High-performance acrylic emulsion for textile printing overlay and preparation method thereof, and printing overlay coating

By using high-performance acrylic emulsion formula in textile printed cover applications, the problem of insufficient water resistance and adhesion resistance of acrylic emulsion is solved, and efficient bonding and adhesion performance is improved, suitable for mass production, and comply with environmental protection standards.

CN116082559BActive Publication Date: 2024-11-01GUANGDONG YINYANG ENVIRONMENT FRIENDLY NEW MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211674213.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-11-01
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

The existing acrylic emulsions have poor water resistance and adhesion resistance in textile printed cover applications, which limit their use and promotion on the market.

Method used

Adopt high-performance acrylic emulsion formula, including deionized water, ethyl acrylate, butyl acrylate, polymerizable vinyl silane, acrylonitrile, special monomers of Roatian wet adhesion, functional monomers, self-crosslinking monomers, emulsification The agent and initiator are introduced into Rhodium wet adhesion special monomers and functional monomers through copolymerization of silicone and vinyl, thereby improving the structure and bonding properties of the colloids and increasing the degree of crosslinking to improve the resistance to adhesion.

Benefits of technology

It significantly improves the bonding and adhesion performance of the textile printed cover, realizes rapid penetration and displays the bottom pattern after encountering water, has good water resistance, avoids the problems of multi-bubble and soft paint film of traditional paint, and is suitable for large-scale continuous production. Environmentally friendly, compliant with European and American environmental protection standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116082559B_ABST
    Figure CN116082559B_ABST
Patent Text Reader

Abstract

The invention discloses a high-performance acrylic emulsion for textile printing overlay and a preparation method thereof, and a printing mask coating, wherein the high-performance acrylic emulsion comprises by weight: 90-110 parts of deionized water, 9-10 parts of ethyl acrylate, 20-40 parts of butyl acrylate, 0.5-0.8 parts of polymerizable vinyl silane, 4-6 parts of acrylic acid, 4-7 parts of acrylonitrile, 0.6-1 parts of Rhodia wet adhesion special monomer, 3.4-6.0 parts of functional monomer, 0.5-1 parts of self-crosslinking monomer, 0.8-1.2 parts of emulsifier and 0.1-0.3 parts of initiator. After the high-performance acrylic emulsion of the present invention is formulated into a water-transparent bottom overlay coating, it has excellent anti-adhesion effect, does not turn white when covering when encountering water, and has fast permeability, can quickly show bottom patterns when encountering water, has soft hand feel, good water resistance, excellent elasticity, and comprehensive performance that is completely comparable to that of polyurethane emulsion, and has very wide market demand and economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile printing coatings, and in particular to a high-performance acrylic emulsion for textile printing overlays and a preparation method thereof, and a printing overlay coating. Background Art

[0002] In recent years, the clothing printing industry has developed rapidly. As a new printing process, overlay printing fits the current personalized, fashionable and rapidly changing consumption trends, and adapts to the transformation from the traditional business model to the new business model of "small batch, personalized, and quick response". It is an important system of technology, fashion, and green in the printing industry, and has become the fastest growing field in the printing industry in recent years. At the same time, overlay printing directly improves the appearance and texture of printed fabrics due to its excellent application performance, thereby improving the layering and added value of the product, and is highly loved by consumers and respected by the market.

[0003] At present, the main types of overlay printing are matte effect overlay, glossy effect overlay, and water-visible bottom effect overlay. Polyurethane resin basically occupies the entire overlay printing coating resin market due to its outstanding comprehensive material properties. Even though acrylic resin has obvious price advantages over polyurethane resin, and acrylic emulsion is easier to produce and adjust than polyurethane emulsion, it has not been able to meet the corresponding requirements in terms of water resistance, anti-adhesion and other overlay coating application properties, thus limiting its use and promotion. The current textile market competition is becoming increasingly fierce. How to improve the competitiveness of enterprises, the continuous pursuit of product quality and performance, and cost control are urgent issues faced by enterprises in every industry.

