A method for reducing the amount of glue applied to polymerized isocyanate plywood
By coating the active anti-seepage agent of the micropore of wood surface cells on the surface of wood veneer, forming a closed film, the problems of formaldehyde pollution and high cost in traditional plywood are solved, and the manufacturing of formaldehyde-free plywood with low glue application is achieved, reducing production Cost and improves glue strength.
Patent Information
- Application Number
- CN202211693518.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-28
AI Technical Summary
The urea-formaldehyde glue used in the manufacturing of traditional plywood leads to formaldehyde contamination, and the high price of polymeric isocyanate (pMDI) adhesives and large glue application volumes lead to excessive production costs, which limits the development of environmentally friendly plywood.
The surface of wood veneer coats the active anti-seepage agent of the micropore of the wood surface to form a closed film, reduce the amount of glue applying of pMDI adhesive, and manufacture low-gluing-free formaldehyde-free plywood sheets through drying and hot pressing.
It effectively reduces the amount of glue applying of pMDI adhesive, reduces production costs, and improves the glue strength while ensuring the physical and chemical properties of plywood, significantly reduces the dependence on high-priced pMDI adhesives.
Smart Images

Figure GDA0004949395250000091
Abstract
Description
Technical Field
[0001] The invention relates to a method for reducing the amount of glue applied to polymerized isocyanate (pMDI) plywood, and belongs to the technical field of plywood preparation. Background Art
[0002] Plywood is one of the important products in the field of wood-based composite materials (artificial boards) production in my country. It has a wide range of uses in furniture, building decoration, automobile interior, rail transit car interior, ship interior and other fields. The manufacture of traditional plywood is made of formaldehyde-containing chemical materials such as urea-formaldehyde and wood veneer through processes such as gluing, assembly, and hot pressing. During the use of this type of plywood, a large amount of toxic carcinogen formaldehyde is released into the environment, causing serious pollution to the indoor living environment where this type of board is used, and causing serious impacts on people's life and health. Therefore, choosing environmentally friendly materials that do not release free formaldehyde as adhesives, and developing and manufacturing environmentally safe formaldehyde-free plywood has become an important problem that needs to be solved in this field, and has become an important development direction for product upgrading in the field of plywood production.
[0003] In the development of environmentally friendly formaldehyde-free adhesive plywood manufacturing technology, the use of formaldehyde-free polymerized isocyanate (pMDI) as an adhesive to manufacture environmentally friendly plywood has become one of the important development directions and a hot topic in the industry. Industrialized products of polymerized isocyanate (pMDI) plywood have appeared in China, but due to the high price of the adhesive and the relatively high amount of glue applied, the high glue cost has seriously restricted the development of this type of plywood products.
[0004] In the field of plywood production, the price of urea-formaldehyde glue required for ordinary plywood production is around 1,500-2,000 yuan / ton, while the price of lower-priced series pMDI adhesive products is around 16,000-20,000 yuan / ton, which is about ten times the price of urea-formaldehyde glue.
[0005] In terms of glue application, the amount of urea-formaldehyde glue applied per square meter of wood veneer in ordinary plywood manufacturing is 80-120g; while the amount of pMDI adhesive applied in formaldehyde-free plywood is 30-50g. Although the amount of pMDI glue applied is 1 / 3 to 1 / 2 of the amount of urea-formaldehyde glue applied, the glue application cost of pMDI environmentally friendly plywood is 3 to 5 times that of ordinary urea-formaldehyde plywood.
[0006] Wood is a porous biomass material formed by various tubular cell structures such as tracheids, vessels, wood fibers, and axial thin-walled cells, and has good permeability to various liquids. Therefore, in the process of gluing wood veneers in plywood manufacturing, a considerable portion of liquid adhesive will penetrate from the surface of the wood veneer to the inside of the wood veneer to varying degrees through the pores of the wood cells. In order to prevent the defective rate caused by the lack of glue on the surface of the wood veneer after gluing due to the penetration of wood, the amount of glue must be increased, which in turn increases the production cost.
[0007] Therefore, under the premise of ensuring the physical and chemical performance indicators of plywood, how to significantly reduce the amount of pMDI adhesive applied and thus significantly reduce production costs has become a technical problem that must be solved for the production and promotion of this type of plywood. Summary of the invention
[0008] The main purpose of the present invention is to provide a method for reducing the amount of polymerized isocyanate (pMDI) plywood glue applied, and to significantly reduce the amount of pMDI adhesive applied while ensuring the physical and chemical performance indicators of the plywood, thereby significantly reducing the production cost.
