Preparation method of ternary material and ternary material
Through co-precipitation method and two-step calcination method, a nickel-cobalt lithium manganate ternary material that meets the preset stoichiometric ratio is prepared, which solves the problem of high mixing degree of Li+ and Ni2+, improves electrochemical performance and production efficiency, and is suitable for for the manufacture of secondary batteries.
Patent Information
- Application Number
- CN202211439136.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-17
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-11-17
AI Technical Summary
It is difficult to prepare lithium nickel cobalt manganate (NCM) ternary materials that meet the preset stoichiometric ratio and have an ideal layered structure with the existing technology, especially when the nickel content is high, resulting in a high degree of mixing of Li+ and Ni2+, affecting Electrochemical properties.
Using co-precipitation method and two-step calcination method, the precursor and lithium salt are first decomposed at low temperature to reduce the mixing degree of Li+ and Ni2+, and the mixing ratio of the precursor and lithium salt is adjusted to ensure the stability of the ternary material. The lithium element content forms a stable layered structure.
It realizes that the stoichiometric ratio of the ternary material meets the preset, reduces the degree of ion mixing, improves the electrochemical performance and production efficiency, simplifies the water washing steps, and is suitable for manufacturing secondary batteries.
Smart Images

Figure CN115745022B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a preparation method of a ternary material and a ternary material. Background Art
[0002] As a new type of green power source, secondary batteries have many advantages such as high specific energy, low self-discharge, high open circuit voltage, no memory effect, long cycle life, and low environmental pollution. They are widely used in digital electronic products, pure electric and hybrid new energy vehicles, and energy storage systems. Lithium-ion batteries are one of the most widely used secondary batteries in commercial applications. The energy density of lithium-ion batteries is usually related to the specific capacity of the positive electrode material. Compared with other positive electrode materials, lithium nickel cobalt manganese oxide (also known as NCM ternary material) has higher specific capacity and lower cost, and therefore has received more and more attention.
[0003] NCM ternary materials have a layered structure, with transition metal ions and O 2- Together they form octahedrons and thus form the main body of the layered structure, Li + It occupies the vacancies between the layers and can be reversibly deintercalated between the layers. 2+ It mainly plays the role of supply capacity, so the higher the nickel content in the ternary material, the higher the theoretical specific capacity. 2+ The radius and Li + Close, with Ni 2+ The increase of Ni 2+ When the molar ratio of Ni to total transition metal ions is greater than 90%, more and more Ni 2+ Will occupy Li + Location, Li + This increases the complexity of the material structure, making it difficult to obtain a ternary material with the same or similar metal ion ratio as the raw material by adjusting the ratio of nickel ions, cobalt ions and manganese ions in the raw material and the amount of lithium salt added. + The NCM ternary material Li is volatile under high temperature conditions. + The content is often lower than the preset content, further reducing the content of active lithium ions in the material. Therefore, in the NCM ternary material obtained by the traditional method, the actual content of metal ions (especially lithium ions) has a large deviation from the feed ratio, and the deviation is difficult to control.
[0004] Therefore, how to prepare a ternary material that meets the preset stoichiometric ratio and has an ideal layered structure has become an urgent problem to be solved. Summary of the invention
[0005] Based on this, the present application provides a preparation method of a ternary material and a ternary material. The preparation method can effectively control the stoichiometric ratio of each element in the prepared ternary material, and make the ternary material have an ideal layered structure and a lower degree of ion mixing, thereby improving the electrochemical performance of the ternary material.
[0006] In a first aspect of the present application, a method for preparing a ternary positive electrode material is provided, comprising the following steps:
[0007] Step S1: In a protective gas atmosphere, 2+ 、Co 2+ and Mn 2+ The mixed solution, the precipitant and the complexing agent are mixed and reacted;
[0008] Step S2, aging, standing, filtering, washing and drying the reaction product of step S1 in sequence to prepare a precursor;
[0009] Step S3, mixing the precursor and the lithium salt, and placing them in an oxygen-containing atmosphere for a first calcination, and cooling them after the calcination to prepare a pre-sintering material;
[0010] Step S4, placing the pre-sintered material in an oxygen-containing atmosphere for a second calcination to prepare a ternary material containing Ni, Co and Mn, wherein the temperature of the second calcination is higher than the temperature of the first calcination.
