A dual antibacterial super-lyophobic coating and preparation method thereof
The dual antibacterial superliquid coating prepared by combining fluorine-containing half cage oligosilsesquioxane, anhydrous ethanol, inorganic nanoparticles and antibacterial peptides with aqueous resins has solved the safety of antibacterial coatings in the prior art. The problem of insufficient performance and stability has achieved the effect of efficient broad-spectrum antibacterial and environmentally friendly construction.
Patent Information
- Application Number
- CN202310103960.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-02-09
AI Technical Summary
The existing antibacterial superliquid coatings have safety and stability problems in industries such as food packaging and medical devices, especially the complex production process and high cost of inorganic antibacterial agent doping methods, as well as the decomposition of organic antibacterial agents and Toxicity issues cannot meet industry requirements.
The combination of fluorine-containing semi-cage oligosilsesquioxane, anhydrous ethanol, inorganic nanoparticles and antimicrobial peptides and high-safe aqueous resins is prepared by ultrasonic treatment and spraying to achieve the The synergistic effect of physical and biological antibacterial.
This coating has excellent antibacterial properties, liquid repellency and high safety. It can have an antibacterial rate of E. coli and Staphylococcus aureus of more than 99%. It uses environmentally friendly solvents, which have high construction efficiency and low cost, and is suitable for food packaging. and medical devices and other fields.
Smart Images

Figure BDA0004074130270000121 
Figure BDA0004074130270000122 
Figure HDA0004074130280000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of antibacterial material preparation, and specifically relates to a dual antibacterial super-lyophobic coating and a preparation method thereof. Background Art
[0002] At present, the world is facing severe challenges from the novel coronavirus infection, and global public health security is under serious threat. People pay more attention to health and hygiene, and put forward higher requirements for the safety of food packaging and medical devices. Bacteria, as a kind of microorganism existing in nature, can easily breed and reproduce on the surface of objects, posing a serious threat to human life and health. Therefore, it is of great significance to develop surface materials that can effectively inhibit bacterial growth and effectively kill bacteria and resist viruses.
[0003] As a special new material, antibacterial super-liquid-repellent coating material has special properties such as antibacterial, self-cleaning, anti-icing, anti-corrosion, anti-fouling, anti-scaling, and fluid drag reduction. It has potential application value in many aspects such as medical equipment, electronic equipment, transportation facilities, clothing and textiles, etc. Therefore, it has attracted much attention from researchers. In recent years, domestic and foreign researchers have mainly prepared antibacterial super-liquid-repellent coating materials by two methods: inorganic antibacterial agent doping and organic antibacterial agent doping. For example, patent document 202111573456.3 discloses a durable antibacterial and antiviral super-amphiphobic coating and a preparation method thereof. The method mixes silica nanoparticles, alcohol solvents, alkaline catalysts, silicates and fluorine-containing organic matter in corresponding proportions to prepare super-amphiphobic modified nano-silica particles, and then mixes fluorocarbon resin, acrylic resin, barium sulfate powder, organic solvents and various additives to prepare a primer. Subsequently, the super-amphiphobic modified nano-silica particles, ultrafine-sized nano-silver powder and anhydrous ethanol are stirred to prepare a topcoat. Finally, the primer is sprayed on the substrate, and after it is dried on the surface, the topcoat is sprayed on the primer to prepare a durable antibacterial and antiviral super-amphiphobic coating. The static contact angles of water and pump oil of the coating are both over 150°, and the antibacterial rates against Escherichia coli and Staphylococcus aureus are both over 99.9%. For another example, patent document with application number 201811054100.7 discloses a super-hydrophobic antibacterial cationic fluoropolymer nano-coating. During the preparation process of the coating, the quaternary ammonium reagent 3-chloropropylene and alkyl-dimethyl tertiary amine are reacted by heating to prepare propylene-alkyl-dimethyl quaternary ammonium salt monomer, i.e., antibacterial cationic monomer, then the antibacterial cationic monomer, fluorine-containing monomer, styrene monomer and acrylic monomer are mixed, and antibacterial cationic fluoropolymer microsphere emulsion is prepared by emulsion polymerization. Finally, the antibacterial cationic fluoropolymer microsphere emulsion is combined with an aqueous curing agent to prepare a super-hydrophobic antibacterial cationic fluoropolymer nano-coating. The coating has good super-hydrophobicity, wear resistance and adhesion, and has good antibacterial properties against Escherichia coli and Staphylococcus aureus.
