Catalysts for exhaust gas purification

By controlling the particle size of barium components in the catalyst layer and reducing the contact between Si elements and the catalyst layer, the problem of anti-degradation of the oxygen storage capacity of Si-SiC composite substrate at high temperatures is solved, and high-temperature durability and NOx purification performance are achieved Improvement.

CN116133736BActive Publication Date: 2024-11-29CATALER CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202180056716.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-19
Publication Date
2024-11-29
Estimated Expiration
2041-07-19

Smart Images

  • Figure CN116133736B_ABST
    Figure CN116133736B_ABST
Patent Text Reader

Abstract

The present invention provides an exhaust gas purification catalyst with excellent high-temperature durability and oxygen storage capacity, which has a substrate containing a silicon-silicon carbide composite material and a catalyst layer containing a barium component. The exhaust gas purification catalyst disclosed in the present invention has a substrate and a catalyst layer in contact with the substrate. The substrate contains a silicon-silicon carbide composite material. The catalyst layer contains a platinum group catalyst, a barium component and an oxygen storage material. The barium component is at least one selected from barium and a barium compound. The barium component is present at least on the surface of the oxygen storage material. The average particle size of the barium component is not less than 100nm and not more than 350nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a catalyst for exhaust gas purification, and more specifically to a catalyst for exhaust gas purification that can be suitably used as an electrically heated catalyst. It should be noted that this application claims priority based on Japanese Patent Application No. 2020-134758 filed on August 7, 2020, and the entire contents of the application are incorporated into this specification as a reference. Background Art

[0002] In recent years, electrically heated catalysts (EHCs) have attracted much attention as catalysts for purifying exhaust gas emitted from engines of automobiles and the like. In order for an exhaust gas purification catalyst for an internal combustion engine to exhibit sufficient purification performance, the temperature of the exhaust gas purification catalyst needs to rise to a temperature at which the catalyst is activated. Since conventional exhaust gas purification catalysts are heated using the heat of the exhaust gas, high purification performance cannot be obtained when the exhaust gas temperature is low, such as when the engine has just been started. In contrast, in an electrically heated catalyst, even when the exhaust gas temperature is low, such as when the engine has just been started, the catalyst temperature can be raised in a short time by electrically heating, thereby activating the catalyst. Therefore, even when the exhaust gas temperature is low, sufficient purification performance can be obtained, thereby improving the purification efficiency of the exhaust gas.

[0003] The typical structure of an electrically heated catalyst has a substrate and a catalyst layer. As a substrate of an electrically heated catalyst, a substrate containing a ceramic SiC (silicon carbide) having electrical conductivity is known. In addition, as such a substrate, a substrate containing a Si-SiC (silicon-silicon carbide) composite material in which Si, which is a low-impedance material having an impedance lower than that of SiC, is combined with SiC is known (for example, refer to Patent Documents 1 and 2). On the other hand, as a catalyst layer of an electrically heated catalyst, a catalyst layer containing a platinum group metal (PGM) as a catalyst component, an oxygen storage material (OSC material), etc. is known (for example, refer to Patent Document 3).

[0004] Prior Art Literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 6052250

[0007] Patent Document 2: Japanese Patent Application Publication No. 2011-194323

[0008] Patent Document 3: Japanese Patent Application Publication No. 2004-351292 Summary of the invention

[0009] Problems to be solved by the invention

[0010] The inventors of the present invention have conducted in-depth research and found the following viewpoint: in an exhaust purification catalyst using a substrate containing a Si-SiC composite material, when exposed to a high temperature environment, Si of the Si-SiC composite material will move to the catalyst layer and diffuse, react with the oxygen storage material, and degrade the oxygen storage material. Here, when barium (Ba) is contained in the catalyst layer in order to suppress platinum group metal poisoning caused by hydrocarbons (HC), the Ba element will promote the diffusion of Si into the catalyst layer, which will promote the degradation of the oxygen storage material. Therefore, when the catalyst layer of the exhaust purification catalyst using a substrate containing a Si-SiC composite material contains a barium component, there will be a problem of low resistance to degradation of the oxygen storage capacity when exposed to a high temperature environment (in other words, the high temperature durability of the oxygen storage capacity).

