Modified lithium-rich manganese-based positive electrode material with stable structure and preparation method thereof, and lithium-ion battery
By introducing Zr(HPO4)2·H2O or Zr(HPO4)2 on the surface of lithium-rich manganese-based cathode materials, a spinel phase and O vacancies are generated, and a phosphate protective layer is formed, which solves the structural instability and surface deterioration of the material. problem, improving energy density and cycle life.
Patent Information
- Application Number
- CN202211620751.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-16
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-12-16
AI Technical Summary
The structural instability of lithium-rich manganese-based cathode materials leads to insufficient energy density and cycle life. Existing doping and surface modification methods are difficult to effectively solve the problems of surface interface degradation and structural damage.
Zr(HPO4)2·H2O or Zr(HPO4)2 is introduced on the surface of lithium-rich manganese-based cathode materials, and spinel phase and O vacancies are generated through high-temperature sintering, and a phosphate inert protective layer is formed to improve the structural stability and stability of the material. Lithium ion diffusion ability.
It significantly improves the first Coulombic efficiency, rate performance and cycle stability of the material, inhibits the escape of lattice oxygen and electrolyte erosion, and extends the cycle life of the material.
Smart Images

Figure CN115692682B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of a lithium ion battery positive electrode material, and in particular to a modified lithium-rich manganese-based positive electrode material with a stable structure, a preparation method thereof, and a lithium ion battery. Background Art
[0002] In today's world, energy innovation represented by lithium-ion batteries has spread to all fields. However, it is difficult for commercial battery systems to meet the increasingly high energy density requirements, such as 350 Wh kg -1 , or even 450 Wh kg -1 Considering that the positive electrode material determines the energy density of the battery, LiCoO2, LiNi x Co y Mn (1-x-y) It is difficult for O2 and LiFePO4 cathodes to achieve such energy density. Lithium-rich manganese-based cathodes have a higher specific capacity (~ 300 mAh g -1 ) and energy density (~1000 Wh kg -1 ) and are widely anticipated. However, the commercial application of lithium-rich manganese-based batteries is hindered by the instability of their structure. Unstable lattice O participates in charge compensation above 4.5 V and becomes oxygen escape. Transition metal ions often occupy lithium sites during the delithiation process, resulting in structural degradation, further leading to capacity decay and voltage decay. In addition, the surface of lithium-rich manganese-based batteries often undergoes parasitic reactions with the electrolyte, resulting in increased impedance and surface damage or even cracks, which deteriorates the lithium ion transfer rate and cycle life. Therefore, a stable structure is the key to the practical application of lithium-rich manganese-based batteries.
[0003] The methods to stabilize the structure are usually doping and surface modification. Li et al. introduced that Al ions occupy the Mn position in the Li@Mn6 superstructure unit, stabilizing the structure of LR and showing a long cycle life ( Advanced Energy Materials, 2021,11, 2101962 Nie et al. reported a Co-free Li-rich layered cathode with significantly improved structural stability by co-doping with F and Cl ( Nano letters, 2021, 21, 8370). However, the bulk doping strategy is difficult to effectively alleviate the degradation of the surface interface, which ultimately leads to structural damage. Surface modification is another useful method to stabilize the structure, including coating, defect engineering, and interface structure design. Among them, the introduction of spinel phase and O vacancies on the surface of lithium-rich manganese-based materials is a common practice, which can effectively improve the rate performance and alleviate the loss of O. Oleic acid, H2SO4, hydrazine hydrate, HCl, and oxalic acid are used to induce spinel phase and O vacancies on the surface of lithium-rich manganese-based materials. However, the immersion of these liquid acids or reducing agents needs to be carefully controlled, otherwise there is a risk of damaging the structure. In addition, although the diffusion of Li ions and the reversibility of O are improved, the surface of the material is still not well protected. Therefore, it is necessary to develop new strategies to obtain more stable structures. Summary of the invention
[0004] To solve the above problems, the present invention provides a modified lithium-rich manganese-based positive electrode material with a stable structure and a preparation method thereof, which can effectively improve the stability of the material structure, solve the problems of poor material rate, poor cycle performance, and low first efficiency; and also provides a lithium-ion battery.
