A method for identifying cuprammonia fiber and lyocell fiber by pyrolysis gas chromatography-mass spectrometry and its application

Through the thermal cracking GC-MS method, gas chromatography-mass spectrometry instrument is used to measure the fiber product, and cuprammonium fiber and lyocell fiber are determined according to the characteristic peak area ratio, which solves the problem of difficult fiber identification in the existing technology and realizes A fast, accurate and environmentally friendly identification method.

CN115993409BActive Publication Date: 2024-10-18FUJIAN FIBER INSPECTION CENT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211404160.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-10
Publication Date
2024-10-18
Estimated Expiration
2042-11-10

AI Technical Summary

Technical Problem

It is difficult to quickly and accurately identify cupro fiber and lyocell fiber with existing technology. The two are very similar in appearance and physical and chemical properties, making it difficult to achieve accurate identification using a single method.

Method used

The thermal cracking GC-MS method is used to measure the thermal cracking products of the fiber through a gas chromatography-mass spectrometry instrument. The determination is based on the characteristic peak area ratio in the total ion chromatogram of the product to realize cuprammonium fiber and lyocell fiber. rapid identification.

Benefits of technology

It achieves reliable fiber identification results within 30 minutes. It has a small sample size, accurate and reliable characterization, good stability and repeatability, avoids the shortcomings of using solvents, and is suitable for large-scale fiber identification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115993409B_ABST
    Figure CN115993409B_ABST
Patent Text Reader

Abstract

The present invention relates to a method and application of thermal cracking gas chromatography-mass spectrometry to identify copper ammonia fiber and lyocell fiber, comprising the following steps: detection: thermal cracking of the fiber to be tested, and the thermal cracking product is measured by a gas chromatography-mass spectrometry instrument to obtain a total ion current chromatogram; analysis and judgment: the total ion current chromatogram includes a first time segment of 2-7.5min and a second time segment of 7.6-11min; the first time segment contains N characteristic product chromatographic peaks, and the total area is S1; the second time segment contains M characteristic product chromatographic peaks, and the total area is S2; according to the result of S2 / S1, the fiber to be tested is judged; or if M=N, according to the S3 value, the fiber to be tested is judged. The method can be applied to quickly and accurately identify copper ammonia fiber and lyocell fiber, and the test result obtained within 30min.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of fiber inspection, and in particular to a method and application of identifying cuprammonia fiber and lyocell fiber by thermal pyrolysis-gas chromatography-mass spectrometry. Background Art

[0002] The qualitative and quantitative determination of fibers is of great significance to the circulation of textile products. In many countries, the law requires that the type of fiber used and its composition must be indicated on textiles. Therefore, it is of great significance to formulate fiber identification standards and component testing methods. Lyocell and cupro fiber are both regenerated cellulose fibers. They use non-petroleum raw materials in the processing process. The finished products and waste are easy to decompose in the natural environment. They are environmentally friendly materials. The molecular structures of these two fibers are very similar, so their appearance and chemical structure are very similar. The microscopy method, combustion method, melting point method and dissolution method specified in the current textile industry series standard FZ / T.01057 cannot identify these two fibers.

[0003] At present, the industry usually uses a variety of methods to comprehensively judge the identification of these two types of fibers: (1) Dissolution method: Liu Zhen et al. used 59.5% sulfuric acid to treat for 30 minutes at room temperature. Lyocell had residues and cuprammonium fiber dissolved, but this method may cause misjudgment due to the presence of other similar dissolving performance fibers; (2) Polarized light microscope method: Liu Zhen et al. found that compared with cuprammonium fiber, Lyocell had obvious notches under a polarized light microscope, but in actual testing, it was found that notches could also be observed on some cuprammonium fibers; (3) Post-coloring microscope observation method: ISO 21915-2 dyes cuprammonium fiber and Lyocell fiber samples with dyes, and uses the different dye uptake rates of cuprammonium fiber and Lyocell to identify them. This method has a complex pre-treatment process and is time-consuming and labor-intensive; (4) Wet expansion performance method: Li Juzhu found through a study of the wet expansion performance of Lyocell and cuprammonium fiber that the instantaneous lateral wet expansion rate of these two fibers in alkaline solution is quite different. Ruan Lingfeng et al. developed a qualitative detection method for cuprammonia fiber and lyocell fiber by taking advantage of the fact that the lateral expansion degree of cuprammonia fiber in sodium hydroxide solution is much higher than that of lyocell fiber. However, this method is more dependent on the experience of the experimenters and is prone to misjudgment.

