Method, device and application for preparing alkylaluminoxane for in-situ olefin oligomerization and polymerization

Using packed column technology to carry water in an inert organic solvent to react with alkyl aluminum solves the problem of the generation of aluminum hydroxy compounds and aluminum oxide in the existing technology, improves the preparation yield and activity of alkyl aluminoxane, and achieves Efficient preparation of alkylaluminoxanes.

CN116023528BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111247230.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-26
Publication Date
2024-10-15
Estimated Expiration
2041-10-26

AI Technical Summary

Technical Problem

It is difficult to effectively avoid the formation of aluminum hydroxyl compounds and aluminum oxide when preparing alkyl aluminoxane with the existing technology, resulting in low reaction yield and unstable product activity. In addition, traditional methods have problems with the adsorption of inorganic salt reaction residues to the product. .

Method used

Packed column technology is used to carry metered water, and the mobile phase is used to drive the reaction between water and alkylaluminum in an inert organic solvent. The reaction conditions are controlled to generate alkylaluminoxane, avoiding the generation of aluminum hydroxy compounds and aluminum trioxide, and improving productivity. rate and activity.

Benefits of technology

It achieves the preparation of alkylaluminoxane with high yield and high activity, avoids the adsorption of inorganic salt residues, and ensures the stability and reaction efficiency of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116023528B_ABST
    Figure CN116023528B_ABST
Patent Text Reader

Abstract

The present invention relates to a method, device and application for preparing alkylaluminoxane for in-situ cutting-in olefin polymerization and polymerization reaction. The method comprises: using a filling column to meter water, and injecting the water into a solution formed by alkyl aluminum and a first inert organic solvent under the drive of a mobile phase to react, obtaining a mixed solution containing alkylaluminoxane, and metering and detecting the alkylaluminoxane in the mixed solution. The method uses the filling column technology to carry a trace amount of metered water, so that the amount of water relative to the amount of alkyl aluminum in the inert organic solvent solution can maximize the generation of alkylaluminoxane instead of aluminum hydroxy compounds or aluminum oxide. In the experimental operation, the relevant configuration and operation technology are combined to make the reaction proceed smoothly and controllably, and the alkylaluminoxane is prepared with high yield. The prepared alkylaluminoxane can be in-situ cut-in olefin polymerization and polymerization reaction, and used as a co-catalyst for olefin polymerization and polymerization reaction, so as to use the alkylaluminoxane efficiently.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of alkylaluminoxane, and in particular relates to a method, a device and application of preparing alkylaluminoxane for in-situ cutting-in olefin oligomerization and polymerization reaction. Background Art

[0002] Alkyl aluminoxane is an important cocatalyst or catalyst for olefin polymerization and polymerization, among which methyl aluminoxane plays the most significant role. The main functions of alkyl aluminoxane are: 1) group exchange reaction with the transition metal in the main catalyst; 2) grabbing the group at the transition metal center to form a cationic single active catalytic center; 3) removing impurities from the reaction system. It has also been reported that the aluminum alkyl group of alkyl aluminoxane is easy to exchange groups with the polymer chain in the main catalyst, which can affect the molecular weight and molecular weight distribution of the polymer product.

[0003] Alkyl aluminoxanes are synthesized by reacting alkyl aluminum with water or a water-containing substance, or by a method that can form RAlO or R2AlOAlR2 (R is an alkyl) structural fragments. Alkyl aluminoxane synthesis for laboratory and industrial use is carried out in an inert organic solvent, and the result is usually a mixture of an organic solution of alkyl aluminoxane and alkyl aluminum. Therefore, when alkyl aluminoxane is used directly as a solution, it is necessary to consider that its structural formula is (RAlO) n ·(AlR3) m or (R2AlOAlR2) n ·(AlR3) m The former is the reaction of one molecule of AlR3 to remove two molecules of RH, and the latter is the reaction of two molecules of AlR3 to remove two molecules of RH. When both reactions exist, the structural formula of the resulting mixture of alkylaluminoxane and alkylaluminum can be expressed as (RAlO) n ·(R2AlOAlR2) l ·(AlR3) m When the volatile substances in the alkylaluminoxane solution are removed by decompression or volatilization, the structural formula of the remaining solid alkylaluminoxane is generally considered to be (RA1O) n or (R2AlOAlR2) n or (RA1O) n ·(R2AlOAlR2) l . However, when alkyl aluminum reacts with water or water-containing substances, aluminum hydroxy compounds or aluminum oxide are also generated, and aluminum hydroxy compounds or aluminum oxide are inactive species. At the same time, the reaction between alkyl aluminum and water is very violent, and it is easy to form inactive aluminum hydroxy compounds or aluminum oxide. Therefore, the reaction between alkyl aluminum and water or water-containing substances requires metering control and reaction condition control to obtain effective alkyl aluminumoxane (RAlO) n ·(AlR3)m or (R2AlOAlR2) n ·(AlR3) m or (RA1O) n ·(R2AlOAlR2) l ·(AlR3) m or (RA1O) n or (R2AlOAlR2) n or (RA1O) n ·(R2AlOAlR2) l It is well known in the art that metering control and reaction condition control require a combination of certain device design and operating techniques.

[0004] The process of forming alkylaluminoxanes by reacting an alkylaluminum with a water-containing material such as a crystalline hydrate is generally referred to by those skilled in the art as the indirect process. Patents DE3240383A1, EP0208561A2, EP0513808A2, US4544762A, US4404744, US4665208, US5041583, US5099050, CN03104815.3, CN97104192.X, CN200410029717.5, CN200910090468.3, CN201010215018.5 and the like report the use of metal salt crystal water compounds for the synthesis of alkyl aluminoxanes, but the metal ions therein are prone to bring colored impurities to the product and also affect the reaction activity of the alkyl aluminoxane. However, this synthesis method also has a weakness, that is, a large amount of inorganic salt reaction residues will adsorb the product and alkyl aluminum, resulting in a large loss and a low reaction yield. There are also reports on the use of porous materials that absorb a certain amount of water, such as silica gel, molecular sieves, alumina, cyclodextrin (CN88106834.9, CN1039587C, CN94119050.1, CN97104192.X, CN201010576012.0, CN201210239141.X), etc., to react with alkyl aluminum to synthesize alkyl aluminoxane. The reaction characteristics and weaknesses are similar to those of the above situation, and the adsorption of alkyl aluminoxane and alkyl aluminum by the reaction residues is also inevitable.

[0005] The method of directly reacting alkylaluminum with water to produce alkylaluminoxane is usually called the direct method by people in the art, but it is well known that the reaction between alkylaluminum and water is very violent. Therefore, the control of the ratio and metering of alkylaluminum and H2O, the concentration adjustment of inert organic solvent, reaction temperature, stirring degree, and the degree of extraction of alkane by-products are very important for synthesizing high-quality and high-yield alkylaluminoxane. These factors put forward extremely high requirements on the corresponding synthetic reaction process control, accident prevention of the reaction device, and safety protection of the operator.

[0006] US4924018 uses a static mixer to fully mix water and toluene to form an emulsion, which is then injected into a reactor through a conduit to react with an alkyl aluminum toluene solution. US4908436 reacts this emulsion and solution through a T-type reactor. US4772736 uses a syringe pump to inject water through a stainless steel conduit. There are three conditions for injection: first, the outlet of the stainless steel pipe is designed to be a structural system that can turn the outflowing water into a mist-like structure; second, a low-pressure nitrogen system is set at the entrance of the pipe to promote water atomization; and third, the atomized water is directly introduced below the liquid level through the blades of a propeller stirrer to quickly disperse the water mist in the alkyl aluminum toluene solution under high shear and vigorous stirring for reaction. US5041585 also mentions a method for synthesizing atomized water. US4937363 instructs an inert gas containing water vapor, i.e., to form a moist inert gas, which is introduced from the bottom of a hollow column and rises along the column wall, thereby contacting and reacting with the alkyl aluminum solution falling from the top membrane method. US5087713 uses ice cubes at -80°C and a dilute solution of an alkyl aluminum in an inert solvent to react under mechanical force or vigorous stirring to generate fluid impact force to produce alkyl aluminum oxane. Sinn et al. (Sinn, H.; Bliemeister, J.; et al. In Ziegler catalyst recent innovations and technological improvements, 1995, p58) further used a frozen ice tray at -40°C and an alkyl aluminum toluene solution to react and synthesize alkyl aluminum oxane. US4730072 and ER257695A use ultrasonic vibration to evenly disperse mutually immiscible water and organic solvents, especially toluene, and then react with the alkyl aluminum solution.

[0007] Compared with the indirect method, the direct method can avoid the adsorption of the reaction salt residue on alkylaluminoxane and alkylaluminum. However, whether it is the direct method or the indirect method, the reaction between alkylaluminum and water molecules is very violent. To control the reaction to produce alkylaluminoxane instead of aluminum hydroxy compounds or aluminum oxide, there are still very high requirements for the synthesis process and synthesis technology.

[0008] In addition, reports show (Prog. Polym. Sci., 1995, Vol. 20, 309-367) that the synthesized alkylaluminoxane solution contains a certain amount of unreacted alkylaluminum, which exists in a free state or in a complex state with the alkylaluminoxane, and forms a coexistence equilibrium state with the alkylaluminoxane in the solution. However, this equilibrium state is unstable and will cause dissociation or decomposition after a certain period of time, forming a solid precipitate that precipitates from the solution. Therefore, when using alkylaluminoxane in industry, it is emphasized to store it at low temperature and use it as soon as possible. Summary of the invention

[0009] The present invention aims at the deficiencies of the prior art and provides a method for preparing an alkylaluminoxane for in-situ cutting-in olefin oligomerization and polymerization reaction. The method utilizes a filling column technology, and the filling column can load a certain amount of water so that the amount of water relative to the amount of alkylaluminum in the inert organic solvent solution can maximize the generation of alkylaluminoxane instead of aluminum hydroxy compound or aluminum oxide. In the experimental operation, the relevant configuration and operation technology are combined to make the reaction proceed smoothly and controllably, and the alkylaluminoxane is prepared with high yield. The prepared alkylaluminoxane can be in-situ cut-in olefin oligomerization and polymerization reaction, and used as a co-catalyst for olefin oligomerization and polymerization reaction, so as to efficiently use the alkylaluminoxane.

[0010] To this end, the first aspect of the present invention provides a method for preparing an alkylaluminoxane for in-situ olefin oligomerization and polymerization reaction, which comprises: using a filling column to meter water, and injecting the water into a solution formed by alkyl aluminum and a first inert organic solvent under the drive of a mobile phase to react, obtaining a mixed solution containing alkylaluminoxane, and metering and detecting the alkylaluminoxane in the mixed solution.

[0011] In some embodiments of the present invention, the water loading capacity of the packed column is 0.1 mL to 1000 mL.

[0012] In the present invention, the water can be injected into the filling column by a micro injection pump.

[0013] In some embodiments of the present invention, the column filler in the packed column is selected from inorganic substances that do not react with water or form a gel with water or organic high molecular polymers that do not react with water or form a gel with water.

[0014] There is no chemical reaction between the column filler and the water molecules in the present invention, and the interaction force between the two is preferably a van der Waals force or a weak hydrogen bond.

[0015] In some embodiments of the present invention, the inorganic substance is selected from at least one of silicon oxide, aluminum oxide, molecular sieve, kaolin, attapulgite, ceramics, metal oxide ceramics and glass fibers. In addition, other inorganic substances that do not interact strongly with water and can be carried by the mobile phase are selected fillers. It is worth noting that: experiments show that silicon oxide, aluminum oxide, molecular sieve, kaolin, attapulgite that are not calcined at high temperature are easy to form gels with water, and water cannot be carried smoothly. Therefore, the selected silicon oxide, aluminum oxide, molecular sieve, kaolin, attapulgite need to be calcined at high temperature and crushed into particles of a certain size for use. The size of the particles depends on whether the rate of the mobile phase is within the control range. Generally, the size of the particles can be 4 to 400 mesh (Note: determined by the American standard mesh number).

[0016] In other embodiments of the present invention, the organic high molecular polymer is selected from at least one of polyethylene, polypropylene, polyvinyl chloride, polytetrafluoroethylene, polystyrene, polyisobutylene, polyisoprene, ethylene-propylene rubber resin, polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polybutyl methacrylate, polymethyl acrylate, polyethyl acrylate, polypropyl acrylate, polybutyl acrylate, polyacrylamide, polycarbonate, polysulfone and polyetheretherketone.

[0017] In the present invention, the column filler can also be an inorganic metal framework compound that does not react with water or form a gel with water. Other high molecular organic compounds and metal organic framework compounds that do not strongly interact with water and can be carried by the mobile phase are all selected fillers.

[0018] In some embodiments of the present invention, the structural formula of the alkyl aluminum is AlR3, wherein R is an alkyl group, which is limited to the alkyl group that can be prepared currently. In some specific embodiments of the present invention, R is an alkyl group with 1 to 20 carbon atoms.

[0019] In some preferred embodiments of the present invention, the alkyl aluminum is selected from at least one of trimethyl aluminum, triethyl aluminum, tri-n-propyl aluminum, tri-n-butyl aluminum, tri-isobutyl aluminum and tri-n-octylaluminum.

[0020] When the alkyl aluminum is a single alkyl aluminum, the method is used to prepare a single alkyl aluminoxane; when the alkyl aluminum is a mixture of two alkyl aluminums, the method is used to prepare a mixed dialkyl aluminoxane; when the alkyl aluminum is a mixture of three or more alkyl aluminums, the method is used to prepare a multi-mixed alkyl aluminoxane.