[0005] To achieve the above object, the present invention provides the following specific technical solutions:
[0006] A method for preparing a modified lithium-rich manganese-based positive electrode material with a stable structure comprises uniformly mixing the lithium-rich manganese-based positive electrode material with Zr(HPO4)2·H2O or Zr(HPO4)2 and then sintering the mixture to obtain the material.
[0007] The present invention introduces Zr(HPO4)2·H2O or Zr(HPO4)2 on the surface of the lithium-rich manganese base. During the high-temperature sintering process, the H in Zr(HPO4)2·H2O or Zr(HPO4)2 can undergo a protonation reaction to exchange ions with the Li in the lithium-rich manganese base, and then react at high temperature to generate a surface with a spinel phase and O vacancies, and leave a layer of inert phosphate protective layer. This unique structure can not only improve the initial coulomb efficiency and rate performance of the lithium-rich manganese base, but also inhibit the escape of surface active O, maintain structural stability, and enhance the lithium ion diffusion capacity. At the same time, the inert phosphate protective layer on the surface can also block the erosion of the electrolyte, ensuring that the material maintains stability during a long cycle.
[0008] Preferably, a liquid phase method is used for uniform mixing, and the preparation method comprises:
[0009] S1. Adding lithium-rich manganese-based positive electrode material and Zr(HPO4)2·H2O or Zr(HPO4)2 into water, stirring continuously to obtain a uniformly mixed precursor mixture, and then performing solid-liquid separation and drying to obtain a precursor powder;
[0010] S2. Sintering the obtained precursor powder.
[0011] Preferably, in step S1, the amount of Zr(HPO4)2·H2O or Zr(HPO4)2 added is 0.5-5 mol% of the molar amount of the lithium-rich manganese-based positive electrode material. Too much Zr(HPO4)2·H2O or Zr(HPO4)2 content will lead to a surface inert layer, hindering performance improvement, while too little Zr(HPO4)2·H2O or Zr(HPO4)2 cannot achieve an effective interface modification effect.
[0012] Preferably, in step S1, the solid content of the precursor mixture is 8-12 g / L, and the stirring time is 12-36 h. The stirring temperature can be room temperature, which can reduce energy consumption. Too low or too high solid content will result in poor adsorption between the lithium-rich manganese base and Zr(HPO4)2·H2O or Zr(HPO4)2, and they cannot be evenly mixed. Too long stirring time will prolong the preparation process, while too short stirring time will result in the inability to evenly mix the two.
[0013] Water can be deionized water, high-purity water, distilled water or other water that does not react with the material. There are many ways to achieve solid-liquid separation, such as filtration, centrifugation and other commonly used solid-liquid separation methods.
[0014] Preferably, the sintering temperature is 400-600°C; the sintering atmosphere is air; the sintering time is 3-9 h; and the sintering heating rate is 3-7°C / min. A suitable sintering system can ensure that Zr(HPO4)2·H2O or Zr(HPO4)2 reacts completely with the lithium-rich manganese base to form the required improved interface.
[0015] Preferably, the lithium-rich manganese-based positive electrode material is obtained by grinding and mixing a lithium-rich manganese-based precursor with a lithium source, calcining by a solid phase method, and cooling.
[0016] Preferably, the lithium-rich manganese-based precursor is selected from Mn 0.667 Ni 0.166 Co 0.166 CO3、Mn 0.667 Ni 0.166 Co 0.166 (OH)2; the lithium source is at least one of lithium carbonate, lithium hydroxide and its hydrate, lithium nitrate, lithium acetate and its hydrate.
[0017] Preferably, the lithium-rich manganese-based precursor is mixed with a lithium source in a molar ratio of the total amount of Ni, Co, and Mn to Li of 1:1.5-1.6. An appropriate excess lithium amount is beneficial to make up for the loss of Li during the sintering process, while excessive Li will lead to the formation of residual lithium on the surface, reducing the electrochemical performance.
[0018] Preferably, the solid phase calcination is carried out in an air atmosphere at 700-1000°C for 8-15 h, and the heating rate is 3-7°C / min. An appropriate heating rate is conducive to maintaining the spherical structure of the material, while a suitable sintering temperature and sintering time can ensure sufficient crystallinity without excessive grain growth.
