Lithium secondary battery and battery module, battery pack and power-consuming device containing same

CN115917816BActive Publication Date: 2024-11-12CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080102371.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-24
Publication Date
2024-11-12
Estimated Expiration
2040-12-24

AI Technical Summary

Technical Problem

铁析出容易破坏SEI膜,也会进一步刺穿隔膜造成电池的短路,安全性较低

Benefits of technology

[0038]本申请的电池模块、电池包和用电装置包括本申请提供的二次电池,因而至少具有与所述二次电池相同的优势。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115917816B_ABST
    Figure CN115917816B_ABST
Patent Text Reader

Abstract

The present application discloses a secondary battery, a battery module, a battery pack and a device containing the secondary battery. The positive electrode includes a positive electrode active material layer, the positive electrode active material layer contains a lithium compensator, and the molecular formula of the lithium compensator is Li x Ni a Cu 1‑a‑b M b O2, where 1 ≤ x ≤ 2, 0 < a < 1, 0 ≤ b < 0.1, and M is selected from one or more of Zn, Sn, Mg, Fe, and Mn. The negative electrode active material includes graphite and a silicon material. The electrolyte contains fluoroethylene carbonate (FEC). The mass percentages of the lithium compensator, the silicon content of the negative electrode, and fluoroethylene carbonate (FEC) satisfy 0.2 × W Si ≤ W FEC ≤ 7.5% - 0.6 × W L . Thus, the cycle life can be improved, a better charge-discharge specific capacity can be obtained, and the amount of self-discharge of the battery can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of lithium secondary batteries, and relates to a lithium secondary battery, and in particular to a lithium secondary battery containing a lithium compensator in a positive electrode active material layer, and a battery module, a battery pack and an electrical device having the lithium secondary battery. Background Art

[0002] Lithium secondary batteries have the advantages of high energy density, long cycle life and no memory effect, and are widely used in many consumer electronic products. In recent years, with the continuous development of electric vehicles and energy storage systems, the requirements for the energy density of lithium secondary batteries are also increasing.

[0003] At the same time, silicon materials have become a potential negative electrode material for lithium secondary batteries with high energy density due to their ultra-high theoretical specific capacity. However, due to the poor conductivity of pure silicon materials and the volume expansion of up to 300%, the solid electrolyte interface film SEI formed on the electrode surface is constantly broken and repaired, consuming more lithium, thus shortening the cycle life of lithium secondary batteries.

[0004] In order to compensate for the consumed lithium, replenishing lithium to the positive electrode is an effective application method. In terms of positive electrode lithium replenishment, the lithium replenisher that is currently being studied more is Li5FeO4. This type of lithium-rich material has a high theoretical specific capacity, but other metal ions (such as iron ions) generated after delithiation will shuttle to the negative electrode for reduction. Iron precipitation can easily destroy the SEI film and further pierce the diaphragm, causing a short circuit in the battery, which has low safety. In addition, Li5FeO4 will also release oxygen after delithiation, causing oxidation of the electrolyte and attenuation of the battery capacity. Summary of the invention

[0005] The present application is made in view of the above technical problems, and its purpose is to provide a lithium secondary battery, including: a positive electrode, a negative electrode and an electrolyte; wherein:

[0006] The positive electrode comprises a positive electrode active material layer, wherein the positive electrode active material layer contains a lithium compensator, and the molecular formula of the lithium compensator is Li x Ni a Cu 1-a-b M b O2, wherein 1≤x≤2, 0<a<1, 0≤b<0.1, and M is selected from one or more of Zn, Sn, Mg, Fe and Mn;

[0007] The negative electrode comprises a negative electrode active material layer, wherein the negative electrode active material layer contains a first negative electrode active material and a second negative electrode active material, wherein the first negative electrode active material is graphite, and the second negative electrode active material is selected from Si, SiO n (0<n<2), one or more of SiC;

[0008] The electrolyte contains fluoroethylene carbonate (FEC);

[0009] The lithium secondary battery meets the following requirements: 0.2×W Si ≤W FEC ≤7.5%-0.6×W L , where W FEC is the mass proportion of the FEC in the electrolyte, W Si is the mass ratio of the silicon element in the second negative electrode active material in the negative electrode active material layer, W L is the mass ratio of the lithium compensator in the positive electrode active material layer.

[0010] According to the above structure, the lithium compensator Li x Ni a C u1-a-b M b O2 can compensate for the lithium consumed in forming and repairing the solid electrolyte interface film SEI, and since the lithium compensator does not contain Fe, it can avoid iron precipitation and damage the SEI film. In addition, a dense SEI film can be formed by the fluoroethylene carbonate (FEC) contained in the electrolyte, making the SEI film difficult to rupture, so that the cycle can maintain a slower capacity decay rate and obtain a better charge and discharge specific capacity. However, too much fluoroethylene carbonate (FEC) will worsen gas production, causing the pole piece to expand, and will cause the metallic copper in the lithium compensator L to dissolve, worsening the self-discharge of the system. Here, by controlling the content of fluoroethylene carbonate (FEC) and lithium compensator, the problem of battery self-discharge caused by the precipitation of transition metal ions in the lithium compensator at the negative electrode can be reduced. According to the lithium secondary battery of the present invention, by controlling the mass ratio of fluoroethylene carbonate (FEC), silicon element and lithium compensator within the above range, the loss of active lithium in the silicon negative electrode can be effectively compensated, the capacity decay rate during the cycle can be maintained at a slower rate to improve the cycle life, and a better charge and discharge specific capacity can be obtained, and the amount of battery self-discharge can be reduced.

[0011] In any embodiment, the W L With the W Si Satisfy the conditions: -2.2% ≤ W L -W Si ≤2.5%.

[0012] Since the initial coulombic efficiency (ratio of initial discharge capacity to charge capacity) of the secondary battery with silicon negative electrode is low, if the silicon content increases, more lithium compensator is needed to supplement the active lithium. By keeping the mass ratio of silicon element and lithium compensator within the above range, the active lithium can be effectively supplemented for the silicon negative electrode, so that the capacity decay rate during circulation and storage is kept at a slower rate, thereby improving the cycle life and storage life, and obtaining a better charge and discharge specific capacity. Among them, when W L ≥W Si -2.2%, the lithium compensator can supplement sufficient active lithium for the silicon negative electrode secondary battery; at the same time, when W L ≤W Si When the value is +2.5%, the ratio of the amount of lithium removed from the negative electrode active material and the amount of lithium inserted into the positive electrode lithium vacancies of the lithium compensator is moderate, thereby further improving the discharge specific capacity of the battery.