[0004] In summary, there is currently no method that can quickly and effectively identify these two fibers. The laboratory usually distinguishes these two fibers based on specific experimental phenomena obtained by multiple methods. Therefore, it is necessary to develop a fast, efficient, stable and repeatable accurate characterization method to identify cuprocell and lyocell fibers to meet market demand. Cuprocell and lyocell fibers are very similar in appearance and physical and chemical properties, and it is difficult to accurately and quickly identify them using a single method with existing technology. Summary of the invention

[0005] In view of the above problems, the present application provides a method for quickly and accurately identifying cuprammonium fiber and lyocell fiber, which can obtain reliable test results within 30 minutes.

[0006] To achieve the above object, the inventor provides a method for identifying cuprammonia fiber and lyocell fiber by thermal pyrolysis gas chromatography-mass spectrometry, comprising the following steps:

[0007] Detection:

[0008] Thermal cracking is performed on the fiber to be tested, and the thermal cracking products are measured by gas chromatography-mass spectrometry to obtain a total ion current chromatogram of the cracking products;

[0009] Analysis and judgment:

[0010] The total ion current chromatogram includes a first time segment of 2-7.5 min and a second time segment of 7.6-11 min; the first time segment contains N characteristic product chromatographic peaks, and the total area of ​​the N chromatographic peaks in the first time segment is S1; the second time segment contains M characteristic product chromatographic peaks, and the total area of ​​the M chromatographic peaks in the second time segment is S2;

[0011] According to the results of S2 / S1, the fiber to be tested is judged

[0012] or

[0013] The total ion current chromatogram includes a first time segment of 2-7.5 min and a second time segment of 7.6-11 min; in the first time segment, there are N characteristic product chromatographic peaks in sequence, with areas of N1, N2, .... Nn respectively; in the second time segment, there are M characteristic product chromatographic peaks in sequence, with areas of M1, M2, .... Mm respectively;

[0014] If M = N, then According to the S3 value, the fiber to be tested is judged.

[0015] Different from the prior art, the above technical solution uses a gas chromatography-mass spectrometry instrument to measure the pyrolysis products, and can quickly make a qualitative judgment on the tested fiber according to the difference in the content of several pyrolysis products of cuprammonia fiber and lyocell fiber. The present invention does not need to use any solvent and is an environmentally friendly and safe qualitative test method. In addition, the present invention also has the advantages of a small amount of test samples, accurate and reliable qualitative analysis, good stability and repeatability, and provides a simple, fast and accurate method for the identification of large quantities of cuprammonia fiber and lyocell fiber.

[0016] In some embodiments, if S2 / S1=1.5-3.2, the fiber to be tested is determined to be lyocell fiber; if S2 / S1=4.8-9.0, the fiber to be tested is determined to be cupro fiber.

[0017] In some embodiments, if S3<85, the fiber to be tested is determined to be lyocell fiber; if S3>142, the fiber to be tested is determined to be cupro fiber.

[0018] In some embodiments, the fiber to be tested is cupro fiber or lyocell fiber.

[0019] In some embodiments, the mass of the fiber to be tested is 0.10-0.90 mg.

[0020] In some embodiments, the thermal cracking temperature is 400-600° C., and the thermal cracking time is 0.1-0.5 min.

[0021] In some embodiments, N=4, the chromatographic peaks are at 5.2 min, 5.6 min, 5.9 min, and 7.1 min. M=4, the chromatographic peaks are at 7.7 min, 8.2 min, 9.8 min, and 10.5 min.

[0022] In some embodiments, the chromatographic parameters of the gas chromatography-mass spectrometry instrument are: the chromatographic column uses DB-17MS; the chromatographic column heating process: the initial temperature is 80°C, and the temperature is increased to 300°C at 20°C / min and maintained for 5 minutes; the carrier gas is He gas; the flow rate is 1.0 mL / min.

[0023] In some embodiments, the chromatographic parameters of the gas chromatography-mass spectrometry instrument are: quadrupole temperature is 150°C, ion source temperature is 230°C, mass spectrometry uses EI source, energy is 70eV, full scan mode is used in the mass-to-charge ratio range of 29-550, and solvent delay is 2min.