[0019] Preferably, in step S1, the drying temperature is 60-120°C and the drying time is 3-24 hours. If the drying temperature is too low, the water between the components cannot be effectively volatilized, and if it is too high, the energy consumption will increase. If the drying time is too short, the material cannot be dried, thereby deteriorating the subsequent sintering effect. If the drying time is too long, the energy consumption will also increase and the experimental process will be prolonged.
[0020] As a general inventive concept, the present invention provides a modified lithium-rich manganese-based positive electrode material with a stable structure, which is prepared by the aforementioned preparation method.
[0021] As a general inventive concept, the present invention also provides a lithium-ion battery comprising the above-mentioned positive electrode material.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) The preparation method of the present invention can form a spinel phase and O vacancies on the surface of a lithium-rich manganese-based lithium-ion battery positive electrode material, and can also form an inert phosphate protective layer on the surface of the positive electrode material; the spinel phase and O vacancies can improve the lithium ion diffusion capacity of the material and enhance the rate performance; the spinel phase and O vacancies can also inhibit the escape of lattice O, improve the first coulomb efficiency, and inhibit voltage decay and capacity decay; the inert phosphate protective layer remaining on the surface can also prevent the erosion of the electrolyte, so that it has good structural stability during long cycles.
[0024] (2) The preparation process is simple, highly reproducible, and easy to promote on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1The figures are comparison diagrams of the electrochemical performance of batteries assembled with the modified lithium-rich manganese-based positive electrode material obtained in Example 1 and the unmodified lithium-rich manganese-based positive electrode material of the comparative example, wherein (a) is a comparison diagram of the first cycle charge and discharge curves, (b) is a dQ / dV ratio diagram corresponding to the first cycle charge and discharge curves, (c) is a rate performance comparison diagram, (d) is a discharge cycle comparison diagram, (e) is a discharge curve diagram of the material assembled from the material of Example 1, (f) is a discharge curve diagram of the material assembled from the comparative example, (g) is an energy density comparison diagram, (h) is the dQ / dV curve corresponding to Figure e, and (i) is the dQ / dV curve corresponding to Figure f.
[0027] Figure 2 The SEM image (a) and element distribution diagrams (b)-(g) of the modified lithium-rich manganese-based positive electrode material obtained in Example 1.
[0028] Figure 3 The differential electrochemical mass spectra of the modified lithium-rich manganese-based positive electrode material (b) obtained in Example 1 and the unmodified lithium-rich manganese-based positive electrode material (a) of the comparative example are shown.
[0029] Figure 4 The in-situ electrochemical XRD patterns of the modified lithium-rich manganese-based positive electrode material (b) obtained in Example 1 and the unmodified lithium-rich manganese-based positive electrode material (a) of the comparative example.
[0030] Figure 5 The electron paramagnetic resonance images of the modified lithium-rich manganese-based positive electrode material obtained in Example 1 and the unmodified lithium-rich manganese-based positive electrode material in the comparative example are shown. DETAILED DESCRIPTION
[0031] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.
[0032] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0034] Example 1: 0.5 mol% modification amount (labeled as S-LR)
[0035] (1) Preparation of lithium-rich manganese-based materials:
[0036] Weigh 0.1 mol Mn 0.667 Ni 0.166 Co0.166 CO3 and 0.1575 mol of LiOH·H2O were ground in a mortar for 2 hours until the materials were completely mixed. Then the mixed materials were placed in a crucible and sintered at 900℃ for 10 hours in a muffle furnace with air as the atmosphere at a heating rate of 5℃ / min. After naturally cooling to room temperature, the lithium-rich manganese-based material Li 1.2 (Mn 0.54 Ni 0.13 Co 0.13 )O2.
[0037] (2) Preparation of precursor solution:
[0038] Weigh 0.5 g of lithium-rich manganese-based material and 0.0089 g of Zr(HPO4)2·H2O into 50 ml of pure water and stir at room temperature of 25°C for 24 h to obtain a uniformly mixed precursor solution;
[0039] (3) Preparation of precursor powder:
[0040] After filtering the precursor mixed solution, the filter cake was dried in an oven at 120 °C for 6 h until completely dry;
[0041] (4) Preparation of final material:
[0042] The precursor powder was placed in a muffle furnace and sintered at 500°C for 4 h at a heating rate of 5°C / min to obtain a Zr(HPO4)2·H2O-modified lithium-rich manganese-based positive electrode material with a modification amount of 0.5 mol%.