[0004] Therefore, the innovative development of a high-performance acrylic emulsion suitable for use in printed overlays is the current development trend and direction of the printing industry, which has broad market demand and economic benefits. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a high-performance acrylic emulsion for textile printing topcoat and a preparation method thereof, and a printing topcoat coating, aiming to solve the problem of poor water resistance and anti-blocking properties of the existing acrylic emulsion.

[0006] The technical solution of the present invention is as follows:

[0007] A high-performance acrylic emulsion for textile printing cover, wherein the high-performance acrylic emulsion comprises, by weight: 90-110 parts of deionized water, 9-10 parts of ethyl acrylate, 20-40 parts of butyl acrylate, 0.5-0.8 parts of polymerizable vinyl silane, 4-6 parts of acrylic acid, 4-7 parts of acrylonitrile, 0.6-1 parts of Rhodia wet adhesion special monomer, 3.4-6.0 parts of functional monomer, 0.5-1 parts of self-crosslinking monomer, 0.8-1.2 parts of emulsifier and 0.1-0.3 parts of initiator.

[0008] The high-performance acrylic emulsion for textile printing cover, wherein the functional monomer is one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, glycidyl acrylate and glycidyl methacrylate.

[0009] In the high-performance acrylic emulsion for textile printing overlay, the self-crosslinking monomer is one or two of diacetone acrylamide and acetoacetoxyethyl methacrylate.

[0010] The high-performance acrylic emulsion for textile printing cover, wherein the emulsifier is one or both of double-bond-containing allyl alkyl succinate sulfonic acid sodium salt and allyl-containing special alcohol ether sulfate.

[0011] In the high-performance acrylic emulsion for textile printing overlay, the polymerizable vinyl silane is one or more of vinyl triethoxy silane, vinyl tri(β-methoxyethoxy) silane and vinyl trimethoxy silane.

[0012] In the high-performance acrylic emulsion for textile printing overlay, the initiator is one or more of ammonium persulfate, sodium persulfate and potassium persulfate.

[0013] A method for preparing a high-performance acrylic emulsion for textile printing overlay, comprising the steps of:

[0014] Preparation of primer A: Add 45-82 parts of deionized water and 0.2-0.3 parts of emulsifier into the polymerization kettle, and heat the polymerization kettle until the temperature reaches 68-72° C. to prepare primer A;

[0015] Preparation of pre-emulsion B: add 20-40 parts of butyl acrylate, 9-10 parts of ethyl acrylate, 0.5-0.8 parts of polymerizable vinyl silane, 4-6 parts of acrylic acid, 4-7 parts of acrylonitrile, 3.4-6.0 parts of functional monomer, 0.5-1 part of self-crosslinking monomer, 0.8-1.2 parts of emulsifier, and 18-25 parts of deionized water into a pre-emulsification tank at room temperature and pressure, and stir to mix into a uniform pre-emulsion B for later use;

[0016] Preparation of initiator solution C: add 0.1-0.3 parts of initiator and 10-20 parts of deionized water into an initiator tank at room temperature and pressure to prepare a uniform initiator C solution;

[0017] When the temperature in the polymerization kettle reaches 68-72°C, add 2%-5% of the total amount of pre-emulsion B and 20%-30% of the total amount of initiator solution C into the polymerization kettle. After 5-10 minutes, add the remaining pre-emulsion B and the remaining initiator solution C dropwise into the polymerization kettle. The total dropping time is controlled within 150-180 minutes.

[0018] When the pre-emulsion B has been added dropwise for 120-150 minutes, 0.6-1.0 parts of Rhodia wet adhesion special monomer are added. After the addition is completed, the temperature in the polymerization kettle is controlled at 72-78°C and kept warm for 0.5-2 hours;

[0019] When the temperature in the polymerization kettle drops to below 50°C, add a defoamer and a mildew and fungicide into the reactor, stir and filter the material to obtain a high-performance acrylic emulsion for textile printing cover.

[0020] A printing finish coating comprises the high-performance acrylic emulsion for textile printing finish of the present invention.

