Electrode sheet and preparation method thereof, secondary battery, battery module, battery pack and power-consuming device

By adopting a composite structure of a porous current collector and a porous separator layer and a lithium source layer in the electrode plate, the problem of lithium ion consumption by the SEI film is solved, the battery performance and life are improved, and the processing of the electrode plate is kept simple. sex and compatibility.

CN115832208BActive Publication Date: 2024-10-11CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210800855.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-08
Publication Date
2024-10-11
Estimated Expiration
2042-07-08

AI Technical Summary

Technical Problem

During the first charge and discharge process of existing liquid lithium-ion batteries, the passivation film (SEI film) formed at the solid-liquid interface between the electrode material and the electrolyte causes lithium ion consumption, reducing the charge-discharge efficiency and cycle performance of the electrode material. Moreover, traditional lithium replenishment technology requires complex changes to the pole piece structure, which increases production costs and has limited improvement in battery life.

Method used

An electrode pole piece is designed, which adopts a stacked porous current collector structure, including an electrode active material filled in the porous current collector and a lithium supplement layer composed of a porous separator layer and a lithium source layer. The lithium source is stably released through the porous separator layer. , achieve long-term lithium replenishment, avoid the negative impact of SEI film formation on battery performance and life, and keep the structure simple in pole piece processing.

Benefits of technology

It achieves a significant improvement in battery performance and lifespan, avoids the adverse effects of the SEI film on battery performance and lifespan, and maintains the simplicity of pole piece processing and the compatibility of previous processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115832208B_ABST
    Figure CN115832208B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of secondary batteries, and in particular to an electrode plate and a preparation method thereof, a secondary battery, a battery module, a battery pack and an electrical device. The electrode plate includes a first active layer, a lithium supplement layer and a second active layer which are stacked; the first active layer and the second active layer include a porous current collector and an electrode active material filled in the porous current collector; the lithium supplement layer includes a first diaphragm layer, a lithium source layer and a second diaphragm layer which are stacked; the first diaphragm layer and the second diaphragm layer have a porous structure. By using a porous diaphragm layer and a lithium source layer to form a lithium supplement layer, the lithium source can be stably released at a certain rate through the pores of the diaphragm layer, so as to achieve long-term lithium supplementation and avoid the adverse effects of the formation of SEI film on battery performance and life. Moreover, the structure of the electrode plate is not complicatedly changed due to the introduction of the lithium supplement layer, and the electrode plate processing can use the previous processes and equipment, providing a electrode plate with a simple structure and significantly improved life and performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to an electrode plate and a preparation method thereof, a secondary battery, a battery module, a battery pack and an electrical device. Background Art

[0002] During the first charge and discharge process of liquid lithium-ion batteries, the electrode material and the electrolyte react at the solid-liquid interface to form a passivation film covering the surface of the electrode material. This passivation film is called the "solid electrolyte interface", or SEI film for short. The formation of the SEI film consumes some lithium ions, increasing the irreversible capacity of the first charge and discharge, and reducing the charge and discharge efficiency and cycle performance of the electrode material. Therefore, in order to avoid the negative impact of the formation of the SEI film on battery performance and life, it is often necessary to supplement the electrode with lithium. Summary of the invention

[0003] Based on this, it is necessary to provide an electrode plate with self-lithium replenishment function and its preparation method, secondary battery, battery module, battery pack and electrical device.

[0004] In a first aspect of the present application, an electrode plate is provided, which includes a first active layer, a lithium supplement layer, and a second active layer stacked in layers;

[0005] The first active layer and the second active layer include a porous current collector and an electrode active material filled in the porous current collector;

[0006] The lithium supplement layer comprises a first diaphragm layer, a lithium source layer and a second diaphragm layer which are stacked; the first diaphragm layer and the second diaphragm layer have a porous structure.

[0007] By using a porous diaphragm layer and a lithium source layer to form a lithium replenishment layer, the lithium source can be stably released at a certain rate through the pores of the diaphragm layer, thereby achieving long-term lithium replenishment and avoiding the adverse effects of the formation of the SEI film on battery performance and life. At the same time, by filling the electrode active material in the porous current collector to form an active layer located on both sides of the lithium replenishment layer, the interconnection between the lithium replenishment agent and the electrode active material, and the interconnection between the electrode active material and the electrolyte can be met. The structure of the pole piece is not complicatedly changed due to the introduction of the lithium replenishment layer. The previous process and equipment can be used in the processing of the pole piece, providing a pole piece with a simple structure and significantly improved life and performance.

[0008] In some embodiments, the porous current collector has a porosity of 78% to 92%, a pore density of 40 PPI to 110 PPI, and a pore size of 500 nm to 3 μm. The porosity, pore density, and pore size are related to the migration speed of active lithium, thereby affecting the lithium replenishment rate. Appropriate parameters can make the migration speed of active lithium moderate, avoid the local accumulation of lithium due to too slow a speed, and avoid the collapse caused by the collapse of the structure due to the excessive release of active lithium from the lithium replenishment layer.

[0009] In some embodiments, the minimum distance between the outer contour edge of the orthographic projection of the lithium source layer on the first diaphragm layer and the outer contour edge of the first diaphragm layer is 0.7 mm to 0.9 mm, and the maximum distance is 1.1 mm to 1.3 mm. By controlling the distance between the edge of the lithium source layer and the edge of the first diaphragm layer, lithium deposition on the side can be avoided.

[0010] In some embodiments, the thickness of the lithium source layer is ≤3 μm. Controlling the thickness of the lithium source layer within a suitable range can avoid adverse effects on the transmission of active materials in the upper and lower layers while meeting the lithium replenishment requirements, and avoid excessive collapse of the pole piece after lithium replenishment.

[0011] In some embodiments, the mass of the lithium source in the lithium source layer is 1% to 5% of the mass of the electrode active material. The amount of the lithium source is controlled within a suitable range, while meeting the basic lithium replenishment requirements of the battery, the proportion of active materials will not be reduced too much, and the reduction of the battery volume capacity is avoided.

