A sandwich structured, sticky and durable oral ulcer membrane and preparation method thereof

By designing the oral ulcer membrane with a sandwich structure, the expansion of the top layer forms suction cup-like adsorption, the problem of oral ulcer membrane dissolution and poor adhesion in saliva in the prior art is solved, and effective bonding and improvement are achieved for a longer time Good healing effect.

CN115737605BActive Publication Date: 2024-11-12HANGZHOU GUILING MEDICAL INSTR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211480923.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-24
Publication Date
2024-11-12
Estimated Expiration
2042-11-24

AI Technical Summary

Technical Problem

The existing oral ulcer membrane dissolves in saliva, has a short dissolution time and poor adhesion, resulting in the problem of shedding.

Method used

Design a sandwich structure with an adhesive and lasting oral ulcer membrane, including a tightly fitted top layer, intermediate layer and adhesive layer. The top layer uses a hydrophilic material that swells in water. The intermediate layer is a waterproof flexible material, and the adhesive layer contains drugs. , through the expansion of the top layer, it forms a suction cup-like adsorption on the mucosa, solving the problem of poor adhesion.

Benefits of technology

The oral ulcer membrane is achieved to swell in water without immediately dissolving, maintaining its morphology for more than 60 minutes, enhancing adhesion, reducing foreign body sensation, avoiding edge warping, significantly reducing the pain of oral ulcers and promoting healing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115737605B_ABST
    Figure CN115737605B_ABST
Patent Text Reader

Abstract

The present invention discloses a viscous and long-lasting oral ulcer membrane with a sandwich structure and a preparation method thereof, wherein the oral ulcer membrane comprises a top layer, an intermediate layer and an adhesive layer that are tightly fitted to form a sandwich structure; the intermediate layer comprises a waterproof flexible material, the top layer comprises a hydrophilic material that swells when in contact with water, and the adhesive layer contacts the oral mucosa and comprises a drug and a hydrophilic material that swells when in contact with water. The present invention designs an oral ulcer membrane with a unique "sandwich" (ABA) sandwich structure, and when the oral ulcer membrane is attached to the surface of the oral mucosa, its outer surface generates a larger expansion volume due to contact with more saliva, thereby causing the oral ulcer membrane to bend inward, so that it can be expanded to form a "sucker-like" shape when in use and firmly adsorbed on the surface of the oral mucosa, thereby solving the pain point of poor adhesion of the existing oral ulcer patch (overcoming the pain point that the existing oral ulcer patch will cause the adhesive layer to absorb water and swell due to long-term saliva soaking, thereby causing the edge of the patch to warp and fall off).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of medical materials and relates to a membrane material, in particular to a sticky and durable oral ulcer membrane with a sandwich structure and a preparation method thereof. Background Art

[0002] Oral ulcers are a common ulcerative injury disease that occurs in the oral mucosa. During an attack, the pain is severe and there is obvious local burning pain. In severe cases, it can also affect eating and speaking, causing great inconvenience to daily life.

[0003] Oral ulcer membranes can reduce the pain caused by oral ulcers and accelerate the healing of oral ulcers. At present, commercially available oral ulcer membranes are mainly made of water-soluble bioadhesive materials, such as propolis, polyvinyl alcohol, chitosan, etc. However, this type of oral ulcer membrane has poor water resistance and will quickly swell and dissolve in the mouth due to saliva and lose its effect. The effective time is usually no more than 15 minutes.

[0004] In order to prevent saliva from dissolving and prolong the effective time, Chinese patent CN 110302144 A prevents saliva from eroding by compounding a waterproof layer on the bioadhesive layer. The waterproof layer can be water-insoluble ethyl cellulose, polymer film, etc. However, saliva soaking will cause the bioadhesive layer to absorb water and swell, which will cause the edge of the patch to warp and fall off. Summary of the invention

[0005] In view of the shortcomings and deficiencies in the prior art, the object of the present invention is to provide a sandwich structured, sticky and durable oral ulcer membrane.

[0006] Another object of the present invention is to provide a method for preparing the above-mentioned sticky and durable oral ulcer film with a sandwich structure.

