Electrodes, batteries, and electrode preparation methods

By designing an electrode structure with a first wrinkled surface on the lithium secondary battery electrode, the problems of increased internal resistance and sudden drop in cycle performance caused by pole piece deformation are solved, and the battery energy density and cycle life are improved.

CN115706203BActive Publication Date: 2024-10-11BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110943030.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-17
Publication Date
2024-10-11
Estimated Expiration
2041-08-17

AI Technical Summary

Technical Problem

During the charging and discharging process of lithium secondary batteries, the deformation of the pole pieces leads to an increase in internal resistance and a sudden drop in cycle performance, which limits the service life and safety performance of the battery.

Method used

Design an electrode, including a current collector layer and an active component layer. A plurality of first protrusions are formed on the side of the active component layer away from the current collector layer to form a first wrinkled surface. Through surface chemical oxidation process and chemical vapor deposition process , Swelling process or thermal deformation process is used to reduce the stress on the outer layer of the pole piece, increase the contact area between the electrode and the electrolyte, and reduce friction.

Benefits of technology

Effectively alleviate the deformation of the pole piece, improve the energy density and cycle life of the battery, reduce the internal resistance, and extend the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115706203B_ABST
    Figure CN115706203B_ABST
Patent Text Reader

Abstract

The embodiment of the present application provides an electrode, a battery and a method for preparing an electrode, wherein the electrode includes a current collector layer and an active component layer, wherein the active component layer covers at least one surface of the current collector layer. The active component layer has a plurality of first protrusions on the side away from the current collector layer, and the plurality of first protrusions can form a first wrinkled surface of the active component layer. The electrode forms a plurality of first protrusions on the side of the active component layer away from the current collector layer, and the plurality of first protrusions can form a first wrinkled surface of the active component layer. The first wrinkled surface can reduce the stress of the outer layer of the pole piece, and alleviate the deformation of the pole piece and the expansion of the battery caused by the expansion of the electrode material. In addition, the first wrinkled surface can also increase the contact area between the electrode and the electrolyte, reduce the friction between the electrode and other components in the battery, and thereby improve the energy density and cycle life of the electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of material forming, and specifically, the present application relates to an electrode, a battery and a method for preparing the electrode. Background Art

[0002] With the continuous expansion of applications in mobile phones, camcorders, laptop computers and electric vehicles, the research and development of batteries has attracted more and more attention. Among them, the development of secondary batteries that can be charged and discharged has always been the focus of attention.

[0003] A general method for manufacturing a lithium secondary battery includes applying a slurry containing a positive electrode active material and a negative electrode active material to respective current collectors, and then winding or laminating together with a separator as an insulator to manufacture and prepare an electrode assembly, inserting the electrode assembly into a battery case, injecting an electrolyte into the battery case and sealing the battery case, and degassing to remove gases generated during initial formation.

[0004] However, the active materials of the battery will experience large pole piece deformation during the charge and discharge process, and the pole piece will rub against the diaphragm during the deformation process, causing damage to the active material layer on the pole piece, which in turn leads to an increase in the internal resistance of the electrode and a sharp drop in the cycle performance, severely limiting the service life and safety performance of the battery. Summary of the invention

[0005] One purpose of the embodiments of the present application is to provide a new technical solution for an electrode, a battery, and a method for preparing an electrode.

[0006] According to a first aspect of an embodiment of the present application, an electrode is provided, comprising:

[0007] a current collector layer;

[0008] An active component layer is covered on at least one surface of the current collector layer, and a side of the active component layer away from the current collector layer has a plurality of first protrusions to form a first wrinkled surface of the active component layer.

[0009] Optionally, top surfaces of the plurality of first protrusions form a first curved surface.

[0010] Optionally, the first protrusion is formed by a surface chemical oxidation process, a chemical vapor deposition process, a swelling process, a thermal deformation process or a prestress release process.

[0011] Optionally, the active component layer covers a first surface and a second surface of the current collector layer, and a surface density of the active component layer located on the first surface is greater than a surface density of the active component layer located on the second surface.

[0012] Optionally, the first protrusion is a linear protrusion, and a plurality of the first protrusions form the first wrinkled surface having a one-dimensional structure.

[0013] Optionally, the first protrusions are point-shaped protrusions, and a plurality of the first protrusions form the first wrinkled surface having a three-dimensional structure.

[0014] Optionally, the first protrusion is a linear protrusion, and a plurality of the first protrusions form the first wrinkled surface having a two-dimensional structure.

[0015] Optionally, the current collector layer has a plurality of second protrusions to form a second wrinkled surface of the current collector layer.

[0016] Optionally, the first protrusion includes a substrate and lines formed on the surface of the substrate, the substrate has a size of micrometer level, and the lines have a size of micrometer level and / or nanometer level.

[0017] Optionally, the first protrusion includes a substrate and lines formed on the surface of the substrate, the size of the substrate is in the millimeter level, and the size of the lines is in the micrometer level and / or millimeter level.

[0018] According to a second aspect of an embodiment of the present application, a battery is provided, comprising the electrode described in the first aspect.