[0012] In some embodiments, the materials of the first diaphragm layer and the second diaphragm layer are independently selected from one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride and carbon fiber. The suitable material not only makes the diaphragm layer have a certain mechanical strength to avoid the obvious collapse of the pole piece after the lithium replenishment is completed, but also has good high temperature resistance, especially local high temperature resistance, to avoid the pole piece overheating during lithium replenishment and cause the diaphragm to be damaged.

[0013] In some embodiments, the first diaphragm layer and the second diaphragm layer independently have one or more of the following features:

[0014] (1) Porosity is 60% to 90%;

[0015] (2) The pore diameter is 10nm~50nm.

[0016] The porosity and pore size of the diaphragm layer also directly affect the lithium replenishment rate. Appropriate porosity and pore size are important prerequisites for the electrode to have a suitable lithium replenishment rate.

[0017] In some embodiments, the thickness of the first diaphragm layer and the second diaphragm layer are independently 1 μm to 7 μm. The thickness of the diaphragm layer also affects the transmission rate of active lithium to a certain extent, and at the same time, provides a certain mechanical strength to avoid obvious collapse of the electrode after lithium replenishment.

[0018] In some embodiments, the electrode plate is a positive electrode plate, and the pore sizes of the first diaphragm layer and the second diaphragm layer are independently 10nm to 30nm. Since the oxidation voltage on the positive electrode side is relatively high, the lithium replenishing material is easy to release active lithium, and setting the pore size smaller is conducive to controlling the lithium replenishing rate.

[0019] When the electrode plate is a positive electrode plate:

[0020] In some embodiments, the lithium source in the lithium source layer includes Li 1+x Ni 0.5 Mn 1.5 O4, Li2NiO2, Li5FeO4, LiF, Li2S, Li2C2O4, LiMn2O4; one or more of Li2O2, Li2O and Li3N; wherein x is selected from any value between 0 and 1.

[0021] In some embodiments, the compaction density of the electrode plate is 3.3 g / cm 3 ~3.5g / cm 3 .

[0022] In some embodiments, the electrode plate is pressed by a secondary calendering process, and the compaction density of the electrode plate during the first pressing is 3.0 g / cm 3 ~3.3g / cm 3 The compaction density of the electrode sheet during the second pressing is 3.3g / cm 3 ~3.5g / cm 3 . The secondary calendering process makes the area close to the lithium replenishment layer (inner layer) have a relatively small compaction density and a relatively large pore size; the area far from the lithium replenishment layer (outer layer, that is, the side that preferentially contacts the electrolyte) has a relatively large compaction density and a relatively small pore size. This is because: the active lithium in the inner layer has a long transmission distance, and it is necessary to increase the appropriate pore size to accelerate its migration; the outer layer has a short transmission distance, and by increasing the compaction, not only more active substances can be filled, but also the pores can be uniform, so that the active lithium released by the lithium replenishment material is released slowly. Therefore, the use of the secondary calendering process can make the electrode have better performance.

[0023] In some embodiments, the electrode plate is a negative electrode plate, and the pore sizes of the first diaphragm layer and the second diaphragm layer are independently 30nm to 50nm. The reduction voltage on the negative electrode side is low, and the lithium replenishment material is released slowly, so a larger pore size is required to increase the lithium replenishment rate to a more suitable range.

[0024] When the electrode plate is a negative electrode plate:

[0025] In some embodiments, the lithium source in the lithium source layer includes one or more of lithium foil, lithium powder, and pre-lithiated graphite.

[0026] In some embodiments, the compaction density of the electrode plate is 1.5 g / cm 3 ~1.7g / cm 3 .

[0027] In some embodiments, the electrode plate is pressed by a secondary calendering process, and the compaction density of the electrode plate during the first pressing is 1.3 g / cm 3 ~1.5g / cm 3 The compaction density of the electrode sheet during the second pressing is 1.5g / cm 3 ~1.7g / cm 3 .

[0028] In a second aspect of the present application, a method for preparing an electrode sheet according to one or more of the above embodiments is provided, which comprises the following steps:

[0029] Filling the electrode active material into the porous current collector to prepare the first active layer and the second active layer;

[0030] Compounding the first separator layer, the lithium source layer and the second separator layer to prepare the lithium replenishing layer;

[0031] The first active layer, the lithium supplement layer and the second active layer are compounded to prepare the electrode plate.

[0032] In some embodiments, the electrode active material is first mixed with a solvent to prepare an electrode slurry with a viscosity of 20000 mPa·s to 30000 mPa·s, and then filled into the porous current collector. By controlling the viscosity of the electrode slurry, the solution more suitable for the present application allows the electrode slurry to be more evenly filled into the pores of the current collector, avoiding the slurry being too thin to flow out of the through hole and excessively deposited in the lower layer, and also avoiding the slurry being too thick to be filled into the lower layer.

[0033] In some embodiments, after the electrode slurry is filled into the porous current collector, the porous current collector is cold pressed, and the thickness of the porous current collector after cold pressing is controlled to be reduced by 20% to 50% compared with that before cold pressing. Controlling the compression amount of the cold pressed pole piece can provide a certain buffer amount for the subsequent hot pressing of the pole piece, so that the hot pressing can be better performed.

[0034] In some embodiments, the first active layer, the lithium supplement layer and the second active layer are composited by hot pressing, and the hot pressing operation satisfies at least one of the following conditions:

[0035] (1) The hot pressing temperature is 80℃~120℃; the appropriate hot pressing temperature can prevent the diaphragm layer material from becoming soft or wrinkled, causing an uneven surface of the electrode, and at the same time, it will not cause the active layer and the lithium supplement layer to be loosely bonded, affecting the release of active lithium.