[0007] The technical solution of the present invention is as follows:

[0008] A sticky and durable oral ulcer membrane with a sandwich structure comprises a top layer, a middle layer and an adhesive layer which are tightly fitted to form a sandwich structure; the middle layer comprises a waterproof flexible material, the top layer comprises a hydrophilic material which swells in water, and the adhesive layer contacts the oral mucosa and comprises a drug and a hydrophilic material which swells in water.

[0009] Furthermore, the thickness of the top layer is greater than or equal to the thickness of the adhesion layer.

[0010] When the oral ulcer film of the present invention is attached to the oral mucosal surface, its outer surface (i.e., the top layer) contacts more saliva and generates a larger expansion volume, thereby causing the oral ulcer film to bend inward, and can be expanded to form a "sucker" shape and firmly adsorbed to the mucosal surface, thereby solving the pain point of poor adhesion of the oral ulcer patch. When the thickness of the top layer is greater than or equal to the thickness of the adhesive layer, the adsorption effect is better.

[0011] Furthermore, the mass ratio of the top layer to the adhesive layer is (1-2):1.

[0012] Furthermore, the hydrophilic material that swells in water includes one or more of hydroxypropyl methylcellulose, polyvinyl alcohol, hydroxyethyl cellulose, xanthan gum, and the like.

[0013] Furthermore, the hydrophilic material that swells in water is a mixture of polyvinyl alcohol and xanthan gum, and the mass ratio of polyvinyl alcohol to xanthan gum is (4-15):1.

[0014] By screening the hydrophilic materials of the top layer and the adhesive layer and selecting the proportion, the hydrophilic materials of the top layer and the adhesive layer will not dissolve immediately in water, but will swell to cause volume expansion and maintain the shape for more than 60 minutes.

[0015] Furthermore, the drug is one or more of chemical pharmaceuticals, traditional Chinese medicine extracts and bio-inorganic materials that promote oral ulcer healing and relieve pain; in the adhesive layer, the mass of the drug accounts for 1-3% of the mass of the hydrophilic material that swells in water.

[0016] Furthermore, the drug is one or more of metronidazole, menthol or bioactive glass.

[0017] Furthermore, the waterproof flexible material includes one or more of ethyl cellulose or silicone resin.

[0018] Furthermore, the thickness of the oral ulcer membrane is 0.08-0.3 mm, and the oral ulcer membrane is a circular membrane with a diameter of 0.5-1.5 cm; the thickness of the middle layer is 0.01-0.03 mm.

[0019] A method for preparing a sandwich-structured sticky and durable oral ulcer membrane comprises the following steps:

[0020] (1) dissolving the hydrophilic material that swells in water in a first solvent to prepare a solution A; dissolving the hydrophilic material that swells in water and a drug in a second solvent to prepare a solution B; and dissolving the waterproof flexible material in a third solvent to prepare a solution C;

[0021] (2) pouring solution B into a glass container and drying it to obtain an adhesive layer; coating solution C on the adhesive layer and drying it to obtain an intermediate layer; then pouring solution A on the intermediate layer and drying it to obtain a three-layer sandwich structure sheet;

[0022] (3) cutting to obtain the sticky and durable oral ulcer membrane with a sandwich structure.

[0023] Further, the thickness of the top layer is greater than or equal to the thickness of the adhesive layer;

[0024] The first solvent and the second solvent are both water;

[0025] The third solvent is anhydrous alcohol or decamethylcyclopentasiloxane;

[0026] The drying temperature is 25-90°C.

[0027] Furthermore, when the waterproof flexible material is ethyl cellulose, the third solvent is anhydrous alcohol; when the waterproof flexible material is silicone resin, the third solvent is decamethylcyclopentasiloxane.

[0028] Furthermore, the hydrophilic material that swells in water accounts for (1-3)% of the total mass of the first solvent and the hydrophilic material that swells in water.

[0029] In the adhesive layer, the hydrophilic material that swells in water accounts for (1-3)% of the total mass of the second solvent, the drug and the hydrophilic material that swells in water. The drug content is 1-4% of the mass of the hydrophilic material.