[0021] In some embodiments of the present invention, the first inert organic solvent is selected from any one of straight-chain hydrocarbons, branched hydrocarbons, cyclic saturated hydrocarbons and aromatic hydrocarbons; preferably, the first inert organic solvent is selected from any one of toluene, xylene, trimethylbenzene, n-pentane, isopentane, neopentane, cyclopentane, methylcyclopentane, n-hexane, n-heptane, cyclohexane, methylcyclohexane, petroleum ether, isoheptane, neoheptane, Isopar E and Isopar F.

[0022] In other embodiments of the present invention, the mobile phase is selected from a second inert organic solvent or a gaseous substance that does not react with water and alkyl aluminum.

[0023] In some specific embodiments of the present invention, the second inert organic solvent is selected from any one of straight-chain hydrocarbons, branched hydrocarbons, cyclic saturated hydrocarbons and aromatic hydrocarbons; further preferably, the second inert organic solvent is selected from any one of toluene, xylene, trimethylbenzene, n-pentane, isopentane, neopentane, cyclopentane, methylcyclopentane, n-hexane, n-heptane, cyclohexane, methylcyclohexane, petroleum ether, isoheptane, neoheptane, Isopar E and Isopar F.

[0024] In some preferred embodiments of the present invention, the second inert organic solvent is the same as the first inert organic solvent, that is, the inert organic solvent used for the mobile phase is consistent with the inert organic solvent used to dissolve the alkyl aluminum.

[0025] In some other specific embodiments of the present invention, the gaseous substance is selected from any one of nitrogen, argon and methane.

[0026] In some embodiments of the present invention, the molar ratio of water to alkyl aluminum is not higher than 1:1. The minimum value of the molar ratio of water to alkyl aluminum depends on the optimal activity of the alkyl aluminoxane obtained after the reaction for a specific co-catalytic reaction or catalytic reaction. In some preferred embodiments of the present invention, the molar ratio of water to alkyl aluminum is 1:(1-10), preferably 1:(1-5).

[0027] In other embodiments of the present invention, the content of alkyl aluminum in the solution is 0.4-80 wt %.

[0028] The amount of the inert organic solvent in the present invention is determined by the following aspects: (1) to ensure a smooth reaction, (2) to avoid the formation of insoluble solid aluminum hydroxy compounds or aluminum oxide to the greatest extent possible, and (3) to ensure that the generated alkylaluminoxane solution of a certain concentration has the best activity for a specific co-catalytic reaction or catalytic reaction.

[0029] In some specific embodiments of the present invention, the content of metallic aluminum in the mixed solution containing alkylaluminoxane is 0.1 to 40.0 wt %; wherein, when the mobile phase is a gaseous substance, the content of metallic aluminum in the mixed solution containing alkylaluminoxane is controlled by adjusting the amount of the first inert organic solvent; when the mobile phase is a second inert organic solvent, the content of metallic aluminum in the mixed solution containing alkylaluminoxane is controlled by adjusting the sum of the amounts of the first inert organic solvent and the second inert organic solvent.

[0030] In some embodiments of the present invention, the reaction temperature is -50 to 110°C, preferably -20 to 90°C, and more preferably -10 to 80°C. In the present invention, the control of the reaction temperature is preferably carried out in steps, wherein the process from the addition of water carried by the gaseous mobile phase or the water carried by the liquid inert organic solvent mobile phase to the reaction of the solution containing the alkyl aluminum is controlled at the lower temperature limit; and the subsequent aging process needs to be controlled at the upper temperature limit. The temperature limits of these two steps refer to a certain temperature range, and the specific temperature of each step is determined based on the optimal performance of the subsequent catalytic activity test. The reaction time of these two steps should also be determined by the optimal performance of the subsequent catalytic activity test.

[0031] In some embodiments of the present invention, the reaction time is 4 to 15 hours, preferably 8 to 12 hours.

[0032] For those skilled in the art, this control is not limited to two-step control. In order to achieve the best performance of the synthesized alkylaluminoxane solution in terms of co-catalysis or catalysis, one or more steps of control are also permitted. The aging process after water is added to react with the solution containing alkylaluminum can be understood as generating a stable alkylaluminoxane, the structural formula of which is as described above (RA10): n ·(AlR3) m or (R2AlOAlR2) n ·(AlR3) m or (RA1O) n ·(R2AlOAlR2) l ·(AlR3) m or (RA1O) n or (R2AlOAlR2) n or (RA1O) n ·(R2AlOAlR2) l .

[0033] In the present invention, the finally obtained mixed solution containing alkylaluminoxane is injected into a sealed container under an inert atmosphere for standby use, and the sealed container is selected from a pressure-resistant glass bottle or a stainless steel bottle.

[0034] The alkylaluminoxane prepared by the present invention preferably includes methylaluminoxane, ethylaluminoxane, n-propylaluminoxane, isopropylaluminoxane, n-butylaluminoxane, isobutylaluminoxane, tert-butylaluminoxane, and n-octylaluminoxane. The alkylaluminoxane that can be synthesized is limited to the R alkyl that can be prepared at present, and other alkylaluminoxanes produced by controlled hydrolysis of other alkylaluminums are not excluded.

[0035] It should be noted that these specific alkylaluminoxanes are just general terms, and the structural formula should include the following types: The structural formula of methylaluminoxane is (MeAlO) n·(AlMe3) m 、(Me2AlOAlMe2) n ·(AlMe3) m 、(MeAlO) n ·(Me2AlOAlMe2) l ·(AlMe3) m 、(MeAlO) n 、(Me2AlOAlMe2) n 、(MeAlO) n ·(Me2AlOAlMe2) l ; The structural formula of ethylaluminoxane is (EtAlO) n ·(AlEt3) m 、(Et2AlOAlEt2) n ·(AlEt3) m 、(EtAlO) n ·(Et2AlOAlEt2) l ·(AlEt3) m 、(EtAlO) n 、(Et2AlOAlEt2) n 、(EtAlO) n ·(Et2AlOAlEt2) l ; The structural formula of n-propylaluminoxane is (nPrAlO) n ·(AlnPr3) m 、(nPr2AlOAlnPr2) n ·(AlnPr3) m 、(nPrAlO) n ·(nPr2AlOAlnPr2) l ·(AlnPr3) m 、(nPrAlO) n 、(nPr2AlOAlnPr2) n 、(nPrAlO) n ·(nPr2AlOAlnPr2) l ; The structural formula of n-butylaluminoxane is (nBuAlO) n ·(AlnBu3) m 、(nBu2AlOAlnBu2) n ·(AlnBu3) m 、(nBuAlO) n ·(nBu2AlOAlnBu2) l ·(AlnBu3) m 、(nBuAlO) n 、(nBu2AlOAlnBu2)n 、(nBuAlO) n ·(nBu2AlOAlnBu2) l ; The structural formula of isobutylaluminoxane is (iBuAlO) n ·(AliBu3) m 、(iBu2AlOAliBu2) n ·(AliBu3) m 、(iBuAlO) n ·(iBu2AlOAliBu2) l ·(AliBu3) m 、(iBuAlO) n 、(iBu2AlOAliBu2) n 、(iBuAlO) n ·(iBu2AlOAliBu2) l ; The structural formula of n-octylaluminoxane is (n-OctylAlO) n ·(Aln-Octyl3) m 、(n-Octyl2AlOAln-Octyl2) n ·(Aln-Octyl3) m 、(n-OctylAlO) n ·(n-Octyl2AlOAln-Octyl2) l ·(Aln-Octyl3) m 、(n-OctylAlO) n 、(n-Octyl2AlOAln-Octyl2) n 、(n-OctylAlO) n ·(n-Octyl2AlOAln-Octyl2) l The structural formulas of other alkylaluminoxanes also basically include these, wherein the alkyl groups need to be replaced accordingly.

[0036] In some embodiments of the present invention, the content of alkylaluminoxane in the mixed solution is measured by detecting the content of metallic aluminum in the mixed solution.

[0037] In the present invention, the method for detecting the content of metallic aluminum in the mixed solution can be: taking a certain amount of the mixed solution containing alkylaluminoxane, hydrolyzing to generate aluminum ions, reacting with an excess of complexing agent disodium ethylenediaminetetraacetate at a relatively low acidity to generate a water-soluble complex, using xylenol orange as an indicator, and back-titrating the excess disodium ethylenediaminetetraacetate with a zinc salt solution. After the zinc ions are complexed with disodium ethylenediaminetetraacetate, the extremely slightly excessive zinc ions form a colored complex with the indicator, which is the titration end point. Finally, the mass percentage of metallic aluminum in the mixed solution containing alkylaluminoxane can be calculated.

[0038] The determination of the amount of alkyl in alkylaluminoxane, for methylaluminoxane and ethylaluminoxane, can be balanced by the amount of methane gas or ethane gas produced by the hydrolysis or acidolysis of a certain amount of alkylaluminoxane solution. The alkanes produced by the hydrolysis or acidolysis of other alkylaluminoxanes are easily miscible with organic solvents, and accurate determination is relatively difficult.

[0039] The mixed solution containing alkylaluminoxane is freed from volatile alkylaluminum and inert organic solvent to obtain solid alkylaluminoxane. The solid alkylaluminoxane is characterized by nuclear magnetic resonance spectroscopy. 1 H. 13 C and 27 The Al spectrum can detect the presence of alkyl groups and metallic aluminum, but it is not sufficient for accurate measurement.

[0040] Solid methylaluminoxane can be detected by UV-vis spectrum and compared with the spectrum reported in the literature to obtain qualitative information.

[0041] The specific method for calculating the conversion yield of alkylaluminum and water in an inert organic solvent to generate alkylaluminoxane is as follows: after the reaction is completed, the solid is collected to the maximum extent by filtration and weighed. Based on the premise that the molar ratio of water to alkylaluminum is not higher than 1:1, the generated solid should be aluminum oxide. Based on this, the reaction conversion yield can be calculated.

[0042] The determination of the content (mass percentage) of metallic aluminum in the mixed solution containing alkylaluminoxane can also be used to calculate the conversion yield of the reaction.

[0043] When the alkyl aluminum is trimethyl aluminum and triethyl aluminum, another measurement method is the methane or ethane gas metering method, that is, collecting the methane or ethane released by the metering reaction, and then balancing the conversion yield of the reaction. This method is applicable only if an inert organic solvent is used as the mobile phase carrying water. If gas is used as the mobile phase carrying water, it cannot be measured.

[0044] In some specific embodiments of the present invention, the method of the present invention specifically comprises the following steps:

[0045] S1, replacing the reactor with an inert gas, wherein the water and oxygen contents in the reactor are less than 1000 ppm, preferably less than 100 ppm after the replacement;

[0046] S2, weighing an alkyl aluminum and a first inert organic solvent to form a solution (reaction solution), injecting the solution into a reactor, and turning on a stirrer; the amount of the reaction solution in the reactor accounts for 1 / 10 to 9 / 10 of the reactor volume, preferably 1 / 2 to 2 / 3;

[0047] S3, setting the reactor to a certain temperature; the reaction temperature is controlled at -50 to 110°C, preferably at -20 to 90°C, and more preferably at -10 to 80°C;

[0048] S4, injecting water into the packing column, introducing the mobile phase, carrying the water in the packing into the solution formed by the alkyl aluminum and the first inert organic solvent in the reactor, and reacting under stirring;

[0049] S5, the alkane gas generated in the reaction is partially dissolved in the generated mixed solution containing alkylaluminoxane and partially released; when no gas is released, the reactor temperature is increased (increased by 50-70° C.) and the reaction is continued for a period of time until the reaction no longer generates gas, and the reaction is terminated;

[0050] S6, collecting the mixed solution containing the alkylaluminoxane under an inert atmosphere, and sealing and storing it for later use.

[0051] The method of the present invention can be used for: (1) preparing a single alkyl aluminoxane by controlled hydrolysis of a single alkyl aluminum; (2) preparing a mixed dialkyl aluminoxane by controlled hydrolysis of a mixture of two alkyl aluminums; (3) preparing a multi-mixed alkyl aluminoxane by controlled hydrolysis of a mixture of three or more alkyl aluminums; and (4) preparing a modified alkyl aluminoxane.

[0052] When the method of the present invention is used for the controlled hydrolysis of a single alkylaluminum to prepare a single alkylaluminoxane, the method specifically comprises the following steps:

[0053] (1) replacing the reactor with an inert gas so that the water, oxygen and other impurities in the reactor are kept at the lowest possible level; specifically, the water and oxygen content in the reactor after the replacement is less than 1000 ppm, preferably less than 100 ppm;

[0054] (2) weighing a certain amount of alkyl aluminum A and a certain amount of a first inert organic solvent to prepare a solution (reaction solution), injecting the solution into a reactor, and turning on a stirrer; the amount of the reaction solution in the reactor accounts for 1 / 10 to 9 / 10 of the reactor volume, preferably 1 / 2 to 2 / 3;

[0055] (3) setting the reactor to a certain temperature; the reaction temperature is controlled at -50 to 110°C, preferably at -20 to 90°C, and more preferably at -10 to 80°C;

[0056] (4) filling a packed column with a certain amount of column filler capable of carrying water, then injecting a certain amount of water, and then introducing a mobile phase inert to water, the column filler and the alkyl aluminum, carrying the water in the filler into the center formed by the alkyl aluminum and the first inert organic solvent in the reactor, and reacting under stirring;

[0057] (5) The alkane gas generated during the reaction partially dissolves in the generated mixed solution containing alkylaluminoxane and partially releases; when the reaction stops until no gas is released, the reactor temperature is increased (by 50 to 70° C.) and the reaction is continued for a period of time until no gas is generated during the reaction, and the reaction is terminated;

[0058] (6) Collect the mixed solution containing alkylaluminoxane under an inert atmosphere, seal it and store it for later use.