[0013] In any embodiment, the W L is 0.1% to 10%, optionally, the W L is 0.2% to 9%, and further optionally, the W L When the amount of lithium compensator added is within the above range, sufficient active lithium can be added to compensate for the lithium loss during the film formation and cycle process of the positive and negative electrodes, ensuring that the ratio of the negative electrode active material to the positive electrode lithium vacancies containing the lithium compensator is appropriate, thereby further improving the discharge capacity of the secondary battery.

[0014] In any embodiment, the W Si is 0.5wt% to 10wt%, optionally, the W Si is 1wt% to 8wt%, and further optionally, the W Si It is 1.5wt%~6wt%.

[0015] Therefore, only by keeping the silicon content within the above range can the cycle life and storage life be effectively improved by adding lithium compensators, and a better charge-discharge specific capacity can be obtained. In this application, when the Si content in the negative electrode is within the above range, on the one hand, the energy density of the secondary battery can be improved; at the same time, the amount of lithium compensator L required can be controlled to improve the cycle, storage life and self-discharge problems of the secondary battery.

[0016] In any embodiment, the W FEC is 0.1wt% to 7.5wt%, optionally, the W FEC is 0.5wt% to 6wt%, and further optionally, the W FEC It is 1wt% to 5wt%.

[0017] Thus, by keeping the content of fluoroethylene carbonate (FEC) within the above range, the cycle life can be improved and the amount of self-discharge can be reduced. It is speculated that the reason may be that when the content of fluoroethylene carbonate (FEC) in the electrolyte is within the above range, a dense SEI film can be formed on the surface of the negative electrode (especially silicon particles), effectively improving the interface side reaction between silicon particles and the electrolyte, thereby improving the cycle life of the secondary battery; at the same time, limiting the upper limit of the content of fluoroethylene carbonate (FEC) can also reduce the dissolution of copper elements in the lithium compensator, improving the problem of increased self-discharge rate of the secondary battery.

[0018] In any embodiment, the specific surface area of ​​the lithium compensator is BET L The value is 0.3m 2 / g~10m 2 / g, optional, the BET L 0.6m 2 / g~3.5m 2 / g.

[0019] Thus, the specific surface area BET of the lithium compensator L The value is within the above range, which can avoid the occurrence of gelation problems during the preparation of the positive electrode sheet, thereby avoiding the decrease in cycle characteristics and discharge capacity ratio. L When within the above range, on the one hand, the lithium compensator does not agglomerate, thereby improving the problem of easy gelation of the positive electrode slurry and increasing the battery cycle life and charge and discharge specific capacity; at the same time, it can also improve the matching degree with the positive electrode active material and enhance the capacity of the lithium compensator, which is conducive to further exerting the contribution of the lithium compensator to the charge and discharge capacity ratio.

[0020] In any embodiment, the volume average particle size D of the lithium compensating agent is v 50 L 1 μm to 20 μm, optionally, the D v 50 L 3μm~13μm.

[0021] Therefore, the volume average particle size D of the lithium compensating agent v 50 L Within the above range, problems such as gelation during the preparation of the positive electrode sheet can be avoided, thereby avoiding the decrease in cycle characteristics and discharge capacity ratio. v 50 L When within the above range, the lithium compensator is not easy to agglomerate, making the positive electrode slurry not easy to gel, thereby improving the battery cycle life and charge and discharge capacity ratio; at the same time, it can also improve the matching degree with the positive electrode active material, enhance the capacity of the lithium compensator, and help further exert the contribution of the lithium compensator to the charge and discharge capacity ratio.

[0022] In any embodiment, the positive electrode further comprises a positive electrode active material, and the positive electrode active material comprises at least one of the compounds represented by formula (I) to formula (III):

[0023] Li 1+x1 Ni a1 Co b1 M' 1-a1-b1 O 2-y1 A y1 (I);

[0024] Li 1+x2 Mn a2 M” 2-a2 O 4-d A' d (II);

[0025] LiFe (1-x3-y3) Mn x3 M'" y3 PO4 (III);

[0026] Wherein, in the formula (I), -0.1≤x1≤0.2, 0<a1<1, 0≤b1≤1, 0<a1+b1<1, 0≤y1<0.2, M' is one or more of Mn, Fe, Cr, Ti, Zn, V, Al, Zr and Ce, A includes one or more of S, N, F, Cl, Br and I; optionally, 0.5≤a1<1, 0<b1<0.5, 0.7≤a1+b1<1, 0≤y<0.1, M is M n and Al, A is one or two of S or F;

[0027] Wherein, in the formula (II), -0.1≤x2≤0.2, 0<a2≤2, 0≤d<1, M″ includes one or more of Ni, Fe, Cr, Ti, Zn, V, Al, Mg, Zr and Ce, A includes one or more of S, N, F, Cl, Br and I;

[0028] Wherein, in the formula (III), 0≤x3≤1, 0≤y3≤0.1, and M''' is selected from one or more transition metal elements and non-transition metal elements except Fe and Mn;

[0029] Optionally, the positive electrode active material includes at least the compound represented by formula (I).

[0030] Therefore, the above-mentioned lithium compensating agent can be used in combination with various positive electrode active materials, which can improve the cycle life and storage life, obtain better charge and discharge specific capacity, and reduce the amount of battery self-discharge.

[0031] In any embodiment, the positive electrode further comprises a positive electrode active material, the positive electrode active material comprises a lithium transition metal oxide having a layered structure, and the volume average particle size D of the lithium compensator is v 50 L The volume average particle size D of the lithium transition metal oxide v 50 N Satisfy: 0.3≤D v 50 L / D v 50 N ≤3.6, optional, 0.7≤D v 50 L / D v 50 N ≤3.

[0032] Thus, by having the particle size ratio of the lithium compensator to the lithium transition metal oxide with a layered structure within the above range, the slurry of the positive electrode active material is not easy to gel, has better stability, and the lithium compensator contributes more to the charge and discharge capacity. In the present application, when the particle size ratio of the lithium compensator to the lithium transition metal oxide with a layered structure is within the above range, the positive electrode material is not easy to gel, which is beneficial to improving the cycle life and charge and discharge specific capacity of the secondary battery; at the same time, it can also improve the matching degree with the positive electrode active material, which is beneficial to the capacity of the lithium compensator and improves the contribution of the lithium compensator to the charge and discharge capacity ratio.

[0033] In any embodiment, the positive electrode further comprises a positive electrode active material, the positive electrode active material comprises a lithium phosphate having an olivine structure, and the volume average particle size D of the lithium compensator is v 50 L The volume average particle size D of the lithium phosphate having an olivine structure v 50 P Satisfies: 1≤D v 50 L / D v 50 P ≤15, optional, 2.5≤D v 50 L / D v 50 P ≤11.

