In-situ coated high voltage positive electrode material and preparation method and use thereof
By forming a benzodifurandione derivative conductive polymer coating layer on the surface of the high-voltage cathode material, the problems of poor cycle stability and rate performance in lithium-ion batteries are solved, and higher battery performance is achieved.
Patent Information
- Application Number
- CN202211710297.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-29
AI Technical Summary
Existing high-voltage cathode materials have poor cycle stability and poor rate performance in lithium-ion batteries, especially due to insufficient ion conductivity of the coating layer, which results in poor electronic and ion conductivity, affecting battery performance.
Benzodifuran dione and its derivatives are used as conductive polymers to form a dense coating layer on the surface of the high-voltage cathode material through in-situ reaction to improve the conductive performance, and oxidative polymerization is performed at a specific temperature and solvent to form a stable conductive layer. Polymer shell.
It effectively suppresses the structural instability and side reactions of the cathode material, improves the cycle stability and rate performance of the battery, enhances the transmission capacity of Li+, and significantly improves the overall performance of the battery.
Smart Images

Figure CN115863651B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery materials, and in particular to an in-situ coated high-voltage positive electrode material, a preparation method and uses thereof. Background Art
[0002] Energy crisis and environmental protection are two issues that people are extremely concerned about in the 21st century. Vigorously developing new energy is the most effective means to solve the above problems. As one of the important new energy products, lithium-ion batteries have been widely used in the fields of 3C products and electric vehicles. And with the continuous development of the economy and society, higher requirements are put forward for the energy density of lithium-ion batteries. The use of high-voltage positive electrode materials is an important way to improve the energy density of lithium-ion batteries, such as nickel-manganese spinel positive electrode materials, high-nickel positive electrode materials, and lithium-rich positive electrode materials. However, under high voltage, the structure of the positive electrode material is unstable and easy to collapse, and the side reaction between the positive electrode material and the electrolyte will cause the electrochemical performance of the lithium-ion battery to decay; in addition, due to the poor electronic conductivity and ionic conductivity of the high-voltage positive electrode material, the rate performance and cycle performance are defective.
[0003] To overcome the above defects, the main solution is currently through element doping and surface coating of positive electrode materials. To a certain extent, the collapse of positive electrode materials and oxidative decomposition of electrolytes under high voltages are alleviated. At present, the coated materials mainly include metals and their metal oxides, which can effectively inhibit the side reactions between positive electrode materials and electrolytes, but usually have disadvantages such as uneven coating, high processing temperature, and poor ionic conductivity, and it is difficult to obtain an ideal coating effect. Polymers, especially conductive polymers, are also often used to coat positive electrode materials to improve the conductivity while protecting the structure of the positive electrode material. For example, the modified high-voltage positive electrode material, preparation method and application disclosed in Chinese patent document CN111509210A, the modified high-voltage positive electrode material includes a high-voltage positive electrode material core and a conductive polymer shell coating its surface, the preparation method includes using a high-voltage positive electrode material, a conductive polymer monomer, a catalyst and an initiator to react in situ or using a high-voltage positive electrode material, a conductive polymer and a coupling agent for direct coating, and the modified high-voltage positive electrode material can react with the electrolyte in the battery through a controllable electrochemical activation process to gradually react to form a new surface dense coating layer. However, the above-mentioned conductive polymers have poor ion conductivity and the coating layer is not conducive to Li + The rapid transmission has limited improvement on overall battery performance. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of poor cycle stability and poor rate performance of batteries prepared from high-voltage positive electrode materials in the prior art, thereby providing an in-situ coated high-voltage positive electrode material and a preparation method and use thereof.
[0005] To this end, the present invention provides the following technical solutions:
[0006] An in-situ coated high-voltage positive electrode material comprises a high-voltage positive electrode material core and a conductive polymer shell coated on the surface of the high-voltage positive electrode material core; the conductive polymer shell comprises a polymer of benzodifurandione and its derivatives; the molecular formula structure of benzodifurandione and its derivatives is shown in Formula 1:
[0007]
[0008] Wherein, R is selected from: H, -CH3, -CH2CH3, -OH, -OCH3 or -OCH2CH3.