[0004] The antibacterial super-lyophobic coating material prepared by two methods of inorganic antibacterial agent doping and organic antibacterial agent doping, although having good lyophobicity and excellent antibacterial performance, realizes the dual antibacterial effect of physical antibacterial and chemical antibacterial to a certain extent, and has a wide range of application value, however, these two technologies have many shortcomings, such as the antibacterial super-lyophobic prepared by the inorganic antibacterial agent doping method, with inorganic silver as the main antibacterial agent, the production process is more complicated, difficult to manufacture, and costly, in addition, the silver antibacterial agent is easy to change color, and the product of the super-lyophobic coating doped with the silver antibacterial agent is coated, and the free silver ions on its surface are easily reduced to elemental silver under sunlight irradiation conditions and present gray or brown, which seriously affects the light transmittance of the product. And the super-lyophobic coating prepared by the organic antibacterial agent doping method, its antibacterial agent is mainly quaternary ammonium salts, organic metals, etc. as the main components, in a solvent environment, the organic antibacterial agent in the antibacterial super-lyophobic coating is easily decomposed and separated, and the decomposition product is toxic, and it is easy to produce drug resistance and cross resistance, in addition, its safety has not been determined so far. Therefore, the existing antibacterial super-lyophobic coating technology cannot meet the safety and stability requirements of industries such as food packaging and medical devices. Summary of the invention
[0005] In response to the problems of poor safety and stability of antibacterial super-lyophobic coating materials in the above-mentioned prior art when applied to food packaging, medical equipment and other industries, the present invention will provide a dual antibacterial super-lyophobic coating and a preparation method thereof. The method incorporates fluorinated semi-cage oligomeric silsesquioxane, anhydrous ethanol, inorganic nanoparticles and antimicrobial peptides into a high-safety aqueous resin to prepare a dual antibacterial super-lyophobic coating having excellent antibacterial properties, lyophobic properties, high safety and stability.
[0006] To achieve the above purpose, the following technical solutions are specifically included:
[0007] A dual antibacterial super-liquid-repellent coating, the preparation raw materials of which include fluorine-containing semi-cage oligomeric silsesquioxane, ethanol, inorganic nanoparticles, antimicrobial peptides and water-based resin.
[0008] The dual antibacterial super-lyophobic coating has the advantages of the physical antibacterial of the super-lyophobic layer and the biological antibacterial of the antibacterial peptide, and can achieve high-efficiency and broad-spectrum antibacterial, with the antibacterial rates against Escherichia coli and Staphylococcus aureus exceeding 99%.
[0009] As a preferred embodiment of the present invention, the mass ratio of the fluorine-containing semi-cage type oligomeric silsesquioxane to ethanol is (15-70):(30-85).
[0010] As a preferred embodiment of the present invention, the mass ratio of the fluorine-containing semi-cage type oligomeric silsesquioxane to the aqueous resin is 1:(20000-200000).
[0011] As a preferred embodiment of the present invention, the mass ratio of the inorganic nanoparticles to the aqueous resin is 1:(50-300).
[0012] As a preferred embodiment of the present invention, the mass ratio of the antimicrobial peptide to the aqueous resin is 1:(1000-5000).
[0013] As a preferred embodiment of the present invention, the inorganic nanoparticles are at least one of silicon dioxide nanoparticles, titanium dioxide nanoparticles, aluminum oxide nanoparticles and zirconium dioxide nanoparticles.
[0014] As a preferred embodiment of the present invention, the size of the inorganic nanoparticles is 5-500 nm.
[0015] As a preferred embodiment of the present invention, the antimicrobial peptide is at least one of nisin, nisin, enterocin and cecropin.
[0016] As a preferred embodiment of the present invention, the water-based resin is at least one of water-based inorganic silicone resin SJ-8050, water-based silicone resin S-227, water-based polyacrylate 3958, water-based polyurethane 2944, water-based epoxy resin S-969, and water-based fluorocarbon resin DF-01L.
[0017] In the dual antibacterial super-lyophobic coating, the solid content of the aqueous resin is 0.1-20%.