[0019] According to a third aspect of the embodiments of the present application, a method for preparing the electrode according to the first aspect is provided, comprising:

[0020] The active component layer is arranged on the surface of the current collector layer, wherein the active component layer comprises an active component and a deformation component, and the deformation component comprises an expansion agent or a shrinkage agent;

[0021] When the deformation component includes a swelling agent, the first protrusion is obtained by swelling the swelling agent;

[0022] Alternatively, when the deformation component includes a shrinking agent, the first protrusion is obtained by shrinking the shrinking agent.

[0023] One technical effect of the embodiment of the present application is:

[0024] The embodiment of the present application provides an electrode, which includes a current collector layer and an active component layer. The electrode forms a plurality of first protrusions on the side of the active component layer away from the current collector layer, and the plurality of first protrusions can form a first wrinkled surface of the active component layer, and the first wrinkled surface can reduce the stress of the outer layer of the pole piece, and alleviate the deformation of the pole piece and the expansion of the battery caused by the expansion of the electrode material. In addition, the first wrinkled surface can also increase the contact area between the electrode and the electrolyte, reduce the friction between the electrode and other components in the battery, and thus improve the energy density and cycle life of the electrode.

[0025] Other features and advantages of the present application will become apparent from the following detailed description of exemplary embodiments of the present application with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the application and, together with the description, serve to explain the principles of the application.

[0027] Figure 1 A schematic diagram of a first wrinkled surface of an electrode provided in an embodiment of the present application;

[0028] Figure 2 A top view of an electrode provided in an embodiment of the present application;

[0029] Figure 3 for Figure 2 Cross-section view of the AA surface;

[0030] Figure 4 A schematic SEM image of a first wrinkled surface of another electrode provided in an embodiment of the present application;

[0031] Figure 5 A schematic diagram of the structure of another electrode provided in an embodiment of the present application;

[0032] Figure 6 for Figure 5 The enlarged view of point A in the middle;

[0033] Figure 7 A schematic SEM image of a first wrinkled surface of another electrode provided in an embodiment of the present application;

[0034] Figure 8 A schematic diagram of the structure of another electrode provided in an embodiment of the present application;

[0035] Fig. 9 for Figure 8 The enlarged view of point B in the middle;

[0036] Fig.10A schematic diagram of a first wrinkled surface of another electrode provided in an embodiment of the present application;

[0037] Fig.11 A schematic diagram of the structure of another electrode provided in an embodiment of the present application;

[0038] Fig.12 for Fig.11 Enlarged view of point C in the middle;

[0039] Fig.13 A top view of an electrode provided in an embodiment of the present application;

[0040] Fig.14 for Fig.13 Cross-section of the middle BB surface;

[0041] Fig.15 A schematic diagram of the structure of a battery provided in an embodiment of the present application.

[0042] Among them: 1-current collector layer; 11-second protrusion; 2-active component layer; 21-first protrusion. DETAILED DESCRIPTION

[0043] Various exemplary embodiments of the present application will now be described in detail with reference to the accompanying drawings. It should be noted that unless otherwise specifically stated, the relative arrangement of components and steps, numerical expressions and numerical values ​​set forth in these embodiments do not limit the scope of the present application.

[0044] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the present application, its application, or uses.

[0045] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered part of the specification.

[0046] In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limiting. Therefore, other examples of the exemplary embodiments may have different values.

[0047] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.

[0048] Reference Figures 1 to 14 , an embodiment of the present application provides an electrode, the electrode comprising:

[0049] A current collector layer 1 and an active component layer 2 , wherein the active component layer 2 covers at least one surface of the current collector layer 1 .

[0050] The active component layer 2 has a plurality of first protrusions 21 on one side away from the current collector layer 1 . The first protrusions 21 may be dot-shaped protrusions or strip-shaped protrusions. The plurality of first protrusions 21 may form a first wrinkled surface of the active component layer 2 .

[0051] Specifically, the first wrinkled surface of the active component layer 2 can be formed only after the wrinkling treatment of the active component layer 2, and the current collector layer 1 can remain straight at this time; or, the first wrinkled surface of the active component layer 2 can also be formed by the combined effect of the wrinkles of the current collector layer 1 and the wrinkles of the active component layer 2.

[0052] Specifically, the first wrinkled surface of the active component layer 2 can regulate the physical and chemical properties of the electrode due to its bionic wrinkled morphology formed by utilizing the instability of the pole piece surface. For example, when the electrode is used in a battery, the first wrinkled surface of the active component layer 2 can improve the distribution of electrolytes and electrodes in the battery. The first wrinkled surface can reduce the outer layer stress of the pole piece, release the self-stress of the electrode, alleviate the deformation of the pole piece and the expansion of the battery caused by the expansion of the electrode material, and help to suppress the overall deformation of the electrode.

[0053] In addition, when the electrode is used in a battery, the first wrinkled surface of the active component layer 2 can increase the contact area between the electrode and the electrolyte and the ion transmission path in the electrode, thereby improving the ion conduction efficiency between the electrode and the electrolyte in the battery, reducing the polarization of the electrode, thereby increasing the cycle life of the electrode, and reducing the internal resistance of the electrode.

[0054] Moreover, the first wrinkled surface of the active component layer 2 can reduce the friction between the electrode and other components in the battery. For example, when the particle size of the material of the active component layer 2 is reduced to the micrometer or nanometer level, the surface area to volume ratio of the active component layer 2 is relatively high, which can achieve anti-adhesion and low friction, thereby improving the deformation, energy density and cycle life of the battery.