[0059] When the method of the present invention is used for preparing mixed dialkyl aluminoxane by controlled hydrolysis of two alkyl aluminum mixtures, the method specifically comprises the following steps:

[0060] (1) replacing the reactor with an inert gas so that the water, oxygen and other impurities in the reactor are kept at the lowest possible level; specifically, the water and oxygen content in the reactor after the replacement is less than 1000 ppm, preferably less than 100 ppm;

[0061] (2) weighing a certain amount of alkyl aluminum A, a certain amount of alkyl aluminum B and a certain amount of a first inert organic solvent to prepare a solution (reaction solution), injecting the solution into a reactor, and turning on a stirrer; the amount of the reaction solution in the reactor accounts for 1 / 10 to 9 / 10 of the volume of the reactor, preferably 1 / 2 to 2 / 3;

[0062] (3) setting the reactor to a certain temperature; the reaction temperature is controlled at -50 to 110°C, preferably at -20 to 90°C, and more preferably at -10 to 80°C;

[0063] (4) filling a packed column with a certain amount of column filler capable of carrying water, then injecting a certain amount of water, and then introducing a mobile phase inert to water, the column filler and the alkyl aluminum, carrying the water in the filler into the center formed by the alkyl aluminum and the first inert organic solvent in the reactor, and reacting under stirring;

[0064] (5) The alkane gas generated in the reaction partially dissolves in the generated mixed solution containing mixed dialkyl aluminoxane and partially releases; when the reaction stops until no gas is released, the reactor temperature is increased (increased by 50 to 70° C.) and the reaction is continued for a period of time until no gas is generated, and the reaction is terminated;

[0065] (6) Collect the mixed solution containing the mixed dialkylaluminoxane under an inert atmosphere, seal it and store it for later use.

[0066] The ratio of the amount of alkylaluminum A and B and the first inert organic solvent, and the concentration of A and B given thereby, depends on the optimal performance of the mixed alkylaluminoxane obtained in the co-catalysis or catalysis. The quantitative concentration of alkylaluminoxane is calibrated by the mass percentage of metallic aluminum, which is consistent with the method for preparing alkylaluminoxane from a single alkylaluminum, but the quantitative concentration cannot be used to calculate the reaction conversion rate or reaction yield.

[0067] The mixed solution containing mixed dialkyl aluminoxane is freed from volatile alkyl aluminum and organic solvent to obtain a solid mixed dialkyl aluminoxane. The solid mixed dialkyl aluminoxane is characterized by nuclear magnetic resonance spectroscopy. 1 H. 13 C and 27 The Al spectrum can detect the presence of alkyl groups and metallic aluminum, but it is not sufficient for accurate measurement.

[0068] The two mixed aluminum alkyls A and B are preferably selected from trimethylaluminum and triethylaluminum, trimethylaluminum and tri-n-propylaluminum, trimethylaluminum and tri-n-butylaluminum, trimethylaluminum and tri-isobutylaluminum, triethylaluminum and tri-n-propylaluminum, triethylaluminum and tri-n-butylaluminum, triethylaluminum and tri-isobutylaluminum, tri-n-propylaluminum and tri-n-butylaluminum, tri-n-propylaluminum and tri-isobutylaluminum, tri-n-propylaluminum and tri-isobutylaluminum.

[0069] The structural formula of the mixed dialkyl aluminoxane prepared by this method can be expressed as follows:

[0070] For mixed methyl ethyl aluminoxane: (MeAlO) m ·(EtAlO) n ·(AlMe3) o ·(AlEt3) p 、(Me2AlOAlMe2) m ·(Et2AlOAlEt2) n ·(AlMe3) o ·(AlEt3) p 、(MeAlO) m ·(Et2AlOAlEt2) n ·(AlMe3) o ·(AlEt3) p 、(EtAlO) m ·(Me2AlOAlMe2) n ·(AlMe3) o ·(AlEt3) p 、(MeAlO) m ·(Me2AlOAlMe2) n·(Et2AlOAlEt2) o ·(AlMe3) p ·(AlEt3) q 、(EtAlO) m ·(Me2AlOAlMe2) n ·(Et2AlOAlEt2) o ·(AlMe3) p ·(AlEt3) q 、(MeAlO) m ·(EtAlO) n ·(Me2AlOAlMe2) o ·(Et2AlOAlEt2) p ·(AlMe3) q ·(AlEt3) r 、(MeAlO) m ·(EtAlO) n 、(Me2AlOAlMe2) m ·(Et2AlOAlEt2) n 、(MeAlO) m ·(Et2AlOAlEt2) n 、(EtAlO) m ·(Me2AlOAlMe2) n 、(MeAlO) m ·(Me2AlOAlMe2) n ·(Et2AlOAlEt2) o 、(EtAlO) m ·(Me2AlOAlMe2) n ·(Et2AlOAlEt2) o 、(MeAlO) m ·(EtAlO) n ·(Me2AlOAlMe2) o ·(Et2AlOAlEt2) p ;

[0071] For methyl-n-propylaluminoxane, it is: (MeAlO) m ·(nPrAlO) n ·(AlMe3) o ·(AlnPr3) p 、(Me2AlOAlMe2) m ·(nPr2AlOAlnPr2) n ·(AlMe3) o ·(AlnPr3) p 、(MeAlO)m ·(nPr2AlOAlnPr2) n ·(AlMe3) o ·(AlnPr3) p 、(nPrAlO) m ·(Me2AlOAlMe2) n ·(AlMe3) o ·(AlnPr3) p 、(MeAlO) m ·(Me2AlOAlMe2) n ·(nPr2AlOAlnPr2) o ·(AlMe3) p ·(AlnPr3) q 、(nPrAlO) m ·(Me2AlOAlMe2) n ·(nPr2AlOAlnPr2) o ·(AlMe3) p ·(AlnPr3) q 、(MeAlO) m ·(nPrAlO) n ·(Me2AlOAlMe2) o ·(nPr2AlOAlnPr2) p ·(AlMe3) q ·(AlnPr3) r 、(MeAlO) m ·(nPrAlO) n 、(Me2AlOAlMe2) m ·(nPr2AlOAlnPr2) n 、(MeAlO) m ·(nPr2AlOAlnPr2) n 、(nPrAlO) m ·(Me2AlOAlMe2) n 、(MeAlO) m ·(Me2AlOAlMe2) n ·(nPr2AlOAlnPr2) o 、(nPrAlO) m ·(Me2AlOAlMe2) n ·(nPr2AlOAlnPr2) o 、(MeAlO) m ·(nPrAlO) n ·(Me2AlOAlMe2) o ·(nPr2AlOAlnPr2)p ;

[0072] For methyl-n-butylaluminoxane: (MeAlO) m ·(nBuAlO) n ·(AlMe3) o ·(AlnBu3) p , (Me2AlOAlMe2) m ·(nBu2AlOAlnBu2) n ·(AlMe3) o ·(AlnBu3) p , (MeAlO) m ·(nBu2AlOAlnBu2) n ·(AlMe3) o ·(AlnBu3) p , (nBuAlO) m ·(Me2AlOAlMe2) n ·(AlMe3) o ·(AlnBu3) p , (MeAlO) m ·(Me2AlOAlMe2) n ·(nBu2AlOAlnBu2) o ·(AlMe3) p ·(AlnBu3) q , (nBuAlO) m ·(Me2AlOAlMe2) n ·(nBu2AlOAlnBu2) o ·(AlMe3) p ·(AlnBu3) q , (MeAlO) m ·(nBuAlO) n ·(Me2AlOAlMe2) o ·(nBu2AlOAlnBu2) p ·(AlMe3) q ·(AlnBu3) r , (MeAlO) m ·(nBuAlO) n , (Me2AlOAlMe2) m ·(nBu2AlOAlnBu2) n , (MeAlO) m ·(nBu2AlOAlnBu2) n , (nBuAlO) m ·(Me2AlOAlMe2) n, (MeAlO) m ·(Me2AlOAlMe2) n ·(nBu2AlOAlnBu2) o , (nBuAlO) m ·(Me2AlOAlMe2) n ·(nBu2AlOAlnBu2) o , (MeAlO) m ·(nBuAlO) n ·(Me2AlOAlMe2) o ·(nBu2AlOAlnBu2) p ;

[0073] For the mixed methyl isobutyl aluminoxane: (MeAlO) m ·(iBuAlO) n ·(AlMe3) o ·(AliBu3) p , (Me2AlOAlMe2) m ·(iBu2AlOAliBu2) n ·(AlMe3) o ·(AliBu3) p , (MeAlO) m ·(iBu2AlOAliBu2) n ·(AlMe3) o ·(AliBu3) p , (iBuAlO) m ·(Me2AlOAlMe2) n ·(AlMe3) o ·(AliBu3) p , (MeAlO) m ·(Me2AlOAlMe2) n ·(iBu2AlOAliBu2) o ·(AlMe3) p ·(AliBu3) q , (iBuAlO) m ·(Me2AlOAlMe2) n ·(iBu2AlOAliBu2) o ·(AlMe3) p ·(AliBu3) q , (MeAlO) m ·(iBuAlO) n ·(Me2AlOAlMe2) o ·(iBu2AlOAliBu2) p·(AlMe3) q ·(AliBu3) r 、(MeAlO) m ·(iBuAlO) n 、(Me2AlOAlMe2) m ·(iBu2AlOAliBu2) n 、(MeAlO) m ·(iBu2AlOAliBu2) n 、(iBuAlO) m ·(Me2AlOAlMe2) n 、(MeAlO) m ·(Me2AlOAlMe2) n ·(iBu2AlOAliBu2) o 、(iBuAlO) m ·(Me2AlOAlMe2) n ·(iBu2AlOAliBu2) o 、(MeAlO) m ·(iBuAlO) n ·(Me2AlOAlMe2) o ·(iBu2AlOAliBu2) p ;

[0074] For the mixed ethyl n-propyl aluminoxane: (EtAlO) m ·(nPrAlO) n ·(AlEt3) o ·(AlnPr3) p 、(Et2AlOAlEt2) m ·(nPr2AlOAlnPr2) n ·(AlEt3) o ·(AlnPr3) p 、(EtAlO) m ·(nPr2AlOAlnPr2) n ·(AlEt3) o ·(AlnPr3) p 、(nPrAlO) m ·(Et2AlOAlEt2) n ·(AlEt3) o ·(AlnPr3) p 、(EtAlO) m ·(Et2AlOAlEt2) n ·(nPr2AlOAlnPr2) o ·(AlEt3) p·(AlnPr3) q 、(nPrAlO) m ·(Et2AlOAlEt2) n ·(nPr2AlOAlnPr2) o ·(AlEt3) p ·(AlnPr3) q 、(EtAlO) m ·(nPrAlO) n ·(Et2AlOAlEt2) o ·(nPr2AlOAlnPr2) p ·(AlEt3) q ·(AlnPr3) r 、(EtAlO) m ·(nPrAlO) n 、(Et2AlOAlEt2) m ·(nPr2AlOAlnPr2) n 、(EtAlO) m ·(nPr2AlOAlnPr2) n 、(nPrAlO) m ·(Et2AlOAlEt2) n 、(EtAlO) m ·(Et2AlOAlEt2) n ·(nPr2AlOAlnPr2) o 、(nPrAlO) m ·(Et2AlOAlEt2) n ·(nPr2AlOAlnPr2) o 、(EtAlO) m ·(nPrAlO) n ·(Et2AlOAlEt2) o ·(nPr2AlOAlnPr2) p ;

[0075] For the mixed ethyl-n-butyl aluminoxane: (EtAlO) m ·(nBuAlO) n ·(AlEt3) o ·(AlnBu3) p 、(Et2AlOAlEt2) m ·(nBu2AlOAlnBu2) n ·(AlEt3) o ·(AlnBu3) p 、(EtAlO) m ·(nBu2AlOAlnBu2)n ·(AlEt3) o ·(AlnBu3) p 、(nBuAlO) m ·(Et2AlOAlEt2) n ·(AlEt3) o ·(AlnBu3) p 、(EtAlO) m ·(Et2AlOAlEt2) n ·(nBu2AlOAlnBu2) o ·(AlEt3) p ·(AlnBu3) q 、(nBuAlO) m ·(Et2AlOAlEt2) n ·(nBu2AlOAlnBu2) o ·(AlEt3) p ·(AlnBu3) q 、(EtAlO) m ·(nBuAlO) n ·(Et2AlOAlEt2) o ·(nBu2AlOAlnBu2) p ·(AlEt3) q ·(AlnBu3) r 、(EtAlO) m ·(nBuAlO) n 、(Et2AlOAlMe2) m ·(nBu2AlOAlnBu2) n 、(EtAlO) m ·(nBu2AlOAlnBu2) n 、(nBuAlO) m ·(Et2AlOAlEt2) n 、(EtAlO) m ·(Et2AlOAlEt2) n ·(nBu2AlOAlnBu2) o 、(nBuAlO) m ·(Et2AlOAlEt2) n ·(nBu2AlOAlnBu2) o 、(EtAlO) m ·(nBuAlO) n ·(Et2AlOAlEt2) o ·(nBu2AlOAlnBu2) p ;

[0076] For the mixed ethyl isobutyl aluminoxane: (EtAlO) m ·(iBuAlO) n ·(AlEt3) o ·(AliBu3) p 、(Et2AlOAlEt2) m ·(iBu2AlOAliBu2) n ·(AlEt3) o ·(AliBu3) p 、(EtAlO) m ·(iBu2AlOAliBu2) n ·(AlEt3) o ·(AliBu3) p 、(iBuAlO) m ·(Et2AlOAlEt2) n ·(AlEt3) o ·(AliBu3) p 、(EtAlO) m ·(Et2AlOAlEt2) n ·(iBu2AlOAliBu2) o ·(AlEt3) p ·(AliBu3) q 、(iBuAlO) m ·(Et2AlOAlEt2) n ·(iBu2AlOAliBu2) o ·(AlEt3) p ·(AliBu3) q 、(EtAlO) m ·(iBuAlO) n ·(Et2AlOAlEt2) o ·(iBu2AlOAliBu2) p ·(AlEt3) q ·(AliBu3) r 、(EtAlO) m ·(iBuAlO) n 、(Et2AlOAlMe2) m ·(iBu2AlOAliBu2) n 、(EtAlO) m ·(iBu2AlOAliBu2) n 、(iBuAlO) m ·(Et2AlOAlEt2) n 、(EtAlO) m·(Et2AlOAlEt2) n ·(iBu2AlOAliBu2) o 、(iBuAlO) m ·(Et2AlOAlEt2) n ·(iBu2AlOAliBu2) o 、(EtAlO) m ·(iBuAlO) n ·(Et2AlOAlEt2) o ·(iBu2AlOAliBu2) p ;