[0011] Therefore, an object of the present invention is to provide an exhaust gas purification catalyst having a substrate containing a Si-SiC composite material and a catalyst layer containing a barium component and having excellent oxygen storage capacity and high-temperature durability.

[0012] Technical means to solve problems

[0013] The exhaust gas purification catalyst disclosed herein comprises a substrate and a catalyst layer in contact with the substrate. The substrate comprises a silicon-silicon carbide composite material. The catalyst layer comprises a platinum group catalyst, a barium component and an oxygen storage material. The barium component is at least one selected from barium and a barium compound. The barium component is present at least on the surface of the oxygen storage material. The average particle size of the barium component is not less than 100 nm and not more than 350 nm.

[0014] According to such a structure, by appropriately controlling the particle size of the barium component, not only can the contact between the Ba element contained in the catalyst layer and the Si element contained in the substrate be reduced, but also the Ba element can be dispersed in the catalyst layer together with the platinum group catalyst. This can inhibit the diffusion of Si into the catalyst layer caused by the Ba element, and can inhibit the degradation of the oxygen storage material caused by Si. As a result, the high-temperature durability of the oxygen storage capacity of the exhaust gas purification catalyst can be improved. That is, according to such a structure, a catalyst for exhaust gas purification having a substrate containing a Si-SiC composite material and a catalyst layer containing a barium component and excellent high-temperature durability of oxygen storage capacity can be provided.

[0015] In a preferred embodiment of the exhaust gas purification catalyst disclosed herein, the average particle size of the barium component is 100 nm or more and 200 nm or less. With such a structure, the high temperature durability of the oxygen storage capacity is further improved.

[0016] In another preferred embodiment of the exhaust gas purification catalyst disclosed herein, the platinum group metal is Pd. According to such a structure, the high temperature durability of the oxygen storage capacity is further improved.

[0017] In still another preferred embodiment of the exhaust gas purifying catalyst disclosed herein, the exhaust gas purifying catalyst further comprises an electrode, and the exhaust gas purifying catalyst is an electrically heated catalyst.

[0018] According to such a structure, an electrically heated catalyst having excellent oxygen storage capacity and high-temperature durability is provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a perspective schematic diagram showing an example of an exhaust gas purification catalyst according to an embodiment.

[0020] Figure 2 yes Figure 1 A schematic cross-sectional view of an example of a layer structure of an exhaust gas purification catalyst.

[0021] Figure 3 yes Figure 1 A schematic cross-sectional view of another example of the layer structure of the exhaust gas purifying catalyst.

[0022] Figure 4 It is a graph showing the evaluation results of the oxygen absorption capacity of the exhaust gas purification catalysts of the examples, comparative examples and reference examples.

[0023] Figure 5 is the NO of the exhaust gas purification catalysts of the examples, comparative examples and reference examples. x A graph showing the evaluation results of purification performance. DETAILED DESCRIPTION

[0024] Hereinafter, several preferred embodiments of the present invention will be described with appropriate reference to the accompanying drawings. Except for matters specifically mentioned in this specification, matters required for implementing the present invention can be grasped as design matters for those skilled in the art based on the prior art in the art. The present invention can be implemented based on the contents disclosed in this specification and the technical knowledge in the art. The following figures are schematic diagrams for understanding the contents of the present invention, and the dimensional relationships (length, width, thickness, etc.) in each figure do not reflect the actual dimensional relationships.

[0025] Figure 1 An example of the exhaust gas purification catalyst according to the present embodiment is schematically shown. Figure 1 This is an example in which the exhaust gas purification catalyst of the present embodiment is configured as an electrically heated catalyst. Figure 2 Schematically Figure 1 Layer structure of an exhaust gas purification catalyst.