[0011] In some embodiments, the molar ratio of the precursor to the lithium element in the lithium salt is 1:(1.01-1.1). Optionally, the molar ratio of the precursor to the lithium element in the lithium salt is 1:1.05.
[0012] In some embodiments, the precipitant and the complexing agent are both provided in the form of alkaline solutions. Optionally, the precipitant is an aqueous sodium hydroxide solution, and the complexing agent is an aqueous ammonia solution.
[0013] In some embodiments, the mixed solution is Ni 2+ 、Co 2+ and Mn 2+ The total concentration of the aqueous solution is 1.5-2.5 mol / L, the precipitant is 0.2-0.3 mol / L sodium hydroxide aqueous solution, and the complexing agent is 3-5 mol / L ammonia aqueous solution. 2+ 、Co 2+ and Mn 2+ The molar ratio is x:y:(1-xy), wherein 0.83≤x<0.98, 0<y<0.2.
[0014] In some embodiments, the Ni2+ 、Co 2+ and Mn 2+ The lithium source comprises at least one of lithium hydroxide, lithium carbonate and lithium nitrate. Optionally, the soluble nickel salt, cobalt salt and manganese salt are each independently selected from at least one of the corresponding sulfate, nitrate and chloride.
[0015] In some embodiments, the reaction in step S1 is carried out at a constant temperature and stirring rate, the constant temperature is 50-60°C, the stirring rate is 800-1200rpm, the reaction time is 12-18h, and the pH value of the reaction system is 10-12; the aging time in step S2 is 8-12h.
[0016] In some embodiments, the mixed solution, the precipitant and the complexing agent are added dropwise independently, with a dropwise addition rate of 0.4-0.6 mL / min.
[0017] In some embodiments, the temperature of the first calcination is 500-600°C, the heating rate is 2.0-3.0°C / min, the time is 5-7h, and the oxygen concentration in the atmosphere is 99-100%. Optionally, the temperature of the first calcination is 550°C, the heating rate is 2.5°C / min, the time is 6h, and the oxygen concentration in the atmosphere is 99.9%.
[0018] In some of the embodiments, the temperature of the second calcination is 740-800° C., the time is 12-18 hours, the heating rate is 1-5° C. / min, and the oxygen concentration in the atmosphere is 99-100%.
[0019] In a second aspect of the present application, a ternary material is provided, wherein the composition of the ternary material is LiNi x Co y Mn 1-x-y , where 0.83≤x<0.98, 0<y<0.2.
[0020] The present application prepares NCM ternary materials with a preset stoichiometric ratio and a stable layered structure by using a coprecipitation and two-step calcination method. First, by setting the first calcination step, the precursor and lithium salt are preliminarily decomposed at a relatively low temperature, which not only removes impurities, but also alleviates the problem of rapid decomposition of lithium salt under high temperature conditions, so that the lithium salt can slowly and evenly enter the precursor and fully react with the precursor, reducing the Li + with Ni 2+ The mixing degree is guaranteed, thereby ensuring that the product has a preset stoichiometric ratio and a stable layered structure.
[0021] Furthermore, by adjusting the mixing ratio of the precursor and the lithium salt, the lithium salt is slightly excessive, which makes up for the Li + The active lithium content lost through volatilization ensures the lithium content in the ternary material.
[0022] Furthermore, by regulating the co-precipitation steps, a spherical precursor with uniform morphology is prepared, so that the prepared ternary material has a good morphology, effectively preventing the agglomeration of the ternary material and improving the dispersibility of the ternary material in the battery positive electrode slurry.
[0023] In addition, the first calcination of the present invention removes moisture from the precursor and lithium salt, reducing the moisture and CO 2 The possibility of reaction on the surface of the material is reduced, thereby reducing the LiOH, Li 2 CO 3 The amount of residual alkali generated is equal to that of the ternary material prepared in the present application, so the ternary material prepared in the present application can be directly used to manufacture secondary batteries, which simplifies the water washing steps in the traditional technology and improves the production efficiency of the secondary batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a scanning electron microscope image of a precursor prepared in one embodiment of the present application;
[0025] Figure 2 This is a scanning electron microscope image of a ternary material prepared in one embodiment of the present application;
[0026] Figure 3 XRD spectra of ternary materials prepared in different embodiments of the present application. DETAILED DESCRIPTION
[0027] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more related listed items. "More than" used herein includes two and more than two items. "Above a certain number" used herein should be understood as a certain number and a range greater than a certain number.