[0018] A method for preparing a dual antibacterial super-lyophobic coating comprises the following steps:
[0019] (1) mixing and dissolving a fluorinated semi-cage type oligomeric silsesquioxane and ethanol, and then subjecting the mixture to ultrasonic treatment to obtain an ethanol solution of the fluorinated semi-cage type oligomeric silsesquioxane;
[0020] (2) mixing the fluorinated semi-cage oligomeric silsesquioxane ethanol solution, inorganic nanoparticles, antimicrobial peptides and aqueous resin to obtain a dual antimicrobial super-lyophobic coating slurry;
[0021] (3) coating the dual antibacterial super-liquid-repellent coating slurry on a carrier and curing the slurry to obtain the dual antibacterial super-liquid-repellent coating.
[0022] As a preferred embodiment of the present invention, the ultrasonic frequency of the ultrasonic treatment is 20-60 kHz.
[0023] As a preferred embodiment of the present invention, the ultrasonic treatment time is 5-60 min.
[0024] As a preferred embodiment of the present invention, the curing time is 12-48 hours.
[0025] As a preferred embodiment of the present invention, the carrier is a carrier made of glass.
[0026] As a preferred embodiment of the present invention, the coating method is at least one of spraying, spin coating, brush coating, and roller coating.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) The present invention introduces low surface energy substances such as fluorine-containing semi-cage oligomeric silsesquioxane and inorganic nanoparticles into a water-based resin to obtain a super-liquid-repellent coating with physical antibacterial properties (physical isolation of bacteria-containing liquids). The coating has a strong repellent effect on water or organic solvents such as glycerol and ethylene glycol, and has excellent liquid repellency.
[0029] (2) The present invention introduces antimicrobial peptides into the super-liquid-repellent coating to prepare a synergistic antimicrobial super-liquid-repellent coating with physical antimicrobial (super-liquid-repellent surface) and biological antimicrobial (antimicrobial peptides). The coating only needs to be mixed with an appropriate amount of antimicrobial peptides to achieve high-efficiency broad-spectrum antibacterial activity, and the antimicrobial rates against Escherichia coli and Staphylococcus aureus are both over 99%.
[0030] (3) The preparation process of the dual antibacterial super-lyophobic coating uses environmentally friendly and non-toxic solvents such as water and ethanol. The equipment used is simple and easy to operate. It can be achieved through simple construction methods such as spraying, brushing, and roller coating. It has high construction efficiency and low preparation cost. It is expected to be used in food packaging, medical equipment and other industries. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is an appearance diagram of the dual antibacterial super-lyophobic coating slurry in Example 1 of the present invention.
[0032] Figure 2 These are pictures of 10 μL water droplets (left) and 10 μL ethylene glycol droplets (right) dropped on the surface of the dual antibacterial super-liquid-repellent coating in Example 1 of the present invention.
[0033] Figure 3 This is a diagram showing the antibacterial effect of the blank control group in the antibacterial experiment in Example 1 of the present invention.
[0034] Figure 4 This is a diagram showing the antibacterial effect of the dual antibacterial super-lyophobic coating in Example 1 of the present invention. DETAILED DESCRIPTION
[0035] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below through specific embodiments.
[0036] In the embodiments of the present invention and the comparative examples, anhydrous ethanol and inorganic nanoparticles are all commercially available analytically pure reagents.
[0037] The fluorinated half-cage oligomeric silsesquioxane can be prepared in-house or purchased on the market. The fluorinated half-cage oligomeric silsesquioxane used in the following examples and comparative examples is of the same type. The preparation process thereof can be found in patent document CN202010348435.0:
[0038] Step 1: 1H, 1H, 2H, 2H-perfluoroalkoxysilane, sodium hydroxide and anhydrous ethanol are mixed evenly, deionized water is added dropwise, and then heated and stirred for reaction. After the reaction is completed, the ethanol solvent is rotary evaporated, and vacuum dried to obtain a fluorinated semi-cage oligomeric silsesquioxane sodium salt;
[0039] Step 2: Add sodium salt of fluorinated semi-cage oligomeric silsesquioxane in batches to concentrated hydrochloric acid, react at room temperature, filter to remove insoluble matter after the reaction is completed, add the filtrate dropwise into crushed ice to precipitate a white solid, which is then washed with water and alcohol and dried in vacuo to obtain fluorinated semi-cage oligomeric silsesquioxane.