[0043] Comparative example: lithium-rich manganese-based (marked as LR)
[0044] Weigh 0.1 mol Mn 0.667 Ni 0.166 Co 0.166 CO3 and 0.1575 mol of LiOH·H2O were ground in a mortar for 2 hours until the materials were completely mixed. Then the mixed materials were placed in a crucible and sintered at 900℃ for 10 hours in a muffle furnace with air as the atmosphere at a heating rate of 5℃ / min. After naturally cooling to room temperature, the lithium-rich manganese-based material Li 1.2 (Mn 0.54 Ni 0.13 Co 0.13 )O2.
[0045] Battery assembly: Weigh 0.08 g of the modified lithium-rich manganese-based positive electrode material obtained in Example 1 of the present invention and the comparative example, add 0.01 g of acetylene black as a conductive agent and 0.01 g of polyvinylidene fluoride as a binder, and N-methylpyrrolidone as a dispersant, mix well and apply the mixture on an aluminum foil to make a positive electrode sheet, and assemble a CR2032 button battery in a vacuum glove box using a metal lithium sheet as a negative electrode, a composite film of PE and PP as a separator, and 1 mol / L LiPF6 / DMC:EC (volume ratio 1:1) as an electrolyte.
[0046] The battery assembled with the positive electrode materials of Example 1 and the comparative example was subjected to charge and discharge tests in the voltage range of 2.0-4.8 V. The results are as follows: Figure 1 As shown. Among them, (a) is a comparison diagram of the first cycle charge and discharge curves, (b) is a dQ / dV ratio diagram corresponding to the first cycle charge and discharge curves, (c) is a rate performance comparison diagram, (d) is a discharge cycle comparison diagram, (e) is a discharge curve diagram of the material assembly of Example 1, (f) is a discharge curve diagram of the material assembly of the comparative example, (g) is an energy density comparison diagram, (h) is the dQ / dV curve corresponding to Figure e, and (i) is the dQ / dV curve corresponding to Figure f.
[0047] from Figure 1 As can be seen from (a), (c), (d), and (g), the first cycle charge and discharge efficiency, rate performance, cycle performance, and energy density of S-LR are better than those of LR, indicating that the electrochemical performance of the modified cathode material has been significantly improved. Among them, at a rate of 0.1 C, the discharge capacity of S-LR is 279.1 mAh g -1 , the first efficiency is 88.4%; and the discharge capacity of LR is 284.1 mAhg -1 The first efficiency is 83.12%. The gram capacity of S-LR is slightly lower because it is coated with inert materials, but its first efficiency is greatly improved. The S-LR discharges at 0.2, 1, 5 and 10 C are 266.5, 243.6, 188.2 and 134.2 mAh g -1 ; The capacity retention rate after 200 cycles at 1 C rate is 84.25%; The LR discharge capacities at 0.2, 1, 5, and 10 C are 266.1, 232.9, 132.7, and 74.9 mAh g, respectively. -1 ; The capacity retention rate is 68.51% after 200 cycles at 1 C rate.
[0048] from Figure 1 (b) It can be seen that S-LR has a small peak at 2.75 V, indicating the presence of spinel phase in the modified cathode material. Figure 1 From the comparison of (e) and (f), it can be seen that the voltage decay of the material in Example 1 during the cycle is significantly slower than that in Comparative Example 1, which shows that the structure of the modified material is more stable. Figure 1 From the comparison between (h) and (i), it can be seen that the modified positive electrode material has fewer harmful phase changes during the cycle, and thus the structure is more stable.
[0049] The SEM image and element distribution diagram of the material prepared in Example 1 are as follows: Figure 2 As shown in Figures 2(a) and 2(b)-(g), it can be seen that the elements of the obtained material are evenly distributed.
[0050] The differential electrochemical mass spectra of the modified lithium-rich manganese-based positive electrode material obtained in Example 1 and the unmodified lithium-rich manganese-based positive electrode material in Comparative Example 1 are shown as follows: Figure 3 (b) and (a). Figure 3 It can be seen that S-LR produces less gas, indicating that less lattice O escapes, indicating that its structure is more stable.