[0021] Beneficial effects: The textile printing overlay high-performance acrylic emulsion of the present invention is copolymerized with silicone, vinyl and acrylic ester to chemically bond silicone and polyacrylate, thereby strengthening the bonding strength of the overlay resin layer to the bottom layer; the textile printing overlay high-performance acrylic emulsion of the present invention is prepared by introducing Rhodia's special wet adhesion monomer, which, as a functional modified monomer, can not only provide hydrogen bonds and intermolecular forces, but also improve the particle structure of the emulsion polymer when added to the emulsion polymerization system, and can quickly reduce the interfacial tension, so that the overprint coating layer can quickly penetrate into the bottom layer after encountering water, so as to achieve the effect of becoming transparent when encountering water and showing the bottom image The effect of the scheme is achieved, avoiding the traditional practice of adding a large amount of penetrant in the paint production, which causes problems such as multiple bubbles, soft paint film and whitening when exposed to water. It can more effectively wet the pigment and filler particles and the surface of the adhered matrix, thereby significantly improving the bonding and adhesion properties of the topcoat, and balancing the disadvantages of the latex film on water molecules brought by the reactive emulsifier itself. The whole emulsion system can maintain sufficient hydrophilicity and low surface energy to enable the topcoat to quickly penetrate water, and at the same time have sufficient water resistance to keep the topcoat from turning white when wetted by water after water penetration, and can show the bottom pattern, and can withstand multiple washings without stratification. The textile printing overlay high-performance acrylic emulsion of the present invention is also introduced into the functional monomers during preparation, so as to improve the wetting property of the emulsion and make it easier to spread on the bottom layer after the emulsion is formed into a film, and the wettability is good, the interface contact area is large, and the adhesion is effectively improved. The polar groups attached to these functional monomers can form intermolecular forces with the polar groups of the overlay bottom layer, and can also effectively improve the adhesion between the layers; and at the same time, the introduction of the self-crosslinking monomer and the sufficient crosslinking degree enhance the dryness of the paint film after film formation, so that the overlay layer has excellent anti-adhesion performance. The textile printing overlay high-performance acrylic emulsion of the present invention has outstanding comprehensive performance of the water-transparent bottom overlay slurry prepared, and can completely replace the polyurethane emulsion, and the production process is simple, the reaction is stable and controllable, the energy consumption is lower, the cost performance is high, and it is very suitable for large-scale continuous production; at the same time, it is environmentally friendly, does not contain APEO, formaldehyde, heavy metals, solvents, etc., and meets the relevant environmental protection standards of Europe and the United States. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a flow chart of a preferred embodiment of a method for preparing a high-performance acrylic emulsion for textile printing cover. DETAILED DESCRIPTION

[0023] The present invention provides a high-performance acrylic emulsion for textile printing finish and a preparation method thereof, and a printing finish coating. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0024] The invention provides a high-performance acrylic emulsion for textile printing overlay, wherein the high-performance acrylic emulsion comprises, by weight, 90-110 parts of deionized water, 9-10 parts of ethyl acrylate, 20-40 parts of butyl acrylate, 0.5-0.8 parts of polymerizable vinyl silane, 4-6 parts of acrylic acid, 4-7 parts of acrylonitrile, 0.6-1 parts of Rhodia wet adhesion special monomer, 3.4-6.0 parts of functional monomer, 0.5-1 parts of self-crosslinking monomer, 0.8-1.2 parts of emulsifier and 0.1-0.3 parts of initiator.

[0025] In the present invention, the ethyl acrylate and butyl acrylate are used as soft monomers to provide the film-forming property and softness of the acrylic resin; acrylic acid can provide carboxyl groups to the polymer, and the carboxyl groups can provide cross-linking groups and can improve the reaction stability and hydrophilicity of the emulsion; acrylonitrile is used as a hard monomer to improve the adhesion and anti-blocking property of the acrylic resin; the introduction of the Rhodia wet adhesion special monomer as a functional modified monomer can significantly improve the bonding property and adhesion between the top layer and the bottom layer of the overlay.