[0040] In the examples and comparative examples of the present invention, the size of the inorganic nanoparticles is 5-500 nm.
[0041] In the examples and comparative examples of the present invention, the ultrasonic frequency of the fluorine-containing semi-cage oligomeric silsesquioxane ethanol solution is 20-60 kHz.
[0042] In the examples and comparative examples of the present invention, the slurry is evenly coated on the glass sheet and left at room temperature for 12-48 hours.
[0043] In the examples and comparative examples of the present invention, the solid content of the water-based resin in the coating is 0.1-20%.
[0044] Example 1
[0045] The present embodiment provides a dual antibacterial super-lyophobic coating, the raw materials for preparing the coating include fluorine-containing semi-cage oligomeric silsesquioxane, anhydrous ethanol, inorganic nanoparticles, antimicrobial peptides, and water-based resin;
[0046] The inorganic nanoparticles are silicon dioxide nanoparticles; the size of the inorganic nanoparticles is 5-500nm;
[0047] The antimicrobial peptide is nisin (CAS: 1414-45-5, molecular weight 3354.07);
[0048] The water-based resin is water-based inorganic silicone resin SJ-8050;
[0049] In the dual antibacterial super-lyophobic coating, the mass content (solid content) of the water-based inorganic silicone resin is 0.1%.
[0050] The present invention provides a method for preparing a dual antibacterial super-lyophobic coating, comprising the following steps:
[0051] (1) mixing a fluorinated half-cage oligomeric silsesquioxane and anhydrous ethanol, stirring and dissolving them, and treating them under 20 kHz ultrasound for 30 minutes to prepare a fluorinated half-cage oligomeric silsesquioxane ethanol solution, wherein the mass content of the fluorinated half-cage oligomeric silsesquioxane is 15%;
[0052] (2) adding a fluorinated semi-cage oligomeric silsesquioxane ethanol solution, inorganic nanoparticles, and antimicrobial peptides to an aqueous resin and mixing them uniformly to obtain a dual antimicrobial super-lyophobic coating slurry, wherein the mass ratio of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:20000, the mass ratio of the inorganic nanoparticles to the aqueous resin is 1:50, and the mass ratio of the antimicrobial peptide to the aqueous resin is 1:1000; the appearance is as follows Figure 1 As shown;
[0053] (3) The dual antibacterial super-liquid-repellent coating slurry is evenly sprayed on a glass sheet, placed at room temperature for 24 hours, and naturally dried and solidified to obtain a dual antibacterial super-liquid-repellent coating; the appearance is as follows Figure 2 shown.
[0054] Example 2
[0055] Compared with Example 1, the difference is:
[0056] The inorganic nanoparticles are titanium dioxide nanoparticles;
[0057] The antimicrobial peptide is pediocin lactic acid;
[0058] The water-based resin is water-based silicone resin S-227;
[0059] In the dual antibacterial super-lyophobic coating, the solid content of the water-based resin is 2%.
[0060] The mass content of the fluorinated semi-cage type oligomeric silsesquioxane in the ethanolic solution of the fluorinated semi-cage type oligomeric silsesquioxane is 20%.
[0061] The mass ratio of the fluorine-containing semi-cage oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:50000;
[0062] The mass ratio of the inorganic nanoparticles to the water-based resin is 1:80;
[0063] The mass ratio of the antimicrobial peptide to the aqueous resin is 1:1500;
[0064] The ultrasonic frequency of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 30kHz;
[0065] The slurry was evenly coated on the glass sheet and left at room temperature for 12 h;
[0066] The coating method is spin coating.
[0067] Example 3
[0068] Compared with Example 1, the difference is:
[0069] The inorganic nanoparticles are aluminum oxide nanoparticles;
[0070] The antimicrobial peptide is enterobactin;
[0071] The water-based resin is water-based fluorocarbon resin DF-01L;
[0072] In the dual antibacterial super-lyophobic coating, the solid content of the water-based resin is 5%;
[0073] The mass content of the fluorinated semi-cage oligomeric silsesquioxane in the ethanol solution of the fluorinated semi-cage oligomeric silsesquioxane is 25%;
[0074] The mass ratio of the fluorine-containing semi-cage oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:80000;
[0075] The mass ratio of the inorganic nanoparticles to the water-based resin is 1:100;
[0076] The mass ratio of the antimicrobial peptide to the aqueous resin is 1:2000;
[0077] The ultrasonic frequency of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 40 kHz;
[0078] The slurry was evenly coated on the glass sheet and left at room temperature for 36 h;
[0079] The coating method is brush application.