[0024] To achieve the above-mentioned purpose, the inventor provides a method for identifying cuprammonia fiber and lyocell fiber by pyrolysis gas chromatography-mass spectrometry and its application in identifying and distinguishing cuprammonia fiber and lyocell fiber.

[0025] Different from the prior art, the above technical solution uses a gas chromatography-mass spectrometry instrument to measure the pyrolysis products, and can quickly make a qualitative judgment on the tested fiber according to the difference in the content of several pyrolysis products of cuprammonia fiber and lyocell fiber. The present invention does not need to use any solvent and is an environmentally friendly and safe qualitative test method. In addition, the present invention also has the advantages of a small amount of test samples, accurate and reliable qualitative analysis, good stability and repeatability, and provides a simple, fast and accurate method for the identification of large quantities of cuprammonia fiber and lyocell fiber.

[0026] The above-mentioned records related to the invention content are only an overview of the technical solution of the present application. In order to enable ordinary technicians in the field to more clearly understand the technical solution of the present application, and then implement it according to the text of the specification and the contents recorded in the drawings, and to make the above-mentioned purpose and other purposes, features and advantages of the present application easier to understand, the following is an explanation in combination with the specific implementation mode and drawings of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The drawings are only used to illustrate the principles, implementation methods, applications, characteristics and effects of the specific embodiments of the present application and other related contents, and shall not be considered as limitations of the present application.

[0028] In the drawings of the specification:

[0029] Figure 1 The thermal pyrolysis-gas chromatography-mass spectrometry total ion current chromatogram of the cuprammonium fiber and the lyocell fiber of Example 1 of the present invention;

[0030] Figure 2 The thermal pyrolysis-gas chromatography-mass spectrometry total ion current chromatogram of the cuprammonium fiber and the lyocell fiber of Example 2 of the present invention;

[0031] Figure 3 The thermal pyrolysis-gas chromatography-mass spectrometry total ion current chromatogram of the cuprammonium fiber and the lyocell fiber of Example 3 of the present invention;

[0032] Figure 4 The thermal pyrolysis-gas chromatography-mass spectrometry total ion current chromatogram of the cuprammonium fiber and the lyocell fiber of Example 4 of the present invention;

[0033] Figure 5 This is a total ion current chromatogram of the thermal pyrolysis-gas chromatography-mass spectrometry of the cuprammonia fiber and lyocell fiber of Example 5 of the present invention.

[0034] Figure 6 This is a total ion current chromatogram of the thermal pyrolysis-gas chromatography-mass spectrometry of the cuprammonia fiber and lyocell fiber of Example 6 of the present invention. DETAILED DESCRIPTION

[0035] In order to explain in detail the possible application scenarios, technical principles, specific schemes that can be implemented, and the purposes and effects that can be achieved, the following is a detailed description of the specific embodiments listed in conjunction with the accompanying drawings. The embodiments described herein are only used to more clearly illustrate the technical solutions of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0036] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.

[0037] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.

[0038] In the description of this application, the term "and / or" is an expression used to describe the logical relationship between objects, indicating that three relationships may exist, for example, A and / or B, which means: A exists, B exists, and A and B exist at the same time. In addition, the character " / " in this article generally indicates that the objects before and after are in an "or" logical relationship.

[0039] In the present application, terms such as “first” and “second” are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship of quantity, priority or sequence between these entities or operations.

[0040] Without further limitations, in this application, the words "include", "comprises", "has" or other similar expressions used in the sentences are intended to cover non-exclusive inclusion. These expressions do not exclude the presence of additional elements in the process, method or product including the elements, so that the process, method or product including a series of elements may include not only those limited elements, but also other elements not explicitly listed, or also include elements inherent to such process, method or product.

[0041] Similar to the understanding in the Examination Guidelines, in this application, expressions such as "greater than", "less than", "exceed" and the like are understood to exclude the number itself; expressions such as "above", "below", "within" and the like are understood to include the number itself. In addition, in the description of the embodiments of this application, "multiple" means more than two (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups", "multiple times", etc., unless otherwise clearly and specifically limited.

[0042] In the description of the embodiments of the present application, space-related expressions used, such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "vertical", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicate the orientation or position relationship based on the orientation or position relationship shown in the specific embodiments or drawings, and are only for the convenience of describing the specific embodiments of the present application or facilitating the reader's understanding, and do not indicate or imply that the referred device or component must have a specific position, a specific orientation, or be constructed or operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.