[0030] The waterproof flexible material accounts for (1-3)% of the total mass of the flexible material and the third solvent.

[0031] The advantages of the present invention are as follows:

[0032] The present invention designs a unique "sandwich" (ABA) structured oral ulcer membrane, which is composited from three layers of materials. The top layer and the adhesive layer are mainly composed of hydrophilic materials that swell in water, while the middle layer is mainly composed of waterproof flexible materials, forming a sandwich structure.

[0033] When the oral ulcer membrane is attached to the surface of the oral mucosa, its outer surface will swell to a larger volume due to contact with more saliva, causing the oral ulcer membrane to bend inward, so that it can swell to form a "suction cup shape" during use and firmly adhere to the surface of the oral mucosa, thereby solving the pain point of poor adhesion of existing oral ulcer patches (overcoming the pain point that the adhesive layer of existing oral ulcer patches will absorb water and swell due to long-term saliva immersion, thereby causing the edge of the patch to warp and fall off).

[0034] Among them, the hydrophilic materials of the top layer and the adhesive layer of the oral ulcer membrane will not dissolve immediately in water, but will swell to cause volume expansion and maintain the shape for more than 60 minutes.

[0035] The oral ulcer membrane of the invention has good biological adhesion, can be well adhered to the ulcer wound surface, and makes the patient feel less foreign body sensation, is easy to use, and has the advantages of repairing ulcer wounds, promoting healing, relieving pain, and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a schematic diagram of the structure of oral ulcer membrane;

[0037] Among them, 1. adhesive layer, 2. middle layer, 3. top layer. DETAILED DESCRIPTION

[0038] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0039] Embodiment 1:

[0040] Table 1. Recipe 1

[0041]

[0042] According to the formula shown in Table 1, the raw materials were weighed, and PVA and xanthan gum were dissolved in water to form solution A. PVA, xanthan gum, menthol and bioglass were dissolved in water and recorded as solution B after being completely dissolved. Ethyl cellulose was dissolved in ethanol and recorded as solution C. Then 80 parts of solution B were poured into a glass container and dried in a 55 degree Celsius oven to obtain an adhesive layer. 10 parts of solution C were applied to the adhesive layer and dried in a 55 degree Celsius oven, and 100 parts of solution A were poured into a glass container and dried in a 55 degree Celsius oven to obtain a three-layer structure sheet.

[0043] Cut with a circular cutter of 1 cm in diameter to obtain the sandwich structured sticky and durable oral ulcer patch. The thickness of the adhesive layer 1 of the oral ulcer patch is 80±5 um, the thickness of the middle layer 2 is 10±5 um, and the thickness of the top layer 3 is 100±5 um.

[0044] The dissolution time of adhesive layer 1 in water is 120±10min; the effective adhesion time of mucous membrane is 90±10min; comfort: little foreign body sensation. No edge warping phenomenon. It can significantly reduce the pain caused by oral ulcers.

[0045] Among them, the definition of effective mucosal adhesion time is: the time from the time the oral ulcer membrane is attached to the oral mucosa of the volunteer to the time it falls off is the effective mucosal adhesion time.

[0046] Definition of edge warping: The edge of the circular oral ulcer patch warps outwards. It may cause the oral ulcer membrane to fall off and increase the foreign body sensation.

[0047] Embodiment 2:

[0048] Table 2. Formulation 2

[0049]

[0050] According to the formula shown in Table 2, weigh the raw materials, dissolve PVA1788 and PVA1799 in water to prepare solution A. Dissolve PVA1788, PVA1799, menthol and bioglass in water, and record them as solution B after they are completely dissolved. Dissolve ethyl cellulose in ethanol and record them as solution C. Then pour 100 parts of solution B into a glass container, dry it in an oven at 55 degrees Celsius, and obtain adhesive layer 1. Apply 10 parts of solution C on adhesive layer 1, dry it in an oven at 55 degrees Celsius, pour 100 parts of solution A into a glass container, and dry it in an oven at 55 degrees Celsius to obtain a three-layer structure sheet.