[0009] Optionally, the core of the high-voltage positive electrode material includes: a lithium-rich solid solution positive electrode material, a high-voltage nickel-manganese spinel positive electrode material or a high-nickel positive electrode material.
[0010] A method for preparing an in-situ coated high-voltage positive electrode material comprises the following steps:
[0011] (1) adding a high voltage positive electrode material into a polar aprotic solvent to obtain a suspension of the high voltage positive electrode material;
[0012] (2) Add benzodifurandione and its derivatives and benzoquinone oxidant to the suspension of the high voltage positive electrode material, stir, and then heat to 100-130° C. under the protection of inert gas, and stir to react for 1-3 hours.
[0013] Optionally, in step (1), the polar aprotic solvent includes dimethyl sulfoxide, N-methylpyrrolidone or N,N-dimethylformamide.
[0014] Optionally, in step (2), the molar ratio of the high voltage positive electrode material, benzodifurandione and its derivatives and benzoquinone oxidant is 1: (0.01-0.04): (0.02-0.06).
[0015] Optionally, in step (2), the molar ratio of the high voltage positive electrode material, benzodifurandione and its derivatives and benzoquinone oxidant is 1:0.02:0.03.
[0016] Optionally, in step (2), the benzoquinone oxidant includes benzoquinone, tetramethylbenzoquinone, tetrahydroxybenzoquinone, p-dimethylquinone, 2,5-dihydroxy-1,4-benzoquinone, tetrafluorobenzoquinone, tetrabromobenzoquinone, tetrachlorobenzoquinone, 2,5-dichloro-p-benzoquinone or 2,5-dibromo-p-benzoquinone; and / or
[0017] In the step (2), the temperature is raised to 100° C. and the reaction is stirred for 2 h.
[0018] The in-situ coated high-voltage positive electrode material or the in-situ coated high-voltage positive electrode material prepared by the preparation method of the in-situ coated high-voltage positive electrode material is used in lithium-ion batteries.
[0019] A lithium ion battery contains the in-situ coated high-voltage positive electrode material or the in-situ coated high-voltage positive electrode material prepared by the method for preparing the in-situ coated high-voltage positive electrode material.
[0020] Optionally, a positive electrode sheet for a lithium-ion battery is included, wherein the preparation of the positive electrode sheet for the lithium-ion battery is as follows: the in-situ coated high-voltage positive electrode material is dispersed into a solution, and then a conductive agent and a binder are added to prepare a slurry, and the obtained slurry is scraped onto an aluminum foil and pressed into shape;
[0021] Optionally, the mass ratio of the in-situ coated high voltage positive electrode material, the conductive agent and the binder is (85-97): (2-10): (1-8);
[0022] Optionally, it also includes a negative electrode sheet, a separator and an electrolyte;
[0023] Optionally, the negative electrode material contained in the negative electrode plate is at least one of lithium metal, graphite, silicon carbon and silicon oxygen material;
[0024] Optionally, the separator is one of PP, PE or PI films, and has a thickness of 6 to 20 μm.
[0025] The technical solution of the present invention has the following advantages:
[0026] 1. The present invention provides an in-situ coated high-voltage positive electrode material, comprising a high-voltage positive electrode material core and a conductive polymer shell coated on the surface of the high-voltage positive electrode material core; the conductive polymer shell comprises a polymer of benzodifurandione and its derivatives; the molecular general structure of the benzodifurandione and its derivatives is shown in Formula 1; in the above-mentioned in-situ coated high-voltage positive electrode material, by selecting a polymer of benzodifurandione and its derivatives, it can be uniformly coated on the surface of the high-voltage positive electrode material to form a dense organic protective layer, which can effectively inhibit the collapse caused by the structural instability of the positive electrode material under high voltage, alleviate the side reaction of the positive electrode material / electrolyte interface, and improve the cycle stability of the battery prepared by the in-situ coated high-voltage positive electrode material. In addition, because the polymer of benzodifurandione and its derivatives is an n-type conductive polymer, it not only has an ultra-high electronic conductivity, but its electron-rich characteristic structure is also conducive to Li + The transmission of electrons and ions is accelerated, which is beneficial to reducing the surface impedance, thereby improving the rate performance of the battery prepared by the in-situ coated high-voltage positive electrode material.