[0080] Example 4
[0081] Compared with Example 1, the difference is:
[0082] The inorganic nanoparticles are zirconium dioxide nanoparticles;
[0083] The antimicrobial peptide is cecropin;
[0084] The water-based resin is water-based polyacrylate 3958;
[0085] In the dual antibacterial super-lyophobic coating, the solid content of the water-based resin is 10%;
[0086] The mass content of the fluorinated semi-cage oligomeric silsesquioxane in the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 30%;
[0087] The mass ratio of the fluorine-containing semi-cage oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:100000;
[0088] The mass ratio of the inorganic nanoparticles to the water-based resin is 1:125;
[0089] The mass ratio of the antimicrobial peptide to the aqueous resin is 1:2500;
[0090] The ultrasonic frequency of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 50 kHz;
[0091] The slurry was evenly coated on the glass sheet and left at room temperature for 48 h;
[0092] The coating method is roller coating.
[0093] Example 5
[0094] Compared with Example 1, the difference is:
[0095] The inorganic nanoparticles are silicon dioxide nanoparticles;
[0096] The antimicrobial peptide is pediocin lactic acid;
[0097] The water-based resin is water-based polyurethane 2944;
[0098] In the dual antibacterial super-lyophobic coating, the solid content of the water-based resin is 12%;
[0099] The mass content of the fluorinated semi-cage type oligomeric silsesquioxane in the ethanolic solution of the fluorinated semi-cage type oligomeric silsesquioxane is 35%;
[0100] The mass ratio of the fluorine-containing semi-cage oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:120000;
[0101] The mass ratio of the inorganic nanoparticles to the water-based resin is 1:150;
[0102] The mass ratio of the antimicrobial peptide to the aqueous resin is 1:3000;
[0103] The ultrasonic frequency of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 60 kHz;
[0104] The slurry was evenly coated on the glass sheet and left at room temperature for 16 h;
[0105] The coating method is spraying.
[0106] Example 6
[0107] Compared with Example 1, the difference is:
[0108] The inorganic nanoparticles are titanium dioxide nanoparticles;
[0109] The antimicrobial peptide is enterobactin;
[0110] The water-based resin is water-based epoxy resin S-969;
[0111] In the dual antibacterial super-lyophobic coating, the solid content of the water-based resin is 14%;
[0112] The mass content of the fluorinated semi-cage type oligomeric silsesquioxane in the ethanol solution of the fluorinated semi-cage type oligomeric silsesquioxane is 40%.
[0113] The mass ratio of the fluorine-containing semi-cage type oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:140000.
[0114] The mass ratio of the inorganic nanoparticles to the water-based resin is 1:200;
[0115] The mass ratio of the antimicrobial peptide to the aqueous resin is 1:3500;
[0116] The ultrasonic frequency of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 30kHz;
[0117] The slurry was evenly coated on the glass sheet and left at room temperature for 20 h;
[0118] The coating method is spin coating.
[0119] Example 7
[0120] Compared with Example 1, the difference is:
[0121] The inorganic nanoparticles are aluminum oxide nanoparticles;
[0122] The antimicrobial peptide is cecropin;
[0123] The water-based resin is water-based inorganic silicone resin SJ-8050;
[0124] In the dual antibacterial super-lyophobic coating, the solid content of the water-based resin is 15%;
[0125] The mass content of the fluorinated semi-cage type oligomeric silsesquioxane in the ethanolic solution of the fluorinated semi-cage type oligomeric silsesquioxane is 45%;
[0126] The mass ratio of the fluorine-containing semi-cage oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:150000;
[0127] The mass ratio of the inorganic nanoparticles to the water-based resin is 1:250;
[0128] The mass ratio of the antimicrobial peptide to the aqueous resin is 1:4000;
[0129] The ultrasonic frequency of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 40 kHz;
[0130] The slurry was evenly coated on the glass sheet and left at room temperature for 22 h;
[0131] The coating method is brush application.