[0051] The in-situ electrochemical XRD patterns of the modified lithium-rich manganese-based positive electrode material obtained in Example 1 and the unmodified lithium-rich manganese-based positive electrode material in Comparative Example 1 are shown as follows: Figure 4 (b) and (a). Figure 4 It can be seen that the (003) peak of S-LR has a lower degree of shift and is closer to the initial value after cycling, indicating that the structure of the modified positive electrode material is more stable.
[0052] Figure 5 The electron paramagnetic resonance images of the modified lithium-rich manganese-based positive electrode material obtained in Example 1 and the unmodified lithium-rich manganese-based positive electrode material in Comparative Example 1 prove that S-LR has more O vacancies than LR, indicating that the modification introduces O vacancies.
[0053] In summary, the modified cathode material introduced O vacancies and spinel phases, the electrochemical performance was significantly improved, and the structural stability was greatly enhanced.
[0054] Example 2: 1 mol% modification amount
[0055] (1) Preparation of lithium-rich manganese-based materials:
[0056] Weigh 0.1 mol Mn 0.667 Ni 0.166 Co 0.166 CO3 and 0.1575 mol of LiOH·H2O were ground in a mortar for 2 hours until the materials were completely mixed. Then the mixed materials were placed in a crucible and sintered at 900℃ for 10 hours in a muffle furnace with air as the atmosphere at a heating rate of 5℃ / min. After naturally cooling to room temperature, the lithium-rich manganese-based material Li 1.2 (Mn 0.54 Ni 0.13 Co 0.13 )O2.
[0057] (2) Preparation of precursor solution:
[0058] Weigh 0.5 g of lithium-rich manganese-based material and 0.0177 g of Zr(HPO4)2·H2O into 50 ml of pure water and stir at room temperature of 25°C for 24 h to obtain a uniformly mixed precursor solution;
[0059] (3) Preparation of precursor powder:
[0060] After filtering the precursor mixed solution, the filter cake was dried in an oven at 120 °C for 6 h until completely dry;
[0061] (4) Preparation of final material:
[0062] The precursor powder was placed in a muffle furnace and sintered at 500°C for 4 h at a heating rate of 5°C / min to obtain a Zr(HPO4)2·H2O-modified lithium-rich manganese-based positive electrode material with a modification amount of 1 mol%.
[0063] Battery assembly: Weigh 0.08 g of the modified lithium-rich manganese-based positive electrode material obtained in this example, add 0.01 g of acetylene black as a conductive agent and 0.01 g of polyvinylidene fluoride as a binder, and N-methylpyrrolidone as a dispersant. After mixing evenly, apply it on an aluminum foil to make a positive electrode sheet. In a vacuum glove box, use a metal lithium sheet as a negative electrode, a composite film of PE and PP as a separator, and 1 mol / LLiPF6 / DMC:EC (volume ratio 1:1) as an electrolyte to assemble a CR2032 button battery.
[0064] The assembled battery has a discharge capacity of 265.2, 240.7, 179.3, and 128.6 mAh g at 0.2, 1, 5, and 10 C, respectively, in the voltage range of 2.0–4.8 V. -1 The assembled battery has a capacity retention rate of 83.29% after 200 cycles at 1 C rate in the voltage range of 2.0-4.8 V.
[0065] Example 3: 1.5 mol% modification amount
[0066] (1) Preparation of lithium-rich manganese-based materials:
[0067] Weigh 0.1 mol Mn 0.667 Ni 0.166 Co 0.166 CO3 and 0.1575 mol of LiOH·H2O were ground in a mortar for 2 hours until the materials were completely mixed. Then the mixed materials were placed in a crucible and sintered at 900℃ for 10 hours in a muffle furnace with air as the atmosphere at a heating rate of 5℃ / min. After naturally cooling to room temperature, the lithium-rich manganese-based material Li1.2 (Mn 0.54 Ni 0.13 Co 0.13 )O2.
