method for preparing a C-type hollow core optical fiber according to any one of claim 1, characterized in that: Before using laser to perform side ablation on the sleeve cladding of the hollow core optical fiber preform, the hollow core optical fiber preform needs to be prepared, including drawing a thick tube into a capillary tube with a desired outer diameter or a hollow core optical fiber preform containing only the sleeve cladding.
9. The method for preparing a C-type hollow core optical fiber according to claim 8, characterized in that: The preparation of the hollow-core optical fiber preform can also include: drawing the rod-shaped object into a small thin rod with a desired outer diameter; inserting a unit body composed of a capillary, a small thin rod or a plurality of capillaries into a large-diameter sleeve for stacking to form a stack; heating and stretching the stack as a whole to obtain a hollow-core optical fiber preform with a microstructure cladding.
10. The method for preparing a C-type hollow core optical fiber according to claim 9, characterized in that: The stacking refers to fixing the position of the capillary tube or the small thin rod in the sleeve by using local heating or auxiliary tube.
11. A C-type hollow core optical fiber prepared by the preparation method according to any one of claims 1 to 10, characterized in that: include: An optical fiber core (2-1) and an optical fiber tube cladding (2-2); The optical fiber sleeve cladding (2-2) is unsealed, and there is a side channel (2-4) on the optical fiber sleeve cladding extending in the length direction by meters and penetrating the outside world and the optical fiber core (2-1). The C-type hollow-core optical fiber comprises an optical fiber microstructure cladding (2-3), which is naturally unsealed and attached to the inner surface of the optical fiber sleeve cladding (2-2), and defines an optical fiber core (2-1) with an effective radius together with the optical fiber sleeve cladding (2-2), and the core (2-1) is connected to the outside world through the naturally unsealed gap of the microstructure cladding (2-3) and the side channel (2-4).
12. The C-type hollow core optical fiber according to claim 11, characterized in that: The optical fiber core (2-1) is filled with a non-solid medium, the matrix material is glass or plastic, and the transmission band is in the range of ultraviolet to terahertz waveband.
13. The C-type hollow core optical fiber according to claim 11, characterized in that: By stripping off the optical fiber coating at any position of the optical fiber (2), the side channel (2-4) can be exposed, thereby facilitating the entry of external environment gas molecules into the fiber core (2-1).
14. The use of the C-type hollow core optical fiber according to claim 11, characterized in that: As a microcavity for the interaction between light and matter, it is used in the fields of gas sensing, microfluidic sensing or gas / liquid lasers.