[0036] (2) After hot pressing, the thickness of the electrode plate is reduced by 50% to 60% compared with that before hot pressing; the appropriate hot pressing plate compression amount can make the sub-layers of the plate have better bonding force, and the plate has a suitable compaction density.

[0037] (3) After hot pressing, the coating weight CW of the electrode active material per unit area on one side is 100 mg / cm 2 ~150mg / cm 2 ; The appropriate coating amount after hot pressing makes the battery have better electrical performance.

[0038] In a third aspect of the present application, a secondary battery is provided, which includes the electrode plate described in one or more of the aforementioned embodiments.

[0039] In a fourth aspect of the present application, a battery module is provided, which includes the aforementioned secondary battery.

[0040] In a fifth aspect of the present application, a battery pack is provided, which includes the aforementioned battery module.

[0041] In a sixth aspect of the present application, there is provided an electrical device comprising one or more of the aforementioned secondary battery, battery module and battery pack. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 is a schematic diagram of a secondary battery according to one embodiment of the present application.

[0043] Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of the present application is shown.

[0044] Figure 3 is a schematic diagram of a battery module according to an embodiment of the present application.

[0045] Figure 4 It is a schematic diagram of a battery pack according to one embodiment of the present application.

[0046] Figure 5 yes Figure 4 An exploded view of a battery pack according to an embodiment of the present application is shown.

[0047] Figure 6 FIG. 1 is a schematic diagram of an electric device using a secondary battery according to an embodiment of the present application as a power source.

[0048] Description of reference numerals:

[0049] 1: battery pack; 2: upper box; 3: lower box; 4: battery module; 5: secondary battery; 51: shell; 52: electrode assembly; 53: cover plate. DETAILED DESCRIPTION

[0050] In order to facilitate the understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0051] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0053] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0054] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0055] The percentage contents involved in this application, unless otherwise specified, refer to mass percentage for solid-liquid mixing and solid-solid mixing, and refer to volume percentage for liquid-liquid mixing.

[0056] The percentage concentrations mentioned in this application, unless otherwise specified, refer to the final concentration, which refers to the percentage of the added component in the system after the addition of the component.

[0057] The temperature parameters in this application, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range of instrument control.

[0058] Due to the formation of SEI film, some lithium ions will be consumed, which will increase the irreversible capacity of the battery's first charge and discharge, and reduce the charge and discharge efficiency and cycle performance of the electrode material. In order to replenish these consumed lithium ions, the pole piece needs to be treated with lithium replenishment. However, in traditional technology, in order to achieve lithium replenishment, the pole piece structure often needs to be redesigned, which is quite different from the existing pole piece structure, and it is inconvenient to use existing processing equipment for processing, which greatly increases the production cost. In addition, traditional technology rarely involves the regulation of the lithium replenishment rate, and it is impossible to achieve long-term lithium replenishment, which has limited effect on improving the battery life.

[0059] Based on the above background, in a first aspect of the present application, an electrode plate is provided, which includes a first active layer, a lithium supplement layer, and a second active layer which are stacked;

[0060] The first active layer and the second active layer include a porous current collector and an electrode active material filled in the porous current collector;

[0061] The lithium supplement layer comprises a first diaphragm layer, a lithium source layer and a second diaphragm layer which are stacked; the first diaphragm layer and the second diaphragm layer have a porous structure.

[0062] By using a porous diaphragm layer and a lithium source layer to form a lithium replenishment layer, the lithium source can be stably released at a certain rate through the pores of the diaphragm layer, thereby achieving long-term lithium replenishment and avoiding the adverse effects of the formation of the SEI film on battery performance and life. At the same time, by filling the electrode active material in the porous current collector to form an active layer located on both sides of the lithium replenishment layer, the interconnection between the lithium replenishment agent and the electrode active material, and the interconnection between the electrode active material and the electrolyte can be met. The structure of the pole piece is not complicatedly changed due to the introduction of the lithium replenishment layer. The previous process and equipment can be used in the processing of the pole piece, providing a pole piece with a simple structure and significantly improved life and performance.

[0063] In some embodiments, a bonding layer may be provided between the first active layer and the lithium replenishing layer, and between the lithium replenishing layer and the second active layer, to increase the bonding strength of the layers and make the contact closer. The material of the bonding layer is preferably a currently known adhesive for pole pieces, such as polyvinylidene fluoride, styrene-butadiene rubber, etc.

[0064] In some embodiments, the porosity of the porous current collector is 78% to 92%, the pore density is 40PPI to 110PPI, and the pore size is 500nm to 3μm. Optionally, the porosity of the porous current collector can also be, for example, 80%, 82%, 84%, 86%, 88% or 90%; the pore density of the porous current collector can also be, for example, 50PPI, 60PPI, 70PPI, 80PPI, 90PPI or 100PPI; the pore size of the porous current collector can also be, for example, 750nm, 1μm, 1.25μm, 1.5μm, 1.75μm, 2μm, 2.25μm, 2.5μm or 2.75μm. The size of the porosity, pore density and pore size is related to the migration speed of active lithium, thereby affecting the lithium replenishment rate. Appropriate parameters can make the migration speed of active lithium moderate, avoiding the local accumulation of lithium and lithium precipitation caused by too slow a speed, and also avoiding the lithium replenishment layer releasing active lithium too quickly, resulting in structural instability and collapse.

[0065] In some embodiments, the minimum distance between the outer contour edge of the orthographic projection of the lithium source layer on the first diaphragm layer and the outer contour edge of the first diaphragm layer is 0.7mm to 0.9mm, and the maximum distance is 1.1mm to 1.3mm. Optionally, the minimum distance can also be 0.8mm, and the maximum distance can also be 1.2mm, for example. At this time, the value range of the distance between the orthographic projection contour of the lithium source layer on the first diaphragm layer and the contour of the first diaphragm layer is 0.8mm to 1.2mm, and the value of the distance can be 0.9mm, 1mm or 1.1mm. By controlling the edge of the lithium source layer to have a certain distance from the edge of the first diaphragm layer, lithium deposition on the side can be avoided.