[0043] The inventor provides a method for identifying cuprammonia fiber and lyocell fiber by pyrolysis-gas chromatography-mass spectrometry, comprising the following steps:

[0044] Detection:

[0045] Thermal cracking is performed on the fiber to be tested, and the thermal cracking products are measured by gas chromatography-mass spectrometry to obtain a total ion current chromatogram of the cracking products;

[0046] Analysis and judgment:

[0047] The total ion current chromatogram includes a first time segment of 2-7.5 min and a second time segment of 7.6-11 min; the first time segment contains N characteristic product chromatographic peaks, and the total area of ​​the N chromatographic peaks in the first time segment is S1; the second time segment contains M characteristic product chromatographic peaks, and the total area of ​​the M chromatographic peaks in the second time segment is S2;

[0048] According to the results of S2 / S1, the fiber to be tested is judged;

[0049] or

[0050] The total ion current chromatogram includes a first time segment of 2-7.5 min and a second time segment of 7.6-11 min; in the first time segment, there are N characteristic product chromatographic peaks in sequence, with areas of N1, N2, .... Nn respectively; in the second time segment, there are M characteristic product chromatographic peaks in sequence, with areas of M1, M2, .... Mm respectively;

[0051] If M = N, then According to the S3 value, the fiber to be tested is judged.

[0052] Different from the prior art, the above technical solution uses a gas chromatography-mass spectrometry instrument to measure the thermal cracking products. According to the different contents of several thermal cracking products of cuprammonia fiber and lyocell fiber, a qualitative judgment can be made quickly on the fiber to be tested.

[0053] At room temperature, because the molecular structure and elemental composition of cuprammonium fiber and lyocell fiber are exactly the same, and their appearance, touch and chemical properties are very similar, conventional fiber identification methods cannot accurately and efficiently distinguish them. During the research process, the inventor found that after high-temperature pyrolysis of cuprammonium fiber and lyocell fiber, there are the same stable characteristic pyrolysis products, and the content difference is not large, which makes it difficult to compare.

[0054] In the process of further research, the inventors compared the chromatograms of cuprammonia fiber and lyocell fiber and found that the total area S1 of N chromatographic peaks in the first time segment of 2-7.5min and the total area S2 of M chromatographic peaks in the second time segment of 7.6-11min both had a relatively stable linear relationship. The S2 / S1 method was designed and adopted for judgment. The difference between cuprammonia fiber and lyocell fiber is large, and it can be clearly judged whether the fiber to be tested is cuprammonia fiber or lyocell fiber.

[0055] At the same time, when M=N, The value can also be judged based on the difference between the cupro fiber and the lyocell fiber in the first time segment and the second time segment.

[0056] In some embodiments, if S2 / S1=1.5-3.2, the fiber to be tested is determined to be a lyocell fiber. The inventor sets this interval based on the S2 / S1 value of 1.62 of the lyocell fiber standard and in combination with the detection values ​​of multiple batches of non-standard lyocell fibers. If S2 / S1=4.8-9.0, the fiber to be tested is determined to be a cuprammonium fiber. The inventor sets this interval based on the S2 / S1 value of 6.35 of the cuprammonium fiber standard and in combination with the detection values ​​of multiple batches of non-standard cuprammonium fibers.

[0057] In some embodiments, if S3<85, the fiber to be tested is determined to be lyocell fiber; if S3>142, the fiber to be tested is determined to be cupro fiber. The inventor sets the threshold value based on the S3 values ​​of lyocell fiber and cupro fiber standards and in combination with the detection values ​​of multiple batches of non-standard lyocell fiber and cupro fiber.

[0058] In some embodiments, the fiber to be tested is cuprammonium fiber or lyocell fiber. It should be noted that, whether abroad or domestically, identifying cuprammonium fiber and lyocell fiber is a difficulty and pain point in the current industry. Since the purpose of the present invention is to provide a method for quickly, efficiently and accurately determining whether a fiber is cuprammonium fiber or lyocell fiber, that is, the identification object of the present invention is cuprammonium fiber and lyocell fiber, rather than other fibers other than cuprammonium fiber or lyocell fiber.

[0059] In some embodiments, the mass of the fiber to be tested is 0.10-0.90 mg. This technical solution can be used to detect a small amount of fiber. In the forensic detection of some special clothing or fabrics, a fiber to be tested can be extracted for detection and determination without damaging the clothing or fabric sample, which is conducive to protecting the integrity of evidence.