[0026] Specifically, the high-performance acrylic emulsion of the present invention is copolymerized with silicone, vinyl and acrylic ester to chemically bond silicone and polyacrylate, thereby strengthening the bonding strength of the top resin layer to the bottom layer; the high-performance acrylic emulsion of textile printing top layer of the present invention is introduced into the preparation of Rhodia (SIPOMER WAME) is a special monomer for wet adhesion. As a functional modified monomer, its special molecular structure can not only provide hydrogen bonds and intermolecular forces, but also improve the particle structure of the emulsion polymer when added to the emulsion polymerization system, which can quickly reduce the interfacial tension, so that the overprint coating layer can quickly penetrate into the bottom layer after encountering water, so as to achieve the effect of becoming transparent when encountering water and showing the bottom pattern, avoiding the traditional practice of adding a large amount of penetrant in the production of coatings, resulting in multiple bubbles, soft paint film and whitening when encountering water, and more effectively wetting the pigment and filler particles and the surface of the adhered matrix, thereby significantly improving the bonding and adhesion properties of the topcoat, balancing the disadvantages of the latex film brought by the reactive emulsifier itself that the adsorption and penetration of water molecules are weakened, so that the entire emulsion system can maintain sufficient hydrophilicity and low surface energy to enable the topcoat to quickly penetrate when encountering water, and at the same time have sufficient water resistance to keep the topcoat from turning white when wetting with water after encountering water penetration, and can show the bottom pattern, and can withstand multiple washings without stratification. Functional monomers are also introduced during the preparation of the textile printing overlay high-performance acrylic emulsion of the present invention, so as to improve the wetting performance of the emulsion and make it easier for the emulsion to spread on the bottom layer after film formation, thereby achieving good wettability and a large interface contact area, and effectively improving the adhesion. In addition, the polar groups attached to these functional monomers can form intermolecular forces with the polar groups of the overlay bottom layer, and can also effectively improve the adhesion between the layers. Meanwhile, the introduction of self-crosslinking monomers and sufficient crosslinking degree enhance the dryness of the paint film after film formation, so that the overlay layer has excellent anti-adhesion performance.

[0027] In this embodiment, the Rhodia wet adhesion special monomer is SIPOMER WAME wet adhesion special monomer, and the main component of SIPOMER WAME is a heterocyclic methacrylate compound. The special molecular structure of SIPOMER WAME product can not only provide hydrogen bonds and intermolecular forces, but also improve the colloid structure of the emulsion polymerization system when it is added to the emulsion polymerization system, reduce the interfacial tension, and more effectively infiltrate the pigment and filler particles and the surface of the adhered matrix, thereby significantly improving the bonding and adhesion performance of the water-based coating.

[0028] In some embodiments, the functional monomer is one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, glycidyl acrylate and glycidyl methacrylate, but is not limited thereto. In this embodiment, the functional monomer provides an appropriate cross-linking group, and the polar group attached to the functional monomer can associate with the polar group of the overprinting bottom layer to form an intermolecular force to improve fastness and adhesion.

[0029] In some embodiments, the self-crosslinking monomer is one or both of diacetone acrylamide and acetoacetoxyethyl methacrylate, but is not limited thereto. In this embodiment, the self-crosslinking monomer significantly improves the water resistance and anti-blocking properties of the emulsion through crosslinking.

[0030] In some embodiments, the emulsifier is one or both of sodium salt of allyl alkyl succinate sulfonate containing double bonds and special alcohol ether sulfate containing allyl groups. In this embodiment, the emulsifier is composed of a reactive emulsifier, which has high reactivity and is connected to the polymer surface through chemical bonds. Therefore, the emulsifier molecules will not migrate to the surface of the paint film, thereby forming a non-chemically bonded emulsifier layer on the surface of the paint film, which will absorb water and swell when in contact with water, causing whitening and reduced water resistance.

[0031] In some embodiments, the polymerizable vinyl silane is one or more of vinyl triethoxysilane, vinyl tri(β-methoxyethoxy)silane and vinyl trimethoxysilane, but is not limited thereto. In this embodiment, the polymerizable vinyl silane can introduce Si-O-Si bonds into the polymer main chain. Since the silicon-oxygen bonds can rotate freely, the forces between polymer molecules can be reduced, so that the sliding properties between polymer molecules are enhanced and the hand feel is soft.

[0032] In some embodiments, the initiator is one or more of ammonium persulfate, sodium persulfate and potassium persulfate, but is not limited thereto. In this embodiment, persulfate is selected as the initiator because its reaction rate is relatively slow, the reaction is easy to control, it is highly safe and cheap.