[0034] Therefore, when the particle size ratio of the lithium compensating agent to the lithium phosphate having an olivine structure is within the above range, the slurry of the positive electrode active material is not easy to gel, has good stability, and the contribution of the lithium compensating agent to the capacity is also high.

[0035] A second aspect of the present application provides a battery module, which includes the secondary battery according to the first aspect of the present application.

[0036] A third aspect of the present application provides a battery pack, which includes a battery module according to the second aspect of the present application.

[0037] A fourth aspect of the present application provides an electrical device comprising at least one of the secondary battery according to the first aspect of the present application, the battery module according to the second aspect of the present application, or the battery pack according to the third aspect of the present application.

[0038] The battery module, battery pack and electric device of the present application include the secondary battery provided by the present application, and thus have at least the same advantages as the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a schematic diagram of a secondary battery according to one embodiment of the present application.

[0040] Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of the present application is shown.

[0041] Figure 3 is a schematic diagram of a battery module according to an embodiment of the present application.

[0042] Figure 4 It is a schematic diagram of a battery pack according to one embodiment of the present application.

[0043] Figure 5 yes Figure 4 An exploded view of a battery pack according to an embodiment of the present application is shown.

[0044] Figure 6 FIG. 1 is a schematic diagram of a device in which a secondary battery according to an embodiment of the present application is used as a power source.

[0045] Description of reference numerals:

[0046] 1 battery pack

[0047] 2 upper box

[0048] 3 lower cabinets

[0049] 4 battery modules

[0050] 5. Secondary battery

[0051] 51 Shell

[0052] 52 electrode assembly

[0053] 53 Top cover assembly DETAILED DESCRIPTION

[0054] In order to make the purpose, technical solution and advantages of the present application clearer, the embodiments of the present application will be described in detail below in conjunction with the accompanying drawings. However, those skilled in the art should understand that these embodiments are only used to illustrate the technical solution of the present application and are not limiting.

[0055] For simplicity, the present application specifically discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, and any upper limit can be combined with any other upper limit to form an undefined range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an undefined range.

[0056] In the description of this article, it should be noted that, unless otherwise specified, "above" and "below" are inclusive of the number itself, and "several" in "one or several" means two or more.

[0057] The above-mentioned summary of the invention of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of examples, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0058] Secondary battery

[0059] The embodiment of the first aspect of the present application provides a secondary battery. The secondary battery includes a positive electrode sheet, a negative electrode sheet and an electrolyte. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet.

[0060] [Negative electrode]

[0061] The negative electrode plate of the present application includes a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, and the negative electrode film layer includes a negative electrode active material.

[0062] In the secondary battery of the present application, the negative electrode active material may include, but is not limited to, graphite and silicon-based materials. The above-mentioned graphite may include artificial graphite, natural graphite or a mixture thereof. The silicon-based material may be selected from one or more of elemental silicon, silicon oxides (such as silicon monoxide), silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. These materials can be obtained through commercial channels. Specifically, the negative electrode active material layer may contain a first negative electrode active material and a second negative electrode active material, wherein the first negative electrode active material is graphite, and the second negative electrode active material is selected from Si, SiO n (0<n<2), SiC or one or more thereof.

[0063] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0064] In the secondary battery of the present application, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0065] In the secondary battery of the present application, the negative electrode film layer generally comprises a negative electrode active material and an optional binder, an optional conductive agent and other optional auxiliary agents, and is generally formed by coating and drying a negative electrode slurry. The negative electrode slurry coating is generally formed by dispersing the negative electrode active material and the optional conductive agent and binder in a solvent and stirring them uniformly. The solvent may be N-methylpyrrolidone (NMP) or deionized water.

[0066] As an example, the conductive agent may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0067] As an example, the binder can be selected from one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0068] Other optional auxiliary agents include, for example, thickeners (such as sodium carboxymethyl cellulose (CMC-Na)).

[0069] [Positive electrode]

[0070] The positive electrode plate includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.

[0071] The positive electrode active material may include at least one of the compounds represented by formula (I) to formula (III):

[0072] Li 1+x1 Ni a1 Co b1 M' 1-a1-b1 O 2-y1 A y1 (I);

[0073] Li 1+x2 Mn a2 M” 2-a2 O 4-d A' d (II);

[0074] LiFe (1-x3-y3) Mn x3 M'" y3 PO4 (III);

[0075] Wherein, in the formula (I), -0.1≤x1≤0.2, 0<a1<1, 0≤b1≤1, 0<a1+b1<1, 0≤y1<0.2, M' is one or more of Mn, Fe, Cr, Ti, Zn, V, Al, Zr and Ce, and A includes one or more of S, N, F, Cl, Br and I; optionally, 0.5≤al<1, 0<b1<0.5, 0.7≤al+b1<1, 0≤y<0.1, M is one or both of Mn and Al, and A is one or both of S or F;

[0076] Wherein, in the formula (II), -0.1≤x2≤0.2, 0<a2≤2, 0≤d<1, M″ includes one or more of Ni, Fe, Cr, Ti, Zn, V, Al, Mg, Zr and Ce, A includes one or more of S, N, F, Cl, Br and I;

[0077] Wherein, in the formula (III), 0≤x3≤1, 0≤y3≤0.1, and M''' is selected from one or more transition metal elements and non-transition metal elements except Fe and Mn.

[0078] The positive electrode sheet also includes a lithium compensator L, the molecular formula of which is Li x Ni a C u1-a-b M bO2, wherein 1≤x≤2, 0<a<1, 0≤b<0.1, and M is selected from one or more of Zn, Sn, Mg, Fe and Mn. Specifically, the lithium compensator L can be a metal oxide with lithium, nickel and copper as main components, and one or more of Zn, Sn, Mg, Fe and Mn can be added in small amounts.

[0079] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0080] In the secondary battery of the present application, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0081] The positive electrode film layer may also optionally include a conductive agent. However, there is no specific limitation on the type of the conductive agent, and those skilled in the art may select it according to actual needs. As an example, the conductive agent used for the positive electrode film layer may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0082] In the present application, the positive electrode sheet can be prepared according to methods known in the art. As an example, the positive electrode active material, conductive agent and binder of the present application can be dispersed in a solvent (such as N-methylpyrrolidone (NMP)) to form a uniform positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet is obtained.

[0083] [Electrolytes]

[0084] In the secondary battery of the present application, there is no specific restriction on the type of electrolyte, which can be selected according to the needs. The electrolyte can be selected from at least one of a solid electrolyte and a liquid electrolyte (ie, an electrolyte solution).

[0085] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte lithium salt and a solvent.

[0086] Optionally, the lithium salt can be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0087] The solvent contains fluoroethylene carbonate (FEC), which can enhance the negative electrode film formation and form a dense solid electrolyte interface film (SEI film).