[0055] The electrode provided in the embodiment of the present application forms a plurality of first protrusions 21 on the side of the active component layer 2 away from the current collector layer 1. The plurality of first protrusions 21 can form a first wrinkled surface of the active component layer 2. The first wrinkled surface can reduce the stress of the outer layer of the pole piece, and alleviate the deformation of the pole piece and the expansion of the battery caused by the expansion of the electrode material. In addition, the first wrinkled surface can also increase the contact area between the electrode and the electrolyte and the transmission path of ions in the electrode, reduce the friction between the electrode and other components in the battery, and thus improve the energy density and cycle life of the electrode.

[0056] Alternatively, see Figures 1 to 3 as well as Fig.13 and Fig.14 The top surfaces of the plurality of first protrusions 21 form a first plane, and the first plane is parallel to the reference plane of the current collector layer 1 .

[0057] Specifically, the current collector layer 1 can maintain a planar shape, such as Fig.14 The current collector layer 1 may also form a protrusion along its thickness direction together with the active component layer 2, but the overall planar shape is maintained, such as Figure 3 When the top surfaces of the plurality of first protrusions 21 form a first plane, the thickness of the plurality of first protrusions 21 can be ensured to be consistent, and the planar structure of the current collector layer 1 can increase the density of the arrangement of the electrodes in the battery, thereby increasing the energy density of the electrodes.

[0058] Optionally, the first protrusion 21 is formed by a molding process, a printing process, a spraying process, a laser sputtering process or a mechanical wrapping process.

[0059] Specifically, since the top surfaces of the plurality of first protrusions 21 form a first plane, that is, the structural dimensions of the plurality of first protrusions 21 are the same or close, the first protrusions 21 can be formed by precise molding. For example, by molding the pole piece with a mold having the dimensions of the plurality of first protrusions 21, the plurality of first protrusions 21 can be formed at one time; or by removing the material of the active component layer 2 between adjacent first protrusions 21 by laser sputtering, the plurality of first protrusions 21 can also be formed quickly.

[0060] Alternatively, see Figures 4 to 12 , the top surfaces of the plurality of first protrusions 21 form a first curved surface.

[0061] Specifically, when the first wrinkled surface of the active component layer 2 is formed, the structural dimensions of the plurality of first protrusions 21 may be different. For example, a large number of first protrusions 21 with larger sizes may be formed at locations where the stress of the pole piece is more concentrated, and a small number of first protrusions 21 with smaller sizes may be formed at locations where the stress of the pole piece is less, so as to maximize the release of the internal stress of the pole piece. Moreover, after the top surfaces of the plurality of first protrusions 21 form the first curved surface, the contact area between the electrode and the electrolyte and the transmission path of ions in the electrode may be increased, thereby improving the ion conduction efficiency between the electrode and the electrolyte in the battery, reducing the polarization of the electrode, and thereby increasing the cycle life of the electrode.

[0062] Optionally, the first protrusion 21 is formed by a surface chemical oxidation process, a chemical vapor deposition process, a swelling process, a thermal deformation process or a prestress release process.

[0063] Specifically, when the first wrinkled surface of the active component layer 2 is formed, compressive stress can be generated in the active component layer 2 through the above-mentioned molding process. When the compressive stress in the active component layer 2 exceeds a critical value, the formation of the first wrinkled surface will be triggered. The wrinkling of the first wrinkled surface is the result of the electrode system seeking to minimize energy, so that the electrode structure achieves a dual balance of stress and energy. Obviously, the electrode with the first wrinkled surface can achieve the function of dynamic self-regulation. When the electrode is deformed, the wrinkle pattern formed on the first wrinkled surface can play a role of "energy storage", thereby reducing the deformation of the electrode piece. For the homogeneous soft active component layer 2 constrained by the rigid current collector layer 1, compressive stress can be induced by constraining expansion or volume growth, thereby triggering the surface instability of the soft active component layer 2, and then forming self-creases.

[0064] In addition, for an electrode comprising a single-layer soft system, for example, the current collector layer 1 and the active component layer 2 are both soft materials, due to the high sensitivity of internal stress to surface soft defects, the first wrinkled surface is generally arranged according to the surface defects of the active component layer 2. For an electrode comprising a single-layer hard system, for example, the current collector layer 1 and the active component layer 2 are both hard materials, due to the high sensitivity of internal stress to surface and internal defects, the first wrinkled surface is generally arranged according to the defect distribution of the active component layer 2.

[0065] Optionally, the active component layer 2 covers the first surface and the second surface of the current collector layer 1, and the surface density of the active component layer 2 located on the first surface is greater than the surface density of the active component layer 2 located on the second surface.

[0066] Specifically, the first surface and the second surface of the current collector layer 1 are two surfaces of the current collector layer 1 that are far away from each other. When the surface density of the active component layer 2 located on the first surface is greater than the surface density of the active component layer 2 located on the second surface, bending stress will be generated inside the current collector layer 1, causing the current collector layer 1 to tend to bend. The bending of the current collector layer 1 cooperates with the first wrinkled surface of the active component layer 2 to obtain a curved electrode, thereby ensuring the structural stability of the electrode.