[0029] Traditional technology uses high-temperature solid-phase sintering to prepare NCM ternary materials, but this method is not well adapted to high-nickel NCM ternary materials (usually Ni 2+ The preparation process of materials with a total molar ratio of transition metal ions greater than 0.8 is due to the fact that the calcination temperature is too high, which exacerbates the Li + Volatilization may reduce the content of active lithium ions, thereby affecting the rate performance of the material. However, the ion diffusion rate in the solid phase is slow, and a sufficiently high calcination temperature is required to promote the diffusion of ions. Therefore, lowering the calcination temperature will also affect the electrochemical performance of the ternary material. Furthermore, as Ni 2+ With the increase of content, Li + and Ni 2+ The degree of mixing is significantly increased, and high temperature conditions may aggravate the mixing effect, so the structural stability of high-nickel NCM ternary materials prepared by traditional technology is poor. 2+ and Li + Mixed arrangement and Li + The volatilization of Li + The addition of transition metal ions to obtain a ternary material with a preset stoichiometric ratio increases the difficulty of production.
[0030] The high nickel ternary materials currently in mass production include LiNi 0.8 Co 0.1 Mn 0.1 O 2 (NCM811), while ternary materials with higher nickel content are still in the research and development stage. This is because as the nickel content increases, the specific capacity of the ternary material increases, but the stability decreases. Therefore, the comprehensive electrochemical performance of high-nickel ternary materials has not been significantly improved. In addition, there is a lot of residual alkali on the surface of high-nickel ternary materials, which need to be washed with water to remove the residual alkali before they can be used to manufacture batteries, which reduces production efficiency and increases manufacturing costs.
[0031] In order to overcome the above problems, one embodiment of the present application provides a method for preparing a ternary material, comprising the following steps:
[0032] Step S1: In a protective gas atmosphere, 2+ 、Co 2+ and Mn 2+ The mixed solution, the precipitant and the complexing agent are mixed and reacted;
[0033] Step S2, aging, standing, filtering, washing and drying the reaction product of step S1 in sequence to prepare a precursor;
[0034] Step S3, mixing the precursor with the lithium salt, placing the mixture in an oxygen-containing atmosphere for a first calcination, and cooling the mixture after the calcination to prepare a pre-sintered material;
[0035] Step S4, placing the pre-sintered material in an oxygen-containing atmosphere for a second calcination to prepare a ternary material containing Ni, Co and Mn, and the temperature of the second calcination is higher than the temperature of the first calcination.
[0036] A spherical precursor was obtained by coprecipitation (specifically corresponding to step S1 and step S2). In step S1, Ni 2+ 、Co 2+ and Mn 2+ The mixing method may be stirring or other methods, which are not limited in this application. 2+ 、Co 2+ and Mn 2+ It can be completely precipitated by coprecipitation reaction, so a precursor substantially consistent with the above ratio can be obtained by regulating the molar ratio of transition metal ions in the raw materials. Transition metal ions are precipitated under the action of a precipitant to obtain a uniform precipitation of various components, and the complexing agent can promote the slow accumulation of transition metal ions on the precipitation surface, control the growth rate and morphology of the precursor particles, and then form a spherical precursor. The aging step in step S2 can promote the growth of precipitated particles and ensure the size of the precursor particles. The coprecipitation method for preparing a precursor has the advantages of simple process, low cost, easy control of preparation conditions, and uniform components in the product.
[0037] In step S3, the precursor and the lithium salt are firstly mixed uniformly in proportion, and then placed in an oxygen atmosphere for the first calcination (i.e., pre-calcination). At this time, the impurities in the raw materials are decomposed by heat and removed from the system, and the precursor and the lithium salt are decomposed into corresponding oxides and undergo a preliminary reaction. Specifically, the first calcination process includes the following three stages: the first stage (less than 250°C) is the decomposition stage of impurities such as water in the system, the second stage (250°C to 450°C) is the decomposition of the precursor into transition metal oxides and the decomposition of the lithium salt into Li 2 O stage, the third stage (450℃~600℃) is the transition metal oxide and Li 2O reacts under the action of oxygen to form a pre-sintered material. The main component of the pre-sintered material includes lithium nickel cobalt manganese oxide, but due to the slightly low calcination temperature, the metal ions in the pre-sintered material are not fully diffused, so it does not have an ideal layered structure. During the second calcination process in step S4, the metal ions in the pre-sintered material are heated, the movement speed is accelerated and migrate to the corresponding position, such as Li + Migrate to the interlayer space of the material, Ni 2+ Migrate to the main body of the layered structure, thereby obtaining a layered ternary material with a stable structure and low degree of cation mixing.