[0088] Optionally, the solvent may also include one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), cyclopentane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0089] In some embodiments, the electrolyte may also optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, and additives that improve battery low temperature performance.

[0090] [Relationship between positive electrode lithium compensator, electrolyte, and negative electrode silicon content]

[0091] In some embodiments, the lithium secondary battery satisfies: 0.2×W Si ≤W FEC ≤7.5%-0.6×W L , where W FEC is the mass proportion of the FEC in the electrolyte, W Si is the mass ratio of the silicon element in the second negative electrode active material in the negative electrode active material layer, W L is the mass proportion of the lithium compensator L in the positive electrode active material layer.

[0092] According to the above lithium ion secondary battery, the lithium compensating agent Li x Ni a C u1-a-b M b O2 can compensate for the lithium consumed by the formation and repair of the solid electrolyte interface film SEI, and, since the lithium compensator does not contain Fe, it can avoid iron precipitation and damage the SEI film. In addition, a dense SEI film can be formed by the fluoroethylene carbonate (FEC) contained in the electrolyte, making the SEI film difficult to rupture, so that the cycle can maintain a slower capacity decay rate and obtain a better charge and discharge specific capacity. However, too much fluoroethylene carbonate (FEC) will deteriorate gas production, and will cause the metal copper in the lithium compensator L to dissolve, deteriorating the self-discharge of the system. By controlling the content of fluoroethylene carbonate (FEC) and lithium compensator, the problem of battery self-discharge caused by the precipitation of transition metal ions in the lithium compensator at the negative electrode can be reduced. According to the above-mentioned lithium secondary battery, the mass proportion of fluoroethylene carbonate (FEC), silicon element, and lithium compensator is within the above-mentioned range, which can effectively compensate for the loss of active lithium in the silicon negative electrode, so that the cycle maintains a slower capacity decay rate and improves the cycle life, and obtains a better charge and discharge specific capacity, and can reduce the amount of battery self-discharge. If fluoroethylene carbonate (FEC) is less than 0.2×W Si If the fluoroethylene carbonate (FEC) is greater than 7.5%-0.6×W L , the transition metal ions in the lithium compensator L are excessively precipitated at the negative electrode, thereby causing the problem of battery self-discharge.

[0093] In the present application, the mass proportion of the FEC in the electrolyte is W FEC The test method known in the art can be used for determination. For details, reference can be made to GB / T 9722-2006 General Rules for Gas Chromatography of Chemical Reagents for testing. As an example, the gas chromatograph Agilgent 7890B can be used to measure the electrolyte to be injected or the electrolyte obtained by centrifugation of the finished battery cell.

[0094] In the present application, the mass proportion of silicon in the second negative electrode active material in the negative electrode active material layer is W SiThe test method known in the art can be used for determination. As an example, the following method can be used for testing: select the plasma emission spectrometer model ICAP7400 of Thermo Fisher Scientific, USA, and measure it by ICP method. The test sample can be a negative electrode sheet after coating and cold pressing, or a negative electrode sheet disassembled from a battery cell (let the battery cell stand at 25°C for 30 minutes; discharge at a constant current of 0.33C to the battery cell discharge termination voltage, then stand for 30 minutes for full discharge, then disassemble the battery cell, take out the negative electrode sheet, rinse it appropriately with DMC solution, and dry it for use).

[0095] In the present application, the lithium compensator L accounts for W of the mass of the positive electrode active material layer. L The measurement can be carried out by a test method known in the art. As an example, the following method can be used for testing: For a mixed electrode of lithium compensator L and positive electrode active materials that do not contain Ni and Cu elements, such as lithium iron phosphate, ICP (such as the plasma emission spectrometer model ICAP7400 of ThermoFisher Scientific, USA) can be used to test and obtain the Ni / Cu ratio and the mass proportion of lithium compensator L. For a mixed electrode of lithium compensator L and positive electrode active materials containing Ni elements, such as lithium nickel cobalt manganese oxide, ICP (plasma emission spectrometer model ICAP7400 of Thermo Fisher Scientific, USA) can be used to first test and obtain the mass proportion of various elements such as Ni, Co, Mn, Cu, etc. in the positive electrode, and then combine it with EDS (OXFORDEDS X-max-50mm 2 ) Perform a mapping test on the surface or cross-section of the positive electrode, find the copper-rich area (corresponding to the lithium compensator L), narrow the range, test the Ni / Cu ratio of the copper-rich area, which is the Ni / Cu ratio of the lithium compensator L, and then obtain the mass proportion of the L material based on the mass proportion of each element in the ICP test.

[0096] In some embodiments, W L With W Si Satisfy the conditions: -2.2% ≤ W L -W Si ≤2.5%.

[0097] Since the initial coulombic efficiency (ratio of initial discharge capacity to charge capacity) of the secondary battery with silicon negative electrode is low, as the silicon content increases, more lithium compensator L is needed to supplement the active lithium. By keeping the mass ratio of silicon element and lithium compensator L within the above range, the loss of active lithium in silicon negative electrode can be effectively compensated, so that the capacity decay rate during circulation and storage is kept at a relatively slow rate, thereby improving the cycle life and storage life, and obtaining a better charge and discharge specific capacity. Among them, when W L ≥WSi -2.2%, the lithium compensator can supplement sufficient active lithium for the silicon negative electrode secondary battery; at the same time, when W L ≤W Si When the content of lithium vacancies in the positive electrode is more than 2.5%, the ratio of the negative electrode active material to the positive electrode lithium vacancies containing the lithium compensator is moderate, thereby further improving the discharge specific capacity of the battery.

[0098] In some embodiments, W L is 0.1% to 10%, optionally, the W L is 0.2% to 9%, and further optionally, the W L When the amount of lithium compensator added is within the above range, sufficient active lithium can be provided for positive and negative electrode film formation, while ensuring that the ratio of negative electrode active material to positive electrode lithium vacancies containing lithium compensator is appropriate, thereby further improving the discharge specific capacity of the secondary battery.

[0099] In some embodiments, W Si 0.5wt%10wt%, optionally, the W Si is 1wt% to 8wt%, and further optionally, the W Si 1.5wt% to 6wt%. By keeping the silicon content within the above range, the cycle life and storage life can be improved, and a better charge-discharge specific capacity can be obtained. In the present application, when the Si content in the negative electrode is within the above range, on the one hand, the energy density, cycle and storage life of the secondary battery can be improved, and at the same time, the amount of lithium compensator L required can be controlled to improve the self-discharge problem of the secondary battery.