[0067] Alternatively, see Figures 4 to 6 The first protrusion 21 is a linear protrusion, and a plurality of the first protrusions 21 form the first wrinkled surface with a one-dimensional structure; for example, a plurality of the first protrusions 21 form imitation litchi leaf wrinkles, and the imitation litchi leaf wrinkles can be formed by a swelling process.

[0068] Specifically, the lychee leaf-like wrinkle structure is a curved microscale wrinkle. In the surface wrinkles represented by lychee leaves, the one-dimensional lychee leaf-like wrinkles formed by linear protrusions can utilize the surface micro-roughness size effect of the linear protrusions to form tiny wrinkles, effectively reducing the adhesion and friction between the interface of the electrode and other components. For example, when the electrode is applied to a battery, in the presence of a liquid electrolyte, when the electrode and other solid interfaces are close to or in contact with each other, the cracks between the surfaces of the adjacent first protrusions 21 form a liquid bridge, and other solid interfaces are in contact with the peaks of the lychee leaf-like wrinkles formed by the first protrusions 21. Due to the small contact area, the gap between the electrode and other solid interfaces is large, and the surface of the lychee leaf-like wrinkles quickly forms a liquid bridge through air condensation. Since other solid interfaces are in contact with multiple peaks on the surface of the lychee leaf-like wrinkles, multiple capillary bridges may be formed, so that the lychee leaf-like wrinkle structure can also maintain low-friction desorption characteristics in liquid electrolytes.

[0069] In a specific embodiment, the active component layer 2 may include graphite and styrene-butadiene rubber, and the solvent of the swelling process is acetone matched with the styrene-butadiene rubber. When the active component layer 2 is formed on one side or both sides of the current collector layer 1, acetone may be sprayed onto the surface of the active component layer 2, and the styrene-butadiene rubber expands and deforms under the swelling action of acetone, and then the first wrinkled surface of the active component layer 2 may be formed by baking, that is, an electrode having the lychee leaf-like wrinkles may be obtained.

[0070] Alternatively, see Figures 10 to 12 The first protrusions 21 are point-shaped protrusions, and a plurality of the first protrusions 21 form the first wrinkled surface with a three-dimensional structure; for example, a plurality of the first protrusions 21 form pseudo-compound eye wrinkles, and the pseudo-compound eye wrinkles are formed by a swelling process.

[0071] Specifically, the compound eye-like wrinkle structure is a curved multi-scale wrinkle.

[0072] The main body of the compound eye structure with a three-dimensional structure is composed of an array of multiple sub-eyes with point-shaped protrusions. This array form makes it compatible with a variety of large-dimensional shapes such as curved surfaces, bends and twists, and can maintain sufficient top substructures (sub-eyes) with corresponding structural strength. This feature is applied to the electrode described in this application to meet the requirements of the electrode sheet when it is deformed at a large-dimensional level (such as curved surfaces, bends, twists, etc.), and the active component layer 2 as a substructure still has a certain structural strength and is not prone to falling off and failure, thereby improving the electrochemical performance of the electrode. In addition, the imitation compound eye fold structure will also increase the surface area of ​​the electrode, improve the contact between the electrode and the electrolyte, and enhance the charge and discharge stability of the electrode and the battery.

[0073] In a specific embodiment, the active component layer 2 includes graphite, ethylene carbonate (EC) and styrene-butadiene rubber, and the solvent of the swelling process is ethanol matched with the styrene-butadiene rubber. When the active component layer 2 is formed on one side or both sides of the current collector layer 1, ethanol can be sprayed on the surface of the active component layer 2, and the styrene-butadiene rubber expands and deforms under the swelling effect of ethanol, and then the first wrinkled surface of the active component layer 2 can be formed by baking, that is, the electrode with the compound eye-like wrinkles is obtained.

[0074] Alternatively, see Figures 7 to 9 The first protrusions 21 are linear protrusions, and a plurality of the first protrusions 21 form the first wrinkled surface having a two-dimensional structure; for example, a plurality of the first protrusions 21 form cyclamen leaf-like wrinkles, and the cyclamen leaf-like wrinkles are formed by a swelling process.

[0075] Specifically, the cyclamen leaf-like wrinkle structure is a two-dimensional curved multi-scale wrinkle composed of linear protrusions. The cyclamen leaf structure can reduce the adhesion and friction between the electrode surface and the outside world, achieve anti-adhesion and low friction, thereby improving the performance of the electrode and the battery using the electrode.

[0076] In a specific embodiment, the active component layer 2 includes graphite and styrene-butadiene rubber, and the solvent of the swelling process is ethanol matched with the styrene-butadiene rubber. When the active component layer 2 is formed on one side or both sides of the current collector layer 1, ethanol can be sprayed on the surface of the active component layer 2, and the styrene-butadiene rubber expands and deforms under the swelling effect of ethanol, and then the first wrinkled surface of the active component layer 2 can be formed by baking, that is, the electrode with the cyclamen leaf-like wrinkles is obtained.

[0077] In addition, the electrode is not limited to the above-mentioned negative electrode, but can also be used as a positive electrode. For example, the active component layer 2 includes lithium iron phosphate and polyvinylidene fluoride (PVDF), and the solvent of the swelling process is ethanol matched with the polyvinylidene fluoride. When the active component layer 2 is formed on one side or both sides of the current collector layer 1, ethanol can be sprayed onto the surface of the active component layer 2, and the polyvinylidene fluoride expands and deforms under the swelling effect of ethanol, and then the first wrinkled surface of the active component layer 2 can be formed by baking, and a multi-scale wrinkled electrode with the cyclamen leaf-like wrinkles can be obtained.