[0132] Example 8
[0133] Compared with Example 1, the difference is:
[0134] The inorganic nanoparticles are zirconium dioxide nanoparticles; the size of the inorganic nanoparticles is 5-500nm;
[0135] The antimicrobial peptide is nisin;
[0136] The water-based resin is water-based silicone resin S-227;
[0137] In the dual antibacterial super-lyophobic coating, the solid content of the water-based resin is 16%;
[0138] The mass content of the fluorinated semi-cage type oligomeric silsesquioxane in the ethanolic solution of the fluorinated semi-cage type oligomeric silsesquioxane is 50%;
[0139] The mass ratio of the fluorine-containing semi-cage oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:160000;
[0140] The mass ratio of the inorganic nanoparticles to the water-based resin is 1:300;
[0141] The mass ratio of the antimicrobial peptide to the aqueous resin is 1:4200;
[0142] The ultrasonic frequency of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 50 kHz;
[0143] The slurry was evenly coated on the glass sheet and left at room temperature for 28 h;
[0144] The coating method is roller coating.
[0145] Example 9
[0146] Compared with Example 1, the difference is:
[0147] The inorganic nanoparticles are silicon dioxide nanoparticles;
[0148] The antimicrobial peptide is pediocin lactic acid;
[0149] The water-based resin is water-based fluorocarbon resin DF-01L;
[0150] In the dual antibacterial super-lyophobic coating, the solid content of the water-based resin is 16.5%;
[0151] The mass ratio of the fluorine-containing semi-cage oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:170000;
[0152] The mass ratio of the inorganic nanoparticles to the water-based resin is 1:55;
[0153] The mass ratio of the antimicrobial peptide to the aqueous resin is 1:4500;
[0154] The ultrasonic frequency of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 60 kHz;
[0155] The slurry was evenly coated on the glass sheet and left at room temperature for 30 h;
[0156] The coating method is spraying.
[0157] Example 10
[0158] Compared with Example 1, the difference is:
[0159] The inorganic nanoparticles are titanium dioxide nanoparticles;
[0160] The antimicrobial peptide is enterobactin;
[0161] The water-based resin is water-based polyacrylate 3958;
[0162] In the dual antibacterial super-lyophobic coating, the solid content of the water-based resin is 17%;
[0163] The mass content of the fluorinated semi-cage oligomeric silsesquioxane in the ethanol solution of the fluorinated semi-cage oligomeric silsesquioxane is 60%;
[0164] The mass ratio of the fluorine-containing semi-cage oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:180000;
[0165] The mass ratio of the inorganic nanoparticles to the water-based resin is 1:175;
[0166] The mass ratio of the antimicrobial peptide to the aqueous resin is 1:4800;
[0167] The ultrasonic frequency of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 20 kHz;
[0168] The slurry was evenly coated on the glass sheet and left at room temperature for 32 h;
[0169] The coating method is spin coating.
[0170] Embodiment 11
[0171] Compared with Example 1, the difference is:
[0172] The inorganic nanoparticles are aluminum oxide nanoparticles;
[0173] The antimicrobial peptide is cecropin;
[0174] The water-based resin is water-based polyurethane 2944;
[0175] In the dual antibacterial super-lyophobic coating, the solid content of the water-based resin is 18%;
[0176] The mass content of the fluorinated semi-cage type oligomeric silsesquioxane in the ethanolic solution of the fluorinated semi-cage type oligomeric silsesquioxane is 65%;
[0177] The mass ratio of the fluorine-containing semi-cage oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:190000;
[0178] The mass ratio of the inorganic nanoparticles to the water-based resin is 1:225;
[0179] The mass ratio of the antimicrobial peptide to the aqueous resin is 1:4900;
[0180] The ultrasonic frequency of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 30kHz;
[0181] The slurry was evenly coated on the glass sheet and left at room temperature for 35 h;
[0182] The coating method is brush application.