[0026] like Figure 1 and Figure 2As shown, the exhaust gas purifying catalyst 10 has a substrate 11 and a catalyst layer 20. The catalyst layer 20 is directly provided on the substrate 11, so that the catalyst layer 20 is in contact with the substrate 11.

[0027] <Base Material>

[0028] The substrate 11 is a member for supporting the catalyst layer 20. The substrate 11 contains a Si-SiC composite material. The substrate 11 can obtain excellent electrical conductivity due to the Si-SiC composite material. In addition, since the Si-SiC composite material can play the role of an impedance heating body, the exhaust gas purification catalyst 10 can be used as an electrically heated catalyst by containing the Si-SiC composite material in the substrate 11.

[0029] The substrate 11 may also contain components other than the Si-SiC composite material within a range that does not significantly impair the effect of the present invention. The ratio of Si to SiC "Si / SiC" in the Si-SiC composite material is not particularly limited and may be the same as the ratio (Si / SiC) of the known Si-SiC composite material used in the substrate of the exhaust gas purification catalyst.

[0030] The shape of the substrate 11 may be the same as that of a known exhaust gas purifying catalyst. For example, the substrate 11 may be a straight flow type or wall flow type honeycomb substrate commonly used in exhaust gas purifying catalysts.

[0031] exist Figure 1 In the example shown, the substrate 11 has a cylindrical shape. The shape of the substrate 11 is not limited thereto, and may be an elliptical cylinder, a polygonal cylinder, etc. The size of the substrate 11 is not particularly limited, and may be the same size as a known exhaust gas purification catalyst used as an electrically heated catalyst.

[0032] Figure 1 and Figure 2 The arrows indicate the flow direction of the exhaust gas. The substrate 11 has a plurality of chambers 15 opened at the ends on both sides of the exhaust gas inlet side and the exhaust gas outlet side, and partition walls 16 separating adjacent chambers 15. The shape of each chamber 15 is not particularly limited, and may be a quadrilateral such as a square, parallelogram, rectangle, trapezoid; other polygons such as a triangle, hexagon, octagon; circle, etc. In the exhaust gas purification catalyst 10 having the substrate 11 shown in the figure, the exhaust gas flowing into the chamber 15 from the end on the exhaust gas inlet side passes through the chamber 15 and flows out from the end on the exhaust gas outlet side.

[0033] A catalyst layer 20 is formed on at least a portion of the substrate 11. Figure 1 Although not shown, the catalyst layer 20 is formed in the chamber 15 .

[0034] <Catalyst layer>

[0035] The catalyst layer 20 contains a platinum group metal as a catalyst component. That is, the catalyst layer 20 contains at least one metal selected from platinum (Pt), rhodium (Rh), palladium (Pd), ruthenium (Ru), osmium (Os) and iridium (Ir). Among them, Pd and Pt have excellent purification performance (oxidation purification ability) of carbon monoxide (CO) and hydrocarbons (HC), and Rh has excellent NO x The purification performance (reduction purification ability) is excellent. Therefore, from the perspective of high purification performance, the platinum group metal contained in the catalyst layer 20 is preferably at least one selected from Pt, Rh and Pd. In addition, when the platinum group catalyst is Pd, Si, which becomes a factor in reducing the oxygen storage capacity, is more likely to diffuse in the catalyst layer. Therefore, from the perspective of a higher effect of improving the high temperature durability of the oxygen storage capacity, Pd is more preferred as the platinum group metal.

[0036] From the perspective of increasing the contact area with the exhaust gas, the platinum group metal is preferably in a microparticle form. Specifically, the average particle size of the platinum group metal is preferably 15 nm or less, more preferably 10 nm or less, further preferably 7 nm or less, and most preferably 5 nm or less. In addition, the average particle size of the platinum group metal is preferably 1 nm or more. The average particle size of the platinum group metal can be obtained by obtaining an electron microscope image (TEM image, etc.) of the platinum group metal as the average value of the particle sizes of 20 or more particles randomly selected in the image.