[0078] Alternatively, see Figure 6 , Fig. 9 and Fig.12 The current collector layer 1 has a plurality of second protrusions 11 to form a second wrinkled surface of the current collector layer 1 .

[0079] Specifically, the second wrinkled surface of the current collector layer 1 can be achieved by having active component layers 2 with different surface densities on both sides of the current collector layer 1. For example, when the surface density of the active component layer 2 located on the first surface and the surface density of the active component layer 2 located on the second surface are different, bending stress will be generated inside the current collector layer 1, so that the current collector layer 1 has a tendency to bend, thereby generating a plurality of second protrusions 11. In addition, the second wrinkled surface of the current collector layer 1 can also be achieved when the first wrinkled surface of the active component layer 2 is molded. For example, when the first wrinkled surface of the active component layer 2 is molded, compressive stress will be generated inside the active component layer 2, and the active component layer 2 is coated on the current collector layer 1, thereby generating bending stress inside the current collector layer 1, thereby generating a plurality of second protrusions 11.

[0080] Optionally, the first protrusion 21 includes a substrate and lines formed on the surface of the substrate, the size of the substrate is micrometer-level, and the size of the lines is nanometer-level.

[0081] Specifically, the structure of the first protrusion can be similar to the micro-nano scale structure of red rose petals, for example, the surface of the front of the first protrusion is densely stacked and arranged with micron-scale nipples, and the surface of the nipples is also covered with a double-layer hierarchical structure formed by nano-scale wrinkles, that is, a combination of micron-scale nipples and nano-scale wrinkles, which improves the layering of the wrinkles of the first protrusion. In addition, the first protrusion 21 can also include a matrix and a texture formed on the surface of the matrix, the size of the matrix is ​​millimeter-level, and the size of the texture is micrometer-level and / or millimeter-level.

[0082] See also Fig.15 , an embodiment of the present application also provides a battery, comprising the above-mentioned electrode.

[0083] Specifically, the electrode may be a positive electrode or a negative electrode. The electrode may be used alone as the positive electrode or the negative electrode of the battery, or may be combined with a common electrode to form a composite electrode.

[0084] In a specific embodiment, see Fig.15 The electrode described in the present application is the negative electrode of the battery, and is connected in parallel with the conventional common electrode A (planar negative electrode) to form a composite negative electrode, while the positive electrode of the battery adopts the common electrode B (planar positive electrode). The negative electrode and the positive electrode of the battery are separated by a diaphragm, and the electrolyte in the battery can be a liquid electrolyte or a solid electrolyte.

[0085] Since the battery uses an electrode formed by the active component layer 2 having a first wrinkled surface, the first wrinkled surface can reduce the stress of the outer layer of the pole piece, and alleviate the deformation of the pole piece and the expansion of the battery caused by the expansion of the electrode material. In addition, the first wrinkled surface can also increase the contact area between the electrode and the electrolyte and the transmission path of ions in the electrode, reduce the friction between the electrode and other components in the battery, and thus improve the energy density and cycle life of the battery.

[0086] The present application also provides a method for preparing the electrode, comprising:

[0087] S101, disposing the active component layer on the surface of the current collector layer, wherein the active component layer includes an active component and a deformation component, and the deformation component includes an expansion agent or a shrinkage agent;

[0088] S102, when the deformation component includes a swelling agent, obtaining a first protrusion by swelling the swelling agent;

[0089] Alternatively, when the deformation component includes a shrinking agent, the first protrusion is obtained by shrinking the shrinking agent.

[0090] When the deformation component in the electrode provided in the embodiment of the present application includes an expansion agent, the expansion agent is swelled by the solvent, and then the swelled active component layer is baked to form a plurality of first protrusions on the active component layer. The plurality of first protrusions can form a first wrinkled surface of the active component layer. The first wrinkled surface can reduce the outer layer stress of the pole piece and alleviate the deformation of the pole piece and the expansion of the battery caused by the expansion of the electrode material. Or when the deformation component in the electrode includes a shrinking agent, the shrinking agent is shrunk by the solvent, and then the shrunk active component layer is baked to form a plurality of first protrusions on the active component layer.

[0091] In addition, the first wrinkled surface can also increase the contact area between the electrode and the electrolyte and the transmission path of ions in the electrode, reduce the friction between the electrode and other components in the battery, and thus improve the energy density and cycle life of the electrode.

[0092] The present application is further described below through specific examples and comparative examples.

[0093] Example 1

[0094] An electrode, wherein the first wrinkled surface is a honeycomb-like wrinkle, the wrinkled structure is formed along the thickness direction of the electrode, and a plurality of first protrusions form a regular hexagonal projection on the electrode.

[0095] The preparation method of the above-mentioned honeycomb-like wrinkled electrode is as follows:

[0096] The active component layer is formed by fixing the graphite active material on both sides of the current collector layer, and then continuously rolled by a gravure mold roller with a bionic honeycomb shape and a silicone roller to obtain an electrode with a honeycomb-like fold pattern.