[0100] In some embodiments, W FEC 0.1wt%~~7.5wt%, optionally, the W FEC is 0.5wt% to 6wt%, and further optionally, the W FEC 1wt% to 5wt%. By keeping the content of fluoroethylene carbonate (FEC) within the above range, the cycle life can be improved and the amount of self-discharge can be reduced. It is speculated that the reason may be that when the content of fluoroethylene carbonate (FEC) in the electrolyte is within the above range, a dense SEI film can be formed on the surface of the negative electrode (especially silicon particles), effectively improving the interface side reaction between silicon particles and the electrolyte, thereby improving the cycle life of the secondary battery; at the same time, it can also reduce the dissolution of copper elements in the lithium compensator, and improve the problem of increased self-discharge rate of the secondary battery.

[0101] [Lithium compensator L]

[0102] In some embodiments, the specific surface area BET of the lithium compensating agent L is L The value is 0.3m 2 / g~10m2 / g, optional, the BET L 0.6m 2 / g~3.5m 2 / g.

[0103] Lithium compensator L contains more lithium, has strong alkalinity, high activity, large particles and is sensitive to water. It is easy to cause gelation and other problems during the preparation of positive electrode sheets, resulting in poor stability of positive electrode slurry and greatly reducing the yield. L When the value is within the above range, gel can be reduced, the cycle life can be further improved, and a better charge-discharge specific capacity can be obtained.

[0104] In the present application, the specific surface area of ​​the lithium compensator L can be measured by a test method known in the art. For specific test methods and steps, refer to the standard: GB / T 19587-2004 "Gas Adsorption BET Method for Determination of Specific Surface Area of ​​Solid Matter". As an example, the instrument model NOVA 2000e can be used, and the following process can be used for testing: (1) Take a certain amount of sample (e.g., 2.0-15.0g); (2) Put the sample into a sample tube, put it into a heating bag, and degas it (degassing conditions are 200°C, 2 hours); (3) After degassing is completed, when the temperature of the degassing station drops to room temperature, remove the sample tube from the degassing station, weigh and calculate the total mass of the sample; (4) Put the sample tube into a test filling rod to test the specific surface area of ​​the sample.

[0105] In some embodiments, the volume average particle size D of the lithium compensator is v 50 L 1 μm to 20 μm, optionally, the D v 50 L The volume average particle size of the lithium compensator is within the above range, which can reduce gelation, ensure cycle life, and obtain a better charge-discharge specific capacity.

[0106] In the present application, the volume average particle size D of the lithium compensator L is v 50 LThe measurement can be carried out by a test method known in the art. As an example, the following method can be used for testing: refer to GB / T 19077-2016 particle size distribution laser diffraction method, and use a laser particle size analyzer (such as the British Malvern Mastersizer 2000E) for measurement. For the positive electrode plate into which the lithium compensator L has been mixed, a scanning electron microscope (SEM, ZEISS SEM Sigma 300) and ion polishing cross-sectional morphology analysis (CP) can also be used to select multiple areas (for example, more than 20 areas), and measure the visible maximum particle size of the lithium compensator L respectively, and then calculate the average value to characterize the volume average particle size D of the lithium compensator L. v 50 L。

[0107] In some embodiments, the positive electrode active material includes a lithium transition metal oxide having a layered structure, and the volume average particle size D of the lithium compensator is v 50 L The volume average particle size D of the lithium transition metal oxide v 50 N Satisfy: 0.3≤D v 50 L / D v 50 N ≤3.6, optional, 0.7≤D v 50 L / D v 50 N ≤3. By keeping the ratio of the volume average particle size of the lithium compensator to the volume average particle size of the lithium transition metal oxide within the above range, gelation can be reduced, cycle life can be guaranteed, and a better charge and discharge specific capacity can be obtained. In the present application, when the particle size ratio of the lithium compensator to the lithium transition metal oxide with a layered structure is within the above range, the positive electrode material is not easy to gel, which is beneficial to improving the cycle life and charge and discharge specific capacity of the secondary battery; at the same time, it can also improve the matching degree with the positive electrode active material, which is beneficial to the capacity of the lithium compensator and enhances the contribution of the lithium compensator to the charge and discharge capacity ratio.

[0108] In the present application, the volume average particle size D of the lithium compensator L is v 50 L The volume average particle size D of the lithium transition metal oxide v 50 N The particle size ratio D v 50 L / D v 50 NThe test method known in the art can be used for determination. As an example, the following method can be used for testing: For the powder layer, the particle size distribution laser diffraction method according to GB / T 19077-2016 can be used to respectively determine the D of the lithium compensator L and the positive electrode active material using a laser particle size analyzer (e.g., Mastersizer 2000E, Malvern, UK). v For the positive electrode sheet mixed with the lithium compensator L, a scanning electron microscope (SEM, ZEISS SEM Sigma 300) and ion polishing cross-sectional morphology analysis (CP) can also be used to select multiple areas (for example, more than 20 areas), respectively measure the visible maximum particle size of the lithium compensator L and the positive electrode active material, and then calculate the particle size ratio after the average value is obtained for each, so as to characterize the volume average particle size D of the lithium compensator L. v 50 L The volume average particle size D of the positive electrode active material v 50 N The particle size ratio D v 50 L / D v 50 N .

[0109] In some embodiments, the positive electrode active material includes a lithium phosphate having an olivine structure, and the volume average particle size D of the lithium compensator is v 50 L The volume average particle size D of the lithium phosphate having an olivine structure v 50 P Satisfies: 1≤D v 50 L / D v 50 P ≤15. Optional, 2.5≤D v 50 L / D v 50 P ≤11. When the volume average particle size of the lithium compensator is within the above range, gel can be reduced, cycle life can be guaranteed, and a better charge and discharge specific capacity can be obtained.

[0110] In the present application, the volume average particle size D of the lithium compensator L is v 50 L The volume average particle size D of the lithium transition metal oxide v 50 P The particle size ratio D v 50 L / D v 50 P Please refer to the above D v 50 L / Dv 50 P The test method is used for determination.

[0111] [Isolation film]

[0112] In some embodiments, the secondary battery further includes a separator. The separator is disposed between the positive electrode sheet and the negative electrode sheet to serve as an isolation. The secondary battery of the present application has no particular restrictions on the type of separator, and any known porous structure separator for secondary batteries can be selected. For example, the separator can be selected from one or more of a glass fiber film, a non-woven film, a polyethylene film, a polypropylene film, a polyvinylidene fluoride film, and a multilayer composite film containing one or more of them.

[0113] In some embodiments, the secondary battery may include an outer packaging, which is used to package the positive electrode sheet, the negative electrode sheet, and the electrolyte.

[0114] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.

[0115] The secondary battery can be prepared by methods known in the art. For example, the positive electrode sheet, the separator and the negative electrode sheet are wound or laminated to form an electrode assembly, wherein the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role; the electrode assembly is placed in an outer package, and the electrolyte is injected and sealed to obtain a secondary battery.