[0027] 2. The present invention provides a method for preparing an in-situ coated high-voltage positive electrode material, comprising the following steps: (1) adding a high-voltage positive electrode material to a polar non-protonic solvent to obtain a suspension of the high-voltage positive electrode material; (2) adding benzodifurandione and its derivatives and a quinone oxidant to the suspension of the high-voltage positive electrode material, stirring, and then heating to 100-130°C under the protection of an inert gas, stirring and reacting for 1-3 hours; the above method is simple and convenient, and the prepared in-situ coated high-voltage positive electrode material has a stable structure, alleviates side reactions at the positive electrode material / electrolyte interface, has high-temperature stable cycle performance, and has high ion and electron conductivity and high rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 It is the high temperature cycle performance test result in the experimental example of the present invention;
[0030] Figure 2 It is the rate performance test result in the experimental example of the present invention. DETAILED DESCRIPTION
[0031] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0032] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0033] The molecular general structure of benzodifurandione and its derivatives in the following embodiments is shown in Formula 1.
[0034]
[0035] Wherein, R is selected from: H, -CH3, -CH2CH3, -OH, -OCH3 or -OCH2CH3.
[0036] Benzodifurandione was purchased from Zhengzhou Yande Biotechnology Co., Ltd.
[0037] High voltage nickel manganese spinel positive electrode material (LiNi 0.5 Mn 1.5 O4(LNMO)) is a commercially available product.
[0038] Example 1
[0039] This embodiment provides an in-situ coated high-voltage positive electrode material, including a high-voltage positive electrode material core and a conductive polymer shell layer coated on the surface of the high-voltage positive electrode material core; wherein the high-voltage positive electrode material core is a high-voltage nickel-manganese spinel positive electrode material core, and the general formula of the high-voltage nickel-manganese spinel positive electrode material is: LiNi 0.5 Mn 1.5 O4(LNMO), the conductive polymer shell is a poly(benzodifurandione) shell.
[0040] This embodiment also provides a method for preparing the above-mentioned in-situ coated high-voltage positive electrode material, comprising the following steps:
[0041] (1) High voltage nickel manganese spinel positive electrode material (LiNi 0.5 Mn 1.5 O4(LNMO)) (30 g) was added to N-methylpyrrolidone solvent (100 mL), and placed in a reaction device, and kept stirring to obtain a high voltage nickel manganese spinel positive electrode material suspension;
[0042] (2) Add benzodifurandione and tetramethylbenzoquinone to the above-mentioned high voltage nickel manganese spinel positive electrode material suspension, wherein the molar ratio of high voltage nickel manganese spinel positive electrode material: benzodifurandione: tetramethylbenzoquinone is 1:0.02:0.03, and stir evenly to form a dispersed system. Under the protection of an inert atmosphere (argon), slowly heat up to 100°C, stir vigorously to react for 2 hours, so that benzodifurandione undergoes oxidative polymerization on the surface of the high voltage nickel manganese spinel positive electrode material to form a conductive polymer coating layer, and then centrifuge and wash, and finally disperse with N-methylpyrrolidone to obtain a high voltage nickel manganese spinel positive electrode material solution in situ coated with a conductive polymer.
[0043] Example 2
[0044] This embodiment provides an in-situ coated high-voltage positive electrode material, including a high-voltage positive electrode material core and a conductive polymer shell layer coated on the surface of the high-voltage positive electrode material core; wherein the high-voltage positive electrode material core is a high-nickel positive electrode material core, and the high-nickel positive electrode material is: LiNi 0.8 Co 0.1 Mn 0.1 O2, the conductive polymer shell is a poly(benzodifurandione) shell.