[0066] It can be understood that when the lithium source layer and the first diaphragm layer are both rectangular and have parallel sides, the aforementioned distance of "the outer contour edge of the positive projection of the lithium source layer on the first diaphragm layer and the outer contour edge of the first diaphragm layer" refers to the vertical distance from a certain side of the lithium source layer to an edge of the first diaphragm layer that is parallel to and closest to the edge.

[0067] In some embodiments, the thickness of the lithium source layer is ≤3 μm. Optionally, the thickness of the lithium source layer may be, for example, ≤2.5 μm, ≤2 μm, ≤1.5 μm, ≤1 μm, or ≤0.5 μm. The thickness of the lithium source layer is controlled within a suitable range, while meeting the lithium replenishment requirements, it can avoid adverse effects on the transmission of active materials in the upper and lower layers, and avoid excessive collapse of the pole piece after the lithium replenishment is completed.

[0068] In some embodiments, the mass of the lithium source in the lithium source layer is 1% to 5% of the mass of the electrode active material. Optionally, the amount of the lithium source can also be, for example, 2%, 3% or 4%. The amount of the lithium source is controlled within a suitable range, while meeting the basic demand for lithium replenishment of the battery, the proportion of active materials will not be reduced too much, and the reduction of the volume capacity of the battery is avoided.

[0069] In some embodiments, the materials of the first diaphragm layer and the second diaphragm layer are independently selected from one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride and carbon fiber. The suitable material not only makes the diaphragm layer have a certain mechanical strength, which can prevent the pole piece from collapsing significantly after the lithium replenishment is completed, but also has good high temperature resistance, especially local high temperature resistance, to prevent the pole piece from overheating during lithium replenishment and causing damage to the diaphragm.

[0070] In some embodiments, the first diaphragm layer and the second diaphragm layer independently have one or more of the following features:

[0071] (1) The porosity is 60% to 90%; alternatively, the porosity may be, for example, 65%, 70%, 75%, 80% or 85%;

[0072] (2) The pore diameter is 10 nm to 50 nm; alternatively, the pore diameter may be 20 nm, 30 nm or 40 nm, for example.

[0073] The porosity and pore size of the diaphragm layer also directly affect the lithium replenishment rate. Appropriate porosity and pore size are important prerequisites for the electrode to have a suitable lithium replenishment rate.

[0074] In some embodiments, the thickness of the first diaphragm layer and the second diaphragm layer are independently 1 μm to 7 μm. Optionally, the thickness of the first diaphragm layer and the second diaphragm layer are independently 2 μm, 3 μm, 4 μm, 5 μm or 6 μm. The thickness of the diaphragm layer also affects the transmission rate of active lithium to a certain extent, and at the same time, provides a certain mechanical strength to avoid obvious collapse of the pole piece after the lithium replenishment is completed.

[0075] In some embodiments, the electrode plate is a positive electrode plate, and the pore sizes of the first diaphragm layer and the second diaphragm layer are independently 10nm to 30nm. Optionally, the pore sizes of the first diaphragm layer and the second diaphragm layer are independently 15nm, 20nm or 25nm. Since the oxidation voltage on the positive electrode side is high, the lithium replenishing material is easy to release active lithium, and setting the pore size smaller is conducive to controlling the lithium replenishing rate.

[0076] When the electrode plate is a positive electrode plate:

[0077] In some embodiments, the lithium source in the lithium source layer includes Li 1+x Ni 0.5 Mn 1.5 O4, Li2NiO2, Li5FeO4, LiF, Li2S, Li2C2O4, LiMn2O4; one or more of Li2O2, Li2O and Li3N; wherein x is selected from any value between 0 and 1, and optionally, x is 0, 0.5 or 1.

[0078] In some embodiments, the compaction density of the electrode sheet is 3.3 g / cm 3 ~3.5g / cm 3 Optionally, the compaction density of the electrode plate can also be, for example, 3.4 g / cm 3 .

[0079] In some embodiments, the electrode plate is pressed by a secondary calendering process, and the compaction density of the electrode plate during the first pressing is 3.0 g / cm 3 ~3.3g / cm 3 The compaction density of the electrode sheet during the second pressing is 3.3g / cm 3 ~3.5g / cm 3 . The secondary calendering process makes the area close to the lithium replenishment layer (inner layer) have a relatively small compaction density and a relatively large pore size; the area far from the lithium replenishment layer (outer layer, that is, the side that preferentially contacts the electrolyte) has a relatively large compaction density and a relatively small pore size. This is because: the active lithium in the inner layer has a long transmission distance, and it is necessary to increase the appropriate pore size to accelerate its migration; the outer layer has a short transmission distance, and by increasing the compaction, not only more active substances can be filled, but also the pores can be uniform, so that the active lithium released by the lithium replenishment material is released slowly. Therefore, the use of the secondary calendering process can make the electrode have better performance.

[0080] In some embodiments, the electrode plate is a negative electrode plate, and the pore sizes of the first diaphragm layer and the second diaphragm layer are independently 30nm to 50nm. The reduction voltage on the negative electrode side is low, and the lithium replenishment material is released slowly, so a larger pore size is required to increase the lithium replenishment rate to a more suitable range.

[0081] When the electrode plate is a negative electrode plate:

[0082] In some embodiments, the lithium source in the lithium source layer includes one or more of lithium foil, lithium powder, and pre-lithiated graphite.

[0083] In some embodiments, the compaction density of the electrode sheet is 1.5 g / cm 3 ~1.7g / cm 3 Optionally, the compaction density of the electrode plate may be, for example, 1.6 g / cm 3 .

[0084] In some embodiments, the electrode plate is pressed by a secondary calendering process, and the compaction density of the electrode plate during the first pressing is 1.3 g / cm 3 ~1.5g / cm 3 The compaction density of the electrode sheet during the second pressing is 1.5g / cm 3 ~1.7g / cm 3 .