[0037] The catalyst layer contains an oxygen storage material (so-called "OSC material"). The OSC material can function as a co-catalyst for exhaust purification. As an OSC material, a known compound known to have oxygen storage capacity can be used, and specific examples thereof include ceria (CeO2) and composite oxides containing ceria. As composite oxides containing ceria, composite oxides containing ceria and zirconium oxide (ZrO2) (ceria-zirconia composite oxides (so-called CZ composite oxides or ZC composite oxides)) and the like can be mentioned. When zirconium oxide is contained in the OSC material, thermal degradation of ceria can be suppressed, so ceria-zirconia composite oxides are preferred as OSC materials.

[0038] OSC materials may contain oxides of rare earth elements for the purpose of improving properties (particularly heat resistance and oxygen absorption and release properties, etc.) Examples of rare earth elements include Sc, Y, La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu.

[0039] When the OSC material is a composite oxide containing cerium oxide, from the perspective of fully exerting its oxygen storage capacity, the content of cerium oxide is preferably 15% by mass or more, more preferably 20% by mass or more. On the other hand, when the content of cerium oxide is too high, the basicity of the OSC material may become too high. Therefore, the content of cerium oxide is preferably 40% by mass or less, more preferably 30% by mass or less.

[0040] OSC materials can also play the role of a carrier of a catalyst, etc. Therefore, in the catalyst layer 20, the platinum group catalyst is typically supported by the OSC material. Alternatively, the catalyst layer 20 may also contain oxides other than OSC materials such as aluminum oxide (Al2O3), titanium oxide (TiO2), zirconium oxide (ZrO2), silicon oxide (SiO2) (preferably aluminum oxide) as a carrier, and the platinum group catalyst may be supported by the oxide carrier, or the platinum group catalyst may be supported by both the OSC material and the oxide carrier. In order to improve heat resistance, etc., oxide carriers other than OSC materials may also be added with a small amount (e.g., 1% by mass or more and 10% by mass or less) of oxides of rare earth elements such as Pr2O3, Nd2O3, La2O3, and Y2O3.

[0041] The catalyst layer 20 contains a barium component. The catalyst layer 20 contains a barium component, which can suppress poisoning of the platinum group metal by hydrocarbons (HC). In addition, when the platinum group metal is Pd, the barium component can suppress agglomeration of Pd.

[0042] The barium component is at least one selected from barium and barium compounds. Examples of barium compounds include barium sulfate, barium acetate, barium nitrate, and barium carbonate. Among them, barium sulfate and barium acetate are preferred, and barium sulfate is more preferred.

[0043] Generally, in order to highly diffuse the barium component into the catalyst layer, the average particle size of the barium component is as small as possible. In particular, when the average particle size is several nanometers (especially about 5 nm), the diffusibility of the barium component is very good.

[0044] However, in the present embodiment, the average particle size of the barium component is not less than 100 nm and not more than 350 nm. By making the average particle size of the barium component much larger than about 5 nm, the contact between the Ba element contained in the catalyst layer 20 and the Si contained in the substrate 11 can be reduced; and by making the average particle size within the range of not less than 100 nm and not more than 350 nm, the Ba element can be dispersed in the catalyst layer 20 together with the platinum group catalyst. Therefore, by making the average particle size of the barium component within the above range, the diffusion of Si into the catalyst layer 20 caused by the Ba element can be suppressed. Therefore, in this way, the degradation of the OSC material caused by Si can be suppressed, and as a result, the high temperature durability of the OSC is improved. From the perspective of higher high temperature durability of the OSC, the average particle size of the barium component is preferably not less than 100 nm and not more than 200 nm, and more preferably not less than 150 nm and not more than 200 nm. Among them, by making the average particle size of the barium component not less than 100 nm, it is not easy to cause damage to the Si-SiC substrate 11, and high NO can also be obtained. x Purification performance.