[0038] The NCM ternary material with a preset stoichiometric content and a stable layered structure was prepared by co-precipitation and two-step calcination. First, by setting the first calcination step, the precursor and lithium salt were preliminarily decomposed at a relatively low temperature, which not only removed impurities but also alleviated the problem of rapid decomposition of lithium salt under high temperature conditions, allowing the molten lithium salt to slowly and evenly enter the precursor and fully react with the precursor, reducing the Li + with Ni 2+ The mixing degree of the precursor and the lithium salt is adjusted to ensure that the product has a preset stoichiometric ratio and a stable layered structure. Furthermore, by adjusting the mixing ratio of the precursor and the lithium salt, the lithium salt is slightly excessive, which makes up for the Li + The content of active lithium lost by volatilization ensures the lithium content in the ternary material. Furthermore, by regulating the coprecipitation step, a spherical precursor with uniform morphology is prepared, so that the prepared ternary material has a good morphology, effectively preventing the agglomeration of the ternary material and improving the dispersibility of the ternary material in the battery positive electrode slurry. In addition, the first calcination of the present application removes the moisture in the precursor and lithium salt, reducing the moisture and CO 2 The possibility of reaction on the surface of the material is reduced, thereby reducing the LiOH, Li 2 CO 3 The amount of residual alkali generated is equal to that of the ternary material prepared in the present application, so the ternary material prepared in the present application can be directly used to manufacture secondary batteries, which simplifies the water washing steps in the traditional technology and improves the production efficiency of the secondary batteries.
[0039] In a specific embodiment, the molar ratio of the precursor to the lithium element in the lithium salt is 1:(1.01-1.1). Specifically, the molar ratio of the precursor to the lithium element in the lithium salt can be 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09 or 1:1. Optionally, the molar ratio of the precursor to the lithium element in the lithium salt is 1:1.05. When the molar ratio of the precursor to the lithium element in the lithium salt is less than 1:1.01, due to Li +The volatilization of lithium will lead to too low active lithium content in the product, thus reducing the specific capacity of NCM ternary materials. When the molar ratio of lithium element in the precursor and lithium salt is greater than 1:1.1, the degree of mixing in NCM ternary materials may be aggravated, and excessive Li will also cause waste of raw materials and increase unnecessary production costs.
[0040] In a specific embodiment, the precipitant and the complexing agent are both provided in the form of an alkaline solution. Optionally, the precipitant is an aqueous sodium hydroxide solution, and the complexing agent is an aqueous ammonia solution. The addition of an aqueous sodium hydroxide solution can increase the pH value of the reaction system and promote the transition metal ions to form hydroxide precursors. Ammonia water can ensure uniform precipitation of transition metal ions, and as much as possible, each component is precipitated in proportion at the same time to prevent agglomeration or uneven composition caused by excessive concentration of the reaction solution.
[0041] In a specific embodiment, the mixed solution is Ni 2+ 、Co 2+ and Mn 2+ The total concentration of the mixed solution is 1.5-2.5 mol / L, the precipitant is 0.2-0.3 mol / L sodium hydroxide aqueous solution, and the complexing agent is 3-5 mol / L ammonia aqueous solution. 2+ 、Co 2+ and Mn 2+ The total concentration can be 1.5mol / L, 1.6mol / L, 1.7mol / L, 1.8mol / L, 1.9mol / L, 2.0mol / L, 2.1mol / L, 2.2mol / L, 2.3mol / L, 2.4mol / L or 2.5mol / L, and the precipitant can be 0.2mol / L, 0.21mol / L, 0.22mol / L, 0.23mol / L, 0.24mol / L, 0.25mol / L The precipitant and the complexing agent may be 3mol / L, 3.2mol / L, 3.4mol / L, 3.6mol / L, 3.8mol / L, 4mol / L, 4.2mol / L, 4.4mol / L, 4.6mol / L, 4.8mol / L or 5mol / L of aqueous sodium hydroxide solution. When the concentrations of the precipitant and the complexing agent are within the above ranges, the complete precipitation of the transition metal ions in the system can be ensured, and the precursor has a spherical morphology, thereby preventing the precursor from being significantly agglomerated.