[0116] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 5 is a square structure as an example.

[0117] In some embodiments, reference Figure 2 , the outer package may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate are enclosed to form a accommodating cavity. The shell 51 has an opening connected to the accommodating cavity, and the cover plate 53 can be covered on the opening to close the accommodating cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the accommodating cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, which can be adjusted according to needs.

[0118] In some embodiments, secondary batteries may be assembled into a battery module. The battery module may contain multiple secondary batteries, and the specific number may be adjusted according to the application and capacity of the battery module.

[0119] Figure 3 4 is an example of a battery module. Figure 3 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0120] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0121] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0122] Figure 4 and Figure 5 1 is a battery pack 1 as an example. Figure 4 and Figure 5 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0123] Electrical devices

[0124] Another aspect of the present application provides an electrical device, the electrical device comprising at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0125] The electrical device may select a secondary battery, a battery module or a battery pack according to its usage requirements.

[0126] Figure 6 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.

[0127] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a secondary battery may be used as a power source.

[0128] Example

[0129] Below, the embodiment of the present application is described. The embodiment described below is exemplary, is only used to explain the present application, and cannot be construed as limiting the present application. If no specific technology or conditions are specified in the embodiment, the technology or conditions described in the literature in this area or the product specification are used. The reagents or instruments used are conventional products that can be obtained commercially without specifying the manufacturer. The content of each component in the embodiment of the present invention, if not otherwise specified, is by mass.

[0130] Embodiment 1:

[0131] Preparation of negative electrode

[0132] Graphite, silicon oxide (the mass proportion of silicon in the negative electrode active material layer is 3%), binder styrene-butadiene rubber (SBR), and thickener sodium carbon methyl cellulose (CMC) are fully stirred and mixed in deionized water at a mass ratio of 94:3:2:1 to form a uniform negative electrode slurry; the negative electrode slurry is coated on the surface of the negative electrode collector copper foil, and the negative electrode sheet is obtained after drying, cold pressing, stripping, and cutting.

[0133] Preparation of positive electrode

[0134] The positive electrode active material lithium nickel cobalt manganese oxide LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811, average particle size D v 50 is 4.3μm), lithium supplement additive LiNi 0.4 Cu 0.55 Mg 0.05 O2 (lithium compensator accounts for 3% of the mass of the positive electrode active material layer and has a specific surface area of ​​0.99m 2 / g, average particle size D v 50 is 8 μm), conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are mixed in a solvent NMP at a mass ratio of 93.5:3:2:1.5 and stirred thoroughly to form a uniform positive electrode slurry; the positive electrode slurry is coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.

[0135] Preparation of electrolyte

[0136] Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed at a mass ratio of 50:50, and then LiPF6 was uniformly dissolved in the above solution to obtain an electrolyte, wherein the concentration of LiPF6 was 1.1 mol / L. Fluorinated ethylene carbonate (FEC) additive was added to the electrolyte at a mass ratio of 0.6%.

[0137] Preparation of secondary batteries

[0138] Stack the positive electrode sheet, separator, and negative electrode sheet in order, so that the separator is between the positive and negative electrodes to play a role of isolation, and wind them to obtain a bare cell. Place the bare cell in an outer package, inject the prepared electrolyte, and seal it.

[0139] (Examples 2 to 6 and Comparative Examples 1 to 4)

[0140] The preparation methods of Examples 2 to 6 and Comparative Examples 1 to 4 are similar to those of Example 1, but the positive electrode active material is adjusted (lithium iron phosphate in Examples 3 to 5 and Comparative Examples 3 to 4, with an average particle size D v 50 is 1.2μm), the content of lithium compensator, the content of Si in the negative electrode and the content of FEC in the electrolyte. The different product parameters are detailed in Table 1.

[0141] Test Section

[0142] 1. Measurement of volume average particle size Dv50 of powder materials:

[0143] The particle size distribution laser diffraction method according to GB / T 19077-2016 is measured using a laser particle size analyzer (e.g., Mastersizer 2000E, Malvern, UK).

[0144] 2. Measurement of specific surface area of ​​powder materials:

[0145] Reference standard: GB / T 19587-2004 "Determination of specific surface area of ​​solid substances by gas adsorption BET method". The instrument model used is NOVA 2000e, and the test is carried out using the following process: (1) Take a certain amount of sample (e.g., 2.0-15.0g); (2) Put the sample into a sample tube, put it into a heating bag, and degas it (degassing conditions are 200℃, 2 hours); (3) After degassing, when the temperature of the degassing station drops to room temperature, remove the sample tube from the degassing station, weigh and calculate the total mass of the sample; (4) Put the sample tube into the test filling rod and test the specific surface area of ​​the sample.

[0146] 3. Charge and discharge specific capacity test:

[0147] After the battery is assembled, it is charged to 4.25V at a gradient rate of 0.05C, 0.1C, and 0.33C at room temperature, and then charged to 0.05C rate at a constant voltage of 4.25V, and the first charging capacity of the battery is recorded; then it is discharged to 2.8V at a constant current rate of 0.33C, and the discharge capacity of the battery is recorded.

[0148] The charge and discharge specific capacity of the battery in the example table is calculated according to the following formula:

[0149]

[0150] 4. 2-day storage voltage drop test:

[0151] The battery was charged at a constant current of 0.33C to 3.85V at room temperature, and then charged at a constant voltage of 3.85V to 0.05C. It was then left at room temperature for 2 days, and the open circuit voltage V2 of the battery was tested two days later.

[0152] Calculate the battery voltage drop per hour according to the following formula:

[0153]

[0154] 5. Cycle life test:

[0155] The battery is charged at room temperature at a constant current of 0.33C to 4.25V, then charged at a constant voltage of 4.25V to a rate of 0.05C, and then discharged at a constant current of 0.33C to 2.8V, which is considered one cycle. Repeat the above cycle test until the discharge capacity decays to 80% of the initial capacity, and the test is stopped to obtain the number of cycles.

[0156] 6. Storage life test:

[0157] Storage life test process: ① Initial capacity test → ② Full charge → ③ 60℃ storage → ④ Capacity test → ⑤ Repeat steps 3 and 4 until the reversible capacity decays to 80% of the initial capacity, which is the storage life in days.

[0158] Step ② (full charge): The battery is charged at room temperature at a constant current rate of 0.33C to 4.25V, and then charged at a constant voltage rate of 4.25V to a rate of 0.05C;

[0159] Steps ①④ (capacity test): fully charge the battery according to step ②, then discharge it to 2.8V at a rate of 0.33C. The reversible capacity is recorded as C. n , the initial capacity is recorded as C0.