[0009] The above object of the present invention is achieved through the following technical solutions:
[0010] A method for reducing the amount of glue applied to polymerized isocyanate plywood, comprising the following steps:
[0011] (1) coating a wood surface cell micropore active anti-seepage agent on the surface of a wood veneer with a certain moisture content before drying;
[0012] (2) Then, the veneer coated with the wood cell active anti-seepage agent is dried to form a layer of reactive wood cell microporous closed membrane on the surface of the veneer while the veneer reaches a specified moisture content after drying;
[0013] (3) Then, the pMDI glue is applied at a low amount, single board assembly is performed, the board is hot pressed, and the edge is trimmed to form a pMDI formaldehyde-free plywood.
[0014] Preferably, in step (1), the wood surface cell microporous active anti-seepage agent is composed of two parts, namely, a wood surface cell sealing film-forming agent and a bonding and curing reaction active agent, and these two materials are mixed and prepared in a certain proportion.
[0015] Preferably, in step (1), the wood surface cell sealing film-forming agent is a polyethylene-modified polyvinyl acetate aqueous emulsion (i.e., modified polyvinyl acetate emulsion) with a concentration of 15-50% (mass %), preferably 25-50%.
[0016] Preferably, in step (1), the bonding curing reaction activator is an aqueous solution of polyvinyl alcohol with a molecular weight of 16,000 to 200,000, with a concentration of 5% to 15% (mass %), preferably 5% to 10%.
[0017] Preferably, in step (1), the volume ratio of the wood surface cell sealing film-forming agent to the curing reaction activator is 1:1 to 5:1.
[0018] Preferably, in step (1), the coating amount of the wood surface cell microporous active anti-seepage agent is 50-80 g per square meter of wood veneer.
[0019] Preferably, in step (1), the drying temperature of the wood veneer of the wood surface cell microporous active anti-seepage agent is 30-50° C., and the drying time exceeds 5-20 min.
[0020] Preferably, in step (3), the amount of glue applied to the polymerized isocyanate plywood is: the amount of glue applied per square meter of processed veneer is less than 15 g.
[0021] Preferably, in step (3), the amount of glue applied to the polymerized isocyanate plywood is: the amount of glue applied per square meter of processed veneer is less than 10 g.
[0022] Preferably, in step (2), the drying temperature is 30-50° C. and the drying time is 10-30 min.
[0023] Preferably, in step (3), the hot pressing process of the slab formed by the slab assembly after applying the MDI adhesive is as follows: hot pressing temperature 140-190°C, hot pressing pressure 0.8-1MPa, hot pressing time 25-90s·mm -1 .
[0024] Another object of the present invention is to provide a wood surface cell micropore active anti-seepage agent.
[0025] The above-mentioned object of the present invention is achieved by the following technical solutions:
[0026] A wood surface cell microporous active anti-seepage agent comprises a wood surface cell sealing film-forming agent and a bonding and curing reaction activating agent, wherein the wood surface cell sealing film-forming agent is a polyethylene-modified polyvinyl acetate aqueous emulsion with a concentration of 15-50%; the bonding and curing reaction activating agent is a 5%-15% aqueous solution of polyvinyl alcohol with a molecular weight of 16000-200000; the volume ratio of the wood surface cell sealing film-forming agent to the curing reaction activating agent is 1:1-5:1.
[0027] Preferably, the wood surface cell sealing film-forming agent is a 25% aqueous emulsion of polyethylene-modified polyvinyl acetate; the bonding and curing reaction activator is a 7% aqueous solution of polyvinyl alcohol with a molecular weight of 18,000; the volume ratio of the wood surface cell sealing film-forming agent to the curing reaction activator is 3:1.
[0028] Another object of the present invention is to provide a formaldehyde-free plywood with a low glue application amount.
[0029] The above-mentioned object of the present invention is achieved by the following technical solutions:
[0030] A formaldehyde-free plywood with a low glue dosage comprises a plywood substrate, a wood cell microporous sealing film and a polymerized isocyanate glue coating layer in sequence.