[0033] In some embodiments, a method for preparing a high-performance acrylic emulsion for a textile printing overlay is also provided, comprising the steps of:

[0034] S10, preparation of primer A: add 45-82 parts of deionized water and 0.2-0.3 parts of emulsifier into the polymerization kettle, and heat the polymerization kettle until the temperature inside reaches 68-72° C. to prepare primer A;

[0035] S20, preparation of pre-emulsion B: add 20-40 parts of butyl acrylate, 9-10 parts of ethyl acrylate, 0.5-0.8 parts of polymerizable vinyl silane, 4-6 parts of acrylic acid, 4-7 parts of acrylonitrile, 3.4-6.0 parts of functional monomer, 0.5-1 part of self-crosslinking monomer, 0.8-1.2 parts of emulsifier, and 18-25 parts of deionized water into a pre-emulsification tank at room temperature and pressure, and stir and mix to form a uniform pre-emulsion B for standby use;

[0036] S30, preparation of initiator solution C: adding 0.1-0.3 parts of initiator and 10-20 parts of deionized water into an initiator tank at normal temperature and pressure to prepare a uniform initiator C solution;

[0037] S40, when the temperature in the polymerization kettle reaches 68-72°C, add 2%-5% of the total amount of pre-emulsion B and 20%-30% of the total amount of initiator solution C into the polymerization kettle, and after 5-10 minutes, dropwise add the remaining pre-emulsion B and the remaining initiator solution C into the polymerization kettle, and the total dropping time is controlled within 150-180 minutes;

[0038] S50, when the pre-emulsion B has been added dropwise for 120-150 minutes, 0.6-1.0 parts of Rhodia wet adhesion special monomer are added, and after the addition is completed, the temperature in the polymerization kettle is controlled at 72-78° C. and kept warm for 0.5-2 hours;

[0039] S60, when the temperature in the polymerization kettle drops to below 50°C, add a defoamer and a mildew-proofing and bactericide into the reactor, stir, filter and discharge the material, and obtain a high-performance acrylic emulsion for textile printing cover.

[0040] The preparation method of the high-performance acrylic emulsion provided by the present invention has simple process, stable and controllable reaction, lower energy consumption, high cost performance, and is very suitable for large-scale continuous production. At the same time, it is environmentally friendly, does not contain APEO, formaldehyde, heavy metals, solvents, etc., and meets relevant environmental protection standards in Europe and the United States.

[0041] In some embodiments, a printing topcoat is also provided, which includes the high-performance acrylic emulsion for textile printing topcoat of the present invention. In this embodiment, the prepared high-performance acrylic emulsion has a dense film and a transparent appearance. The water-transparent bottom printing topcoat prepared by the high-performance acrylic emulsion has excellent anti-adhesion effect, high hiding rate, no whitening when exposed to water, fast permeability, can quickly show the bottom pattern when exposed to water, has a soft feel, good water resistance, and excellent elasticity.

[0042] The present invention will be further explained below by means of specific embodiments:

[0043] Example 1

[0044] A high-performance acrylic emulsion for textile printing cover, the raw material composition of which includes the following components in parts by weight: 100 parts of deionized water; 30 parts of butyl acrylate; 9 parts of ethyl acrylate; 0.6 parts of polymerizable vinyl silane; 4 parts of acrylic acid; 4 parts of acrylonitrile; 0.6 parts of SIPOMER WAME, a special monomer for wet adhesion, 3.6 parts of functional monomers; 1 part of self-crosslinking monomer emulsifier; 0.8 parts of emulsifier; and 0.2 parts of initiator.

[0045] Furthermore, the functional monomer is hydroxyethyl acrylate.

[0046] Furthermore, the emulsifier is a sodium salt of allyl alkyl succinate sulfonate containing a double bond.

[0047] Furthermore, the polymerizable vinyl silane is vinyl triethoxy silane.

[0048] Furthermore, the self-crosslinking monomer is diacetone acrylamide.

[0049] Furthermore, the initiator is sodium persulfate.