[0042] In a specific embodiment, Ni in the mixed solution 2+ 、Co 2+ and Mn 2+The molar ratio is x:y:(1-xy), wherein 0.83≤x<0.98, 0<y<0.2. Specifically, x can be 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.89, 0.90, 0.91, 0.92, 0.93, 0.94, 0.945, 0.95, 0.96, 0.97 or 0.98, and y can be 0.01, 0.03, 0.05, 0.07, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19 or 0.195.
[0043] In a specific embodiment, Ni 2+ 、Co 2+ and Mn 2+ The nickel salt is provided by soluble nickel salt, cobalt salt and manganese salt respectively. Optionally, the soluble nickel salt, cobalt salt and manganese salt are each independently selected from at least one of the corresponding sulfate, nitrate and chloride. Further optionally, the nickel salt is NiSO 4 6H 2 O, cobalt salt is CoSO 4 7H 2 O, manganese salt is MnSO 4 ·H 2 O. The production cost is reduced by selecting conventional nickel salts, cobalt salts and manganese salts.
[0044] In a specific embodiment, the lithium source includes at least one of lithium hydroxide, lithium carbonate and lithium nitrate. Optionally, the lithium source is LiOH·H 2 O. Since the melting point of lithium hydroxide is about 471°C, it can form a molten state during the first calcination process, and then can be more evenly mixed with the precursor, reducing the amount of lithium residue on the surface of the material and improving the specific capacity of the material.
[0045] In a specific embodiment, the reaction in step S1 is carried out at a constant temperature and stirring rate, the constant temperature is 50-60°C, the stirring rate is 800-1200rpm, the reaction time is 12-18h, and the pH value of the reaction system is 10-12. The aging time in step S2 is 8-12h. Specifically, the constant temperature can be 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C or 60°C, the stirring rate can be 800rpm, 850rpm, 900rpm, 950rpm, 1000rpm, 1050rpm, 1100rpm, 1150rpm or 1200rpm, the reaction time can be 12h, 13h, 14h, 15h, 16h, 17h or 18h, and the pH value of the reaction system can be 10, 10.5, 11, 11.5, 12. The aging time in step S2 can be 8h, 8.5h, 9h, 9.5h, 10h, 10.5h, 11h, 11.5h or 12h. By regulating the reaction temperature, stirring rate, reaction time of step S1, the pH value of the reaction system and the aging time of step S2, a spherical precursor with uniform size is obtained. It should be noted that before step S1, a step of adding a reaction base liquid can be included, and the base liquid can be deionized water, and a base is added to the above-mentioned deionized water to adjust the pH value to between 10 and 12.
[0046] In a specific embodiment, the mixed solution, the precipitant and the complexing agent are added dropwise respectively, and the dropwise acceleration rate is 0.4 to 0.6 mL / min. Specifically, the dropwise acceleration rate can be 0.4 mL / min, 0.42 mL / min, 0.44 mL / min, 0.46 mL / min, 0.48 mL / min, 0.5 mL / min, 0.52 mL / min, 0.54 mL / min, 0.56 mL / min, 0.58 mL / min or 0.6 mL / min. It should be noted that the mixed solution, the precipitant and the complexing agent are added dropwise to the bottom solution at the same time. The uniform growth of the precursor is ensured by regulating the dropwise acceleration rate.
[0047] In a specific embodiment, the temperature of the first calcination is 500-600° C., the heating rate is 2.0-3.0° C. / min, the time is 5-7 hours, and the oxygen concentration in the atmosphere is 99-100%. Specifically, the temperature of the first calcination can be 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C, the heating rate can be 2.0°C / min, 2.1°C / min, 2.2°C / min, 2.3°C / min, 2.4°C / min, 2.5°C / min, 2.6°C / min, 2.7°C / min, 2.8°C / min, 2.9°C / min or 3.0°C / min, the time can be 5h, 5.5h, 6h, 6.5h or 7h, and the oxygen concentration can be 99%, 99.1%, 99.2%, 99.3%, 99.4%, 99.5%, 99.6%, 99.7%, 99.8%, 99.9% or 100%. Optionally, the temperature of the first calcination is 550°C, the heating rate is 2.5°C / min, the time is 6h, and the oxygen concentration in the atmosphere is 99.9%. By regulating the temperature, heating rate, time and oxygen concentration of the first calcination, impurities in the raw materials can be effectively removed, the decomposition of the precursor and the lithium salt can be promoted, and the generated transition metal oxide is conducive to the full reaction with the molten lithium salt to obtain a pre-sintered material that meets the preset stoichiometric ratio. In addition, since the first calcination removes moisture from the system and reduces the amount of residual alkali on the surface of the material, the subsequent washing step is simplified and the production efficiency is improved.