[0060] In some embodiments, the thermal cracking temperature is 400-600° C., and the thermal cracking time is 0.1-0.5 min. The thermal cracking temperature and time affect the thermal cracking products and content. At 400-600° C. and 0.1-0.5 min, the fiber to be tested can achieve sufficient thermal cracking.

[0061] In some embodiments, N=4, the chromatographic peaks are at 5.2 min, 5.6 min, 5.9 min, and 7.1 min. M=4, the chromatographic peaks are at 7.7 min, 8.2 min, 9.8 min, and 10.5 min.

[0062] In the first time segment of 2-7.5 min, four characteristic products common to cuproammonia fiber and lyocell fiber with large content differences were selected (5.2 min, 5.6 min, 5.9 min, 7.1 min), and the S1 value was calculated.

[0063] In the second time segment of 7.6-11 min, four characteristic products common to cuproammonia fiber and lyocell fiber with large content differences were selected (7.7 min, 8.2 min, 9.8 min, 10.5 min) to calculate the S2 value.

[0064] The ratio S1 / S2 of the total area S1 of the four chromatographic peaks in the first time segment and the total area S2 of the four chromatographic peaks in the second time segment above, both have a relatively stable linear relationship. By using the S2 / S1 method for judgment, the difference between cuprammonia fiber and lyocell fiber is large, and it can be clearly judged whether the fiber to be tested is cuprammonia fiber or lyocell fiber.

[0065] In some embodiments, the chromatographic parameters of the gas chromatography-mass spectrometry instrument are: the chromatographic column uses DB-17MS; the chromatographic column heating process: the initial temperature is 80°C, and the temperature is increased to 300°C at 20°C / min and maintained for 5 minutes; the carrier gas is He gas; the flow rate is 1.0 mL / min.

[0066] In some embodiments, the chromatographic parameters of the gas chromatography-mass spectrometry instrument are: quadrupole temperature is 150°C, ion source temperature is 230°C, mass spectrometry uses EI source, energy is 70eV, full scan mode is used in the mass-to-charge ratio range of 29-550, and solvent delay is 2min.

[0067] Example 1

[0068] The standard samples of cuprammonium fiber and lyocell fiber were cut into small pieces respectively, and 0.50 mg of the sample was weighed and kneaded into a ball and placed in the pyrolysis cup A and pyrolysis cup B of the pyrolysis instrument. The pyrolysis cups A and B containing the test samples were placed in the sample introduction plate of the pyrolysis instrument, and pyrolyzed at a pyrolysis temperature of 500°C for 0.2 min. The pyrolysis products were measured by gas chromatography-mass spectrometry (specific experimental parameters are shown in Table 1) to obtain Figure 1 Total ion current chromatograms of the cleavage products are shown.

[0069] Then, the characteristic product chromatographic peaks of the total ion current chromatogram obtained above were extracted, and the sum of the peak area intensities S1 at 5.2 min, 5.6 min, 5.9 min, and 7.1 min and the peak area intensities S2 at 7.7 min, 8.2 min, 9.8 min, and 10.5 min were counted.

[0070] The calculated S2 / S1 values ​​of cuproammonia fiber and lyocell fiber standards are 6.35 and 1.62 respectively.

[0071] Table 1 Gas chromatography-mass spectrometry method test parameters

[0072]

[0073] Example 2

[0074] The sample to be tested was cut into small pieces, 0.55 mg of the sample was weighed and kneaded into a ball and placed in the pyrolysis cup A of the pyrolysis instrument. The pyrolysis cup A containing the test sample was placed in the sample inlet of the pyrolysis instrument, and pyrolyzed at a pyrolysis temperature of 400°C for 0.2 min. The pyrolysis products were measured by gas chromatography-mass spectrometry (specific experimental parameters are shown in Table 1) to obtain Figure 2 Total ion current chromatograms of the cleavage products are shown.

[0075] Then, the characteristic product chromatographic peaks of the total ion current chromatogram obtained above were extracted, and the sum of the peak area intensities S1 at 5.2min, 5.6min, 5.9min, and 7.1min and the peak area intensities S2 at 7.7min, 8.2min, 9.8min, and 10.5min were counted. The S2 / S1 value of the sample to be tested was calculated to be 8.68, S2 / S1=4.8-9.0, and the fiber was determined to be cuprammonium fiber.