[0085] In a second aspect of the present application, a method for preparing an electrode sheet according to one or more of the above embodiments is provided, which comprises the following steps:

[0086] Filling the electrode active material into the porous current collector to prepare a first active layer and a second active layer;

[0087] Compounding the first separator layer, the lithium source layer and the second separator layer to prepare a lithium supplement layer;

[0088] The first active layer, the lithium supplement layer and the second active layer are compounded to prepare an electrode plate.

[0089] In some embodiments, the electrode active material is first mixed with a solvent to form an electrode slurry with a viscosity of 20000mPa·s to 30000mPa·s, and then filled into the porous current collector. Optionally, the viscosity of the electrode slurry can also be, for example, 22000mPa·s, 24000mPa·s, 26000mPa·s or 28000mPa·s. By controlling the viscosity of the electrode slurry, the solution more suitable for the present application allows the electrode slurry to be more evenly filled into the pores of the current collector, avoiding the slurry from flowing out of the through hole when it is too thin, excessive deposition in the lower layer, and also avoiding the slurry from being too concentrated to be filled into the lower layer.

[0090] In some embodiments, after the electrode slurry is filled into the porous current collector, the porous current collector is cold pressed, and the thickness of the porous current collector after cold pressing is controlled to be reduced by 20% to 50% compared with that before cold pressing. Optionally, the thickness of the porous current collector after cold pressing is reduced by 30% or 40% compared with that before cold pressing. Controlling the compression amount of the cold pressed pole piece can provide a certain buffer amount for the subsequent hot pressing of the pole piece, so that hot pressing can be better performed.

[0091] In some embodiments, the first active layer, the lithium supplement layer and the second active layer are composited by hot pressing, and the hot pressing operation satisfies at least one of the following conditions:

[0092] (1) The hot pressing temperature is 80° C. to 120° C.; optionally, the hot pressing temperature may be 90° C., 100° C. or 110° C. The appropriate hot pressing temperature can prevent the diaphragm layer material from becoming soft or wrinkled, causing an uneven surface of the electrode, and at the same time, will not cause the active layer and the lithium supplement layer to be loosely bonded, affecting the release of active lithium.

[0093] (2) The thickness of the electrode plate after hot pressing is reduced by 50% to 60% compared with that before hot pressing; optionally, the thickness of the electrode plate after hot pressing is reduced by 55% compared with that before hot pressing. Appropriate hot pressing plate compression can provide better bonding between the sub-layers of the plate, and the plate has a suitable compaction density.

[0094] (3) The coating weight CW of the electrode active material per unit area on one side after hot pressing is 100 mg / cm 2 ~150mg / cm 2 Optionally, the coating weight CW after hot pressing can also be 110 mg / cm 2 、120mg / cm 2 、130mg / cm 2 or 140mg / cm 2 The appropriate coating amount after hot pressing makes the battery have better electrical performance.

[0095] In a third aspect of the present application, a secondary battery is provided, which includes an electrode plate according to one or more of the aforementioned embodiments.

[0096] In a fourth aspect of the present application, a battery module is provided, which includes the aforementioned secondary battery.

[0097] In a fifth aspect of the present application, a battery pack is provided, which includes the aforementioned battery module.

[0098] In a sixth aspect of the present application, there is provided an electrical device comprising one or more of the aforementioned secondary battery, battery module and battery pack.

[0099] In addition, the secondary battery, battery module, battery pack, and electric device of the present application will be described below with reference to the drawings as appropriate.

[0100] In one embodiment of the present application, a secondary battery is provided.

[0101] Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.

[0102] At least one of the positive electrode sheet and the negative electrode sheet of the secondary battery provided in the present application is the electrode sheet with lithium supplementation function provided in the first aspect of the present application. For example, the positive electrode sheet adopts the electrode sheet provided in the first aspect of the present application, and the negative electrode sheet adopts the conventional negative electrode sheet, or the negative electrode sheet adopts the electrode sheet provided in the first aspect of the present application, and the positive electrode sheet adopts the conventional positive electrode sheet. The structure, material, etc. of the conventional positive electrode sheet or negative electrode sheet are as follows:

[0103] Positive electrode

[0104] The positive electrode plate includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes the positive electrode active material of the first aspect of the present application.

[0105] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0106] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0107] In some embodiments, the positive electrode active material may adopt a positive electrode active material for a battery that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0108] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0109] In some embodiments, the positive electrode film layer may further include a conductive agent, which may include, for example, at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0110] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0111] Negative electrode

[0112] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0113] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0114] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0115] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0116] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0117] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0118] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0119] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0120] Electrolytes

[0121] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.

[0122] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0123] In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0124] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0125] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0126] Isolation film

[0127] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.

[0128] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0129] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0130] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0131] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0132] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 5 is a square structure as an example.

[0133] In some embodiments, reference Figure 2 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0134] In some embodiments, secondary batteries may be assembled into a battery module. The number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.

[0135] Figure 3 4 is an example of a battery module. Figure 3 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0136] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0137] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.

[0138] Figure 4 and Figure 5 1 is a battery pack 1 as an example. Figure 4 and Figure 5 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0139] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. Among them, the mobile device may be, for example, a mobile phone, a laptop computer, etc.; the electric vehicle may be, for example, a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., but are not limited thereto.

[0140] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.

[0141] Figure 6The power consumption device 6 is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the power consumption device's requirements for high power and high energy density of secondary batteries, a battery pack or a battery module can be used.

[0142] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.