[0031] Preferably, the amount of glue applied to the wood surface cell microporous anti-seepage agent on the plywood is: the amount of glue applied to each square meter of processed veneer is 40-90g.
[0032] Preferably, the amount of glue applied to the polymerized isocyanate plywood is: the amount of glue applied per square meter of processed veneer is less than 15 g.
[0033] Beneficial effects:
[0034] The method for reducing the amount of glue applied to a polymeric isocyanate (pMDI) plywood of the present invention reduces or blocks the deep penetration of the pMDI adhesive into the interior of a wood veneer during the gluing process by adopting a wood surface cell blocking technology with a low production cost, so that most of the adhesive can be retained on the surface of the wood veneer after gluing, thereby preventing the phenomenon of lack of glue on the surface of the veneer caused by the deep penetration of the pMDI adhesive into the interior of the veneer, thereby solving the problem of increased production cost caused by increasing the amount of glue applied due to lack of glue on the surface of the glued veneer. DETAILED DESCRIPTION
[0035] Unless otherwise specified, the raw materials used in the following examples are conventional raw materials available on the market in this field, the equipment used is conventional equipment in this field, the method used is a conventional method, and the units are volume units.
[0036] The method of reducing the amount of glue applied to pMDI plywood of the present invention comprises the following specific processes:
[0037] (1) coating a wood veneer with a certain moisture content with an active wood surface cell microporous anti-seepage agent on the surface of the veneer before drying;
[0038] (2) then, drying the veneer coated with the wood cell active anti-seepage agent, so that the veneer reaches a specified moisture content through the drying process, and a layer of reactive wood cell microporous closed membrane is formed on the surface of the veneer;
[0039] (3) Then, the process of applying pMDI glue at a low amount, assembling single boards, hot pressing the boards, trimming and finishing the boards are performed to finally form a new formaldehyde-free plywood;
[0040] In step (1), the active wood surface cell microporous anti-seepage agent is composed of two parts: a wood surface cell sealing film-forming agent and a bonding and curing reaction activator; the two chemical materials are mixed and prepared in a certain manner; wherein the main component of the wood surface cell sealing film-forming agent is a polyethylene-modified polyvinyl acetate aqueous emulsion with a concentration of 25-50%; the bonding and curing reaction activator is a polyvinyl alcohol (molecular weight 16000-200000) aqueous solution with a concentration of 5%-15%; in the formula of the active wood surface cell microporous anti-seepage agent (blocking agent), the mixing ratio (volume ratio) of the wood surface cell sealing film-forming agent and the bonding and curing reaction activator is 1:1-5:1;
[0041] In step (3), the method for manufacturing the pMDI plywood is carried out according to the following process:
[0042] 1) Coat a layer of the prepared "wood surface cell microporous anti-seepage agent" on the surface of the preliminarily dried wood veneer, with the coating amount being 40-90g per square meter of wood veneer;
[0043] 2) Further drying the wood veneer coated with the plugging agent; the drying temperature of the wood veneer coated with the plugging agent is 30-50°C, and the drying time is 10-30 minutes;
[0044] 3) Applying low-dose MDI adhesive to the dried wood veneer, the amount of glue applied is: the amount of glue applied per square meter of processed veneer is 15g or less, and can be less than 10g under further optimization of other process conditions;
[0045] 4) Single plate assembly;
[0046] 5) The slab is sent to the hot press for hot pressing. The hot pressing process is: hot pressing temperature 140-190℃, hot pressing pressure 0.8-1MPa, hot pressing time 25-90s.mm -1 ;
[0047] 6) Trim the pressed sheet and cut it into the specified size;
[0048] 7) Store the cut pMDI plywood in the warehouse (while balancing the moisture content of the board).