[0050] The above textile printing overlay high-performance acrylic emulsion comprises the following steps:

[0051] a. Preparation of the reaction tank primer A: Add 60 parts of deionized water and 0.2 parts of emulsifier to a polymerization reactor with a stirrer, a condenser and a feeding device, and heat the reactor to a temperature of 68°C;

[0052] b. Preparation of pre-emulsion B: Add 30 parts of butyl acrylate, 9 parts of ethyl acrylate, 0.6 parts of polymerizable vinyl silane, 4 parts of acrylic acid, 4 parts of acrylonitrile, 3.6 parts of functional monomer, 1 part of self-crosslinking monomer, 0.6 parts of emulsifier, and 20 parts of deionized water to a pre-emulsion tank with a monomer metering tank and a stirrer at room temperature and pressure, stir and mix into a uniform pre-emulsion, and stir for 30 minutes for standby use;

[0053] c. Preparation of initiator solution C: 0.2 parts of initiator and 20 parts of deionized water were added to an initiator tank with a stirrer and a constant flow dropping device at room temperature and pressure to prepare a uniform initiator solution;

[0054] d. When the temperature in the polymerization kettle reaches 68°C, 2% of the total amount of pre-emulsion B and 30% of the total amount of initiator solution C are added to the kettle. After 5 minutes, the remaining pre-emulsion B and 70% of the initiator solution C are simultaneously added dropwise to the polymerization kettle through a constant flow pump feeding device and a constant flow dripping metering device. The total dripping time is controlled at 180 minutes;

[0055] e. When the pre-emulsion is added dropwise to 120 minutes, add 0.6 parts of SIPOMER WAME, a special monomer for wet adhesion, and continue to add dropwise after stirring for 5 minutes;

[0056] f. After the addition is completed, the temperature in the polymerization reactor is controlled at 75°C for 1 hour;

[0057] g. Cool down to below 50°C, add defoamer and mildew-proof fungicide to the reactor, stir for 20 minutes, filter the material, and you can get a high-performance acrylic emulsion for textile printing cover.

[0058] Example 2

[0059] A textile printing cover high-performance acrylic emulsion, the raw material composition of which includes the following components by weight: 100 parts of deionized water; 40 parts of butyl acrylate; 10 parts of ethyl acrylate; 0.5 parts of polymerizable vinyl silane; 5 parts of acrylic acid; 7 parts of acrylonitrile; 0.8 parts of SIPOMER WAME, a special monomer for wet adhesion, 5 parts of functional monomers; 1 part of self-crosslinking monomer emulsifier; 1 part of emulsifier; 0.2 parts of initiator.

[0060] Furthermore, the functional monomer is glycidyl methacrylate.

[0061] Furthermore, the emulsifier is a sodium salt of allyl alkyl succinate sulfonate containing a double bond.

[0062] Furthermore, the vinyltrimethoxysilane.

[0063] Furthermore, the self-crosslinking monomer is diacetone acrylamide.

[0064] Furthermore, the initiator is ammonium persulfate.

[0065] The above textile printing overlay high-performance acrylic emulsion comprises the following steps:

[0066] a. Preparation of reaction tank primer A: Add 60 parts of deionized water and 0.3 parts of emulsifier to a polymerization reactor with a stirrer, a condenser and a feeding device, and heat the reactor to a temperature of 70°C;

[0067] b. Preparation of pre-emulsion B: add 40 parts of butyl acrylate, 10 parts of ethyl acrylate, 0.5 parts of polymerizable vinyl silane, 5 parts of acrylic acid, 7 parts of acrylonitrile, 5 parts of functional monomer, 1 part of self-crosslinking monomer, 0.7 parts of emulsifier, and 20 parts of deionized water to a pre-emulsion tank with a monomer metering tank and a stirrer at room temperature and pressure, stir and mix to form a uniform pre-emulsion, and stir for 30 minutes for standby use;

[0068] c. Preparation of initiator solution C: 0.2 parts of initiator and 20 parts of deionized water were added to an initiator tank with a stirrer and a constant flow dropping device at room temperature and pressure to prepare a uniform initiator solution;

[0069] d. When the temperature in the polymerization kettle reaches 70°C, 5% of the total amount of pre-emulsion B and 30% of the total amount of initiator solution C are added to the kettle. After 5 minutes, the remaining pre-emulsion B and 70% of the initiator solution C are added dropwise to the polymerization kettle through a constant flow pump feeding device and a constant flow dripping metering device. The total dripping time is controlled at 180 minutes;