[0143] The present application is further described in detail below in conjunction with specific examples and comparative examples. Experimental parameters not specified in the following specific examples are preferably referred to the instructions given in the present application documents, and may also refer to the experimental manual of the art or other experimental methods known in the art, or refer to the experimental conditions recommended by the manufacturer. It is understandable that the instruments and raw materials used in the following examples are more specific, and in other specific embodiments, they may not be limited thereto; the weight of the relevant components mentioned in the embodiments of the present application specification may not only refer to the specific content of each component, but may also represent the proportional relationship of the weight between the components, therefore, as long as the content of the relevant components of the present application specification is proportionally enlarged or reduced, it is within the scope disclosed in the embodiments of the present application specification. Specifically, the weight described in the present application embodiment specification may be mass units known in the chemical and chemical fields such as μg, mg, g, and kg.

[0144] Example 1

[0145] (1) Preparation of positive electrode sheet:

[0146] a. Preparation of the first / second active layer:

[0147] NCM622, PVDF (polyvinylidene fluoride), and SP (conductive carbon) are mixed in a mass ratio of 80:10:10 to obtain a positive electrode active material; the positive electrode active material is dissolved in NMP (N-methylpyrrolidone) to prepare a positive electrode slurry with a viscosity of 20000 mPa·s, which is filled into a porous aluminum current collector (porosity 85%, pore density 50 PPI, pore size 1 μm), and then cold pressed to reduce the thickness by 25% compared with that before cold pressing to obtain a first active layer; the above steps are repeated to prepare a second active layer;

[0148] b. Preparation of positive electrode lithium replenishment layer:

[0149] Select two sheets of polyvinylidene fluoride with a thickness of 2 μm, a porosity of 70%, and a pore size of 15 nm as the first diaphragm layer and the second diaphragm layer respectively; use Li2NiO2 as a lithium source (the amount used is 5% of the mass of the positive electrode active material in step a), press it on the first diaphragm layer to form a 1 μm thick lithium source layer, and make the distance between the orthographic projection contour of the lithium source layer on the first diaphragm layer and the contour of the first diaphragm layer be 1 mm, and then press the second diaphragm layer on the surface of the lithium source layer to obtain a positive electrode lithium supplement layer;

[0150] c. Preparation of positive electrode sheet:

[0151] The first active layer, the positive electrode lithium supplement layer and the second active layer are composited and hot pressed at 100°C, and the thickness after hot pressing is reduced by 50% compared with that before hot pressing, and the distribution amount of the positive electrode active material is 125 mg / cm 2 The compacted density is 3.4 g / cm 3 The positive electrode;

[0152] (2) Preparation of negative electrode sheet:

[0153] Graphite, SBR (styrene butadiene rubber), and SP (conductive carbon) were mixed in a mass ratio of 90:5:5, then dissolved in deionized water, stirred evenly to obtain a negative electrode slurry, and coated on the surface of copper foil. After drying, cold pressing was performed to obtain a compaction density of 1.6 g / cm 3 The negative electrode.

[0154] (3) The positive electrode sheet, the separator, and the negative electrode sheet are wound, hot pressed, injected, and packaged to obtain a lithium-ion battery, and then subjected to formation (0.1C constant current charging to 3.0V, 0.2C constant current charging to 3.75V) and first-cycle lithium source activation (0.33C constant current charging to 4.50V, constant voltage charging to 0.05C, and 0.33C constant current discharge to 2.5V).

[0155] Example 2

[0156] The method is basically the same as Example 1, except that the porosity of the porous aluminum current collector is 70%.

[0157] Example 3

[0158] It is basically the same as Example 1, except that the porosity of the porous aluminum current collector is 95%.

[0159] Example 4

[0160] It is basically the same as Example 1, except that the pore density of the porous aluminum current collector is 30 PPI.

[0161] Example 5

[0162] It is basically the same as Example 1, except that the pore diameters of the first diaphragm layer and the second diaphragm layer are 5 nm.

[0163] Example 6

[0164] It is basically the same as Example 1, except that the pore diameters of the first diaphragm layer and the second diaphragm layer are 55 nm.

[0165] Example 7

[0166] The method is basically the same as Example 1, except that in step (1)a, the viscosity of the positive electrode slurry is 15000 mPa·s.

[0167] Example 8

[0168] The method is basically the same as Example 1, except that in step (1)a, the viscosity of the positive electrode slurry is 32000 mPa·s.

[0169] Example 9

[0170] The method is basically the same as Example 1, except that in step (1) b, the width of the lithium source layer is 0.3 mm smaller than the width of the electrode.

[0171] Example 10

[0172] The method is basically the same as Example 1, except that in step (1) b, the amount of Li2NiO2 used is 10% of the mass of the positive electrode active material.

[0173] Embodiment 11

[0174] Basically the same as Example 1, except that in step (1) c, the hot pressing temperature is 150°C.

[0175] Example 12

[0176] The method is basically the same as Example 1, except that in step (1) b, the Li2NiO2 lithium source is replaced by an equal mass of Li5FeO4.

[0177] Embodiment 13

[0178] It is basically the same as Example 11, except that the amount of Li5FeO4 used is 3% of the mass of the positive electrode active material.

[0179] Embodiment 14

[0180] The method is basically the same as Example 1, except that in step (1) b, the Li2NiO2 lithium source is replaced by an equal mass of Li2O.

[0181] Embodiment 15

[0182] It is basically the same as Example 13, except that the amount of Li2O used is 3% of the mass of the positive electrode active material.