[0049] Example 1
[0050] A method for manufacturing a plywood with a low pMDI plywood glue application comprises the following steps:
[0051] (1) Preparation of wood surface cell microporous anti-seepage agent:
[0052] Preparation of 5 parts by volume of a 5% aqueous solution of polyvinyl alcohol: Use commercially available polyvinyl alcohol with a molecular weight of 18,000 to prepare a 5% aqueous solution. The preparation method is as follows: add 50 g of polyvinyl alcohol to a three-necked flask, then add 950 g of purified water while stirring, and slowly heat up while stirring. Heat to 95°C within 1-2 hours, maintain for 30 minutes, cool down, discharge, and bottle for later use;
[0053] 3 parts by volume of a 50% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 5 parts by volume of a 5% polyvinyl alcohol aqueous solution are poured into a container, stirred at room temperature to form a uniform mixed solution, and a wood surface cell microporous anti-seepage agent is prepared;
[0054] (2) Preparation of wood veneer: logs are peeled to produce wood veneers with a thickness of 1-3 mm; the wood veneers are initially dried to a moisture content of 12-16% by drying on site;
[0055] (3) Applying "active wood surface cell microporous anti-seepage agent" to wood veneer: The wood veneer after preliminary drying is passed through a glue coating machine to apply "active wood surface cell microporous anti-seepage agent" on the wood surface; the coating amount per square meter of the wood veneer surface is 60g;
[0056] (4) Secondary drying of wood veneer to form a film: The veneer coated with "active wood surface cell microporous anti-seepage agent" is subjected to secondary drying treatment in a veneer dryer; the drying temperature is 40°C, the drying time is 20 minutes, and after drying, the moisture content of the veneer is 8-10%, and a sealing film is formed on the surface of the veneer;
[0057] (5) Gluing: Spray pMDI adhesive on the surface of the dried wood veneer at a glue application rate of 15 g per square meter;
[0058] (6) Assembly: The veneers after gluing are assembled in an orthogonal stacking manner to form slabs, and the compression ratio of the finished board to the slab is controlled at 1:1.2;
[0059] (7) Hot pressing: The slab is sent into a hot press for hot pressing. The hot pressing process is as follows: hot pressing temperature 150°C, hot pressing pressure 1 MPa, hot pressing time 45 s.mm -1 ;
[0060] (8) Trimming the pressed sheet to the specified size;
[0061] (9) The cut pMDI plywood is stored in the warehouse (while further balancing the moisture content of the board).
[0062] Example 2
[0063] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: 2 parts of 50% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 4 parts of 5% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container by volume, and stirred at room temperature to form a uniform mixed solution.
[0064] Example 3
[0065] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: 1.5 parts of 50% polyethylene-modified polyacetic acid emulsion (viscosity of 5000-10000, film-forming agent) and 3 parts of 5% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container by volume, and stirred at room temperature to form a uniform mixed solution;
[0066] In step (5), the amount of pMDI adhesive applied is changed to 10 g per square meter.
[0067] Example 4
[0068] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 1 part of a 50% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 2 parts of a 5% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container and stirred at room temperature to form a uniform mixed solution.
[0069] Example 5
[0070] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 2 parts of 45% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 3 parts of 5% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container and stirred at room temperature to form a uniform mixed solution.
[0071] Example 6
[0072] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: 3 parts of 45% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 4 parts of 5% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container by volume, and stirred at room temperature to form a uniform mixed solution;
[0073] In step (5), the amount of pMDI adhesive applied is changed to 10 g per square meter.
[0074] Example 7
[0075] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 3 parts of 40% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 3 parts of 5% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container and stirred at room temperature to form a uniform mixed solution.
[0076] Example 8
[0077] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 3 parts of 35% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 2 parts of 5% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container and stirred at room temperature to form a uniform mixed solution.
[0078] Example 9
[0079] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 1.5 parts of a 35% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 1 part of a 10% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container and stirred at room temperature to form a uniform mixed solution.
[0080] Example 10
[0081] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 2 parts of 35% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity 5000-10000, film-forming agent) and 2 parts of 10% polyvinyl alcohol aqueous solution are prepared into a 10% aqueous solution, the preparation method being: adding 100g of PVC into a three-necked flask, adding 900g of purified water while stirring, and starting to slowly heat up while stirring, heating to 95°C within 1-2h, keeping the temperature for 30min, then cooling to 40°C, discharging and bottling for standby use) into a container, stirring at room temperature to form a uniform mixed solution.
[0082] In step (1), the amount of pMDI adhesive applied was changed to 10 g per square meter.
[0083] Embodiment 11
[0084] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 3 parts of 30% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 2 parts of 5% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container and stirred at room temperature to form a uniform mixed solution.
[0085] Example 12
[0086] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 3 parts of 30% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 1 part of 10% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container and stirred at room temperature to form a uniform mixed solution.
[0087] In step (5), the amount of pMDI adhesive applied is changed to 10 g per square meter.