[0077] For mixed n-propyl n-butyl aluminoxane: (nBuAlO) m ·(nPrAlO) n ·(AlnBu3) o ·(AlnPr3) p 、(nBu2AlOAlnBu2) m ·(nPr2AlOAlnPr2) n ·(AlnBu3) o ·(AlnPr3) p 、(nBuAlO) m ·(nPr2AlOAlnPr2) n ·(AlnBu3) o ·(AlnPr3) p 、(nPrAlO) m ·(nBu2AlOAlnBu2) n ·(AlnBu3) o ·(AlnPr3) p 、(nBuAlO) m ·(nBu2AlOAlnBu2) n ·(nPr2AlOAlnPr2) o ·(AlnBu3) p ·(AlnPr3) q 、(nPrAlO) m ·(nBu2AlOAlnBu2) n ·(nPr2AlOAlnPr2) o ·(AlnBu3) p ·(AlnPr3) q 、(nBuAlO) m ·(nPrAlO) n ·(nBu2AlOAlnBu2) o ·(nPr2AlOAlnPr2) p·(AlnBu3) q ·(AlnPr3) r 、(nBuAlO) m ·(nPrAlO) n 、(nBu2AlOAlnBu2) m ·(nPr2AlOAlnPr2) n 、(nBuAlO) m ·(nPr2AlOAlnPr2) n 、(nPrAlO) m ·(nBu2AlOAlnBu2) n 、(nBuAlO) m ·(nBu2AlOAlnBu2) n ·(nPr2AlOAlnPr2) o 、(nPrAlO) m ·(nBu2AlOAlnBu2) n ·(nPr2AlOAlnPr2) o 、(nBuAlO) m ·(nPrAlO) n ·(nBu2AlOAlnBu2) o ·(nPr2AlOAlnPr2) p ;

[0078] For mixed n-butyl isobutyl aluminoxane: (nBuAlO) m ·(iBuAlO) n ·(AlnBu3) o ·(AliBu3) p 、(nBu2AlOAlnBu2) m ·(iBu2AlOAliBu2) n ·(AlnBu3) o ·(AliBu3) p 、(nBuAlO) m ·(iBu2AlOAliBu2) n ·(AlnBu3) o ·(AliBu3) p 、(iBuAlO) m ·(nBu2AlOAlnBu2) n ·(AlnBu3) o ·(AliBu3) p 、(nBuAlO) m ·(nBu2AlOAlnBu2) n ·(iBu2AlOAliBu2)o ·(AlnBu3) p ·(AliBu3) q 、(iBuAlO) m ·(nBu2AlOAlnBu2) n ·(iBu2AlOAliBu2) o ·(AlnBu3) p ·(AliBu3) q 、(nBuAlO) m ·(iBuAlO) n ·(nBu2AlOAlnBu2) o ·(iBu2AlOAliBu2) p ·(AlnBu3) q ·(AliBu3) r 、(nBuAlO) m ·(iBuAlO) n 、(nBu2AlOAlnBu2) m ·(iBu2AlOAliBu2) n 、(nBuAlO) m ·(iBu2AlOAliBu2) n 、(iBuAlO) m ·(nBu2AlOAlnBu2) n 、(nBuAlO) m ·(nBu2AlOAlnBu2) n ·(iBu2AlOAliBu2) o 、(iBuAlO) m ·(nBu2AlOAlnBu2) n ·(iBu2AlOAliBu2) o 、(nBuAlO) m ·(iBuAlO) n ·(nBu2AlOAlnBu2) o ·(iBu2AlOAliBu2) p .

[0079] The method of the present invention is also applicable to a mixture of three or more alkyl aluminums. Obviously, the composition and structure of the obtained multi-mixed alkyl aluminoxane are more complex. The significance of the preparation of multi-mixed alkyl aluminoxane is still shown by the performance of its use as a co-catalyst or catalyzer. People in this field can all realize it.

[0080] The ratio of the amount of alkyl aluminum A, B, C (or the above components) and the first inert organic solvent, and the concentration of A, B, C (or the above components) given thereby, still depends on the optimal performance of the co-catalysis or catalysis achieved by the prepared multi-mixed alkyl aluminumoxane. Specifically, the following steps are included:

[0081] (1) replacing the reactor with an inert gas so that the water, oxygen and other impurities in the reactor are kept at the lowest possible level; specifically, the water and oxygen content in the reactor after the replacement is less than 1000 ppm, preferably less than 100 ppm;

[0082] (2) weighing a certain amount of alkyl aluminum A, a certain amount of alkyl aluminum B, a certain amount of C and a certain amount of a first inert organic solvent to prepare a solution (reaction solution), injecting the solution into a reactor, and turning on a stirrer; the amount of the reaction solution in the reactor accounts for 1 / 10 to 9 / 10 of the volume of the reactor, preferably 1 / 2 to 2 / 3;

[0083] (3) setting the reactor to a certain temperature; the reaction temperature is controlled at -50 to 110°C, preferably at -20 to 90°C, and more preferably at -10 to 80°C;

[0084] (4) filling a packed column with a certain amount of column filler capable of carrying water, then injecting a certain amount of water, and then introducing a mobile phase inert to water, the column filler and the alkyl aluminum, carrying the water in the filler into the center formed by the alkyl aluminum and the first inert organic solvent in the reactor, and reacting under stirring;

[0085] (5) The alkane gas generated in the reaction partially dissolves in the generated mixed solution containing multi-mixed alkyl aluminoxane and partially releases; when the reaction stops until no gas is released, the reactor temperature is increased (increased by 50-70° C.) and the reaction is continued for a period of time until no gas is generated, and the reaction is terminated;

[0086] (6) Collect the mixed solution containing the poly-mixed alkyl aluminoxane under an inert atmosphere, and seal it for storage.

[0087] The quantitative concentration of mixed alkyl aluminoxane using the mass percentage of metallic aluminum is consistent with the above-mentioned method of synthesizing alkyl aluminoxane from a single alkyl aluminum, but the quantitative concentration cannot be used to calculate the reaction conversion rate or reaction yield. The mixed solution containing mixed alkyl aluminoxane is removed of volatile alkyl aluminum and organic solvent to obtain a solid mixed alkyl aluminoxane. The NMR spectrum shows that 1 H. 13 C and 27 The Al spectrum can detect the presence of polyalkyl groups and metallic aluminum, but it is not sufficient for accurate measurement.

[0088] The three mixed alkyl aluminums A, B and C are preferably selected from trimethyl aluminum, triethyl aluminum and tri-n-propyl aluminum; trimethyl aluminum, triethyl aluminum and tri-n-butyl aluminum; trimethyl aluminum, triethyl aluminum and tri-isobutyl aluminum; trimethyl aluminum, tri-n-propyl aluminum and tri-n-butyl aluminum; trimethyl aluminum, tri-n-propyl aluminum and tri-isobutyl aluminum; triethyl aluminum, tri-n-propyl aluminum and tri-n-butyl aluminum; triethyl aluminum, tri-n-propyl aluminum and tri-isobutyl aluminum; tri-n-propyl aluminum, tri-n-butyl aluminum and tri-isobutyl aluminum. The structural formula of the multi-mixed alkyl aluminoxane is complex, as can be appreciated by those skilled in the art.

[0089] The modified alkyl aluminoxane can be prepared by using the method of the present invention to obtain a single alkyl aluminoxane, and further adding other alkyl aluminums to react with the synthesized single alkyl aluminoxane. Specifically, the modified alkyl aluminoxane comprises the following steps:

[0090] (1) replacing the reactor with an inert gas so that the water, oxygen and other impurities in the reactor are kept at the lowest possible level; specifically, the water and oxygen content in the reactor after the replacement is less than 1000 ppm, preferably less than 100 ppm;

[0091] (2) weighing a certain amount of alkyl aluminum A and a certain amount of a first inert organic solvent to form a solution (reaction solution), injecting the solution into a reactor, and turning on a stirrer; the amount of the reaction solution in the reactor accounts for 1 / 10 to 9 / 10 of the reactor volume, preferably 1 / 2 to 2 / 3;

[0092] (3) setting the reactor to a certain temperature; the reaction temperature is controlled at -50 to 110°C, preferably at -20 to 90°C, and more preferably at -10 to 80°C;

[0093] (4) filling a packed column with a certain amount of column filler capable of carrying water, then injecting a certain amount of water, and then introducing a mobile phase inert to water, the column filler and the alkyl aluminum, carrying the water in the filler into the center formed by the alkyl aluminum and the first inert organic solvent in the reactor, and reacting under stirring;

[0094] (5) The alkane gas generated in the reaction partially dissolves in the generated mixed solution containing multi-mixed alkyl aluminoxane and partially releases; when the reaction stops until no gas is released, the reactor temperature is increased (increased by 50-70° C.) and the reaction is continued for a period of time until no gas is generated, and the reaction is terminated;

[0095] (6) Weigh a certain amount of alkyl aluminum B, inject it into the reactor, and start the stirrer; set the reactor to a certain temperature (the reaction temperature is controlled at -50 to 110° C., preferably controlled at -20 to 90° C., and further preferably controlled at -10 to 80° C.), and stir for a certain time to obtain a mixed solution containing modified alkyl aluminumoxane;

[0096] (7) Collect the mixed solution containing the modified alkylaluminoxane under an inert atmosphere, seal it and store it for later use.

[0097] The ratio of the amounts of alkylaluminum A and the first inert organic solvent, and the concentration of A given thereby, as well as the amount of alkylaluminum B added, still depend on the optimal co-catalytic or catalytic performance achieved by the prepared modified alkylaluminoxane.

[0098] The quantitative concentration of the modified alkylaluminoxane is calibrated by the mass percentage of metallic aluminum, which is consistent with the above-mentioned method of synthesizing alkylaluminoxane from a single alkylaluminum. The quantitative concentration can also be used to calculate the reaction conversion rate or reaction yield, wherein the first step of controlled hydrolysis is the calculation control step, and the second step of the exchange reaction between the two aluminum alkyl groups can be regarded as a complete conversion reaction. The mixed solution containing the modified alkylaluminoxane is removed from the volatile alkylaluminum and the organic solvent to obtain a solid modified alkylaluminoxane. The nuclear magnetic resonance spectrum shows that the solid modified alkylaluminoxane is 1.14 wt. % and 1.3 wt. % respectively. 1 H. 13 C and 27 The Al spectrum can detect the presence of two alkyl groups and metallic aluminum, but it is not sufficient for accurate measurement.

[0099] The alkylaluminum A and B are preferably selected from trimethylaluminum and triethylaluminum, trimethylaluminum and tri-n-propylaluminum, trimethylaluminum and tri-n-butylaluminum, trimethylaluminum and tri-isobutylaluminum, triethylaluminum and tri-n-propylaluminum, triethylaluminum and tri-n-butylaluminum, triethylaluminum and tri-isobutylaluminum, tri-n-propylaluminum and tri-n-butylaluminum, tri-n-propylaluminum and tri-isobutylaluminum, tri-n-propylaluminum and tri-isobutylaluminum. The alkylaluminum A and B may be further preferably selected from trimethylaluminum and triethylaluminum, trimethylaluminum and tri-n-propylaluminum, trimethylaluminum and tri-n-butylaluminum, trimethylaluminum and tri-isobutylaluminum.

[0100] The structural formula of the prepared modified alkylaluminoxane is complex, which may be due to the continuous change in the ratio of the amounts of A and B. More importantly, when the groups in A and B change, the amount of group exchange during the exchange reaction is difficult to quantify.

[0101] For example, when alkyl aluminum A and B are preferably selected from trimethyl aluminum and triethyl aluminum, ethyl-modified methylaluminoxane is obtained, and the names of other modified aluminoxanes can be given by analogy, namely n-propyl-modified methylaluminoxane, n-butyl-modified methylaluminoxane, isobutyl-modified methylaluminoxane, methyl-modified ethylaluminoxane, n-propyl-modified ethylaluminoxane, n-butyl-modified ethylaluminoxane, isobutyl-modified ethylaluminoxane, methyl-modified n-propylaluminoxane, ethyl-modified n-propylaluminoxane, n-butyl-modified n-propylaluminoxane, isobutyl-modified n-propylaluminoxane, methyl-modified n-butylaluminoxane, ethyl-modified n-butylaluminoxane, n-propyl-modified n-butylaluminoxane, isobutyl-modified n-butylaluminoxane, methyl-modified isobutylaluminoxane, ethyl-modified isobutylaluminoxane, n-propyl-modified isobutylaluminoxane, and n-butyl-modified isobutylaluminoxane.

[0102] The second aspect of the present invention provides an apparatus for preparing alkylaluminoxane used in the method as described in the first aspect of the present invention, which comprises a reactor with a stirring device and a filling column connected to a first feed port at the top of the reactor.

[0103] In some embodiments of the present invention, a second feed port is further provided at the top of the reactor, and the second feed port is used to be connected to an inlet pipeline of a solution formed by alkyl aluminum and a first inert organic solvent;

[0104] The top of the reactor is also provided with a gas outlet for removing the gas generated during the reaction from the reactor.

[0105] In the present invention, the inlet pipeline of the solution formed by the alkyl aluminum and the first inert organic solvent can be further connected to a first micro-injection pump, and the first micro-injection pump is used to pump the solution formed by the alkyl aluminum and the first inert organic solvent into the reactor.