[0045] Among them, the average particle size of the barium component can be obtained, for example, in the following manner. First, collect a portion of the catalyst layer 20 from the exhaust purification catalyst 10 as a sample. Next, use an electron microscope (for example, a scanning electron microscope (SEM), a transmission electron microscope (TEM), etc.) to take an electron microscope image of the sample. Next, select more than 20 particles that can be seen as a whole from the particles of the barium component that appear in the electron microscope image, and obtain the area of ​​each selected particle. Calculate the diameters of circles with areas equal to these areas respectively, and then find the arithmetic mean of these diameters. The arithmetic mean is used as the average particle size.

[0046] The average particle size of the barium component can be adjusted, for example, by controlling the average particle size of the barium source in the method of preparing the catalyst layer using a slurry containing the barium source.

[0047] The barium component is present at least on the surface of the OSC material. The barium component is typically supported by the OSC material. Alternatively, the catalyst layer 20 may further contain an oxide support other than the above-mentioned OSC material, and the barium component may be supported by both the OSC material and the oxide support. In this case, for example, 10% by mass or more, 30% by mass or more, or 50% by mass or more of the barium component is supported by the OSC material.

[0048] The dispersion form of the barium component in the catalyst layer 20 is not particularly limited, but since the catalyst layer 20 is typically prepared from a slurry mixed with a platinum group catalyst source, a barium source, an OSC material, and an oxide support as required, the barium component is uniformly dispersed in the catalyst layer 20 .

[0049] There is no particular limitation on the content of the barium component in the catalyst layer 20. The ratio of the mass of the barium component calculated as sulfate to the mass of the platinum group element is preferably 1 / 80 to 20.

[0050] The catalyst layer 20 may further contain components other than those mentioned above (e.g., binders, additives, etc.). Examples of binders include alumina sol, silica sol, etc. Examples of additives include NO x Adsorbents, stabilizers, etc.

[0051] The content of the platinum group metal in the catalyst layer 20 is not particularly limited. For example, it is 0.01% to 8% by mass, or 0.1% to 5% by mass, relative to the total mass of the OSC material and the oxide support other than the OSC material contained in the catalyst layer 20 .

[0052] The size of the catalyst layer 20 is not particularly limited and can be appropriately determined according to the size of the chamber 15 of the substrate 11, the flow rate of exhaust gas supplied to the exhaust gas purifying catalyst 10, etc. The thickness of the catalyst layer 20 can be 1 μm to 500 μm, or 5 μm to 200 μm.

[0053] The catalyst layer 20 may be formed only on a portion of the surface of the substrate 11. For example, the catalyst layer 20 may be formed only on the front portion of the substrate 11 (e.g., only from the end of the exhaust gas inlet side of the substrate 11 to 30% of the area in the exhaust gas flow direction) or only on the rear portion of the substrate 11 (e.g., only from the end of the exhaust gas outlet side of the substrate 11 to 30% of the area in the exhaust gas flow direction). In addition, the catalyst layer 20 may have the same composition throughout the layer, or may have different compositions within the scope of the present embodiment. For example, in the catalyst layer 20, the front and rear portions of the substrate 11 may contain different platinum group catalysts.

[0054] The exhaust gas purifying catalyst 10 may include elements other than the substrate 11 and the catalyst layer 20 .

[0055] exist Figure 1 In the example shown, the exhaust gas purification catalyst 10 is configured as an electrically heated catalyst. Therefore, in addition to the substrate 11 and the catalyst layer 20, the exhaust gas purification catalyst 10 also has an electrode 40. The electrode 40 can be the same as the electrode of the known electrically heated catalyst, and the electrode 40 can be a metal electrode, a carbon electrode, etc. In the example shown in the figure, the electrode 40 has an electrode layer 42 and an electrode terminal 44 arranged on the outer surface of the substrate 11. The electrode layer 42 has the function of diffusing the current. However, the structure of the electrode 40 is not limited to this, as long as it can be powered to the substrate 11.