[0045] This embodiment also provides a method for preparing the above-mentioned in-situ coated high-voltage positive electrode material, comprising the following steps:
[0046] (1) High nickel positive electrode material (LiNi 0.8 Co 0.1 Mn 0.1 O2) (30 g) was added to dimethyl sulfoxide (100 mL), and placed in a reaction device, and stirred continuously to obtain a high-nickel positive electrode material suspension;
[0047] (2) Add benzodifurandione and p-dimethylquinone to the above-mentioned high-nickel positive electrode material suspension, wherein the molar ratio of high-nickel positive electrode material: benzodifurandione: p-dimethylquinone is 1:0.01:0.06, and stir evenly to form a dispersed system. Under the protection of an inert atmosphere (argon), slowly heat to 130°C, vigorously stir and react for 1 hour, so that benzodifurandione undergoes oxidative polymerization on the surface of the high-nickel positive electrode material to form a conductive polymer coating layer, and then centrifuge and wash, and finally disperse with N-methylpyrrolidone to obtain a high-nickel positive electrode material solution in situ coated with a conductive polymer.
[0048] Example 3
[0049] This embodiment provides an in-situ coated high-voltage positive electrode material, comprising a high-voltage positive electrode material core and a conductive polymer shell layer coated on the surface of the high-voltage positive electrode material core; wherein the high-voltage positive electrode material core is a lithium-rich solid solution positive electrode material core, and the lithium-rich solid solution positive electrode material is 0.4Li2MnO3·0.6LiNi 0.2 Mn 0.6 Co 0.2 O2, the conductive polymer shell is a poly(benzodifurandione) shell.
[0050] This embodiment also provides a method for preparing the above-mentioned in-situ coated high-voltage positive electrode material, comprising the following steps:
[0051] (1) Adding a lithium-rich solid solution positive electrode material (30 g) into an N,N-dimethylformamide solvent (100 mL), placing the mixture in a reaction device, and continuously stirring the mixture to obtain a lithium-rich solid solution positive electrode material suspension;
[0052] (2) Add benzodifurandione and tetrafluorobenzoquinone to the above lithium-rich solid solution positive electrode material suspension, wherein the molar ratio of lithium-rich solid solution positive electrode material: benzodifurandione: tetrafluorobenzoquinone is 1:0.04:0.02, and stir evenly to form a dispersed system. Under the protection of an inert atmosphere (argon), slowly heat to 120°C, vigorously stir and react for 3 hours, so that benzodifurandione undergoes oxidative polymerization on the surface of the lithium-rich solid solution positive electrode material to form a conductive polymer coating layer, and then centrifuge and wash, and finally disperse with N-methylpyrrolidone to obtain a lithium-rich solid solution positive electrode material solution coated with a conductive polymer in situ.
[0053] Example 4
[0054] The difference between this embodiment and embodiment 1 is that the conductive polymer shell layer is a poly(benzodifurandione) shell layer replaced by a polymer shell layer of a benzodifurandione derivative; the benzodifurandione derivative is:
[0055]
[0056] Wherein, R is -CH3; the compound was purchased from Zhengzhou Yande Biotechnology Co., Ltd.
[0057] Example 5
[0058] The difference between this embodiment and embodiment 1 is that the conductive polymer shell layer is a poly(benzodifurandione) shell layer replaced by a polymer shell layer of a benzodifurandione derivative; the benzodifurandione derivative is:
[0059]
[0060] Wherein, R is -CH2CH3; the compound was purchased from Zhengzhou Yande Biotechnology Co., Ltd.
[0061] Example 6
[0062] The difference between this embodiment and embodiment 1 is that the conductive polymer shell layer is a poly(benzodifurandione) shell layer replaced by a polymer shell layer of a benzodifurandione derivative; the benzodifurandione derivative is:
[0063]
[0064] Wherein, R is -OH; the compound was purchased from Zhengzhou Yande Biotechnology Co., Ltd.
[0065] Example 7
[0066] The difference between this embodiment and embodiment 1 is that the conductive polymer shell layer is a poly(benzodifurandione) shell layer replaced by a polymer shell layer of a benzodifurandione derivative; the benzodifurandione derivative is:
[0067]
[0068] Wherein, R is -OCH3; the compound was purchased from Zhengzhou Yande Biotechnology Co., Ltd.