[0106] In addition, since a certain amount of reaction heat will be generated and gas products will overflow during the reaction process, alkyl aluminum, alkyl aluminoxane, inert organic solvents, especially low-boiling methane, ethane, propane and butane gas phases in the reaction system will inevitably be brought out, so it is necessary to configure a condenser and a collector at the gas outlet to collect the condensed alkyl aluminum or alkyl aluminum solution or alkyl aluminoxane solution or solvent brought out. The collected liquid can be returned to the reaction system through the second feed port for mixing and metering.

[0107] In some embodiments of the present invention, the bottom of the reactor is also provided with a discharge port for discharging the reaction product from the reactor.

[0108] In some other embodiments of the present invention, the reactor is further provided with an inert gas inlet, which is connected to an inert gas inlet pipeline for introducing an inert gas into the reactor to collect a mixed liquid containing alkylaluminoxane under an inert atmosphere.

[0109] In the present invention, the reactor may also be provided with a safety pressure relief port. In addition, other devices such as a pressure gauge or meter, a temperature gauge or meter, a thermostat controller of the reactor (note: a device for maintaining the reactor at a set temperature), a visual window, a random sampling port, etc. also need to be configured.

[0110] The reactor can allow the reaction temperature to be between -80 and 150°C and the pressure to be between 0 and 150 atm. The facilities and configurations equipped with the reactor also need to withstand the same temperature and pressure. The stirring device equipped with the reactor can ensure smooth stirring of the reaction materials, and a blade-type stirrer is preferred.

[0111] The shape and filling volume of the filling column of the present invention are determined by calculating the amount of synthesized alkylaluminoxane, and a cylinder of a certain length is preferred. The filling column can be placed horizontally, vertically, or at any angle between these two placement forms (i.e., within 0 to 90 degrees).

[0112] In the present invention, the filling volume of the packed column enables the water carrying capacity of the packed column to be in the range of 0.1 mL to 1000 mL.

[0113] In some embodiments of the present invention, a first interface and a second interface are provided on the top of the packed column; the first interface and the second interface are used to connect to a water (eg, pure water) inlet pipeline and a mobile phase inlet pipeline, respectively.

[0114] In the present invention, the mobile phase inlet pipeline includes two pipelines, namely, an inlet pipeline for a gaseous substance that does not react with water and alkyl aluminum and a second inert organic solvent inlet pipeline.

[0115] In some other embodiments of the present invention, a third interface may be further provided at the top of the filling column, and the third interface is used to be connected to the first pressure gauge.

[0116] In the present invention, the water inlet pipeline and the second inert organic solvent inlet pipeline can be further connected to the second micro-injection pump and the third micro-injection pump respectively, so as to pump the water and the second inert organic solvent into the packed column respectively.

[0117] In some embodiments of the present invention, an outlet is provided at the bottom of the packed column, and the outlet is connected to the first feed port of the reactor through a conduit. The conduit enables the aqueous mobile phase passing through the column packing to enter the solution formed by the alkyl aluminum and the first inert organic solvent homogeneously and evenly for reaction. It is particularly pointed out that if the conduit cannot or cannot well enable the aqueous mobile phase passing through the column packing to enter the solution formed by the alkyl aluminum and the first inert organic solvent homogeneously and evenly, it is necessary to consider equipping a certain configuration such as a static mixer or an atomizer to achieve the purpose of such functionalization.

[0118] Among alkyl aluminum compounds, trimethyl aluminum reacts most violently with water, with high heat release and high release of methane gas; triethyl aluminum is similar, with high heat release and high release of ethane gas. Other alkyl aluminum compounds also show high heat release, but the alkanes produced show gradually better solubility in the solution as the number of carbon atoms increases. The heat generated in the reaction system can be controlled by the thermostat of the reactor to adjust the reaction smoothly. Part of the generated alkane gas is dissolved in the generated mixed solution containing alkyl aluminoxane, part is released through the gas outlet of the reactor, and part will affect the effluent phase of the filling column. Therefore, for the effluent phase of the filling column, when it is a gas mobile phase, it is necessary to adjust the gas pressure of the filling column to be slightly greater than the pressure of the reaction system to prevent the effluent phase from being blocked; when it is a liquid mobile phase, a metering injection pump needs to be configured to also prevent the effluent phase from being blocked.

[0119] The alkylaluminoxane prepared in the first aspect of the present invention can be directly used for olefin polymerization or polymerization reaction, which relates to a technology of in-situ cutting-in of alkylaluminoxane into olefin polymerization or polymerization reaction. One is that the alkylaluminoxane solution collected under an inert atmosphere can be directly transferred to the olefin polymerization or polymerization reaction device for use after metering detection and packaging; the other is that after in-situ metering detection but without packaging, it is directly transferred to the olefin polymerization or polymerization reaction device for use, which method requires transportation through a pipeline.

[0120] For the production and in-situ use of alkylaluminoxane, it is necessary to prepare alkylaluminum raw materials with stable properties. This is easy to achieve. For the production and in-situ use of alkylaluminoxane, it is also necessary to perform real-time analysis of alkylaluminoxane. This is also easy to achieve.

[0121] The third aspect of the present invention provides a method for ethylene polymerization, which comprises: in a reactor, contacting ethylene with a solution containing a catalyst and a co-catalyst, and then polymerizing ethylene; the co-catalyst is an alkylaluminoxane prepared by the method described in the first aspect of the present invention, and the catalyst is a chromium-based catalyst.

[0122] In some specific embodiments of the present invention, the method for ethylene polymerization specifically includes: selecting a high-temperature pressure reactor, replacing the reactor with nitrogen, and connecting ethylene gas of a certain pressure. Under ethylene atmosphere, add a certain amount of organic solvent and a certain amount of co-catalyst alkylaluminoxane (prepared by the method described in the first aspect of the present invention). Raise to a certain temperature, stir for a certain time, and add a certain amount of catalyst solution. After the reaction reaches the set time, stop stirring, turn off the ethylene gas, and cool to about 5°C. After slowly unloading the pressure, pour the product after the reaction into an ethanol solution acidified with hydrochloric acid, and add water to separate the organic component product. After the liquid phase product is dried over anhydrous sodium sulfate, it is qualitatively and quantitatively analyzed by GC-FID. The solid product is collected by filtration, and vacuum dried to constant weight at a certain temperature, and the mass percentage is calculated separately.

[0123] A fourth aspect of the present invention provides a method for preparing polypropylene, comprising the following steps:

[0124] S1, mixing the calcined silica gel and the organic solution containing the alkylaluminoxane prepared by the method described in the first aspect of the present invention, and obtaining an alkylaluminoxane-silica gel solid after heating, filtering, washing and drying;

[0125] S2, mixing the alkylaluminoxane-silica gel solid with an organic solution containing a metallocene compound and reacting the mixture to obtain an alkylaluminoxane-silica gel supported metallocene catalyst;

[0126] S3, in the reactor, in the presence of an impurity remover, contacting propylene with the alkylaluminoxane-silica gel supported metallocene catalyst to carry out a polymerization reaction to obtain polypropylene.

[0127] In some embodiments of the present invention, in step S2, the structure of the metallocene compound is as shown in formula (1):

[0128]

[0129] Wherein, R is hydrogen or a C1-C5 alkyl group.

[0130] In some other embodiments of the present invention, the amount of the alkylaluminoxane-silica gel supported metallocene catalyst is 0.00001-100 mg / g propylene, and the amount of the impurity remover is 0-100 mmol / g propylene.

[0131] In the present invention, the polymerization reaction after the propylene contacts the alkylaluminoxane-silica gel supported metallocene catalyst can also be carried out in the presence of an impurity remover and hydrogen, and the amount of hydrogen used is 0 to 0.10 g / g propylene.

[0132] In some preferred embodiments of the present invention, the content of metallocene in the alkylaluminoxane-silica gel supported metallocene catalyst is 0.2-1.0 wt %.

[0133] In other preferred embodiments of the present invention, the impurity remover is an alkyl aluminum, preferably triisobutyl aluminum.

[0134] In some embodiments of the present invention, the organic solvent in the organic solution is selected from at least one of toluene, xylene and trimethylbenzene.

[0135] In other embodiments of the present invention, the polymerization reaction temperature is -40 to 200°C, and the time is 0.016 to 60 hours.

[0136] In the present invention, the isotacticity [mmmm] of the polypropylene prepared by the above method is greater than 90%, and can reach up to 99.7%.

[0137] In some specific embodiments of the present invention, the method for preparing polypropylene specifically comprises:

[0138] (1) Preparation of catalyst

[0139] A certain amount of silica gel calcined at a certain temperature is weighed, and a certain amount of the prepared mixed solution containing alkyl aluminoxane and the corresponding pure solvent is added, heated to a certain temperature, and stirred for a certain period of time, filtered, the solid is collected, and washed with a pure solvent, and the solid is vacuum dried to obtain a solid powder of alkyl aluminoxane-silica gel.

[0140] A certain amount of alkylaluminoxane-silica gel is weighed, a solvent is added to form a suspension, and an organic solution containing a metallocene compound is added to react while stirring. After the reaction is completed, the solid is collected by filtration, washed with a pure solvent until the washed solvent is colorless, and the solid is vacuum dried to obtain a solid powder, which is stored in a glove box for standby use. The metallocene content of the alkylaluminoxane-silica gel supported metallocene catalyst with a determined metallocene content can be obtained by measuring and calculating the amount of feed and the metallocene content of the washed liquid.

[0141] (2) Catalytic reaction

[0142] A high-temperature and high-pressure reactor is selected. After the reactor is completely replaced with nitrogen, a certain amount of propylene is introduced. In the propylene atmosphere, a certain amount of alkyl aluminum is added. The reaction is stirred for a certain period of time to remove impurities.

[0143] The pressurized catalyst device is dried and transferred into a glove box, and a recorded amount of alkylaluminoxane-silica gel-supported metallocene catalyst is added, and a small amount of solvent is added to mix well to form a slurry. The device is removed from the glove box and installed on a high-pressure reactor device to conduct polymerization experiments.

[0144] The polymerization experiment conditions are as follows: set a certain temperature, pressure and reaction time, add a measured amount of alkyl aluminum-silica gel supported metallocene catalyst in a slurry state into the reactor, and start the reaction.

[0145] After the reaction is completed, the unreacted propylene is recovered, and the residue is purged into the receiving bin with high-pressure N2, supplemented by another high-pressure steam purge, and then purged with air to obtain dry polypropylene, which is weighed, and the activity is calculated and spectrographically detected. (Unless otherwise specified, this reaction operation method is used in the following.) BRIEF DESCRIPTION OF THE DRAWINGS

[0146] The present invention will be further described below in conjunction with the accompanying drawings.

[0147] Figure 1 The device for preparing alkylaluminoxane used in the method described in the embodiment of the present invention; the meanings of the reference numerals in the accompanying drawings are as follows:

[0148] 1-inert gas inlet pipeline; 2-first micro-injection pump; 3-inlet pipeline of the solution formed by alkyl aluminum and the first inert organic solvent; 4-second micro-injection pump; 5-water (e.g., pure water) inlet pipeline; 6-filling column; 7-inlet pipeline of the gaseous substance that does not react with water and alkyl aluminum; 8-second inert organic solvent inlet pipeline; 9-third micro-injection pump; 10-first pressure gauge; 11-atomizer; 12-stirring device; 13-second pressure gauge; 14-condensed water inlet; 15-condensed water outlet; 16-reflux condenser; 17-collector; 18-venting pipeline; 19-reactor; 20-thermostatic controller; 21-discharge port; 22-first feed port; 23-second feed port; 24-inert gas inlet; 25-gas outlet; 26-first interface; 27-second interface.

[0149] Figure 2 Schematic diagram of the structure of the metallocene compound used in embodiments 29, 30 and 32 of the present invention.

[0150] Figure 3 Schematic diagram of the structure of the metallocene compound used in embodiment 31 of the present invention. DETAILED DESCRIPTION

[0151] In order to make the present invention easier to understand, the present invention will be further described in detail below in conjunction with examples, which are merely illustrative and are not intended to limit the scope of application of the present invention. The raw materials or components used in the present invention can be obtained by commercial routes or conventional methods unless otherwise specified.

[0152] The apparatus used in Examples 1-27 for preparing alkylaluminoxane is as follows: Figure 1The device comprises a reactor 19 with a stirring device 12, and a packing column 6 connected to a first feed port 22 at the top of the reactor 19;

[0153] The top of the reactor 19 is also provided with a second feed port 23, which is connected to the inlet pipeline 3 of the solution formed by the alkyl aluminum and the first inert organic solvent; the inlet pipeline 3 of the solution formed by the alkyl aluminum and the first inert organic solvent is further connected to the first micro-injection pump 2; the top of the reactor 19 is also provided with a gas outlet 25 for removing the gas generated during the reaction from the reactor, and a reflux condenser 16 and a collector 17 are arranged at the gas outlet 25, and the bottom and top of the reflux condenser 16 are respectively provided with a condensate inlet 14 and a condensate outlet 15, and the collector 17 is also provided with a venting pipeline 18; the bottom of the reactor 19 is also provided with a discharge port 21 for discharging the reaction product from the reactor; the reactor 19 is also provided with an inert gas inlet 24, and the inert gas inlet 24 is connected to the inert gas inlet pipeline 1; the reactor 19 can also be provided with a second pressure gauge 13 and a thermostat 20;

[0154] The top of the filling column 6 is provided with a first interface 26 and a second interface 27; the first interface 26 and the second interface 27 are respectively connected to a water (e.g., pure water) inlet pipeline 5 and a mobile phase inlet pipeline; the mobile phase inlet pipeline includes an inlet pipeline 7 for a gaseous substance that does not react with water and alkyl aluminum and a second inert organic solvent inlet pipeline 8; the water inlet pipeline 5 and the second inert organic solvent inlet pipeline 8 are further connected to a second micro-injection pump 4 and a third micro-injection pump 9, respectively; a third interface is also provided at the top of the filling column, and the third interface is connected to a first pressure gauge 10; an outlet is provided at the lower part of the filling column, and the outlet is connected to a first feed port 22 of the reactor through a conduit; an atomizer 11 is provided at the bottom of the conduit.