[0088] Embodiment 13
[0089] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 3 parts of 25% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 1 part of 10% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container and stirred at room temperature to form a uniform mixed solution.
[0090] Embodiment 14
[0091] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 2 parts of 30% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 1 part of 10% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container and stirred at room temperature to form a uniform mixed solution.
[0092] In step (5), the amount of pMDI adhesive applied is changed to 10 g per square meter.
[0093] Embodiment 15
[0094] The other steps are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 3 parts of 25% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 1 part of 15% polyvinyl alcohol (PVC) aqueous solution (PVC is prepared into a 15% aqueous solution, the preparation method is: add 150g PVC into a three-necked flask, then add 850g pure water while stirring, start to slowly heat up, heat up while stirring, heat to 95°C within 1-2h, keep it for 30min, then cool down to 40°C, discharging and bottling for use as an adhesive curing reaction activator) are poured into a container, stirred at room temperature to form a uniform mixed solution.
[0095] In step (5), the amount of pMDI adhesive applied is changed to 10 g per square meter.
[0096] Example 16
[0097] The other parts are the same as those in Example 1, except that: in step (1), the preparation of the wood surface cell microporous anti-seepage agent in Example 1 is changed to: by volume, 2 parts of 25% polyethylene-modified polyvinyl acetate aqueous emulsion (viscosity of 5000-10000, film-forming agent) and 2 parts of 15% polyvinyl alcohol aqueous solution (adhesive curing reaction activator) are poured into a container and stirred at room temperature to form a uniform mixed solution.
[0098] In step (1), the amount of pMDI adhesive applied was changed to 10 g per square meter.
[0099] Comparative Example 1
[0100] The other steps are the same as those in Example 1, except that: in the preparation process of Example 1, the veneer is not coated with a wood surface cell microporous anti-seepage agent and is not dried for the second time.
[0101] Comparative Example 2
[0102] The other steps are the same as those in Example 1, except that: first, in the preparation process of Example 1, the veneer is not coated with a wood surface cell microporous anti-seepage agent and is not dried for the second time;
[0103] Secondly, the amount of pMDI adhesive applied was changed to 10g per square meter.
[0104] Comparative Example 3
[0105] The other steps are the same as those in Example 1, except that: first, in the preparation process of Example 1, the veneer is not coated with a wood surface cell microporous anti-seepage agent and is not dried for the second time;
[0106] Secondly, the amount of pMDI adhesive applied was changed to 40g per square meter.
[0107] The appearance of the wood surface cell microporous anti-seepage agent prepared in the above examples is a white emulsion without mechanical impurities.
[0108] The properties and bonding strength of the plywood prepared in the above embodiments and comparative examples were tested according to the following standards:
[0109] 1. GB / T 14074—2016. Test methods for wood adhesives and their resins[S]. Beijing: China Standards Press, 2016;
[0110] 2. GB / T 17657—2013. Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels[S]. Beijing: China Standards Press, 2013.
[0111] The bonding strength test is carried out in accordance with Class I bonding strength test regulations, and its 28h bonding strength is tested.
[0112] 28h bonding strength: Place the specimen in boiling water for 4h, then dry it in an air convection drying oven at (60±3)℃ for 20h, and then boil it in boiling water for 4h. After taking it out, place it in room temperature water, cool it for 10min, and then test it immediately.
[0113] The test results are listed in Table 1
[0114] Table 1 Test results
[0115]
[0116] The test results show that the average bonding strength of the plywood prepared in Comparative Example 1, which has not been treated with the microporous active anti-seepage agent for wood veneer, just reaches the requirement of Class I bonding strength (0.7MPa), but more than 40% of the test pieces fail to meet the requirements; the average bonding strength of the plywood prepared in Comparative Example 2 with a lower application amount fails to meet the requirement of Class I bonding strength; the bonding strength of Examples 1-16 with the same application amount level is significantly improved compared with Comparative Examples 1 and 2, indicating that the coating of the microporous active anti-seepage agent for wood veneer can greatly improve the bonding strength under the condition of low pMDI application amount.
[0117] Glue application amount 15g / m 2 Examples 2, 7 and 13, with a sizing amount of 40 g / m 2 The bonding strength of Example 3 is basically the same, indicating that the microporous active anti-seepage agent for wood veneer helps to reduce the amount of pMDI used and significantly reduce the board's dependence on high-priced pMDI adhesives. 2 At the same coating amount of the wood veneer microporous active anti-seepage agent, the comprehensive glue cost is 75% of that in Example 3.