[0070] e. When the pre-emulsion is added dropwise to 120 minutes, add 0.8 parts of SIPOMER WAME, a special monomer for wet adhesion, and continue to add dropwise after stirring for 5 minutes;

[0071] f. After the addition is completed, the temperature in the polymerization reactor is controlled at 72°C for 1 hour;

[0072] g. Cool down to below 50°C, add defoamer and mildew-proof fungicide to the reactor, stir for 20 minutes, filter the material, and you can get a high-performance acrylic emulsion for textile printing cover.

[0073] Example 3

[0074] A textile printing cover high-performance acrylic emulsion, the raw material composition of which includes the following components in parts by weight: 110 parts of deionized water; 20 parts of butyl acrylate; 10 parts of ethyl acrylate; 0.8 parts of polymerizable vinyl silane; 5 parts of acrylic acid; 5 parts of acrylonitrile; 1.0 parts of SIPOMER WAME, a special monomer for wet adhesion, 3.4 parts of functional monomers; 1 part of self-crosslinking monomer emulsifier; 1 part of emulsifier; 0.3 parts of initiator.

[0075] Furthermore, the functional monomer is glycidyl methacrylate.

[0076] Furthermore, the emulsifier is a sodium salt of allyl alkyl succinate sulfonate containing a double bond.

[0077] Furthermore, the vinyltrimethoxysilane.

[0078] Furthermore, the self-crosslinking monomer is diacetone acrylamide.

[0079] Furthermore, the initiator is ammonium persulfate.

[0080] The above textile printing overlay high-performance acrylic emulsion comprises the following steps:

[0081] a. Preparation of reaction tank primer A: Add 70 parts of deionized water and 0.3 parts of emulsifier to a polymerization reactor with a stirrer, a condenser and a feeding device, and heat the reactor to a temperature of 70°C;

[0082] b. Preparation of pre-emulsion B: Add 20 parts of butyl acrylate, 10 parts of ethyl acrylate, 0.8 parts of polymerizable vinyl silane, 5 parts of acrylic acid, 5 parts of acrylonitrile, 3.4 parts of functional monomer, 1 part of self-crosslinking monomer, 0.7 parts of emulsifier, and 20 parts of deionized water to a pre-emulsification tank with a monomer metering tank and a stirrer at room temperature and pressure, stir and mix into a uniform pre-emulsion, and stir for 30 minutes for standby use;

[0083] c. Preparation of initiator solution C: 0.3 parts of initiator and 20 parts of deionized water were added to an initiator tank with a stirrer and a constant flow dropping device at room temperature and pressure to prepare a uniform initiator solution;

[0084] d. When the temperature in the polymerization kettle reaches 70°C, 5% of the total amount of pre-emulsion B and 30% of the total amount of initiator solution C are added to the kettle. After 5 minutes, the remaining pre-emulsion B and 70% of the initiator solution C are added dropwise to the polymerization kettle through a constant flow pump feeding device and a constant flow dripping metering device. The total dripping time is controlled at 180 minutes;

[0085] e. When the pre-emulsion is added dropwise for 120 minutes, add 1.0 parts of SIPOMER WAME, a special monomer for wet adhesion, and continue to add dropwise after stirring for 5 minutes;

[0086] f. After the addition is completed, the temperature in the polymerization reactor is controlled at 78°C for 1 hour;

[0087] g. Cool down to below 50°C, add defoamer and mildew-proof fungicide to the reactor, stir for 20 minutes, filter the material, and you can get a high-performance acrylic emulsion for textile printing cover.

[0088] The textile printing topcoat high-performance acrylic emulsion prepared in Examples 1-3 of the present invention is used to prepare a topcoat coating that becomes transparent when in contact with water. The specific preparation method is as follows: 50 parts of the prepared emulsion and 30 parts of water are added into a dispersion kettle, and then 0.5 parts of a dispersant and 0.5 parts of a wetting agent are added, and stirred for 5-10 minutes. Then 15 parts of aluminum silicate powder are added, and dispersed at high speed for 20-30 minutes. After the dispersion is completed, 0.5 parts of a defoamer and 0.5 parts of ammonia water are added to defoam at a low speed for 5-10 minutes, and then 3 parts of a thickener are slowly added at a medium speed to thicken to a certain viscosity to obtain a topcoat coating that becomes transparent when in contact with water.