[0183] Example 12
[0184] Compared with Example 1, the difference is:
[0185] The inorganic nanoparticles are zirconium dioxide nanoparticles;
[0186] The antimicrobial peptide is nisin;
[0187] The water-based resin is water-based epoxy resin S-969;
[0188] In the dual antibacterial super-lyophobic coating, the solid content of the water-based resin is 20%;
[0189] The mass content of the fluorinated semi-cage type oligomeric silsesquioxane in the ethanolic solution of the fluorinated semi-cage type oligomeric silsesquioxane is 70%;
[0190] The mass ratio of the fluorine-containing semi-cage oligomeric silsesquioxane ethanol solution to the aqueous resin is 1:200000;
[0191] The mass ratio of the inorganic nanoparticles to the water-based resin is 1:275;
[0192] The mass ratio of the antimicrobial peptide to the aqueous resin is 1:5000;
[0193] The ultrasonic frequency of the fluorinated semi-cage oligomeric silsesquioxane ethanol solution is 40 kHz;
[0194] The slurry was evenly coated on the glass sheet and left at room temperature for 38 h;
[0195] The coating method is roller coating.
[0196] Comparative Example 1
[0197] Compared with Example 1, the difference is that the comparative example does not add fluorine-containing semi-cage type oligomeric silsesquioxane.
[0198] Comparative Example 2
[0199] Compared with Example 1, the difference is that no antimicrobial peptide is added in this comparative example.
[0200] Comparative Example 3
[0201] Compared with Example 1, the difference is that the present comparative example does not add antimicrobial peptide and fluorine-containing semi-cage type oligomeric silsesquioxane.
[0202] Antibacterial activity test of dual antibacterial super-lyophobic coating:
[0203] Preparation of coating samples for the embodiments and comparative examples: Prepare 3 pieces of PET film for each sample to be coated with a double antibacterial super-liquid-repellent coating, and prepare 1 piece of PET film without antibacterial treatment as a control. (Note: Using more than 3 antibacterial treated samples helps to reduce errors) Prepare a bottom PET film with a size of (50±2) mm×(50±2) mm and a covering PET film with a size of (40±2) mm×(40±2) mm respectively. When preparing the sample, be careful to avoid contamination of the sample by microorganisms or organic matter. The sample is cleaned, disinfected or sterilized (70% alcohol scrub) before testing.
[0204] Take the stock solution of Staphylococcus aureus (200 μL) and add it to a test tube containing sterile Luria-Bertani (LB) broth (10 mL), then culture it in an incubator at 30°C and 170 rpm for 20 to 24 h. Use LB broth to dilute the bacteria to a concentration of 6.0 × 10 5CFU / mL. For each sample (control group and experimental group in sample preparation), take Staphylococcus aureus culture solution (400μL) and inoculate it to the bottom PET film of (50±2)mm×(50±2)mm and cover the (40±2)mm×(40±2)mm cover film on the bacterial solution, and gently press down the film to spread the bacterial solution to the surroundings, making sure that the bacterial solution does not overflow from the edge of the film. After incubation at 37°C for 24h, 0.1ml of the bacterial solution was aspirated from the film, and then a series of ten-fold dilutions were made with LB broth. Finally, 100μL of the diluted solution was spread on the agar medium and cultured at 37°C for 24h, and the bacterial colonies of each sample were counted. Three groups of antibacterial experiments were carried out on each sample at the same time, and the average value was used as the experimental result. The calculation of bacterial inhibition rate is shown as follows:
[0205]
[0206] Where R is the inhibition rate, M and N are the number of colonies on the culture medium of the blank control group and the experimental group, respectively.
[0207] The surface bacterial colonies of the blank control group in Example 1 are as follows: Figure 3 As shown in Figure 2, a large number of colonies appeared on the surface of the culture medium. The antibacterial effect of the dual antibacterial super-lyophobic coating of Example 1 is as follows: Figure 4 As shown, the number of colonies on the culture medium surface was 6, and the antibacterial rate reached 99.6%.
[0208] The antibacterial effects of the coating samples of the embodiments and comparative examples are shown in Table 1.
[0209] Table 1 Antibacterial effect of coating samples of embodiments and comparative examples
[0210]
[0211] It can be seen from the antibacterial effect of the coating in the examples that the antibacterial effect of the dual antibacterial super-lyophobic coating of the present invention on Staphylococcus aureus is greater than 99%.
[0212] Contact angle and rolling angle test:
[0213] The coatings prepared in the examples and comparative examples were placed at room temperature. After 48 hours, the contact angles of water (10 μL) and ethylene glycol (10 μL) were tested. The results are shown in Table 2.