[0097] The side length of the regular hexagon of the above-mentioned mold is 1 cm, the rolling speed is 3 m / min, and the rolling pressure is not greater than 50 MPa.

[0098] Example 2

[0099] An electrode, wherein the first wrinkled surface is a lychee leaf-like wrinkle, and the wrinkle structure is a curved micro-scale wrinkle.

[0100] The preparation method of the above-mentioned litchi leaf wrinkle electrode is as follows:

[0101] The mixed material of graphite active material and styrene-butadiene rubber is fixed on the A and B surfaces of the current collector layer to form an active component layer, where the surface density of the active material on the A surface is 6 g / cm 2 The active material surface density of surface B is 4 g / cm 2 , a planar electrode is obtained, and then the planar electrode is placed in an oven and baked for 1 hour. Due to the different surface densities of active materials on the AB surface, stress is generated, and a curved electrode can be obtained;

[0102] After the curved electrode is cold pressed, acetone is sprayed on the A surface to moisten it, causing the styrene-butadiene rubber in the A surface to swell. After 30 minutes, the electrode is placed in an oven and baked for 1 hour to obtain an electrode with a lychee leaf-like wrinkle pattern.

[0103] Example 3

[0104] An electrode, wherein the first wrinkle surface is a compound eye-like wrinkle, and the wrinkle structure is a curved multi-scale wrinkle.

[0105] The preparation method of the compound eye-like wrinkled electrode is as follows:

[0106] The active component layer is formed by fixing the mixed material of graphite active material, ethylene carbonate and styrene-butadiene rubber on the A and B surfaces of the current collector layer, where the surface density of the active material on the A surface is 6 g / cm 2 The active material surface density of surface B is 4 g / cm 2 , a planar electrode is prepared, and then the planar electrode is placed in an oven and baked for 1 hour. During the baking process, ethylene carbonate volatilizes, and stress is generated due to the different surface densities of active substances on the AB surface, so that a curved surface electrode with a microstructure can be obtained;

[0107] After the curved surface electrode is cold pressed, ethanol is sprayed on the A surface to moisten it, causing the styrene-butadiene rubber in the A surface to swell. After 30 minutes, the electrode is baked under a far-infrared lamp for 1 hour to obtain an electrode with a compound eye-like wrinkle pattern.

[0108] Example 4

[0109] An electrode, wherein the first wrinkled surface is a wrinkle imitating a cyclamen leaf, and the wrinkle structure is a curved multi-scale wrinkle.

[0110] The preparation method of the cyclamen leaf-like wrinkled electrode is as follows:

[0111] The mixed material of graphite active material and styrene-butadiene rubber is fixed on the A and B surfaces of the current collector layer to form an active component layer, where the surface density of the active material on the A surface is 6 g / cm 2 The active material surface density of surface B is 4 g / cm 2 , a planar electrode is obtained, and then the planar electrode is placed in an oven and baked for 1 hour. Due to the different surface densities of active materials on the AB surface, stress is generated, and a curved electrode can be obtained;

[0112] After the curved surface electrode is cold pressed, ethanol is sprayed on the A surface to moisten it, and the styrene-butadiene rubber in the A surface swells. After 24 hours, the electrode is placed in an oven and baked for 1 hour to obtain an electrode with a cyclamen leaf-like wrinkle pattern.

[0113] Example 5

[0114] An electrode, wherein the first wrinkled surface is a wrinkle imitating a cyclamen leaf, and the wrinkle structure is a multi-scale wrinkle.

[0115] The preparation method of the cyclamen leaf-like wrinkled electrode is as follows:

[0116] A mixed material of lithium iron phosphate active material and polyvinylidene fluoride is fixed on both sides of the current collector layer to form an active component layer to obtain a planar electrode;

[0117] The surface of the planar electrode was sprayed with ethanol to wet it, and the polyvinylidene fluoride in the electrode was swollen. After 24 hours, the electrode was placed in an oven and baked for 1 hour to obtain an electrode with a cyclamen leaf-like wrinkle pattern.

[0118] Example 6

[0119] An electrode, wherein the first wrinkled surface is a honeycomb-like wrinkle, the wrinkled structure is formed along the thickness direction of the electrode, and a plurality of first protrusions form a regular hexagonal projection on the electrode.

[0120] The preparation method of the above-mentioned honeycomb-like wrinkled electrode is as follows:

[0121] The active component layer is formed by fixing the graphite active material on both sides of the current collector layer, and then the local active component layer is vaporized by laser sputtering to cause thermal expansion, fragmentation and peeling, thereby obtaining an electrode with a honeycomb-like fold pattern.

[0122] Example 7

[0123] A battery, such as Fig.15 The electrode with the honeycomb-like pleated pattern obtained in Example 1 is used as the outer negative electrode sheet, the flat electrode without formed pleats in Example 1 is used as the inner negative electrode sheet, the positive electrode sheet is prepared with the spinel structure as the main active material, the negative electrode sheet and the positive electrode sheet are separated by a porous isolation membrane, the electrolyte is prepared with a non-aqueous electrolyte and an organic solution, and the shell is a metal shell.