[0160] Step 3 (60°C storage): Place the fully charged battery in a 60°C constant temperature box and take out the battery every 15 or 30 days to test the reversible capacity.

[0161] The capacity retention rate of the battery after storage at 60°C is calculated according to the following formula:

[0162]

[0163] 7. Slurry gel test:

[0164] Different D v 50 L The lithium compensator L and active material (LFP or NCM), conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an N-methylpyrrolidone solvent (NMP) system in an appropriate weight ratio, sealed with plastic wrap, left to stand for one day, and then observed whether the slurry is gelled.

[0165] The above-mentioned tests were performed on Examples 1 to 6 and Comparative Examples 1 to 4, and the evaluation results are summarized in Table 2.

[0166]

[0167] From Tables 1 and 2, it can be seen that in the secondary batteries of Examples 1 to 6, the following conditions are satisfied: 0.2×W Si ≤W FEC ≤7.5%-0.6×W L , where W FEC is the mass proportion of the FEC in the electrolyte, W Si is the mass ratio of the silicon element in the second negative electrode active material in the negative electrode active material layer, W L is the mass proportion of the lithium compensator in the positive electrode active material layer. In the secondary batteries of Examples 1 to 6, the 2-day storage voltage drop (mV / h) (self-discharge) is maintained at a low level, the cycle life is maintained at a high level, and a higher charge and discharge specific capacity can be obtained. Moreover, it can be seen from Examples 1 to 6 that regardless of whether the positive electrode active material is lithium nickel cobalt manganese oxide or lithium iron phosphate, the secondary battery that satisfies the above relationship can achieve good self-discharge characteristics, a higher cycle life, and a higher charge and discharge specific capacity. This is because, through the lithium compensator Li x Ni a Cu 1-a-b M bO2 can compensate for the lithium consumed in forming and repairing the solid electrolyte interface film SEI, and since the lithium compensator does not contain Fe, it can avoid iron precipitation and damage to the SEI film. In addition, the fluoroethylene carbonate (FEC) contained in the electrolyte can form a dense SEI film, making it difficult for the SEI film to break, so that the cycle can maintain a slower capacity decay rate and obtain a better charge and discharge specific capacity. However, too much fluoroethylene carbonate (FEC) will worsen gas production, cause the pole piece to expand, and cause the metallic copper in the lithium compensator L to dissolve, worsening the self-discharge of the system. By controlling the content of fluoroethylene carbonate (FEC) and lithium compensator, the problem of battery self-discharge caused by the precipitation of transition metal ions in the lithium compensator at the negative electrode can be reduced.

[0168] In contrast, in Comparative Example 1, the content of FEC in the electrolyte is too little, making it difficult to form a dense SEI film at the negative electrode, resulting in reduced cycle life and discharge specific capacity. In Comparative Example 2, the content of FEC in the electrolyte is too much, resulting in the precipitation of transition metal ions in the lithium compensator at the negative electrode, resulting in excessive voltage drop in 2-day storage, resulting in self-discharge problems, and the charge-discharge specific capacity is also low. The same problem also occurs in Comparative Examples 3 and 4, where lithium iron phosphate is used as the positive electrode active material.

[0169] (Examples 7 to 18)

[0170] The preparation methods of Examples 7 to 18 are similar to those of Example 1, but the product parameters of the content of the lithium compensator, the content of Si in the negative electrode, and the content of FEC in the electrolyte are adjusted. The different product parameters are detailed in Table 3.

[0171] The above tests were performed on Examples 7 to 18, and the evaluation results are summarized in Table 4.

[0172]

[0173] From Tables 3 and 4, it can be seen that in the secondary batteries of Examples 7 to 16, the following conditions are satisfied: -2.2% ≤ W L -W Si ≤2.5%. And meet: W L 0.1%~10%; W Si 0.5wt% to 10wt%. L , W SiSatisfying the above relationship can obtain better storage life and cycle life. This is because the first coulomb efficiency (ratio of first discharge capacity to charge capacity) of the secondary battery with silicon negative electrode is low. If the silicon content increases, more lithium compensators are needed to supplement the active lithium. By keeping the mass ratio of silicon element and lithium compensator within the above range, the loss of active lithium in the silicon negative electrode can be effectively compensated, so that the cycle and storage can maintain a slower capacity decay rate to improve the cycle life and storage life, and obtain a better charge and discharge specific capacity. In addition, as the content of lithium compensator L increases, the charge specific capacity tends to increase. In addition, as the Si content increases, due to the presence of lithium compensator L in a content that satisfies the above relationship, the discharge specific capacity of Examples 14 to 16 only decreases slightly.

[0174] (Examples 19 to 24)

[0175] The preparation methods of Examples 19 to 24 are similar to those of Example 2, but the specific surface area, D v Product parameters of 50 particle size, different product parameters are detailed in Table 5.

[0176] The above tests were performed on Examples 19 to 24, and the evaluation results are summarized in Table 6.

[0177]

[0178] From Tables 5 and 6, it can be seen that in the secondary batteries of Examples 19 to 22, BET L The value is 0.5m 2 / g~8m 2 / g, volume average particle size D v 50 L The positive electrode slurry is 1.3 μm to 16 μm, the positive electrode slurry does not gel or slightly gels, and can obtain a better cycle life and charge-discharge specific capacity. This is because the lithium compensator within the above range is not easy to agglomerate and the slurry has good stability. The obtained secondary battery can obtain an excellent cycle life and charge-discharge specific capacity. In addition, in the secondary batteries of Examples 19 to 22, the volume average particle size D of the lithium compensator is v 50 L The volume average particle size D of the lithium transition metal oxide v 50 N Satisfy: 0.3≤D v 50 L / D v 50 N ≤3.6. When the particle size ratio is within the above range, the slurry of the positive electrode active material is not easy to gel, has better stability, and the contribution of the lithium compensator to the charge and discharge capacity is also higher, so that excellent cycle life and charge and discharge specific capacity can be obtained.

[0179] (Examples 25 to 30)

[0180] The preparation methods of Examples 25 to 30 are similar to those of Example 5, but the specific surface area, D v Product parameters of 50 particle size, different product parameters are detailed in Table 7.

[0181] The above tests were performed on Examples 25 to 30, and the evaluation results are summarized in Table 8.

[0182]

[0183] From Tables 7 and 8, it can be seen that in the secondary batteries of Examples 25 to 28, the volume average particle size D of the lithium compensator is v 50 L The volume average particle size D of lithium phosphate with olivine structure v 50 P Satisfies: 1≤D v 50 L / D v 50 P ≤15. When the particle size ratio is within the above range, the slurry of the positive electrode active material is not easy to gel, has good stability, and the contribution of the lithium compensator to the charge and discharge capacity is also high, so that excellent cycle life and charge and discharge specific capacity can be obtained.