[0155] Example 1

[0156] The reactor was replaced with N2 atmosphere 5 times. Weigh 24g of trimethylaluminum, measure 100mL of toluene, prepare a solution (the content of trimethylaluminum in the solution is 21.7wt%), inject it into the reactor, turn on the stirring device, and set the reaction temperature to 0°C. Fill the column with 15-mesh silicon oxide porcelain powder, compact it, and inject pure water until the entire column is evenly wetted. Then pump pure water at a rate of 0.01mL / min through a metering injection pump, control the molar ratio of water to trimethylaluminum reaction to be 1:1, and open the N2 valve, adjust the flow rate to 15mL / min, and carry the water in the column packing into the alkyl aluminum solution in the reactor for reaction. The reaction lasts for 10h. The reaction temperature is further raised to 50°C and reacted for 10min. N2 and the methane gas produced in the reaction are vented through a -50°C condenser, and the condensed liquid is recovered into the reactor. After the reaction is completed, cool to room temperature, collect the solution of the product under an inert atmosphere, sample and analyze it, and then seal and store it for standby use.

[0157] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.2%, and the yield of methylaluminoxane was 87%.

[0158] Example 2

[0159] The reaction time at 0° C. in Example 1 was adjusted to 8 h. Finally, the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0160] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.0%, and the yield of methylaluminoxane was 92%.

[0161] Example 3

[0162] The reaction time at 0° C. in Example 1 was adjusted to 6 h. Finally, the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0163] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 7.7%, and the yield of methylaluminoxane was 87%.

[0164] Example 4

[0165] The reaction time at 0° C. in Example 1 was adjusted to 4 h. Finally, the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0166] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 7.7%, and the yield of methylaluminoxane was 87%.

[0167] Example 5

[0168] The reactor was replaced with N2 atmosphere 5 times. Weigh 30g of trimethylaluminum, measure 100mL of toluene, prepare a solution (the content of trimethylaluminum in the solution is 25.7wt%), inject it into the reactor, turn on the stirring device, and set the reaction temperature to 0°C. Fill the column with 15-mesh silicon oxide porcelain powder, compact it, and inject pure water until the entire column is evenly wetted. Then pump pure water at a rate of 0.01mL / min through a metering injection pump, control the molar ratio of water to trimethylaluminum reaction to be 1:2, and open the N2 valve, adjust the flow rate to 15mL / min, and carry the water in the column packing into the alkyl aluminum solution in the reactor for reaction. The reaction lasts for 10h. The reaction temperature is further raised to 50°C and reacted for 10min. N2 and the methane gas produced in the reaction are vented through a -50°C condenser, and the condensed liquid is recovered into the reactor. Cool to room temperature, collect the solution of the product under an inert atmosphere, sample and analyze, and then seal and store for standby use.

[0169] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 11.6%, and the yield of methylaluminoxane was 88%.

[0170] Example 6

[0171] The amount of trimethylaluminum in Example 5 was adjusted to 36 g, and the content of trimethylaluminum in the prepared solution was 29.4 wt %. Finally, the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0172] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 13.1%, and the yield of methylaluminoxane was 86%.

[0173] Example 7

[0174] The amount of trimethylaluminum in Example 5 was adjusted to 42 g, and the content of trimethylaluminum in the prepared solution was 32.7 wt %. Finally, the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0175] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 15.7%, and the yield of methylaluminoxane was 84%.

[0176] Example 8

[0177] The amount of trimethylaluminum in Example 5 was adjusted to 48 g, and the content of trimethylaluminum in the prepared solution was 35.7 wt %. Finally, the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0178] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 18.3%, and the yield of methylaluminoxane was 88%.

[0179] Example 9

[0180] The reactor was replaced with N2 atmosphere 5 times. Weigh 24g of trimethylaluminum, measure 20mL of toluene, prepare a solution, inject it into the reactor, turn on the stirring device, and set the reaction temperature to -20℃. Fill the column with 15-mesh silicon oxide porcelain powder, compact it, and inject pure water until the entire column is evenly wetted. Then pump pure water at a rate of 0.01mL / min through a metering injection pump to control the molar ratio of water to trimethylaluminum reaction to be 1:2. Then pump toluene at a rate of 0.20mL / min through another metering injection pump, and carry the water in the column packing into the alkyl aluminum solution in the reactor for reaction. The reaction lasts for 6h. The reaction temperature is further raised to 50℃ and reacted for 10min. The methane gas produced in the reaction is vented through a -50℃ condenser, and the condensed liquid is recovered into the reactor. Cool to room temperature, collect the solution of the product under an inert atmosphere, sample and analyze, and then seal and store for standby use.

[0181] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 9.3%, and the yield of methylaluminoxane was 92%.

[0182] Example 10

[0183] The reactor was replaced with N2 atmosphere 5 times. Weigh 24g of trimethylaluminum, measure 20mL of heptane, prepare a solution, inject it into the reactor, turn on the stirring device, and set the reaction temperature to -20℃. Fill the column with 15-mesh silicon oxide porcelain powder, compact it, and inject pure water until the entire column is evenly wetted. Then pump pure water at a rate of 0.01mL / min through a metering injection pump, and control the molar ratio of water to trimethylaluminum reaction to be 1:2. Then pump heptane at a rate of 0.20mL / min through another metering injection pump, and carry the water in the filler into the alkyl aluminum solution in the reactor for reaction. The reaction lasts for 6h. The reaction temperature is further raised to 50℃ and reacted for 10min. The methane gas produced in the reaction is vented through a -50℃ condenser, and the condensed liquid is recovered into the reactor. Cool to room temperature, collect the solution of the product under an inert atmosphere, sample and analyze, and then seal and store for standby use.

[0184] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.7%, and the yield of methylaluminoxane was 89%.

[0185] Embodiment 11

[0186] The reactor was replaced with N2 atmosphere 5 times. Weigh 24g of trimethylaluminum, measure 20mL of methylcyclohexane, prepare a solution, inject it into the reactor, turn on the stirring device, and set the reaction temperature to -20℃. Fill the column with 15-mesh silicon oxide porcelain powder, compact it, and inject pure water until the entire column is evenly wetted. Then pump pure water at a rate of 0.01mL / min through a metering injection pump to control the molar ratio of water to trimethylaluminum reaction to be 1:2. Methylcyclohexane is then pumped in at a rate of 0.20mL / min through another metering injection pump, and the water in the column packing is carried into the alkyl aluminum solution in the reactor for reaction. The reaction lasts for 6h. The reaction temperature is further raised to 50℃ and the reaction is carried out for 10min. The methane gas produced in the reaction is vented through a -50℃ condenser, and the condensed liquid is recovered into the reactor. Cool to room temperature, collect the solution of the product under an inert atmosphere, sample and analyze it, and then seal and store it for standby use.

[0187] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.5%, and the yield of methylaluminoxane was 86%.

[0188] Example 12

[0189] The reactor was replaced with N2 atmosphere 5 times. Weigh 24g of trimethylaluminum, measure 20mL of Isopar E, prepare a solution, inject it into the reactor, turn on the stirring device, and set the reaction temperature to -20℃. Fill the column with 15-mesh silicon oxide porcelain powder, compact it, and inject pure water until the entire column is evenly wetted. Then pump pure water at a rate of 0.01mL / min through a metering injection pump to control the reaction molar ratio of water to trimethylaluminum to be 1:2. Then pump Isopar E at a rate of 0.20mL / min through another metering injection pump, and carry the water in the column packing into the alkyl aluminum solution in the reactor for reaction. The reaction lasted 6h. The reaction temperature was further raised to 50℃ and reacted for 10min. The methane gas produced in the reaction was vented through a -50℃ condenser, and the condensed liquid was recovered into the reactor. Cool to room temperature, collect the solution of the product under an inert atmosphere, sample and analyze, and then seal and store for standby use.

[0190] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.6%, and the yield of methylaluminoxane was 87%.

[0191] Example 13

[0192] The reactor was replaced with N2 atmosphere 5 times. Weigh 24g of trimethylaluminum and 6g of triethylaluminum, measure 100mL of toluene, prepare a solution, inject it into the reactor, turn on the stirring device, and set the reaction temperature to 0°C. Fill the column with 15-mesh silicon oxide porcelain powder, compact it, and inject pure water until the entire column is evenly wetted. Then pump pure water at a rate of 0.01mL / min through a metering injection pump, control the reaction molar ratio of water to alkyl aluminum to 1:2, and open the N2 valve, adjust the flow rate to 15mL / min, and carry the water in the column packing into the alkyl aluminum solution in the reactor for reaction. The reaction lasted 10h. The reaction temperature was further raised to 50°C and reacted for 10min. N2 and the methane gas produced in the reaction were vented through a -50°C condenser, and the condensed liquid was recovered into the reactor. Cool to room temperature, collect the solution of the product under an inert atmosphere, sample and analyze, and then seal and store for standby use.

[0193] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylethylaluminoxane solution was 11.4%, and the yield of methylethylaluminoxane was 92%.

[0194] Embodiment 14

[0195] The reactor was replaced with N2 atmosphere 5 times. Weigh 24g of trimethylaluminum and 6g of triisobutylaluminum, measure 100mL of toluene, prepare a solution, inject it into the reactor, turn on the stirring device, and set the reaction temperature to 0°C. Fill the column with 15-mesh silicon oxide porcelain powder, compact it, and inject pure water until the entire column is evenly wetted. Then pump pure water at a rate of 0.01mL / min through a metering injection pump, control the reaction molar ratio of water to alkyl aluminum to 1:2, and open the N2 valve, adjust the flow rate to 15mL / min, and carry the water in the column packing into the alkyl aluminum solution in the reactor for reaction. The reaction lasted 10h. The reaction temperature was further raised to 50°C and reacted for 10min. N2 and the methane gas produced in the reaction were vented through a -50°C condenser, and the condensed liquid was recovered into the reactor. Cool to room temperature, collect the solution of the product under an inert atmosphere, sample and analyze, and then seal and store for standby use.

[0196] Through hydrolysis and titration analysis, the mass percentage of aluminum in the methyl isobutyl aluminoxane solution was 11.8%, and the yield of methyl isobutyl aluminoxane was 93%.

[0197] Embodiment 15

[0198] The reactor was replaced with N2 atmosphere 5 times. Weigh 24g of trimethylaluminum, 3g of triethylaluminum and 3g of triisobutylaluminum, measure 100mL of toluene, prepare a solution, inject it into the reactor, turn on the stirring device, and set the reaction temperature to 0°C. Fill the column with 15-mesh silicon oxide porcelain powder, compact it, and inject pure water until the entire column is evenly wetted. Then pump pure water at a rate of 0.01mL / min through a metering injection pump, control the reaction molar ratio of water to alkyl aluminum to 1:2, and open the N2 valve, adjust the flow rate to 15mL / min, and carry the water in the column packing into the alkyl aluminum solution in the reactor for reaction. The reaction lasted for 10h. The reaction temperature was further raised to 50°C and reacted for 10min. N2 and the methane gas produced in the reaction were vented through a -50°C condenser, and the condensed liquid was recovered into the reactor. Cool to room temperature, collect the solution of the product under an inert atmosphere, sample and analyze, and then seal and store for standby use.

[0199] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylethylisobutylaluminoxane solution was 11.6%, and the yield of methylethylisobutylaluminoxane was 90%.

[0200] Example 16

[0201] The reactor was replaced with N2 atmosphere 5 times. Weigh 24g of trimethylaluminum, measure 100mL of toluene, prepare a solution, inject it into the reactor, turn on the stirring device, and set the reaction temperature to 0°C. Fill the column with 15-mesh silicon oxide porcelain powder, compact it, and inject pure water until the entire column is evenly wetted. Then pump pure water into the column at a rate of 0.01mL / min through a metering injection pump, control the reaction molar ratio of water to trimethylaluminum to 1:2, open the N2 valve, adjust the flow rate to 15mL / min, and carry the water in the column packing into the alkyl aluminum solution in the reactor for reaction. The reaction lasts for 10h.

[0202] Add 6 g of triethylaluminum and stir to react for 1 h. Further raise the reaction temperature to 50°C and react for 10 min. N2 and methane gas produced in the reaction are vented through a -50°C condenser, and the condensed liquid is recovered into the reactor. Cool to room temperature, collect the product solution under an inert atmosphere, take samples for analysis, and then seal and store for later use.

[0203] Through hydrolysis and titration analysis, the mass percentage of aluminum in the ethyl-modified methylaluminoxane solution was 12.5%, and the yield of ethyl-modified methylaluminoxane was 90%.

[0204] Embodiment 17

[0205] The reactor was replaced with N2 atmosphere 5 times. Weigh 24g of trimethylaluminum, measure 100mL of toluene, prepare a solution, inject it into the reactor, turn on the stirring device, and set the reaction temperature to 0°C. Fill the column with 15-mesh silicon oxide porcelain powder, compact it, and inject pure water until the entire column is evenly wetted. Then pump pure water into the column at a rate of 0.01mL / min through a metering injection pump, control the reaction molar ratio of water to trimethylaluminum to 1:2, open the N2 valve, adjust the flow rate to 15mL / min, and carry the water in the column packing into the alkyl aluminum solution in the reactor for reaction. The reaction lasts for 10h.