[0048] In a specific embodiment, the temperature of the second calcination is 740-800°C, the time is 12-18h, the heating rate is 1-5°C / min, and the oxygen concentration in the atmosphere is 99-100%. Specifically, the temperature of the second calcination can be 740°C, 750°C, 760°C, 770°C, 780°C, 790°C or 800°C, the time can be 12h, 13h, 14h, 15h, 16h, 17h or 18h, the heating rate can be 1°C / min, 2°C / min, 3°C / min, 4°C / min or 5°C / min, and the oxygen concentration can be 99%, 99.1%, 99.2%, 99.3%, 99.4%, 99.5%, 99.6%, 99.7%, 99.8%, 99.9% or 100%. By adjusting the temperature, heating rate, time and oxygen concentration of the second calcination, the metal ions in the pre-sintered material can be fully diffused to obtain a ternary material with an ideal layered structure. And because the temperature of the second calcination is lower than the calcination temperature of the traditional high-temperature curing method, the degree of lithium-nickel mixing in the ternary material is reduced, and the structural stability of the material is improved.
[0049] Furthermore, one embodiment of the present application provides a ternary material prepared according to the preparation method described above, wherein the composition of the ternary material is LiNi x Co y Mn 1-x-y , where 0.83≤x<0.98, 0<y<0.2.
[0050] In order to make it easier to understand and implement the present application, the following more specific and detailed embodiments and comparative examples which are easier to implement are provided as references. Through the description and performance results of the following specific embodiments and comparative examples, the embodiments of the present application and their advantages will also be apparent.
[0051] Unless otherwise specified, the raw materials used in the following test examples can be purchased from the market.
[0052] Example 1
[0053] (1) Preparation of precursor
[0054] Dissolve the sulfates of Ni, Co, and Mn in a certain volume of distilled water at a molar ratio of 0.95:0.03:0.02, with a molar concentration of 2 mol / L; prepare a 4 mol / L sodium hydroxide solution as a precipitant; prepare a certain molar concentration of ammonia water as a complexing agent, and conduct a coprecipitation experiment in a constant temperature water bath of 50-60°C. Add a small amount of base liquid to a four-necked flask, add an appropriate amount of ammonia water and stir, keep the pH value of the base liquid between 10 and 12, add nitrogen to the base liquid, and exhaust the air in the four-necked flask. Use a peristaltic pump to drop the transition metal salt solution, sodium hydroxide solution, and ammonia water into the four-necked flask at a certain feed rate, and stir vigorously at a certain speed throughout the reaction. After the solution is added, keep the four-necked flask sealed, and continue to stir at a certain speed to complete the reaction and grow the particles. Let it stand after the end. After the addition is completed, the stirring speed is maintained at a constant level. The total reaction time is 12 to 18 hours. After the reaction is completed, the mixture is aged, allowed to stand for 24 hours, filtered, washed, and dried to obtain the precursor Ni 0.95 Co 0.03 Mn 0.02 (OH) 2 .
[0055] (2) Preparation of pre-sintering materials
[0056] The precursor prepared in (1) was mixed with LiOH·H 2 O was mixed at a molar ratio of 1:1.05, and the first calcination was carried out at 550°C, the heating rate was 2.5°C / min, the calcination time was 6h, and the oxygen concentration in the calcination atmosphere was 99.9%. After the first calcination was completed, the sample was cooled to room temperature to obtain a pre-sintered material.
[0057] (3) Preparation of ternary materials
[0058] The pre-sintered material prepared in (2) was calcined for the second time at 740°C, with a heating rate of 2.5°C / min, a calcination time of 12h, and an oxygen concentration of 99.9% in the calcination atmosphere. After the second calcination, the sample was cooled to room temperature and post-treated to obtain a ternary material.