[0069] Example 8
[0070] This embodiment also provides a method for preparing a lithium ion battery using the in-situ coating high voltage positive electrode material of embodiment 1, comprising the following steps:
[0071] 1) Add a conductive agent and a binder to the high-voltage nickel-manganese spinel positive electrode material solution coated with a conductive polymer in situ to make a slurry, and then evenly scrape the slurry on an aluminum foil, press it into shape, and obtain a positive electrode sheet for a lithium-ion battery. Among them, the mass ratio of positive electrode material: conductive agent: binder is 93:5:2. At the same time, the conductive agent and binder are both conventional conductive agents and binders in the field. The conductive agent selected in this embodiment is carbon black, and the binder is polyvinylidene fluoride.
[0072] 2) The above-mentioned high-voltage nickel-manganese spinel positive electrode plate with in-situ coating of conductive polymer is used as the positive electrode, the metal lithium plate is used as the negative electrode plate, the diaphragm is selected as a polypropylene film (PP film) with a thickness of 13 μm, and the electrolyte is selected as 1M LiPF6 (EC (ethylene carbonate): EMC (ethyl methyl carbonate): DMC (dimethyl carbonate) = 1:1:1 vol%) + 3% FEC (fluoroethylene carbonate), and a button battery is assembled.
[0073] Example 9
[0074] This embodiment also provides a method for preparing a lithium ion battery using the in-situ coating high voltage positive electrode material of embodiment 2, comprising the following steps:
[0075] 1) Add a conductive agent and a binder to the in-situ coated high-voltage positive electrode material solution to make a slurry, then evenly scrape the slurry on an aluminum foil, press and form, and obtain a positive electrode sheet for a lithium-ion battery. Among them, the mass ratio of positive electrode material: conductive agent: binder is 85:10:5. At the same time, the conductive agent and binder are conventional conductive agents and binders in the field. The conductive agent selected in this embodiment is carbon black, and the binder is polyvinylidene fluoride.
[0076] 2) The positive electrode sheet made of the above-mentioned in-situ coated high-voltage positive electrode material is used as the positive electrode, the metal lithium sheet is used as the negative electrode sheet, the diaphragm is a polyethylene film (PE film) with a thickness of 6 μm, and the electrolyte is 1M LiPF6 (EC:EMC:DMC=1:1:1vol%)+3% FEC (fluoroethylene carbonate), and a button battery is assembled.
[0077] Example 10
[0078] This embodiment also provides a method for preparing a lithium ion battery using the in-situ coating high voltage positive electrode material of embodiment 3, comprising the following steps:
[0079] 1) Add a conductive agent and a binder to the in-situ coated high-voltage positive electrode material solution to make a slurry, then evenly scrape the slurry on an aluminum foil, press and form, and obtain a positive electrode sheet for a lithium-ion battery. Among them, the mass ratio of positive electrode material: conductive agent: binder is 97:2:1. At the same time, the conductive agent and binder are conventional conductive agents and binders in the field. The conductive agent selected in this embodiment is carbon black, and the binder is polyvinylidene fluoride.
[0080] 2) The positive electrode sheet made of the above-mentioned in-situ coated high-voltage positive electrode material is used as the positive electrode, the metal lithium sheet is used as the negative electrode sheet, the diaphragm is a polyimide film (PI film) with a thickness of 20 μm, and the electrolyte is 1M LiPF6 (EC:EMC:DMC=1:1:1vol%)+3% FEC (fluoroethylene carbonate), and a button battery is assembled.
[0081] Embodiment 11
[0082] This embodiment also provides a method for preparing a lithium ion battery using the in-situ coating high voltage positive electrode material of embodiment 4, comprising the following steps:
[0083] 1) Add a conductive agent and a binder to the in-situ coated high-voltage positive electrode material solution to make a slurry, then evenly scrape the slurry on an aluminum foil, press and form it to obtain a positive electrode sheet for a lithium-ion battery. Among them, the mass ratio of positive electrode material: conductive agent: binder is 90:2:8. At the same time, the conductive agent and binder are conventional conductive agents and binders in the field. The conductive agent selected in this embodiment is carbon black, and the binder is polyvinylidene fluoride.