[0183] Example 16

[0184] (1) Preparation of positive electrode sheet:

[0185] NCM622, PVDF, and SP were mixed in a mass ratio of 80:10:10 to obtain a positive electrode active material; the positive electrode active material was dissolved in NMP (N-methylpyrrolidone) to prepare a positive electrode slurry with a viscosity of 20000 mPa·s, which was filled into a porous aluminum current collector (porosity 85%, pore density 50 PPI, pore size 1 μm), and then cold pressed to reduce the thickness by 25% compared with that before cold pressing, and obtain a compacted density of 3.4 g / cm 3 The positive electrode;

[0186] (2) Preparation of negative electrode sheet:

[0187] a. Preparation of the first / second active layer:

[0188] Graphite, SBR and SP were mixed in a mass ratio of 90:5:5 to obtain a positive electrode active material; the positive electrode active material was dissolved in NMP (N-methylpyrrolidone) to prepare a positive electrode slurry with a viscosity of 30000 mPa·s, which was filled into a porous aluminum current collector (porosity 85%, pore density 50 PPI, pore size 1 μm), and then cold pressed to reduce the thickness by 25% compared with that before cold pressing to obtain a first active layer; the above steps were repeated to prepare a second active layer;

[0189] b. Preparation of negative electrode lithium replenishment layer:

[0190] Select two sheets of polyvinylidene fluoride with a thickness of 2 μm, a porosity of 70%, and a pore size of 40 nm as the first diaphragm layer and the second diaphragm layer respectively; use lithium foil as a lithium source (the amount used is 1% of the mass of the negative electrode active material in step a), press it on the first diaphragm layer to form a 1 μm thick lithium source layer, and make the distance between the positive projection contour of the lithium source layer on the first diaphragm layer and the contour of the first diaphragm layer be 1 mm, and then press the second diaphragm layer on the surface of the lithium source layer to obtain a negative electrode lithium supplement layer;

[0191] c. Preparation of negative electrode sheet:

[0192] The first active layer, the negative electrode lithium supplement layer and the second active layer are composited and hot pressed at 100°C, and the thickness after hot pressing is reduced by 50% compared with that before hot pressing, and the distribution amount of the negative electrode active material is 125 mg / cm 2 , the compacted density is 1.6 g / cm 3 The negative electrode;

[0193] (3) The positive electrode sheet, the separator, and the negative electrode sheet are wound, hot pressed, injected, and packaged to obtain a lithium-ion battery, and then subjected to formation (0.1C constant current charging to 3.0V, 0.2C constant current charging to 3.75V) and first-cycle lithium source activation (0.33C constant current charging to 4.50V, constant voltage charging to 0.05C, and 0.33C constant current discharge to 2.5V).

[0194] Comparative Example 1

[0195] (1) Preparation of positive electrode sheet:

[0196] NCM622, PVDF and SP were mixed in a mass ratio of 80:10:10 to obtain a positive electrode active material; the positive electrode active material was dissolved in NMP (N-methylpyrrolidone) to prepare a positive electrode slurry with a viscosity of 20000 mPa·s, which was filled into a porous aluminum current collector (porosity 85%, pore density 50 PPI, pore diameter 1 μm), and then cold pressed to reduce the thickness by 25% compared with that before cold pressing to obtain a positive electrode sheet;

[0197] (2) Preparation of negative electrode sheet:

[0198] Graphite, SBR, and SP (mixed in a mass ratio of 90:5:5, dissolved in deionized water, stirred evenly to obtain a negative electrode slurry, and coated on the surface of copper foil, dried, and cold pressed to obtain a compaction density of 1.6 g / cm 3 The negative electrode.

[0199] (3) The positive electrode sheet, the separator, and the negative electrode sheet are wound, hot pressed, injected, and packaged to obtain a lithium-ion battery, and then subjected to formation (0.1C constant current charging to 3.0V, 0.2C constant current charging to 3.75V) and first-cycle lithium source activation (0.33C constant current charging to 4.50V, constant voltage charging to 0.05C, and 0.33C constant current discharge to 2.5V).

[0200] Characterization Tests:

[0201] The batteries prepared in the above embodiments and comparative examples were subjected to the following performance tests:

[0202] (1) Battery first cycle capacity test:

[0203] The lithium-ion secondary battery was placed in a thermostat at 25°C, and charged at room temperature at a constant current of 0.5C until the voltage was higher than 4.35V, and further charged at a constant voltage of 4.35V until the current was lower than 0.05C, so that it was in a fully charged state of 4.35V, and then the lithium-ion secondary battery was discharged at a constant current of 0.33C until the voltage was 2.5V (cut-off voltage), which was one cycle. The discharge capacity D was recorded; the first-cycle discharge capacity D0 of the comparative example 1 without lithium supplementation was used as the benchmark, and the improvement of the first-cycle capacity of each embodiment relative to the comparative example 1 was calculated as (D-D0) / D0.

[0204] (2) Cycle life test:

[0205] Place the lithium-ion secondary battery in a 25°C constant temperature box, charge it at a constant current of 0.5C at room temperature until the voltage is higher than 4.35V, and further charge it at a constant voltage of 4.35V until the current is lower than 0.05C, so that it is in a fully charged state of 4.35V, and then discharge the lithium-ion secondary battery at a constant current of 0.33C until the voltage is 2.5V (cut-off voltage), which is 1 cycle. Repeat the cycle, record the discharge capacity D2 of each cycle, and stop the test when D2 / D1=80% and record the number of cycles.

[0206] The results are listed in Table 1:

[0207] Table 1

[0208]

[0209]