[0068] (2) Preparation of precursor solution:
[0069] Weigh 0.5 g of lithium-rich manganese-based material and 0.0267 g of Zr(HPO4)2·H2O into 50 ml of pure water and stir at room temperature of 25°C for 24 h to obtain a uniformly mixed precursor solution;
[0070] (3) Preparation of precursor powder:
[0071] After filtering the precursor mixed solution, the filter cake was dried in an oven at 120 °C for 6 h until completely dry;
[0072] (4) Preparation of final material:
[0073] The precursor powder was placed in a muffle furnace and sintered at 500 °C for 4 h at a heating rate of 5 °C / min to obtain a Zr(HPO4)2·H2O-modified lithium-rich manganese-based cathode material with a modification amount of 1.5 mol%.
[0074] Battery assembly: Weigh 0.08 g of the modified lithium-rich manganese-based positive electrode material obtained in this example, add 0.01 g of acetylene black as a conductive agent and 0.01 g of polyvinylidene fluoride as a binder, and N-methylpyrrolidone as a dispersant. After mixing evenly, apply it on an aluminum foil to make a positive electrode sheet. In a vacuum glove box, use a metal lithium sheet as a negative electrode, a composite film of PE and PP as a separator, and 1 mol / LLiPF6 / DMC:EC (volume ratio 1:1) as an electrolyte to assemble a CR2032 button battery.
[0075] The assembled battery has a discharge capacity of 264.3, 239.3, 175.6 and 126.6 mAh g at 0.2, 1, 5 and 10 C, respectively, in the voltage range of 2.0–4.8 V. -1 The assembled battery has a capacity retention rate of 82% after 200 cycles at 1 C rate in the voltage range of 2.0-4.8 V.
[0076] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a modified lithium-rich manganese-based positive electrode material with a stable structure, characterized in that: A lithium-rich manganese-based positive electrode material is mixed with Zr(HPO4)2·H2O or Zr(HPO4)2 and then sintered to obtain the positive electrode; the preparation method comprises: S1. Adding lithium-rich manganese-based positive electrode material and Zr(HPO4)2·H2O or Zr(HPO4)2 into water, stirring continuously to obtain a uniformly mixed precursor mixture, and performing solid-liquid separation and drying to obtain a precursor powder; S2. Sintering the obtained precursor powder to obtain a product; the sintering atmosphere is air.
2. The method for preparing a modified lithium-rich manganese-based positive electrode material with a stable structure according to claim 1, characterized in that: In step S1, the amount of Zr(HPO4)2·H2O or Zr(HPO4)2 added is 0.5-5 mol% of the molar amount of the lithium-rich manganese-based positive electrode material.
3. The method for preparing a modified lithium-rich manganese-based positive electrode material with a stable structure according to claim 1, characterized in that: In step S1, the solid content of the precursor mixture is 8-12 g / L; and the stirring time is 12-36 h.
4. The method for preparing a modified lithium-rich manganese-based positive electrode material with a stable structure according to claim 1, characterized in that: The sintering temperature is 400-600° C. and the sintering time is 3-9 hours.
5. The method for preparing a modified lithium-rich manganese-based positive electrode material with a stable structure according to claim 1, characterized in that: The lithium-rich manganese-based positive electrode material is obtained by grinding and mixing a lithium-rich manganese-based precursor and a lithium source, calcining by a solid phase method, and cooling.
6. The method for preparing a modified lithium-rich manganese-based positive electrode material with a stable structure according to claim 5, characterized in that: The lithium-rich manganese-based precursor is selected from Mn 0.667 Ni 0.166 Co 0.166 CO3、Mn 0.667 Ni 0.166 Co 0.166 (OH)2; the lithium source is at least one of lithium carbonate, lithium hydroxide and its hydrate, lithium nitrate, lithium acetate and its hydrate; the lithium-rich manganese-based precursor and the lithium source are mixed according to the molar ratio of the total amount of Ni, Co, Mn to Li of 1:1.5-1.
6.
7. The method for preparing a modified lithium-rich manganese-based positive electrode material with a stable structure according to claim 5, characterized in that: The solid phase calcination is carried out in an air atmosphere at 700-1000° C. for 8-15 hours.
8. A modified lithium-rich manganese-based positive electrode material with a stable structure, characterized in that: The method is described in any one of claims 1 to 7.
9. A lithium ion battery, characterized in that: Comprising the positive electrode material as claimed in claim 8.