[0206] Add 6 g of triisobutylaluminum and stir to react for 1 h. Further raise the reaction temperature to 50°C and react for 10 min. N2 and methane gas produced in the reaction are vented through a -50°C condenser, and the condensed liquid is recovered into the reactor. Cool to room temperature, collect the product solution under an inert atmosphere, take samples for analysis, and then seal and store for later use.

[0207] Through hydrolysis and titration analysis, the mass percentage of aluminum in the isobutyl-modified methylaluminoxane solution was 11.7%, and the yield of the isobutyl-modified methylaluminoxane was 87%.

[0208] Embodiment 18

[0209] The reactor was replaced with N2 atmosphere 5 times. Weigh 24g of trimethylaluminum, measure 100mL of toluene, prepare a solution, inject it into the reactor, turn on the agitator, and set the reaction temperature to 0℃. Fill the 15-mesh alumina porcelain powder into the column, compact it, and inject pure water until the entire column is evenly wetted. Then, pure water is pumped in at a rate of 0.01mL / min through a metering injection pump, and the reaction molar ratio of water to trimethylaluminum is controlled to be 1:2. The N2 valve is opened, and the flow rate is adjusted to 15mL / min, and the water in the column filler is carried into the alkyl aluminum solution in the reactor for reaction. The reaction lasts for 10h. The reaction temperature is further raised to 50℃ and the reaction is carried out for 10min. N2 and the methane gas produced in the reaction are vented through a -50℃ condenser, and the condensed liquid is recovered into the reactor. Cool to room temperature, collect the solution of the product under an inert atmosphere, take samples for analysis, and then seal and store for standby use.

[0210] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.3%, and the yield of methylaluminoxane was 88%.

[0211] Embodiment 19

[0212] The column packing in Example 18 was replaced with 15-mesh kaolin porcelain powder. Finally, the product solution was collected under an inert atmosphere, sampled for analysis, and then sealed and stored for later use.

[0213] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.4%, and the yield of methylaluminoxane was 90%.

[0214] Embodiment 20

[0215] The column packing in Example 18 was replaced with 15-mesh attapulgite porcelain powder. Finally, the product solution was collected under an inert atmosphere, sampled for analysis, and then sealed and stored for later use.

[0216] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.4%, and the yield of methylaluminoxane was 90%.

[0217] Embodiment 21

[0218] The column packing in Example 18 was replaced with a particulate polyethylene resin, and finally the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0219] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.7% and the yield of methylaluminoxane was 91%.

[0220] Embodiment 22

[0221] The column packing in Example 18 was replaced with particulate polypropylene resin, and finally the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0222] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.6%, and the yield of methylaluminoxane was 90%.

[0223] Embodiment 23

[0224] The column packing in Example 18 was replaced with particulate polystyrene resin, and finally the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0225] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.6%, and the yield of methylaluminoxane was 90%.

[0226] Embodiment 24

[0227] The column packing in Example 18 was replaced with particulate polymethyl methacrylate resin, and finally the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0228] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.5%, and the yield of methylaluminoxane was 90%.

[0229] Embodiment 25

[0230] The column packing in Example 18 was replaced with particulate polyvinyl chloride resin, and finally the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0231] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.4%, and the yield of methylaluminoxane was 86%.

[0232] Embodiment 26

[0233] The column packing in Example 18 was replaced with a particulate polycarbonate resin, and finally the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0234] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.5%, and the yield of methylaluminoxane was 88%.

[0235] Embodiment 27

[0236] The column packing in Example 18 was replaced with particulate polyetheretherketone resin, and finally the product solution was collected under an inert atmosphere, sampled and analyzed, and then sealed and stored for later use.

[0237] The hydrolysis and titration analysis showed that the mass percentage of aluminum in the methylaluminoxane solution was 8.5%, and the yield of methylaluminoxane was 88%.

[0238] Embodiment 28

[0239] A fresh toluene solution of a chromium catalyst with a concentration of 1 mmol / L was prepared in the glove box, and 10 mL of the toluene solution of the chromium catalyst was measured and set aside. The reactor was installed, preheated to 100°C, vacuum dried and cooled to room temperature, replaced with an ethylene atmosphere, and 50 mL of toluene, 10 mL of the toluene solution of the chromium catalyst, and 1 mL of MAO toluene solution (toluene solution with a specification of 10% wt) were added, and the mixture was rapidly heated to 60°C. At the same time, the ethylene pressure was increased to 3 MPa, and the stirring rate was 800 rpm, which was maintained for 60 min. The reaction system was then rapidly cooled to 0°C, the pressure was released, the gas was collected with a gas collector, the solid polymer was collected by filtration and dried and weighed, and the mass percentage was calculated separately. The liquid was quenched by adding 10 mL of anhydrous ethanol and 1 mL of 10% hydrochloric acid, shaken, allowed to stand, and 5 g of n-heptane internal standard was added for gas phase analysis. The catalyst activity was calculated by gas chromatography analysis to be 7.4×10 6 g / mol Cr·h, of which the selectivity of C6 is 32.3wt%, the selectivity of C8 is 66.1wt%, and the selectivity of C 10+ The selectivity is 1.6wt% and the polymer content is 0.38wt%.

[0240] Embodiment 29

[0241] 1. Preparation of catalyst

[0242] Weigh 2 g of silica gel calcined at 600°C, add 10 mL of MAO (methylaluminoxane) toluene solution (10% wt toluene solution) and 20 mL of pure toluene solvent, heat to 80°C, stir for 24 hours, filter, collect the solid, and wash it 3 times with toluene solvent. Vacuum dry the solid for 24 hours to obtain solid powdered MAO-silica gel.

[0243] Weigh a certain amount of MAO-silica gel, add toluene solvent to form a suspension, add the toluene solution of the metallocene zirconium compound while stirring evenly, and react overnight. Filter and collect the solid, wash with toluene solvent until the washed solvent is colorless, and vacuum dry the solid for 24 hours to obtain a solid powdered metallocene catalyst, which is stored in a glove box for later use. The catalyst with a determined zirconium content can be obtained by measuring and calculating the amount of feed and the zirconium content of the washed liquid.

[0244] Selection Figure 2 The metallocene zirconium compound shown was used, and the Al / Zr ratio was controlled to be 200:1 to prepare catalyst SC-1, in which the zirconium content was 0.268 wt% (29.4 μmol / g).

[0245] 2. Catalytic reaction

[0246] A 300 mL high-pressure reactor was selected, vacuumed in an oil bath at 100°C, and replaced with nitrogen three times before use.

[0247] The pressurized catalyst adding device is dried and transferred into the glove box, and the measured catalyst is added, and a small amount of solvent is added to mix well. The glove box is removed and installed on the high-pressure reactor device to carry out the polymerization experiment.

[0248] 200 mg of SC-1 catalyst was selected, no impurity remover was used, the reaction time was 180 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, and the amount of propylene pressed in was 50 g.

[0249] Finally, 23.5 g of polymer was obtained, and the calculated activity was 2.35×10 6 g(PP)·mol -1 (Zr)·h -1 .

[0250] Embodiment 30

[0251] 1. Preparation of catalyst

[0252] Weigh 2 g of silica gel calcined at 600°C, add 10 mL of MAO toluene solution (10% wt toluene solution) and 20 mL of pure toluene solvent, heat to 80°C, stir for 24 hours, filter, collect the solid, and wash it 3 times with toluene solvent. Vacuum dry the solid for 24 hours to obtain solid powdered MAO-silica gel.

[0253] Weigh a certain amount of MAO-silica gel, add toluene solvent to form a suspension, add the toluene solution of the metallocene zirconium compound while stirring evenly, and react overnight. Filter and collect the solid, wash with toluene solvent until the washed solvent is colorless, and vacuum dry the solid for 24 hours to obtain a solid powdered metallocene catalyst, which is stored in a glove box for later use. The catalyst with a determined zirconium content can be obtained by measuring and calculating the amount of feed and the zirconium content of the washed liquid.

[0254] Selection Figure 2 The metallocene zirconium compound shown in the figure controls the Al / Zr ratio to be 50:1, 100:1, and 200:1, respectively, to prepare catalysts SC-2A (zirconium content is 0.846wt%, 100.2μmol / g), SC-2B (zirconium content is 0.430wt%, 47.2μmol / g), and SC-2C (zirconium content is 0.268wt%, 29.4μmol / g), respectively.

[0255] 2. Catalytic reaction

[0256] A 2000 mL high pressure reactor was selected, vacuumed in an oil bath at 100°C, and replaced with nitrogen three times before use.

[0257] Operation 1

[0258] 105 mg of SC-2A catalyst and 8 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 500:1) were selected. The reaction time was 180 minutes, the reaction temperature was 75° C., the propylene pressure was >3.9 MPa, and the propylene amount was 523 g.

[0259] Finally, 92 g of polymer was obtained, and the calculated polymerization activity was 4.00 × 10 7 g(PP)·mol -1 (Zr)·h -1 The Mn, Mw and PDI values ​​measured by high temperature gel permeation chromatography (GPC) were 131324, 325745 and 2.48, respectively. 13 The isotacticity measured by C NMR spectrum is [mmmm] 99.4%. The melting point test value is 151.33℃. (Note: The analysis of PP is selective.)

[0260] Operation 2

[0261] 105 mg of SC-2B catalyst and 3.2 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 200:1) were selected. The reaction time was 180 minutes, the reaction temperature was 75° C., the propylene pressure was >3.9 MPa, and the propylene amount was 526 g.

[0262] Finally, 64 g of polymer was obtained, and the calculated polymerization activity was 2.78×10 7 g(PP)·mol -1 (Zr)·h -1 .

[0263] Operation Three

[0264] 106 mg of SC-3C catalyst and 3.2 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 200:1) were selected. The reaction time was 180 minutes, the reaction temperature was 75° C., the propylene pressure was >3.9 MPa, and the propylene amount was 519 g.

[0265] Finally, 57 g of polymer was obtained, and the calculated polymerization activity was 2.45×10 7 g(PP)·mol -1 (Zr)·h -1 .

[0266] Embodiment 31

[0267] 1. Preparation of catalyst

[0268] The preparation steps are basically the same as those in Example 29, except that Figure 3 The metallocene compounds shown in the figure have an Al / Zr ratio of 193:1, 227:1, and 340:1, respectively, to prepare catalysts SC-3A (zirconium content of 0.40wt%, 28.4μmol / g), SC-3B (zirconium content of 0.30wt%, 25.0μmol / g), and SC-3C (zirconium content of 0.20wt%, 16.7μmol / g), respectively.

[0269] 2. Catalytic reaction

[0270] A 2000 mL high pressure reactor was selected, vacuumed in an oil bath at 100°C, and replaced with nitrogen three times before use.

[0271] Operation 1

[0272] 105 mg of SC-3A catalyst and 8 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 500:1) were selected. The reaction time was 180 minutes, the reaction temperature was 75° C., the propylene pressure was >3.9 MPa, and the propylene amount was 522 g.

[0273] Finally, 80 g of polymer was obtained, and the calculated polymerization activity was 3.48×107 g(PP)·mol -1 (Zr)·h -1 The Mn, Mw and PDI values ​​measured by high temperature GPC are 133064, 313745 and 2.36 respectively. 13 The isotacticity measured by C NMR spectrum is [mmmm] 99.3%. The melting point is 149.43°C.

[0274] Operation 2

[0275] 105 mg of SC-3B catalyst and 3.2 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 200:1) were selected. The reaction time was 180 minutes, the reaction temperature was 75° C., the propylene pressure was >3.9 MPa, and the propylene amount was 516 g.

[0276] Finally, 52 g of polymer was obtained, and the calculated polymerization activity was 2.26×10 7 g(PP)·mol -1 (Zr)·h -1 .

[0277] Operation Three

[0278] 106 mg of SC-3C catalyst and 3.2 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 200:1) were selected. The reaction time was 180 minutes, the reaction temperature was 75° C., the propylene pressure was >3.9 MPa, and the propylene amount was 518 g.

[0279] Finally, 43 g of polymer was obtained, and the calculated polymerization activity was 1.85×10 7 g(PP)·mol -1 (Zr)·h -1 .

[0280] Embodiment 32

[0281] 1. Preparation of catalyst

[0282] The preparation steps are basically the same as those in Example 29, except that Figure 2 The metallocene compounds shown in the figure have an Al / Zr ratio of 193:1, 194:1, and 195:1, respectively, to prepare catalysts SC-4A (zirconium content: 0.40wt%, 28.4μmol / g), SC-4B (zirconium content: 0.40wt%, 28.5μmol / g), and SC-4C (zirconium content: 0.40wt%, 28.7μmol / g), respectively.

[0283] 2. Catalytic reaction

[0284] A 2000 mL high pressure reactor was selected, vacuumed in an oil bath at 100°C, and replaced with nitrogen three times before use.

[0285] Operation 1

[0286] 98 mg of SC-4A catalyst and 15 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 549:1) were selected. The reaction time was 240 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, and the propylene amount was 528.7 g.

[0287] Finally, 450 g of polymer was obtained, and the calculated polymerization activity was 1.098×10 8 g(PP)·mol -1 (Zr)·h -1 The Mn, Mw and PDI values ​​measured by high temperature GPC are 162913, 377577 and 2.317 respectively. 13 The isotacticity measured by C NMR spectrum is [mmmm] 99.6%. The melting point is 151.4°C.

[0288] Operation 2

[0289] 60 mg of SC-4A catalyst and 15 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 896:1) were selected. The reaction time was 330 minutes, the reaction temperature was 75° C., the propylene pressure was >3.9 MPa, and the propylene amount was 518 g.

[0290] Finally, 860 g of polymer was obtained, and the calculated polymerization activity was 1.772×10 8 g(PP)·mol -1 (Zr)·h -1 The Mn, Mw and PDI values ​​measured by high temperature GPC are 104205, 226218 and 2.17 respectively. 13 The isotacticity measured by C NMR spectrum is [mmmm] 98.4%. The melting point test value is 152.2 / 161.4℃.