[0056] Figure 3 Another example of the exhaust gas purification catalyst according to the present embodiment is shown. Figure 3 The exhaust purification catalyst 10' shown has a second catalyst layer 30 in addition to the first catalyst layer 20. The first catalyst layer 20 has the same structure as above. The second catalyst layer 30 contains a catalyst. The type of catalyst contained in the second catalyst layer 30 is not particularly limited. Here, by making the second catalyst layer 30 contain a platinum group element different from the platinum group element contained in the first catalyst layer 20 as a catalyst, the exhaust purification performance of the exhaust purification catalyst 10 can be improved. In addition, the second catalyst layer 30 may contain an oxide carrier, an OSC material, etc. for supporting the catalyst. The second catalyst layer 30 may contain Ba or may not contain it. When the second catalyst layer 30 contains Ba particles, the average particle size thereof is not particularly limited, and may be less than 100 nm, may be greater than 350 nm, and may be in the range of more than 100 nm and less than 350 nm.

[0057] As an example of the exhaust gas purification catalyst 10', the first catalyst layer 20 contains Pd, an oxide carrier (such as alumina) carrying Pd, Ba having an average particle size of 100 nm to 350 nm, and an OSC material (such as a CZ composite material) carrying Ba. On the other hand, the second catalyst layer 30 contains Rh, an oxide carrier (such as alumina) carrying Rh, and an OSC material (such as a CZ composite material).

[0058] The exhaust gas purification catalyst 10 can be manufactured, for example, as follows. First, prepare a substrate 11 containing a Si-SiC composite material. In addition, the constituent components of the catalyst layer 20 (for example, a platinum group metal source (for example, a solution containing ions of platinum group metals, etc.), an OSC material, a Ba source (for example, barium sulfate, barium acetate, etc.)) and a dispersion medium are mixed to prepare a slurry for forming the catalyst layer 20. The slurry is applied to the chamber 15 of the substrate 11 and dried, and fired as needed. The catalyst layer 20 is thereby formed on the substrate 11. Then, the electrode 40 is assembled according to conventional methods.

[0059] The exhaust gas purification catalyst 10 can be used for exhaust gas purification of an internal combustion engine according to a known method. Specifically, the exhaust gas purification catalyst 10 can be configured in an exhaust system (particularly an exhaust pipe) of an automobile engine for use. Here, the exhaust gas purification catalyst 10 is configured as an EHC. In this case, for example, it is electrically connected to the automobile to supply power from the battery of the automobile. The internal combustion engine is, for example, a gasoline engine, a diesel engine, etc., preferably a gasoline engine.

[0060] The exhaust gas purifying catalyst 10 suppresses a decrease in oxygen storage capacity when exposed to high temperatures (for example, 900° C. or 1000° C.) for a long period of time. Therefore, the exhaust gas purifying catalyst 10 is excellent in high temperature durability of oxygen storage capacity.

[0061] The above description is about the case where the exhaust gas purification catalyst of the present embodiment is configured as an electrically heated catalyst. However, the exhaust gas purification catalyst of the present embodiment can also be used as a particulate filter such as a gasoline particulate filter (GPF) and a diesel particulate filter (DPF). When the particulate filter is regenerated, the particulates are heated to be burned. Therefore, when used as a particulate filter, the deterioration of the oxygen storage capacity during the heating can be suppressed.

[0062] The present invention will be described in more detail below with reference to examples, but the present invention is not intended to be limited to these examples.

[0063] <Preparation of Exhaust Gas Purification Catalyst>

[0064] [Example 1]

[0065] As a substrate, a honeycomb substrate made of Si-SiC composite material (volume 551mL, number of chambers 600cpsi, partition wall thickness 5 mils, chamber shape is square, substrate length 50mm) is prepared. Palladium nitrate solution, La2O3 composite Al2O3 powder, CZ composite oxide powder with trace amounts of Pr2O3, Nd2O3, La2O3 and Y2O3 added, barium sulfate with an average particle size of 100nm, Al2O3-based adhesive and ion exchange water are mixed to prepare a Pd-containing slurry. The Pd-containing slurry is flowed into the above-mentioned substrate, and the excess slurry is blown off with a blower, thereby coating the substrate wall with the slurry. Next, the substrate is placed in a dryer set at 120°C and dried for 2 hours. Then, the substrate is fired at 500°C in an electric furnace for 2 hours to form a Pd catalyst layer as the first catalyst layer.