[0076] Example 3

[0077] The sample to be tested was cut into small pieces, 0.52 mg of the sample was weighed and kneaded into a ball and placed in the pyrolysis cup A of the pyrolysis instrument. The pyrolysis cup A containing the test sample was placed in the sample inlet of the pyrolysis instrument, and pyrolyzed at a pyrolysis temperature of 450°C for 0.2 min. The pyrolysis products were measured by a gas chromatography-mass spectrometry instrument (specific experimental parameters are shown in Table 1) to obtain Figure 3 Total ion current chromatograms of the cleavage products are shown.

[0078] Then, the characteristic product chromatographic peaks of the total ion current chromatogram obtained above were extracted, and the sum of the peak area intensities S1 at 5.2 min, 5.6 min, 5.9 min, and 7.1 min and the peak area intensities S2 at 7.7 min, 8.2 min, 9.8 min, and 10.5 min were counted.

[0079] The calculated S2 / S1 value of the sample to be tested is 8.07, S2 / S1=4.8-9.0, and the fiber is determined to be cuprammonia fiber.

[0080] Example 4

[0081] The sample to be tested was cut into small pieces, 0.58 mg of the sample was weighed and kneaded into a ball and placed in the pyrolysis cup A of the pyrolysis instrument. The pyrolysis cup A containing the test sample was placed in the sample inlet of the pyrolysis instrument, and pyrolyzed at a pyrolysis temperature of 550°C for 0.2 min. The pyrolysis products were measured by gas chromatography-mass spectrometry (specific experimental parameters are shown in Table 1) to obtain Figure 4 Total ion current chromatograms of the cleavage products are shown.

[0082] Then, the characteristic product chromatographic peaks of the total ion current chromatogram obtained above were extracted, and the sum of the peak area intensities S1 at 5.2 min, 5.6 min, 5.9 min, and 7.1 min and the peak area intensities S2 at 7.7 min, 8.2 min, 9.8 min, and 10.5 min were counted.

[0083] The calculated S2 / S1 value of the sample to be tested is 1.89, S2 / S1=1.5-3.2, and the fiber is determined to be Lyocell fiber.

[0084] Example 5

[0085] The sample to be tested was cut into small pieces, 0.53 mg of the sample was weighed and kneaded into a ball and placed in the pyrolysis cup A of the pyrolysis instrument. The pyrolysis cup A containing the test sample was placed in the sample inlet of the pyrolysis instrument, and pyrolyzed at a pyrolysis temperature of 600°C for 0.2 min. The pyrolysis products were measured by gas chromatography-mass spectrometry (specific experimental parameters are shown in Table 1) to obtain Figure 5 Total ion current chromatograms of the cleavage products are shown.

[0086] Then, the characteristic product chromatographic peaks of the total ion current chromatogram obtained above were extracted, and the sum of the peak area intensities S1 at 5.2 min, 5.6 min, 5.9 min, and 7.1 min and the peak area intensities S2 at 7.7 min, 8.2 min, 9.8 min, and 10.5 min were counted.

[0087] The calculated S2 / S1 value of the sample to be tested is 1.92, S2 / S1=1.5-3.2, and the fiber is determined to be Lyocell fiber.

[0088] Example 6

[0089] The sample to be tested was cut into small pieces, 0.56 mg of the sample was weighed and kneaded into a ball and placed in the pyrolysis cup A of the pyrolysis instrument. The pyrolysis cup A containing the test sample was placed in the sample inlet of the pyrolysis instrument, and pyrolyzed at a pyrolysis temperature of 600°C for 0.2 min. The pyrolysis products were measured by gas chromatography-mass spectrometry (specific experimental parameters are shown in Table 1) to obtain Figure 6 The total ion current chromatogram of the pyrolysis product is shown. The characteristic product chromatogram peaks of the total ion current chromatogram obtained above are then extracted, and the peak area intensities at 7.7min, 8.2min, 9.8min, and 10.5min in the second time range are divided and compared with the peak area intensities at 5.2min, 5.6min, 5.9min, and 7.1min in the first time range in sequence. Finally, all the divided comparison values ​​are squared and added to obtain the total value.

[0090] Since S3=167.6 (>142), the fiber is determined to be cuprammonium fiber.