[0291] Operation Three

[0292] 60 mg of SC-4A catalyst, 3 mL of triethylaluminum (concentration of 100 μmol / mL, aluminum-zirconium ratio of about 1195:1) were selected, the reaction time was 180 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 538 g, and the hydrogen amount was 0.02 g.

[0293] Finally, 80 g of polymer was obtained, and the calculated polymerization activity was 3.186×10 7 g(PP)·mol -1 (Zr)·h -1 .

[0294] Operation Four

[0295] 35 mg of SC-4A catalyst, 2.5 mL of triethylaluminum (concentration of 100 μmol / mL, aluminum-zirconium ratio of about 1707:1) were selected, the reaction time was 180 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 512 g, and the hydrogen amount was 0.02 g.

[0296] Finally, 35 g of polymer was obtained, and the calculated polymerization activity was 2.389×10 7 g(PP)·mol -1 (Zr)·h -1 .

[0297] Operation Five

[0298] 65 mg of SC-4A catalyst, 20 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1792:1) were selected, the reaction time was 270 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 659 g, and the hydrogen amount was 0.026 g.

[0299] Finally, 600 g of polymer was obtained, and the calculated polymerization activity was 2.206×10 8 g(PP)·mol -1 (Zr)·h -1 The Mn, Mw and PDI values ​​measured by high temperature GPC are 80551, 188015 and 2.33 respectively. 13 The isotacticity measured by C NMR spectrum is [mmmm] 99.7%. The melting point test value is 151.83 / 152.2℃.

[0300] Operation Six

[0301] 40 mg of SC-4A catalyst, 20 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1707:1) were selected, the reaction time was 180 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 628.6 g, and the hydrogen amount was 1.365 g.

[0302] Finally, 270 g of polymer was obtained, and the calculated polymerization activity was 1.613×10 8 g(PP)·mol -1 (Zr)·h -1 .

[0303] Operation seven

[0304] 30 mg of SC-4A catalyst, 20 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 2389:1) were selected, the reaction time was 360 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 658.8 g, and the hydrogen amount was 0.052 g.

[0305] Finally, 390 g of polymer was obtained, and the calculated polymerization activity was 3.106×10 8 g(PP)·mol -1 (Zr)·h -1 The Mn, Mw and PDI values ​​measured by high temperature GPC were 47736, 146937 and 3.08, respectively.

[0306] Operation eight

[0307] 30 mg of SC-4A catalyst, 20 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 2389:1) were selected, the reaction time was 180 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 357.2 g, and the hydrogen amount was 0.06 g.

[0308] Finally, 205 g of polymer was obtained, and the calculated polymerization activity was 1.633×10 8 g(PP)·mol -1 (Zr)·h -1 The melting point test value is 154.03℃.

[0309] Operation Nine

[0310] 30 mg of SC-4A catalyst, 10 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1195:1) were selected, the reaction time was 420 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 682 g, and the hydrogen amount was 0.06 g.

[0311] Finally, 540 g of polymer was obtained, and the calculated polymerization activity was 4.301×10 8 g(PP)·mol -1 (Zr)·h -1 .

[0312] Operation 10

[0313] 20 mg of SC-4A catalyst, 3.5 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 627:1) were selected, the reaction time was 180 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 657 g, and the hydrogen amount was 0.06 g.

[0314] Finally, 10 g of polymer was obtained, and the calculated polymerization activity was 1.195×107 g(PP)·mol -1 (Zr)·h -1 .

[0315] Operation Eleven

[0316] 20 mg of SC-4A catalyst, 7 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1254:1) were selected, the reaction time was 180 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 651 g, and the hydrogen amount was 0.06 g.

[0317] Finally, 45 g of polymer was obtained, and the calculated polymerization activity was 5.376×10 7 g(PP)·mol -1 (Zr)·h -1 .

[0318] Operation 12

[0319] 20 mg of SC-4A catalyst, 10 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1792:1) were selected, the reaction time was 180 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 654 g, and the hydrogen amount was 0.06 g.

[0320] Finally, 82 g of polymer was obtained, and the calculated polymerization activity was 9.797×10 7 g(PP)·mol -1 (Zr)·h -1 .

[0321] Operation Thirteen

[0322] 20 mg of SC-4A catalyst, 10 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1792:1) were selected, the reaction time was 180 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 652 g, and the hydrogen amount was 0.06 g.

[0323] Finally, 92 g of polymer was obtained, and the calculated polymerization activity was 1.099×10 8 g(PP)·mol -1 (Zr)·h -1 .

[0324] Operation 14

[0325] 30 mg of SC-4A catalyst, 10 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1195:1) were selected, the reaction time was 420 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 670 g, and the hydrogen amount was 0.06 g.

[0326] Finally, 530 g of polymer was obtained, and the calculated polymerization activity was 4.221×10 8 g(PP)·mol -1 (Zr)·h -1 .

[0327] Operation 15

[0328] 30 mg of SC-4B catalyst, 10 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1195:1) were selected, the reaction time was 480 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 684 g, and the hydrogen amount was 0.06 g.

[0329] Finally, 610 g of polymer was obtained, and the calculated polymerization activity was 4.859×10 8 g(PP)·mol -1 (Zr)·h -1 .

[0330] Operation 16

[0331] 30 mg of SC-4B catalyst, 10 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1195:1) were selected, the reaction time was 240 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 687.5 g, and the hydrogen amount was 0.06 g.

[0332] Finally, 533 g of polymer was obtained, and the calculated polymerization activity was 4.245×10 8 g(PP)·mol -1 (Zr)·h -1 The melting point test value is 155.46℃.

[0333] Operation 17

[0334] 30 mg of SC-4B catalyst, 10 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1195:1) were selected, the reaction time was 240 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 688.6 g, and the hydrogen amount was 0.06 g.

[0335] Finally, 405 g of polymer was obtained, and the calculated polymerization activity was 3.226×10 8 g(PP)·mol -1 (Zr)·h -1 .

[0336] Operation 18

[0337] 30 mg of SC-4C catalyst, 10 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1195:1) were selected, the reaction time was 180 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 680 g, and the hydrogen amount was 0.06 g.

[0338] Finally, 530 g of polymer was obtained, and the calculated polymerization activity was 4.221×10 8 g(PP)·mol -1 (Zr)·h -1 .

[0339] Operation 19

[0340] 20 mg of SC-4C catalyst, 10 mL of triisobutylaluminum (concentration of 150 μmol / mL, aluminum-zirconium ratio of about 1792:1) were selected, the reaction time was 180 minutes, the reaction temperature was 75°C, the propylene pressure was >3.9 MPa, the propylene amount was 681 g, and the hydrogen amount was 0.06 g.

[0341] Finally, 145 g of polymer was obtained, and the calculated polymerization activity was 1.732×10 8 g(PP)·mol -1 (Zr)·h -1 .

[0342] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. A method for preparing an alkylaluminoxane for in-situ olefin oligomerization and polymerization, wherein include: The method comprises the following steps: using a packed column to meter water, and injecting the water into a solution formed by alkyl aluminum and a first inert organic solvent under the drive of a mobile phase to react, obtaining a mixed solution containing alkyl aluminoxane, and metering and detecting the alkyl aluminoxane in the mixed solution; the mobile phase is selected from a second inert organic solvent or a gaseous substance that does not react with water and alkyl aluminum; the molar ratio of water to alkyl aluminum is not higher than 1:1, The water loading capacity of the packed column is 0.1 mL to 1000 mL; The column filler in the packed column is selected from inorganic substances that do not react with water or form gel with water or organic high molecular polymers that do not react with water or form gel with water; The inorganic substance is selected from at least one of silicon oxide, aluminum oxide, molecular sieve, kaolin, attapulgite, ceramics, metal oxide ceramics and glass fibers; The organic high molecular polymer is selected from at least one of polyethylene, polypropylene, polyvinyl chloride, polytetrafluoroethylene, polystyrene, polyisobutylene, polyisoprene, ethylene-propylene rubber resin, polymethyl methacrylate, polyethyl methacrylate, polypropyl methacrylate, polybutyl methacrylate, polymethyl acrylate, polyethyl acrylate, polypropyl acrylate, polybutyl acrylate, polyacrylamide, polycarbonate, polysulfone and polyetheretherketone; The alkyl aluminum is selected from at least one of trimethyl aluminum, triethyl aluminum, tri-n-propyl aluminum, tri-n-butyl aluminum, tri-isobutyl aluminum and tri-n-octylaluminum; The first inert organic solvent is selected from any one of toluene, xylene, trimethylbenzene, n-pentane, isopentane, neopentane, cyclopentane, methylcyclopentane, n-hexane, n-heptane, cyclohexane, methylcyclohexane, petroleum ether, isoheptane, neoheptane, Isopar E and Isopar F.

2. The method according to claim 1, It is characterized in that The second inert organic solvent is selected from any one of straight-chain hydrocarbons, branched-chain hydrocarbons, cyclic saturated hydrocarbons and aromatic hydrocarbons.

3. The method according to claim 2, It is characterized in that The second inert organic solvent is selected from any one of toluene, xylene, trimethylbenzene, n-pentane, isopentane, neopentane, cyclopentane, methylcyclopentane, n-hexane, n-heptane, cyclohexane, methylcyclohexane, petroleum ether, isoheptane, neoheptane, Isopar E and Isopar F.

4. The method according to claim 3, It is characterized in that The second inert organic solvent is the same as the first inert organic solvent.

5. The method according to claim 1, It is characterized in that The gaseous substance is selected from any one of nitrogen, argon and methane.

6. The method according to claim 1, It is characterized in that The molar ratio of water to alkyl aluminum is 1:(1-10).

7. The method according to claim 6, It is characterized in that The molar ratio of water to alkyl aluminum is 1:(1-5).

8. The method according to claim 1, It is characterized in that The content of alkyl aluminum in the solution is 0.4-80 wt %.

9. The method according to claim 8, It is characterized in that The content of metallic aluminum in the mixed solution containing alkylaluminoxane is 0.1 to 40.0 wt %; wherein, when the mobile phase is a gaseous substance, the content of metallic aluminum in the mixed solution containing alkylaluminoxane is controlled by adjusting the amount of the first inert organic solvent; when the mobile phase is a second inert organic solvent, the content of metallic aluminum in the mixed solution containing alkylaluminoxane is controlled by adjusting the sum of the amounts of the first inert organic solvent and the second inert organic solvent.

10. The method according to claim 1, It is characterized in that The reaction temperature is -50 to 110° C., and the reaction time is 4 to 15 hours.

11. The method according to claim 10, It is characterized in that The reaction temperature is -20 to 90°C, and the reaction time is 8 to 12 hours.

12. The method according to claim 11, It is characterized in that The reaction temperature is -10 to 80°C.

13. The method according to claim 1, It is characterized in that The content of alkylaluminoxane in the mixed solution is measured by detecting the content of metal aluminum in the mixed solution.

14. An apparatus for preparing alkylaluminoxane used in the method according to any one of claims 1 to 13, comprising a reactor with a stirring device, and a packed column connected to a first feed port at the top of the reactor.

15. The device according to claim 14, It is characterized in that The top of the reactor is also provided with a second feed port, which is used to be connected to an inlet pipeline of a solution formed by alkyl aluminum and a first inert organic solvent; The top of the reactor is also provided with a gas outlet for removing the gas generated during the reaction from the reactor.

16. The device according to claim 15, It is characterized in that The gas outlet is provided with a condenser and a collector.

17. The device according to claim 14 or 15, It is characterized in that The bottom of the reactor is also provided with a discharge port for discharging the reaction product out of the reactor.

18. The device according to claim 14, It is characterized in that The top of the packing column is provided with a first interface and a second interface; the first interface and the second interface are used to be connected to a water inlet pipeline and a mobile phase inlet pipeline respectively.

19. The device according to claim 14, It is characterized in that The lower part of the packing column is provided with an outlet, and the outlet is connected to the first feed inlet of the reactor through a conduit.

20. A method for the polymerization of ethylene, wherein include: In the reactor, ethylene is contacted with a solution containing a catalyst and a co-catalyst to carry out ethylene oligomerization; The co-catalyst is an alkylaluminoxane prepared by the method as described in any one of claims 1 to 13; and the catalyst is a chromium-based catalyst.

21. A method for preparing polypropylene, wherein The following steps are involved: S1, mixing the calcined silica gel and an organic solution containing the alkylaluminoxane prepared by the method according to any one of claims 1 to 13, and obtaining an alkylaluminoxane-silica gel solid after heating, filtering, washing and drying; S2, mixing the alkylaluminoxane-silica gel solid with an organic solution containing a metallocene compound and reacting the mixture to obtain an alkylaluminoxane-silica gel supported metallocene catalyst; S3, in the reactor, in the presence of an impurity remover, contacting propylene with the alkylaluminoxane-silica gel supported metallocene catalyst to carry out a polymerization reaction to obtain polypropylene.

22. The method according to claim 21, It is characterized in that In step S2, the structure of the metallocene compound is shown in formula (1): Where R is hydrogen or C 1 ~C 5 of alkyl.

23. The method according to claim 21, It is characterized in that The amount of the alkylaluminoxane-silica gel supported metallocene catalyst is 0.00001-100 mg / g propylene, and the amount of the impurity remover is 0-100 mmol / g propylene.

24. The method according to claim 23, It is characterized in that The content of metallocene in the alkylaluminoxane-silica gel supported metallocene catalyst is 0.2-1.0 wt %.

25. The method according to claim 21, It is characterized in that The impurity remover is alkyl aluminum.

26. The method according to claim 25, It is characterized in that The impurity remover is triisobutylaluminum.

27. The method according to claim 21, It is characterized in that The organic solvent in the organic solution is selected from at least one of toluene, xylene and trimethylbenzene; and / or The polymerization reaction temperature is -40 to 200° C., and the reaction time is 0.016 to 60 hours.