[0124] Example 8

[0125] A battery, using the electrode with the imitation litchi leaf wrinkle pattern obtained in Example 2 as the negative electrode, using the spinel structure as the main active material to prepare the positive electrode, the negative electrode and the positive electrode are separated by a porous isolation membrane, the electrolyte is prepared by non-aqueous electrolyte and organic solution, and the shell is a metal shell.

[0126] Example 9

[0127] A battery, wherein the electrode with the compound eye fold pattern obtained in Example 3 is used as a negative electrode, a positive electrode is prepared with a spinel structure as a main active material, the negative electrode and the positive electrode are separated by a porous isolation membrane, the electrolyte is prepared with a non-aqueous electrolyte and an organic solution, and the shell is a metal shell.

[0128] Example 10

[0129] A battery, wherein the electrode with the cyclamen leaf wrinkle pattern obtained in Example 4 is used as a negative electrode, a positive electrode is prepared with a spinel structure as a main active material, the negative electrode and the positive electrode are separated by a porous isolation membrane, an electrolyte is prepared with a non-aqueous electrolyte and an organic solution, and the shell is a metal shell.

[0130] Embodiment 11

[0131] A battery, with a graphite flat electrode as a negative electrode, and an electrode with a cyclamen leaf wrinkle pattern obtained in Example 5 as a positive electrode, the negative electrode and the positive electrode are separated by a porous isolation membrane, the electrolyte is prepared by a non-aqueous electrolyte and an organic solution, and the shell is a metal shell.

[0132] Example 12

[0133] A battery, using the simulated honeycomb graphite electrode of Example 6 as a negative electrode sheet, using the simulated honeycomb lithium iron phosphate electrode obtained in Example 6 as a positive electrode sheet, the negative electrode sheet and the positive electrode sheet are separated by a porous isolation membrane, the electrolyte is prepared by a non-aqueous electrolyte and an organic solution, and the shell is an aluminum-plastic film.

[0134] Comparative Example 1

[0135] A pole piece, the planar electrode negative pole piece without formed wrinkles in Example 1.

[0136] Comparative Example 2

[0137] A pole piece, the curved surface electrode negative pole piece without wrinkles in Example 2.

[0138] Comparative Example 3

[0139] A pole piece, the curved electrode negative pole piece without wrinkles in Example 3.

[0140] Comparative Example 4

[0141] A pole piece, the curved electrode negative pole piece without formed wrinkles in Example 4.

[0142] Comparative Example 5

[0143] A pole piece, the planar electrode negative pole piece without formed wrinkles in Example 5.

[0144] Comparative Example 6

[0145] A pole piece, the planar electrode negative pole piece without formed wrinkles in Example 6.

[0146] Comparative Example 7

[0147] A battery using the electrode of Comparative Example 1. The preparation method is the same as that of Example 7.

[0148] Comparative Example 8

[0149] A battery using the electrode sheet of Comparative Example 2. The preparation method is the same as that of Example 8.

[0150] Comparative Example 9

[0151] A battery using the electrode sheet of Comparative Example 3. The preparation method is the same as that of Example 9.

[0152] Comparative Example 10

[0153] A battery using the electrode sheet of Comparative Example 4. The preparation method is the same as that of Example 10.

[0154] Comparative Example 11

[0155] A battery using the electrode of Comparative Example 5. The preparation method is the same as that of Example 11.

[0156] Comparative Example 12

[0157] A battery using the electrode sheet of Comparative Example 6. The preparation method is the same as that of Example 12.

[0158] The electrodes and batteries of the above embodiments and comparative examples were tested as follows:

[0159] Fluid retention test

[0160] The electrolyte retention test is used to evaluate the electrode's ability to absorb and retain electrolyte.

[0161] The rich electrode surface structure will improve the liquid retention capacity, which is of great significance to the life of the electrolyte-containing battery encapsulated in a soft package. Specifically, improving the liquid absorption capacity is conducive to the battery retaining more electrolyte, making the battery life longer.

[0162] Specific test method:

[0163] By cutting the electrode into a size of 10cm*20cm, weighing it as W1, then immersing it in the electrolyte, taking it out and weighing W2, the percentage of (W2-W1) / W1 is calculated as the liquid retention rate m. The larger m is, the better the ability of the electrode to absorb and retain electrolyte.

[0164] The test results of the embodiment electrode and the comparative example electrode are shown in Table 1.

[0165] Table 1

[0166]

[0167] It can be seen from Table 1 that the liquid retention rate of the electrode provided by the embodiment of the present application is improved by more than 42% compared with the liquid retention rate of the electrode of the traditional comparative example.

[0168] Expansion test

[0169] The expansion test includes both the evaluation of the degree of expansion of the electrode and the impact of the expansion on the battery using the above electrode.

[0170] The test method is:

[0171] The battery using the above electrodes was tested in three states: uncharged, fully charged, and charged after 100 cycles. The thicknesses of the electrode sheets were h1, h2, and h3, and the thicknesses of the batteries were H1, H2, and H3, respectively.

[0172] The expansion coefficient of the electrode after full charge is P1 = (h2-h1) / h1;

[0173] After 100 cycles, the expansion coefficient of the electrode is P2 = (h3-h1) / h1;

[0174] The expansion coefficient of the battery after full charge is P3 = (H2-H1) / H1;

[0175] After 100 cycles, the expansion coefficient of the battery is P4 = (H3-H1) / H1.