[0091] Cuprammonia fiber and lyocell fiber are very similar in appearance and physical and chemical properties, and it is difficult to accurately and quickly identify them with a single method in the prior art. The inventor found in the research process that cuprammonia fiber and lyocell fiber have slight differences in physical and chemical parameters such as crystallinity, crystal orientation and degree of polymerization, and these slight differences will manifest as differences in the composition and proportion of pyrolysis products during the pyrolysis process. The present invention can easily measure the pyrolysis products and proportions of cuprammonia fiber and lyocell fiber by a pyrolysis-gas chromatography-mass spectrometry instrument, without using any solvent, and can qualitatively identify cuprammonia fiber and lyocell fiber within half an hour. This identification method can not only quickly identify these two fibers in large quantities, but also has the advantages of a small amount of sample required for testing, accurate and reliable qualitative analysis, and good stability and repeatability.

[0092] Finally, it should be noted that although the above embodiments have been described in the specification and drawings of this application, this does not limit the scope of patent protection of this application. All technical solutions generated by replacing or modifying equivalent structures or equivalent processes based on the essential concept of this application using the contents recorded in the specification and drawings of this application, as well as directly or indirectly implementing the technical solutions of the above embodiments in other related technical fields, are included in the scope of patent protection of this application.

Claims

1. A method for identifying cuprammonia fiber and lyocell fiber by thermal pyrolysis gas chromatography-mass spectrometry, characterized in that: The following steps are involved: Detection: The fiber to be tested is subjected to thermal pyrolysis, and the thermal pyrolysis products are measured by gas chromatography-mass spectrometry to obtain a total ion current chromatogram of the pyrolysis products; Analysis and judgment: The total ion current chromatogram includes a first time segment of 2-7.5 min and a second time segment of 7.6-11 min; the first time segment contains N characteristic product chromatographic peaks, and the total area of ​​the N chromatographic peaks in the first time segment is S1; the second time segment contains M characteristic product chromatographic peaks, and the total area of ​​the M chromatographic peaks in the second time segment is S2; When N=4, the chromatographic peaks are at 5.2min, 5.6min, 5.9min, and 7.1min; when M=4, the chromatographic peaks are at 7.7min, 8.2min, 9.8min, and 10.5min; according to the result of S2 / S1, the fiber to be tested is judged, and if S2 / S1=1.5-3.2, the fiber to be tested is judged to be lyocell fiber; If S2 / S1=4.8-9.0, the fiber to be tested is determined to be cuprammonium fiber; or The total ion current chromatogram includes a first time segment of 2-7.5 min and a second time segment of 7.6-11 min; in the first time segment, there are N characteristic product chromatographic peaks in sequence, with areas of N1, N2, .... Nn respectively; in the second time segment, there are M characteristic product chromatographic peaks in sequence, with areas of M1, M2, .... Mm respectively; When N=4, the chromatographic peaks are at 5.2min, 5.6min, 5.9min, and 7.1min; when M=4, the chromatographic peaks are at 7.7min, 8.2min, 9.8min, and 10.5min; According to the S3 value, the fiber to be tested is judged; if S3<85, the fiber to be tested is judged to be lyocell fiber; if S3>142, the fiber to be tested is judged to be cuprammonium fiber; The thermal cracking temperature is 400-600°C, and the thermal cracking time is 0.1-0.5min; The chromatographic parameters of the gas chromatography-mass spectrometry instrument are as follows: the chromatographic column uses DB-17MS; the chromatographic column heating process: the initial temperature is 80°C, the temperature is increased to 300°C at 20°C / min and maintained for 5 minutes; the carrier gas is He gas; the flow rate is 1.0 mL / min; the full scan mode is used to scan in the mass-to-charge ratio range of 29-550 of the mass spectrometer.

2. The method for distinguishing cuprammonium fiber and lyocell fiber according to claim 1, characterized in that: The fiber to be tested is cuprammonium fiber or lyocell fiber.

3. The method for distinguishing cuprammonium fiber and lyocell fiber according to claim 1, characterized in that: The mass of the fiber to be tested is 0.10-0.90 mg.

4. The method for distinguishing cuprammonium fiber and lyocell fiber according to claim 1, characterized in that: The mass spectrometry parameters of the gas chromatography-mass spectrometry instrument are as follows: quadrupole temperature is 150°C, ion source temperature is 230°C, mass spectrometry uses EI source, energy is 70 eV, and solvent delay is 2 min.

5. Use of the method for identifying cuprammonium fiber and lyocell fiber by pyrolysis gas chromatography-mass spectrometry according to any one of claims 1 to 4 in identifying and distinguishing cuprammonium fiber and lyocell fiber.