[0051] The adhesive layer 1 of the obtained oral ulcer patch is 100±5um thick, the middle layer 2 is 10±5um thick, and the top layer 3 is 100±5um thick.

[0052] The dissolution time of the adhesive layer 1 in water is 150±10min; the effective adhesion time of the mucous membrane is 110±10min; comfort: little foreign body sensation. No edge warping. It can significantly reduce the pain caused by oral ulcers.

[0053] Embodiment 3:

[0054] Table 3. Recipe 3

[0055]

[0056]

[0057] According to the formula shown in Table 3, the raw materials are weighed, and PVA and xanthan gum are dissolved in water to prepare solution A. PVA, xanthan gum, menthol and bioglass are dissolved in water, and the solution B is recorded after complete dissolution. Silicone resin (soft film) is dissolved in decamethylcyclopentasiloxane and recorded as solution C. Then 100 parts of solution B are poured into a glass container, and after drying in a 55 degree Celsius oven, an adhesive layer 2 is obtained. 10 parts of solution C are applied to the adhesive layer 2, and after drying in a 55 degree Celsius oven, 150 parts of solution A are poured into a glass container, and after drying in a 55 degree Celsius oven, a three-layer structure sheet is obtained.

[0058] The adhesive layer 1 of the obtained oral ulcer patch has a thickness of 100±10 um, the thickness of the middle layer 2 is 10±5 um, and the thickness of the top layer 3 is 150±5 um.

[0059] The dissolution time of adhesive layer 1 in water is 130±10min; the effective adhesive time of mucous membrane is 100±10min; comfort: strong foreign body sensation. No edge warping. It can significantly reduce the pain caused by oral ulcers.

[0060] Embodiment 4:

[0061] Table 4. Recipe 4

[0062]

[0063]

[0064] The raw materials were weighed according to the formula shown in Table 4, and PVA1788 and PVA1799 were dissolved in water to prepare solution A. PVA1788, xanthan gum, menthol, and bioglass were dissolved in water, and after complete dissolution, they were recorded as solution B. Ethyl cellulose was dissolved in ethanol and recorded as solution C. Then 100 parts of solution B were poured into a glass container, and after drying in an oven at 55 degrees Celsius, an adhesive layer 1 was obtained. 10 parts of solution C were coated on the adhesive layer 1, and after drying in an oven at 55 degrees Celsius, 100 parts of solution A were poured into a glass container, and after drying in an oven at 55 degrees Celsius, a three-layer structure sheet was obtained.

[0065] The adhesive layer 1 of the obtained oral ulcer patch is 100±5um thick, the middle layer 2 is 10±5um thick, and the top layer 3 is 100±5um thick.

[0066] The dissolution time of the adhesive layer 1 in water is 120±10min; the effective adhesion time of the mucous membrane is 100±10min; comfort: little foreign body sensation. No edge warping. It can significantly reduce the pain caused by oral ulcers.

[0067] Comparative Example 1:

[0068] Table 5 Recipe 5

[0069]

[0070] According to the formula shown in Table 5, raw materials were weighed, PVA1788, xanthan gum, menthol, and bioglass were dissolved in water, and after they were completely dissolved, the solution was poured into a glass container and dried in an oven at 55 degrees Celsius to obtain an adhesive layer 1. The thickness of the adhesive layer 1 of the obtained oral ulcer patch was 200±10 um.

[0071] The dissolution time of the adhesive layer 1 in water is 130±10min; the effective adhesion time of the mucosa is 30±10min; comfort: little foreign body sensation. No edge warping phenomenon. It can significantly reduce the pain caused by oral ulcers, but the effective time is significantly shorter than that of Example 1.

[0072] Comparative Example 2:

[0073] Table 6 Recipe 6

[0074]

[0075] The raw materials were weighed according to the formula shown in Table 6, PVA1788, menthol and bioglass were dissolved in water, and after they were completely dissolved, the solution was poured into a glass container and dried in an oven at 55 degrees Celsius to obtain an adhesive layer 1. The thickness of the adhesive layer 1 of the obtained oral ulcer patch was 200±10 um.