[0084] 2) The positive electrode sheet made of the above-mentioned in-situ coated high-voltage positive electrode material is used as the positive electrode, the metal lithium sheet is used as the negative electrode sheet, the diaphragm is a polyimide film (PI film) with a thickness of 10 μm, and the electrolyte is 1M LiPF6 (EC:EMC:DMC=1:1:1vol%)+3% FEC (fluoroethylene carbonate), and a button battery is assembled.
[0085] Example 12
[0086] The method for preparing a lithium-ion battery using the in-situ coating high-voltage positive electrode material of Example 5, Example 6 or Example 7 is the same as that of Example 8.
[0087] Experimental example
[0088] Experimental materials: button cell prepared in Example 8; control: high voltage nickel manganese spinel positive electrode material without in-situ coating (general formula: LiNi 0.5 Mn 1.5 O4(LNMO)) was prepared into a button cell according to the method of Example 8.
[0089] Experimental methods:
[0090] High temperature cycle performance test: Under 45℃ test environment, ① first charge at 0.1C constant current to 4.8V, charge at constant voltage to current ≤0.05C, let stand for 10min, discharge at 0.1C to voltage ≤3.5V, let stand for 10min. ② Keep the charging procedure unchanged, charge at 0.5C to 4.8V. ③ Keep the discharge procedure unchanged, discharge at 1C to 3.5V. ② and ③ processes are cycled 100 times;
[0091] Rate performance test: first charge at 0.2C constant current to 4.8V, charge at constant voltage to current ≤0.05C, let stand for 10min, discharge at 0.2C to voltage ≤3.5V, let stand for 10min. Keep the charge and discharge procedure unchanged, and change the charge and discharge rate in the order of 0.5C, 1C, 2C, 5C, 10C, 0.2C to perform charge and discharge cycles;
[0092] Experimental results:
[0093] 1. High temperature cycle performance test results
[0094] The results are as follows Figure 1 As shown, the high-temperature cycle performance of the in-situ coated conductive polymer and the uncoated modified high-voltage nickel-manganese spinel positive electrode materials prepared in Example 1 at 100 cycles. Compared with the uncoated modified positive electrode material, the capacity retention rate of the high-voltage positive electrode material in-situ coated with the conductive polymer increased from 56.4% to 92.5%, indicating that the conductive polymer layer formed on the surface effectively protects the positive electrode material, inhibits the collapse of the positive electrode material and the side reaction between the positive electrode material and the electrolyte, improves the cycle stability of the material, and thus improves the cycle stability of the entire battery system.
[0095] 2. Rate performance test results
[0096] The results are as follows Figure 2 As shown in the figure, the specific capacity of the cathode material coated with conductive polymer in situ is 113 mAh g at 5C and 10C rates, respectively. -1 and 94mAh g -1 Compared with the uncoated modified cathode material, the specific capacity at 5C and 10C rates is 28 mAh g -1 and 9mAh g -1 There has been a significant improvement, indicating that the conductive polymer coating layer designed in the present invention has excellent electronic conductivity and ionic conductivity, thereby being able to significantly improve its rate performance.
[0097] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. An in-situ coated high voltage positive electrode material for lithium ion batteries, characterized in that: It comprises a high-voltage positive electrode material core and a conductive polymer shell layer coated on the surface of the high-voltage positive electrode material core; the conductive polymer shell layer comprises a polymer of benzodifurandione and its derivatives; the molecular formula structure of benzodifurandione and its derivatives is shown in Formula 1: Wherein, R is selected from: H, -CH3, -CH2CH3, -OH, -OCH3 or -OCH2CH3.
2. The in-situ coated high voltage positive electrode material for lithium ion battery according to claim 1, characterized in that: The core of the high-voltage positive electrode material includes: a lithium-rich solid solution positive electrode material, a high-voltage nickel-manganese spinel positive electrode material or a high-nickel positive electrode material.