[0118] After being treated with wood veneer microporous active anti-seepage agent, 10g / m 2 Under the conditions of pMDI glue application, the board has easily reached Class I bonding strength, which has greatly reduced the comprehensive glue cost of environmentally friendly pMDI plywood.
[0119] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent structural transformation made using the contents of the present invention specification, or directly or indirectly applied to the technical field attached to other related products, are also included in the patent protection scope of the present invention.
Claims
1. A method for reducing the amount of glue applied to polymerized isocyanate plywood, the steps of which are as follows: (1) Before drying a wood veneer with a certain moisture content, a wood surface cell microporous active anti-seepage agent is first coated on the surface of the veneer; the wood surface cell microporous active anti-seepage agent is composed of a wood surface cell sealing film-forming agent and a bonding and curing reaction activator; the wood surface cell sealing film-forming agent is a polyethylene-modified polyvinyl acetate aqueous emulsion with a concentration of 15-50%; the bonding and curing reaction activator is a polyvinyl alcohol aqueous solution with a molecular weight of 16000-200000 with a concentration of 5%-15%; the volume ratio of the wood surface cell sealing film-forming agent to the curing reaction activator is 1:1-5:1; (2) drying the veneer coated with the wood surface cell microporous active anti-seepage agent obtained in step (1) to achieve a specified moisture content after drying, thereby forming a layer of reactive wood cell microporous closed membrane on the surface of the veneer; (3) Applying pMDI glue at a low amount, assembling single boards, hot pressing the boards, trimming and finishing them into boards, and finally forming pMDI formaldehyde-free plywood.
2. The method for reducing the amount of glue applied to polymerized isocyanate plywood according to claim 1, characterized in that: In step (1), the coating amount of the wood surface cell microporous active anti-seepage agent is 50-80g per square meter of wood veneer.
3. The method for reducing the amount of glue applied to polymerized isocyanate plywood according to claim 2, characterized in that: In step (1), the drying temperature of the wood veneer with the wood surface cell microporous active anti-seepage agent is 30-50° C. and the drying time is 5-20 min.
4. The method for reducing the amount of glue applied to polymerized isocyanate plywood according to claim 1, characterized in that: In step (3), the amount of glue applied to the polymerized isocyanate plywood is: the amount of glue applied per square meter of single board is less than 15 g.
5. The method for reducing the amount of glue applied to polymerized isocyanate plywood according to claim 4, characterized in that: In step (3), the amount of glue applied to the polymerized isocyanate plywood is: the amount of glue applied per square meter of single board is less than 10 g.
6. The method for reducing the amount of glue applied to polymerized isocyanate plywood according to claim 1, characterized in that: In step (2), the drying temperature is 30-50°C and the drying time is 10-30 min. In step (3), the hot pressing process is: hot pressing temperature is 140-190°C, hot pressing pressure is 0.8-1 MPa, and hot pressing time is 25-90 s·mm. -1 .
7. A wood surface cell micropore active anti-seepage agent, characterized in that: The invention comprises a wood surface cell sealing film-forming agent and a bonding and curing reaction activator, wherein the wood surface cell sealing film-forming agent is a polyethylene-modified polyvinyl acetate aqueous emulsion with a concentration of 15%-50%; the bonding and curing reaction activator is a polyvinyl alcohol aqueous solution with a molecular weight of 16000-200000 with a concentration of 5%-15%; and the volume ratio of the wood surface cell sealing film-forming agent to the curing reaction activator is 1:1-5:
1.
8. The wood surface cell micropore active anti-seepage agent according to claim 7, characterized in that: The wood surface cell sealing film-forming agent is a 25% aqueous emulsion of polyethylene-modified polyvinyl acetate; the bonding and curing reaction activator is a 15% aqueous solution of polyvinyl alcohol with a molecular weight of 16,000 to 200,000; the volume ratio of the wood surface cell sealing film-forming agent to the curing reaction activator is 3:
1.
9. A formaldehyde-free plywood with low glue application, comprising a plywood substrate, a wood cell microporous sealing membrane and a polymerized isocyanate coating layer, characterized in that: The wood cell microporous closed membrane is obtained by coating the wood surface cell microporous active anti-seepage agent as claimed in claim 7 or 8.