[0184] Those skilled in the art should understand that the above-mentioned embodiments are only some specific embodiments for implementing the present invention, and in practical applications, various changes and modifications may be made thereto in form and details, all of which fall within the scope of protection of this application.

Claims

1. A lithium secondary battery, comprising: A positive electrode, a negative electrode, and an electrolyte; characterized in that, The positive electrode includes a positive electrode active material layer, the positive electrode active material layer contains a lithium compensator, and the molecular formula of the lithium compensator is Li x Ni a Cu 1-a-b M b O2, where 1 ≤ x ≤ 2, 0 < a < 1, 0 ≤ b < 0.1, and M is selected from one or more of Zn, Sn, Mg, Fe, and Mn; The negative electrode includes a negative electrode active material layer, and the negative electrode active material layer contains a first negative electrode active material and a second negative electrode active material. The first negative electrode active material is graphite, and the second negative electrode active material is selected from one or more of Si, SiO n (0 < n < 2), and SiC; the electrolyte contains fluoroethylene carbonate (FEC); The lithium secondary battery meets the following requirements: , where W FEC is the mass proportion of the FEC in the electrolyte, W Si is the mass ratio of the silicon element in the second negative electrode active material in the negative electrode active material layer, W L is the mass ratio of the lithium compensator in the positive electrode active material layer.

2. The lithium secondary battery according to claim 1, characterized in that: The W L With the W Si Satisfy the conditions: -2.2%≤W L -W Si ≤2.5%.

3. The lithium secondary battery according to claim 1, characterized in that: The W L It is 0.1%~10%.

4. The lithium secondary battery according to claim 3, characterized in that: The W L It is 0.2%~9%.

5. The lithium secondary battery according to claim 3, characterized in that The W L It is 0.3%~8%.

6. The lithium secondary battery according to any one of claims 1 to 5, characterized in that The W Si It is 0.5wt%~10wt%.

7. The lithium secondary battery according to claim 6, characterized in that: The W Si It is 1wt%~8wt%.

8. The lithium secondary battery according to claim 6, characterized in that The W Si It is 1.5wt%~6wt%.

9. The lithium secondary battery according to any one of claims 1 to 5, characterized in that The W FEC 0.1wt%~7.5wt%.

10. The lithium secondary battery according to claim 9, characterized in that: The W FEC It is 0.5wt%~6wt%.

11. The lithium secondary battery according to claim 9, characterized in that: The W FEC It is 1wt%~5wt%.

12. The lithium secondary battery according to any one of claims 1 to 5, characterized in that: The specific surface area of ​​the lithium compensator is BET L The value is 0.3m 2 / g~10m 2 / g.

13. The lithium secondary battery according to claim 12, characterized in that: The BET L 0.5m 2 / g~8m 2 / g.

14. The lithium secondary battery according to claim 12, characterized in that: The BET L 0.6m 2 / g~3.5m 2 / g.

15. The lithium secondary battery according to any one of claims 1 to 5, characterized in that: The volume average particle size D of the lithium compensator v 50 L 1μm~20μm.

16. The lithium secondary battery according to claim 15, characterized in that: The D v 50 L 1.3μm~16μm.

17. The lithium secondary battery according to claim 15, characterized in that: The D v 50 L 3μm~13μm.

18. The lithium secondary battery according to any one of claims 1 to 5, characterized in that: the positive electrode further includes a positive electrode active material, and the positive electrode active material includes at least one of the compounds represented by formula (I) to formula (III): Li 1+x1 Ni a1 Co b1 m' 1-a1-b1 O 2-y1 A y1 (I); Li 1+x2 Mr a2 M'' 2-a2 O 4-d A' d (II); LiFe (1-x3-y3) Mn x3 M’’’ y3 PO4(III); wherein, in formula (I), -0.1 ≤ x1 ≤ 0.2, 0 < a1 < 1, 0 ≤ b1 ≤ 1, 0 < a1 + b1 < 1, 0 ≤ y1 < 0.2, M' is one or more of Mn, Fe, Cr, Ti, Zn, V, Al, Zr, and Ce, and A includes one or more of S, N, F, Cl, Br, and I; wherein, in formula (II), -0.1 ≤ x2 ≤ 0.2, 0 < a2 ≤ 2, 0 ≤ d < 1, M'' includes one or more of Ni, Fe, Cr, Ti, Zn, V, Al, Mg, Zr, and Ce, and A' includes one or more of S, N, F, Cl, Br, and I; wherein, in formula (III), 0 ≤ x3 ≤ 1, 0 ≤ y3 ≤ 0.1, and M''' is selected from one or several of transition metal elements other than Fe and Mn and non-transition metal elements.

19. The lithium secondary battery according to claim 18, characterized in that: 0.5 ≤ a1 < 1, 0 < b1 < 0.5, 0.7 ≤ a1 + b1 < 1, 0 ≤ y < 0.1, M is one or both of Mn and Al, and A is one or both of S and F.

20. The lithium secondary battery according to claim 18, characterized in that: The positive electrode active material includes at least the compound represented by formula (I).

21. The lithium secondary battery according to any one of claims 1 to 5, characterized in that: The positive electrode further comprises a positive electrode active material, wherein the positive electrode active material comprises a lithium transition metal oxide having a layered structure, and the volume average particle size D of the lithium compensator is v 50 L The volume average particle size D of the lithium transition metal oxide v 50 N Satisfy: 0.3≤D v 50 L / D v 50 N ≤3.

6.

22. The lithium secondary battery according to claim 21, characterized in that: 0.7≤D v 50 L / D v 50 N ≤3。 23. The lithium secondary battery according to any one of claims 1 to 5, characterized in that: The positive electrode further comprises a positive electrode active material, wherein the positive electrode active material comprises a lithium phosphate having an olivine structure, and the volume average particle size D of the lithium compensator is v 50 L The volume average particle size D of the lithium phosphate having an olivine structure v 50 P Satisfies: 1≤D v 50 L / D v 50 P ≤15.

24. The lithium secondary battery according to claim 23, characterized in that: 2.5≤D v 50 L / D v 50 P ≤11。 25. A battery module, characterized in that: A lithium secondary battery according to any one of claims 1-24.

26. A battery pack, characterized in that: A lithium secondary battery according to any one of claims 1-24, or a battery module according to claim 25.

27. An electrical device, characterized in that: A lithium secondary battery according to any one of claims 1-24, or a battery module according to claim 25, or a battery pack according to claim 26; wherein the lithium secondary battery, the battery module, or the battery pack is used as a power source for the electrical device.