[0210] Analyzing the data in Table 1, it can be seen from the comparison of Examples 1 to 3 that the porosity of the current collector has a certain influence on the lithium replenishment rate. The appropriate porosity makes the lithium replenishment rate moderate, and lithium precipitation will not be caused by excessive lithium replenishment, nor will local deposition be caused by too slow lithium replenishment. Therefore, the capacity and cycle life of the battery can be effectively improved. Comparing Example 1 and Example 4, it can be seen that the pore density of the current collector will also affect the lithium replenishment rate, thereby affecting the cycle life. Comparing Examples 1, 5 to 6, it can be seen that the pore size of the diaphragm layer will also affect the lithium replenishment rate. Due to the high positive electrode potential, the relatively small pore size can control the lithium replenishment rate not to be too fast, but if the pore size is too small (such as Example 5), it will also cause the lithium replenishment material to be unable to be released normally, and the degree of improvement in the cycle life is very limited. Comparing Examples 1, 7 to 8, it can be seen that when the viscosity of the electrode slurry is too high or too low, the filling uniformity of the slurry in the porous current collector will decrease, thereby affecting the cycle performance. Comparing Examples 1 and 9, it can be seen that when the contour distance between the lithium source layer and the first diaphragm layer is too small, lithium precipitation will occur, resulting in limited capacity improvement. Comparing Examples 1 and 10, it can be seen that when the amount of lithium source is too high, the improvement in cycle life is already relatively limited, but the cost will be greatly increased; and although the first-cycle capacity of the battery will be improved due to the increase in lithium source, the lithium source will occupy the position of the active material, resulting in a decrease in the amount of active material in the pole piece, which will cause the overall volume capacity of the battery to decrease. Comparing Examples 1 and 11, it can be seen that if the hot pressing temperature is too high, the diaphragm layer will become wrinkled, making the contact between the lithium supplement layer and the active layer not close enough, affecting the release of active lithium, and causing a decrease in cycle life. Comparing Example 1 and Comparative Example 1, it can be seen that compared with the pole piece that has not been supplemented with lithium, the scheme of the present application can significantly improve the cycle life of the battery.

[0211] It can be seen from Examples 12 to 15 that the solution of the present application is applicable to a variety of lithium sources, and it can be seen from Example 16 that the present application is also applicable to negative electrode lithium replenishment.

[0212] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0213] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the specification and drawings may be used to interpret the contents of the claims.

Claims

1. An electrode plate, characterized in that: It includes a first active layer, a lithium supplement layer and a second active layer which are stacked; The first active layer and the second active layer include a porous current collector and an electrode active material filled in the porous current collector; The lithium supplement layer includes a first separator layer, a lithium source layer, and a second separator layer which are stacked, and the first separator layer and the second separator layer have a porous structure.

2. The electrode plate according to claim 1, characterized in that: The porous current collector has a porosity of 78% to 92%, a pore density of 40 PPI to 110 PPI, and a pore diameter of 500 nm to 3 μm.

3. The electrode plate according to claim 1, characterized in that: The minimum distance between the outer contour edge of the orthographic projection of the lithium source layer on the first diaphragm layer and the outer contour edge of the first diaphragm layer is 0.7 mm to 0.9 mm, and the maximum distance is 1.1 mm to 1.3 mm.

4. The electrode plate according to claim 1, characterized in that: The thickness of the lithium source layer is ≤3 μm.

5. The electrode plate according to claim 1, characterized in that: The mass of the lithium source in the lithium source layer is 1% to 5% of the mass of the electrode active material.

6. The electrode plate according to claim 1, characterized in that: The materials of the first diaphragm layer and the second diaphragm layer are independently selected from one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride and carbon fiber.

7. The electrode plate according to claim 1, characterized in that: The first diaphragm layer and the second diaphragm layer independently have one or more of the following characteristics: (1) Porosity is 60% to 90%; (2) The pore diameter is 10nm to 50nm.

8. The electrode plate according to claim 1, characterized in that: The thickness of the first diaphragm layer and the second diaphragm layer are independently 1 μm to 7 μm.

9. The electrode sheet according to any one of claims 1 to 8, characterized in that: The electrode plate is a positive electrode plate, and the pore sizes of the first diaphragm layer and the second diaphragm layer are independently 10 nm to 30 nm.

10. The electrode plate according to claim 9, characterized in that: The lithium source in the lithium source layer includes Li 1+ x Ni 0.5 Mn 1.5 O4, Li2NiO2, Li5FeO4, LiF, Li2S, Li2C2O4, LiMn2O4; one or more of Li2O2, Li2O and Li3N; wherein x is selected from any value between 0 and 1.

11. The electrode plate according to claim 9, characterized in that: The compaction density of the electrode plate is 3.3 g / cm 3 ~3.5g / cm 3 .

12. The electrode sheet according to any one of claims 1 to 8, characterized in that: The electrode plate is a negative electrode plate, and the pore sizes of the first diaphragm layer and the second diaphragm layer are independently 30 nm to 50 nm.

13. The electrode plate according to claim 12, characterized in that: The lithium source in the lithium source layer includes one or more of lithium foil, lithium powder and pre-lithiated graphite.

14. The electrode plate according to claim 12, characterized in that: The compaction density of the electrode plate is 1.5 g / cm 3 ~1.7g / cm 3 .

15. The method for preparing an electrode sheet according to any one of claims 1 to 14, characterized in that: The following steps are involved: Filling the electrode active material into the porous current collector to prepare the first active layer and the second active layer; Compounding the first separator layer, the lithium source layer and the second separator layer to prepare the lithium replenishing layer; The first active layer, the lithium supplement layer and the second active layer are compounded to prepare the electrode plate.

16. The preparation method according to claim 15, characterized in that: The electrode active material is first mixed with a solvent to prepare an electrode slurry with a viscosity of 20000 mPa·s to 30000 mPa·s, and then filled into the porous current collector.

17. The preparation method according to claim 16, characterized in that: After the electrode slurry is filled into the porous current collector, the porous current collector is cold pressed, and the thickness of the porous current collector after cold pressing is controlled to be reduced by 20% to 50% compared with that before cold pressing.

18. The preparation method according to any one of claims 15 to 17, characterized in that: The first active layer, the lithium supplement layer and the second active layer are composited by hot pressing, and the hot pressing operation satisfies at least one of the following conditions: (1) The temperature of hot pressing is 80℃~120℃; (2) After hot pressing, the thickness of the electrode sheet is reduced by 50% to 60% compared with that before hot pressing; (3) After hot pressing, the coating weight CW of the electrode active material per unit area on one side is 100 mg / cm 2 ~150mg / cm 2 .

19. A secondary battery, characterized in that: The invention comprises the electrode plate as claimed in any one of claims 1 to 14.

20. An electrical device, characterized in that: Includes the secondary battery as claimed in claim 19.