[0176] The test results are shown in Tables 2 to 5:

[0177] Table 2

[0178]

[0179] Table 3

[0180]

[0181] Table 4

[0182]

[0183]

[0184] Table 5

[0185]

[0186] It can be seen from Table 2 that the expansion degree of the electrode provided by the embodiment of the present application after the electrode is fully charged is only 79% or even lower than the expansion degree of the electrode provided by the conventional comparative example, and the expansion degree of the electrode provided by the embodiment 4 after the electrode is fully charged is only 47% of the expansion degree of the electrode provided by the conventional comparative example 4;

[0187] It can be seen from Table 3 that the expansion degree of the electrode provided by the embodiment of the present application after 100 cycles is only 75% or even lower than that of the electrode provided by the conventional comparative example, and the expansion degree of the electrode provided by the embodiment 4 after 100 cycles after the electrode is fully charged is only 38% of that of the electrode provided by the conventional comparative example 4;

[0188] It can be seen from Table 4 that the expansion degree of the battery after the electrode provided in the embodiment of the present application is fully charged is only 73% or even lower than the expansion degree of the electrode provided in the conventional comparative example, and the expansion degree of the electrode provided in the battery after the battery is fully charged is only 28% of the expansion degree of the battery provided in the conventional comparative example 9;

[0189] It can be seen from Table 5 that the expansion degree of the battery after the electrode provided in the embodiment of the present application is cycled 100 times is only 90% or even lower than the expansion degree of the electrode provided in the conventional comparative example, and the expansion degree of the battery provided in Example 9 after the electrode is fully charged and cycled 100 times is only 54% of the expansion degree of the battery provided in the conventional comparative example 9.

[0190] Life test

[0191] The battery's full charge-discharge (1C)-full charge (1C) interval is called a cycle. Repeated cycles, and then measuring the remaining capacity retention rate of a specified number of cycles can show the battery's cycle life. High-rate charging and discharging can accelerate the life test.

[0192] The test results are shown in Table 6:

[0193] Table 6

[0194]

[0195] It can be seen from Table 6 that, compared with batteries using traditional planar electrodes, the battery using the electrode provided in the embodiment of the present application has an enhanced cycle life, whether after a low number of charge and discharge cycles of 50 and 100 times, or after a high number of charge and discharge cycles of 150 and 200 times.

[0196] Although some specific embodiments of the present application have been described in detail by way of example, it should be understood by those skilled in the art that the above examples are only for illustration, not for limiting the scope of the present application. It should be understood by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present application. The scope of the present application is defined by the appended claims.

Claims

1. An electrode, characterized in that: include: Current collector layer (1); An active component layer (2), the active component layer (2) covering at least one surface of the current collector layer (1), the active component layer (2) having a plurality of first protrusions (21) on a side away from the current collector layer (1) to form a first wrinkled surface of the active component layer (2); The active component layer includes a deformation component, and the deformation component includes a swelling agent or a shrinking agent. The first protrusion is obtained by swelling the swelling agent or shrinking the shrinking agent.

2. The electrode according to claim 1, characterized in that The top surfaces of the plurality of first protrusions (21) form a first curved surface.

3. The electrode according to claim 2, characterized in that The first protrusion (21) is formed by a molding process, a printing process, a spraying process, a laser sputtering process, a mechanical wrapping process, a surface chemical oxidation process, a chemical vapor deposition process, a swelling process, a thermal deformation process or a prestress release process.

4. The electrode according to claim 3, characterized in that The active component layer (2) covers the first surface and the second surface of the current collector layer (1), and the surface density of the active component layer (2) located on the first surface is greater than the surface density of the active component layer (2) located on the second surface.

5. The electrode according to claim 2, characterized in that The first protrusions (21) are linear protrusions, and a plurality of the first protrusions (21) form the first wrinkled surface having a one-dimensional structure.

6. The electrode according to claim 2, characterized in that The first protrusions (21) are point-shaped protrusions, and a plurality of the first protrusions (21) form the first wrinkled surface having a three-dimensional structure.

7. The electrode according to claim 2, characterized in that The first protrusions (21) are linear protrusions, and a plurality of the first protrusions (21) form the first wrinkled surface having a two-dimensional structure.

8. The electrode according to claim 1, characterized in that The current collector layer (1) has a plurality of second protrusions (11) thereon to form a second wrinkled surface of the current collector layer (1).

9. The electrode according to claim 1, characterized in that The first protrusion (21) comprises a base and lines formed on the surface of the base, the base has a size of micrometer level, and the lines have a size of micrometer level and / or nanometer level.

10. The electrode according to claim 1, characterized in that The first protrusion (21) comprises a base and a pattern formed on the surface of the base, the size of the base is in the millimeter level, and the size of the pattern is in the micrometer level and / or millimeter level.

11. A battery, characterized in that: The electrode comprises the electrode according to any one of claims 1 to 10.

12. A method for preparing the electrode according to any one of claims 1 to 10, characterized in that: include: The active component layer is arranged on the surface of the current collector layer, wherein the active component layer comprises an active component and a deformation component, and the deformation component comprises an expansion agent or a shrinkage agent; When the deformation component includes a swelling agent, the first protrusion is obtained by swelling the swelling agent; Alternatively, when the deformation component includes a shrinking agent, the first protrusion is obtained by shrinking the shrinking agent.