[0076] The dissolution time of adhesive layer 1 in water is 6 minutes; the effective adhesion time of mucous membrane is 3 minutes; comfort: little foreign body sensation. No edge warping phenomenon. It can hardly relieve the pain caused by oral ulcers.

[0077] Comparative Example 3:

[0078] Table 7 Recipe 7

[0079]

[0080] According to the formula shown in Table 7, the raw materials were weighed, PVA1788, menthol, and bioglass were dissolved in water, and after they were completely dissolved, the solution was poured into a glass container and dried in an oven at 55 degrees Celsius to obtain an adhesive layer 1. Then, an ethanol solution of ethyl cellulose was applied on the adhesive layer 1 to obtain a double-layer structure oral ulcer patch;

[0081] The thickness of the adhesive layer 1 of the obtained oral ulcer patch is 110±10 um. The dissolution time of the adhesive layer 1 in water is 120±10 min; the effective adhesion time of the mucosa is 50±10 min; comfort: severe foreign body sensation. There is obvious edge warping phenomenon. The pain caused by oral ulcer can be significantly reduced.

[0082] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the above embodiments do not limit the protection scope of the present invention in any form, and all technical solutions obtained by equivalent replacement and the like fall within the protection scope of the present invention.

Claims

1. A sandwich structured, sticky and durable oral ulcer membrane, characterized in that: The oral ulcer membrane comprises a top layer, a middle layer and an adhesive layer which are closely attached to form a sandwich structure; the middle layer comprises a waterproof flexible material, the top layer comprises a hydrophilic material which swells in water, and the adhesive layer contacts the oral mucosa and comprises a drug and a hydrophilic material which swells in water; The thickness of the top layer is greater than or equal to the thickness of the adhesive layer; When the oral ulcer membrane is attached to the oral mucosal surface, the outer surface expands to a larger volume due to contact with saliva, so that the oral ulcer membrane bends inward and expands to form a "suction cup" when used, and is firmly adsorbed on the oral mucosal surface without edge warping; The hydrophilic material that swells in water is a mixture of polyvinyl alcohol and xanthan gum, and the mass ratio of polyvinyl alcohol to xanthan gum is (4-15):1; The waterproof flexible material includes one or more of ethyl cellulose or silicone resin.

2. A sandwich structured sticky and durable oral ulcer membrane as claimed in claim 1, characterized in that: The mass ratio of the top layer to the adhesive layer is (1-2):

1.

3. A sandwich structured sticky and durable oral ulcer membrane according to any one of claims 1 to 2, characterized in that: The drug is one or more of chemical pharmaceuticals, Chinese herbal medicine extracts and bio-inorganic materials that promote oral ulcer healing and relieve pain; In the adhesive layer, the mass of the drug accounts for 1-3% of the mass of the water-swellable hydrophilic material.

4. A sandwich structured sticky and durable oral ulcer membrane according to any one of claims 1 to 2, characterized in that: The thickness of the oral ulcer membrane is 0.08-0.3 mm, and the oral ulcer membrane is a circular membrane with a diameter of 0.5-1.5 cm.

5. A method for preparing a sandwich structured sticky and durable oral ulcer film according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: (1) dissolving the hydrophilic material that swells in water in a first solvent to prepare a solution A; dissolving the hydrophilic material that swells in water and a drug in a second solvent to prepare a solution B; and dissolving the waterproof flexible material in a third solvent to prepare a solution C; (2) pouring solution B into a glass container and drying it to obtain an adhesive layer; coating solution C on the adhesive layer and drying it to obtain an intermediate layer; Then, solution A is poured onto the middle layer and dried to obtain a sheet with a three-layer sandwich structure; (3) cutting to obtain the sticky and durable oral ulcer membrane with a sandwich structure.

6. The preparation method according to claim 5, characterized in that: The thickness of the top layer is greater than or equal to the thickness of the adhesive layer; The first solvent and the second solvent are both water; the third solvent is anhydrous alcohol or decamethylcyclopentasiloxane; The drying temperature is 25-90°C.