3. A method for preparing an in-situ coated high-voltage positive electrode material for a lithium-ion battery as claimed in claim 1 or 2, characterized in that: The steps include: (1) adding a high voltage positive electrode material into a polar aprotic solvent to obtain a suspension of the high voltage positive electrode material; (2) Add benzodifurandione and its derivatives and benzoquinone oxidant to the suspension of the high voltage positive electrode material, stir, and then heat to 100-130° C. under the protection of inert gas, and stir to react for 1-3 hours.
4. The method for preparing an in-situ coated high-voltage positive electrode material for a lithium-ion battery according to claim 3, characterized in that: In the step (1), the polar aprotic solvent includes dimethyl sulfoxide, N-methylpyrrolidone or N,N-dimethylformamide.
5. The method for preparing an in-situ coated high-voltage positive electrode material for a lithium-ion battery according to claim 3 or 4, characterized in that: In the step (2), the molar ratio of the high voltage positive electrode material, benzodifurandione and its derivatives and benzoquinone oxidant is 1: (0.01-0.04): (0.02-0.06).
6. The method for preparing an in-situ coated high-voltage positive electrode material for a lithium-ion battery according to claim 3 or 4, characterized in that: In the step (2), the molar ratio of the high voltage positive electrode material, benzodifurandione and its derivatives and benzoquinone oxidant is 1:0.02:0.
03.
7. The method for preparing an in-situ coated high-voltage positive electrode material for a lithium-ion battery according to claim 3 or 4, characterized in that: In the step (2), the benzoquinone oxidant includes benzoquinone, tetramethylbenzoquinone, tetrahydroxybenzoquinone, p-dimethylquinone, 2,5-dihydroxy-1,4-benzoquinone, tetrafluorobenzoquinone, tetrabromobenzoquinone, tetrachlorobenzoquinone, 2,5-dichloro-p-benzoquinone or 2,5-dibromo-p-benzoquinone; and / or In the step (2), the temperature is raised to 100° C. and the reaction is stirred for 2 h.
8. Use of the in-situ coated high-voltage positive electrode material for lithium-ion batteries as claimed in claim 1 or 2 or the in-situ coated high-voltage positive electrode material prepared by the preparation method of the in-situ coated high-voltage positive electrode material for lithium-ion batteries as claimed in any one of claims 3 to 7 in lithium-ion batteries.
9. A lithium ion battery, characterized in that: An in-situ coated high-voltage positive electrode material for a lithium-ion battery as claimed in claim 1 or 2 or an in-situ coated high-voltage positive electrode material prepared by the preparation method of an in-situ coated high-voltage positive electrode material for a lithium-ion battery as claimed in any one of claims 3-7.
10. The lithium-ion battery according to claim 9, characterized in that: The invention comprises a positive electrode plate for a lithium ion battery. The preparation of the positive electrode plate for the lithium ion battery is as follows: the in-situ coated high voltage positive electrode material is dispersed into a solution, a conductive agent and a binder are added to make a slurry, the obtained slurry is scraped and coated on an aluminum foil, and pressed into shape.
11. The lithium ion battery according to claim 10, characterized in that: The mass ratio of the in-situ coated high-voltage positive electrode material, the conductive agent and the binder is (85-97): (2-10): (1-8).
12. The lithium ion battery according to claim 10, characterized in that: It also includes a negative electrode plate, a separator and an electrolyte.
13. The lithium ion battery according to claim 12, characterized in that: The negative electrode material contained in the negative electrode plate is at least one of lithium metal, graphite, silicon carbon and silicon oxygen material; And / or, the separator is one of PP, PE or PI films, with a thickness of 6 to 20 μm.
Citation Information
Patent Citations
Rigid conjugated polymer based on benzodifurandione and derivatives thereof as well as preparation and application of rigid conjugated polymer
CN110862517A
Modified high-voltage positive electrode material and preparation method and application thereof
CN111509210A
Cited By
In-situ coated active material with olivine structure and preparation method and application thereof
CN122291464A