[0214] Table 1 Coating contact angle and rolling angle results of the embodiments and comparative examples
[0215] Water contact angle Water rolling angle Ethylene glycol contact angle Glycol Slip Angle Example 1 162.7° 1.7° 153.2° 14.8° Example 2 160.4° 1.2° 152.5° 15.2° Example 3 163.5° 1.9° 156.1° 13.4° Example 4 157.3° 2.6° 153.8° 19.3° Example 5 160.7° 3.7° 156.3° 16.7° Example 6 164.3° 4.2° 152.8° 13.4° Example 7 158.4° 5.1° 155.7° 14.6° Example 8 161.3° 3.2° 156.1° 13.9° Example 9 162.5° 2.3° 154.2° 12.8° Example 10 161.8° 2.7° 155.7° 16.5° Embodiment 11 159.6° 3.4° 153.1° 12.7° Example 12 162.9° 1.9° 152.9° 17.3° Comparative Example 1 124.3° 22.3° 103.4° 35.2° Comparative Example 2 154.9° 5.1° 151.8 15.5° Comparative Example 3 122.5° 21.9° 106.1° 32.4°
[0216] It can be seen from the contact angle and rolling angle results of the examples that the dual antibacterial super-lyophobic coating of the present invention has a strong repelling effect on water and ethylene glycol.
[0217] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A dual antibacterial super-liquid-repellent coating, It is characterized in that It is made of fluorinated semi-cage oligomeric silsesquioxane, ethanol, inorganic nanoparticles, antimicrobial peptides and water-based resin; the mass ratio of the fluorinated semi-cage oligomeric silsesquioxane to the water-based resin is 1:(20000-200000); the mass ratio of the antimicrobial peptide to the water-based resin is 1:(1000-5000); the mass ratio of the inorganic nanoparticles to the water-based resin is 1:(50-300); the mass ratio of the fluorinated semi-cage oligomeric silsesquioxane to ethanol is (15-70):(30-85); The antimicrobial peptide is at least one of nisin, pediocin, enterocin, and cecropin; The solid content of the water-based resin is 0.1-20%.
2. The dual antibacterial super-lyophobic coating according to claim 1, It is characterized in that The inorganic nanoparticles are at least one of silicon dioxide nanoparticles, titanium dioxide nanoparticles, aluminum oxide nanoparticles and zirconium dioxide nanoparticles; and the size of the inorganic nanoparticles is 5-500 nm.
3. The dual antibacterial super-lyophobic coating according to claim 1, It is characterized in that The water-based resin is at least one of water-based inorganic silicone resin SJ-8050, water-based silicone resin S-227, water-based polyacrylate 3958, water-based polyurethane 2944, water-based epoxy resin S-969, and water-based fluorocarbon resin DF-01L.
4. The method for preparing the dual antibacterial super-lyophobic coating according to any one of claims 1 to 3, It is characterized in that The following steps are involved: (1) mixing and dissolving a fluorinated semi-cage type oligomeric silsesquioxane and ethanol, and then subjecting the mixture to ultrasonic treatment to obtain an ethanol solution of the fluorinated semi-cage type oligomeric silsesquioxane; (2) mixing the fluorinated semi-cage oligomeric silsesquioxane ethanol solution, inorganic nanoparticles, antimicrobial peptides and aqueous resin to obtain a dual antimicrobial super-lyophobic coating slurry; (3) coating the dual antibacterial super-liquid-repellent coating slurry on a carrier and curing the slurry to obtain the dual antibacterial super-liquid-repellent coating.
5. The method for preparing the dual antibacterial super-lyophobic coating according to claim 4, It is characterized in that The ultrasonic frequency of the ultrasonic treatment is 20-60kHz; the time of the ultrasonic treatment is 5-60min; the curing time is 12-48h; the coating method is at least one of spraying, spin coating, brush coating, and roller coating.
Citation Information
Patent Citations
Superhydrophobic antibacterial cationic fluorine-containing polymer nanocoating
CN110885592A
Durable antibacterial and antiviral super-amphiphobic coating and preparation method thereof
CN114058223A
Superhydrophobicity coating based on waterborne emulsion and preparing method and application thereof
CN106433364A
Antibacterial and antifouling medical table cloth and manufacturing method of same
CN106585034A
Fluorinated semi-polyhedral oligomeric silsesquioxane, and preparation method and application thereof