[0059] Example 2
[0060] It is basically the same as Example 1, except that the temperature of the second calcination in (3) is 760°C.
[0061] Example 3
[0062] It is basically the same as Example 1, except that the temperature of the second calcination in (3) is 780°C.
[0063] Example 4
[0064] The method is basically the same as Example 1, except that the temperature of the second calcination in (3) is 800°C.
[0065] Comparative Example 1
[0066] The ternary material was prepared by a conventional method, and the specific steps were basically the same as those in Example 1, except that the precursor obtained in (1) was directly reacted with LiOH·H 2 O was mixed in a substance ratio of 1:1, and then directly calcined at 740°C for 15 hours, with an oxygen concentration of 99% in the calcination atmosphere. The sample was cooled to room temperature and post-treated to obtain a ternary material.
[0067] Comparative Example 2
[0068] The same as Example 1, except that the precursor obtained in (1) was mixed with LiOH·H 2 O are mixed at a molar ratio of 1:1.05, and then calcined according to the step (3).
[0069] Comparative Example 3
[0070] The same as Example 1, except that: in (2), the precursor and LiOH·H 2 The molar ratio of O is 1:1.
[0071] Performance Testing
[0072] (1) XRD test
[0073] XRD tests were performed on Examples 1 to 4 and Comparative Examples 1 to 3 using (Bruker axs D8-Focus). Figure 1is the XRD spectra of Examples 1 to 4, Figure 1 It can be seen that all examples have hexagonal layered structures and good crystallinity. The intensity ratio of the (003) diffraction peak to the (104) diffraction peak of each sample is shown in Table 1. Generally, when the ratio of I(003) / I(104) is larger, it can be considered that Li + with Ni 2+ The lower the degree of mixing.
[0074] (2) Element content test
[0075] The actual molar content of metal elements in Examples 1 to 4 and Comparative Examples 1 to 3 was tested by ICP. The test results are shown in Table 1.
[0076] Test example
[0077] A button cell was prepared using the ternary materials of Examples 1 to 4 and Comparative Examples 1 to 3. Specifically, the above-mentioned ternary material, acetylene black (conductive agent), and polyvinylidene fluoride (binder) were added to the solvent N-methylpyrrolidone at a molar mass ratio of 95:3:2, and mixed evenly to obtain a positive electrode slurry. The above-mentioned slurry was then coated on an aluminum foil and dried in a vacuum drying oven at 80°C for 20 hours to obtain a positive electrode sheet. The positive electrode sheet was then cut into positive electrode discs with a diameter of 12 mm, and the above-mentioned positive electrode discs, isolation membranes, and negative lithium sheets were assembled into a button cell in a glove box, and 1 mol / L of electrolyte (composed of a mixed solution of EC and DEC in a mass ratio of 1:1) was injected. After standing for 12 hours, the above-mentioned button cell was subjected to the first charge and discharge and cycle performance tests using a blue electric test system, and the specific test conditions were as follows.
[0078] (3) First charge and discharge test
[0079] The charge and discharge tests were carried out at room temperature with a voltage range of 2.8 to 4.3 V and a current density of 0.33C.
[0080] (4) Cyclic performance test
[0081] The button cell was charged to 4.3V at a constant current density of 0.5C and then discharged to 2.5V for one cycle. The capacity of the battery was tested after 50 cycles.
[0082] Table 1
[0083]
[0084] As shown in Table 1, the I(003) / I(104) of Examples 1 to 4 are all higher than those of the comparative example, indicating that the Li + with Ni 2 +The degree of mixing is lower than that of the comparative example. From the battery performance test data, it can be seen that the specific capacity and capacity retention rate of each embodiment are higher than those of the comparative example. Among them, the I(003) / I(104) of Example 3 is the largest, and its layered structure Li + with Ni 2+ The mixing degree is the lowest, the first discharge specific capacity is the highest, and the capacity retention rate after 50 cycles is the highest. In addition, the measured element content of the ternary materials obtained in each embodiment is basically consistent with the molar ratio of the raw materials, that is, the chemical composition of the ternary materials obtained in each embodiment is basically consistent with LiNi 0.95 Co 0.03 Mn 0.02 O 2 .