[0089] The performance of the water-transparent base coating sample 1 and sample 2 prepared with the commercial polyurethane emulsion were compared. The results are shown in Table 1:

[0090] Table 1 Performance test results

[0091]

[0092]

[0093] From the above test results, it can be seen that the water-transparent bottom cover coating prepared by the high-performance acrylic emulsion for printing cover in Examples 1-3 has excellent anti-adhesion effect, does not turn white when exposed to water, has fast permeability, can quickly show the bottom pattern when exposed to water, has a soft feel, good water resistance, and excellent elasticity, and has very broad market demand and economic benefits.

[0094] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A high performance acrylic emulsion for textile printing overlay, characterized in that: The high-performance acrylic emulsion comprises, by weight: 90-110 parts of deionized water, 9-10 parts of ethyl acrylate, 20-40 parts of butyl acrylate, 0.5-0.8 parts of polymerizable vinyl silane, 4-6 parts of acrylic acid, 4-7 parts of acrylonitrile, 0.6-1 parts of Rhodia wet adhesion special monomer, 3.4-6.0 parts of functional monomer, 0.5-1 parts of self-crosslinking monomer, 0.8-1.2 parts of emulsifier and 0.1-0.3 parts of initiator; the functional monomer The monomer is one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, glycidyl acrylate and glycidyl methacrylate; the self-crosslinking monomer is one or two of diacetone acrylamide and acetoacetoxyethyl methacrylate; the polymerizable vinyl silane is one or more of vinyl triethoxysilane, vinyl tri(β-methoxyethoxy)silane and vinyl trimethoxysilane; the Rhodia wet adhesion special monomer is SIPOMER WAME wet adhesion special monomer; the emulsifier is one or two of sodium salt of allyl alkyl succinate sulfonate containing double bonds and special alcohol ether sulfate containing allyl groups; The method for preparing the high-performance acrylic emulsion for textile printing overlay comprises the following steps: Preparation of primer A: Add 45-82 parts of deionized water and 0.2-0.3 parts of emulsifier into the polymerization kettle, and heat the polymerization kettle until the temperature reaches 68-72° C. to prepare primer A; Preparation of pre-emulsion B: add 20-40 parts of butyl acrylate, 9-10 parts of ethyl acrylate, 0.5-0.8 parts of polymerizable vinyl silane, 4-6 parts of acrylic acid, 4-7 parts of acrylonitrile, 3.4-6.0 parts of functional monomer, 0.5-1 part of self-crosslinking monomer, 0.8-1.2 parts of emulsifier, and 18-25 parts of deionized water into a pre-emulsification tank at room temperature and pressure, and stir to mix into a uniform pre-emulsion B for later use; Preparation of initiator solution C: add 0.1-0.3 parts of initiator and 10-20 parts of deionized water into an initiator tank at room temperature and pressure to prepare a uniform initiator solution C; When the temperature in the polymerization kettle reaches 68-72°C, add 2%-5% of the total amount of pre-emulsion B and 20%-30% of the total amount of initiator solution C into the polymerization kettle. After 5-10 minutes, add the remaining pre-emulsion B and the remaining initiator solution C dropwise into the polymerization kettle. The total dropping time is controlled within 150-180 minutes. When the pre-emulsion B has been added dropwise for 120-150 minutes, 0.6-1.0 parts of Rhodia wet adhesion special monomer are added. After the addition is completed, the temperature in the polymerization kettle is controlled at 72-78°C and kept warm for 0.5-2 hours; When the temperature in the polymerization kettle drops to below 50°C, add a defoamer and a mildew and fungicide into the reactor, stir and filter the material to obtain a high-performance acrylic emulsion for textile printing cover.

2. The high performance acrylic emulsion for textile printing overlay according to claim 1, characterized in that: The initiator is one or more of ammonium persulfate, sodium persulfate and potassium persulfate.