[0085] From the comparison between Comparative Example 2 and Example 1, it can be seen that the present invention obtains a large I(003) / I(104) and Li + with Ni 2+ The ternary material with a low mixing degree can improve the specific capacity and capacity retention rate of the material. From the comparison between Comparative Example 3 and Example 1, it can be seen that the present application obtains a ternary material with a high active lithium content by adjusting the molar ratio of the precursor to the lithium salt, thereby improving the specific capacity of the ternary material. In addition, Comparative Example 1 is a ternary material obtained by a traditional method. From the test results, it can be seen that its Li + with Ni 2+ The degree of mixing is the highest, and both the specific capacity and capacity retention rate are poor.
[0086] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0087] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the description and drawings may be used to interpret the contents of the claims.
Claims
1. A method for preparing a ternary material, characterized in that: The following steps are involved: Step S1: In a protective gas atmosphere, 2+ 、Co 2+ and Mn 2+ The mixed solution, the precipitant and the complexing agent are mixed and reacted; the precipitant and the complexing agent are provided in the form of alkaline solutions, and the mixed solution, the precipitant and the complexing agent are added dropwise independently; Ni in the mixed solution 2+ 、Co 2+ and Mn 2+ The molar ratio is x: y: (1-xy), where 0.90≤x<0.98, 0<y<0.1; Step S2, aging, standing, filtering, washing and drying the reaction product of step S1 in sequence to prepare a precursor; Step S3, mixing the precursor with a lithium source, placing the mixture in an oxygen-containing atmosphere for a first calcination, and cooling the mixture after the calcination to prepare a pre-sintered material; the molar ratio of the precursor to the lithium element in the lithium source is 1:(1.01-1.1); Step S4, placing the pre-sintered material in an oxygen-containing atmosphere for a second calcination to prepare a ternary material containing Ni, Co and Mn, wherein the temperature of the second calcination is higher than the temperature of the first calcination; The temperature of the first calcination is 550°C, the heating rate is 2.5min, the time is 6h, and the oxygen concentration in the atmosphere is 99.9%; the temperature of the second calcination is 780°C~800°C, the time is 12h~18h; the heating rate of the second calcination is 1~5°C / min, and the oxygen concentration in the atmosphere is 99~100%.
2. The method for preparing the ternary material according to claim 1, characterized in that: The molar ratio of the precursor to the lithium element in the lithium source is 1:1.
05.
3. The method for preparing the ternary material according to claim 1 or 2, characterized in that: The precipitant is a sodium hydroxide aqueous solution, and the complexing agent is an ammonia aqueous solution.
4. The method for preparing the ternary material according to claim 1 or 2, characterized in that: The mixed solution is Ni 2+ 、Co 2+ and Mn 2+ The total concentration of the aqueous solution is 1.5-2.5 mol / L, the precipitant is 0.2-0.3 mol / L sodium hydroxide aqueous solution, and the complexing agent is 3-5 mol / L ammonia aqueous solution.
5. The method for preparing the ternary material according to claim 1 or 2, characterized in that: The Ni 2+ 、Co 2+ and Mn 2+ The lithium source is provided by soluble nickel salt, cobalt salt and manganese salt respectively, and the lithium source includes at least one of lithium hydroxide, lithium carbonate and lithium nitrate.
6. The method for preparing the ternary material according to claim 5, characterized in that: The soluble nickel salt, cobalt salt and manganese salt are each independently selected from at least one of the corresponding sulfates, sulfate hydrates, nitrates, nitrate hydrates, chlorides and chloride hydrates.
7. The method for preparing the ternary material according to claim 1 or 2, characterized in that: The reaction in step S1 is carried out at a constant temperature and stirring rate, wherein the constant temperature is 50-60° C., the stirring rate is 800-1200 rpm, the reaction time is 12-18 h, and the pH value of the reaction system is 10-12.
8. The method for preparing the ternary material according to claim 1 or 2, characterized in that: The aging time in step S2 is 8 to 12 hours.
9. The method for preparing the ternary material according to claim 1 or 2, characterized in that: The dropping rate is 0.4-0.6 mL / min.
10. A ternary material, characterized in that: The ternary material is prepared by the preparation method according to any one of claims 1 to 9, and the composition of the ternary material is LiNi x Co y Mn 1-x-y , where 0.83≤x<0.98, 0<y<0.2.