[0066] In addition, a rhodium nitrate solution, La2O3 composite Al2O3 powder, CZ composite oxide powder with trace amounts of Pr2O3, Nd2O3, La2O3 and Y2O3 added, Al2O3-based binder and ion exchange water are mixed to prepare a Rh-containing slurry. The Rh-containing slurry is flowed into the substrate formed with the above-mentioned Pd catalyst layer, and the excess slurry is blown off with a blower, so that the wall surface of the substrate formed with the above-mentioned Pd catalyst layer is coated with the slurry. Next, the substrate is placed in a dryer set at 120°C and dried for 2 hours. Then, the substrate is fired at 500°C in an electric furnace for 2 hours to form a Rh catalyst layer as a second catalyst layer on the Pd catalyst layer.

[0067] As described above, the exhaust gas purifying catalyst of Example 1 in which the Pd catalyst layer and the Rh catalyst layer were sequentially laminated on the substrate was obtained. In this exhaust gas purifying catalyst, the Pd loading amount was 2 g / L and the Rh loading amount was 0.15 g / L.

[0068] [Other Examples and Comparative Examples]

[0069] The exhaust gas purification catalyst was prepared in the same manner as in Example 1 except that a compound having an average particle size shown in the following table was used as the barium component. The average particle size of barium sulfate having an average particle size of 50 nm or more was adjusted by wet pulverization. In addition, water-soluble Ba was used when preparing the slurry of barium sulfate having an average particle size of 5 nm.

[0070] [Reference example]

[0071] As a substrate, a cordierite honeycomb substrate (volume 551 mL, number of cells 600 cpsi, partition wall thickness 4 mils, cell shape square, substrate length 50 mm) was prepared. An exhaust gas purification catalyst was prepared in the same manner as in Example 1 except that the cordierite substrate was used and a compound having an average particle size shown in the following table was used as a barium component.

[0072] [Table 1]

[0073] Barium composition Average particle size (nm) Comparative Example 1 Barium acetate 5 Comparative Example 2 Barium sulfate 50 Example 1 Barium sulfate 100 Example 2 Barium sulfate 150 Example 3 Barium sulfate 200 Example 4 Barium sulfate 350 Comparative Example 3 Barium sulfate 400 Comparative Example 4 Barium sulfate 500 Reference Example 1 Barium acetate 5 Reference Example 2 Barium sulfate 50 Reference Example 3 Barium sulfate 100 Reference Example 4 Barium sulfate 200 Reference Example 5 Barium sulfate 350 Reference Example 6 Barium sulfate 400 Reference Example 7 Barium sulfate 500

[0074] The average particle size of the barium acetate used was evaluated using TEM, and the average particle size of the barium sulfate used was evaluated using FE-SEM and a laser diffraction particle size distribution measuring device. In addition, a portion of the catalyst layer of the exhaust gas purification catalyst prepared as described above was taken as a sample, and an SEM image of the sample was obtained using FE-SEM, and the average particle size was calculated as the average value of the particle sizes of 20 particles in the SEM image. It was confirmed that the average particle size was the same as the average particle size of the barium acetate used and the barium sulfate used.

[0075] <High temperature durability test>

[0076] The exhaust gas purification catalysts of the embodiments, comparative examples and reference examples were installed in the exhaust system of a V-type 8-cylinder gasoline engine installed on a table, and a 50-hour durability test was carried out at a catalyst bed temperature of 1000°C including a specified fuel cut-off condition.

[0077] <Evaluation of oxygen storage capacity (OSC)>

[0078] The exhaust gas purification catalysts of the embodiments, comparative examples and reference examples after the above-mentioned durability test were installed in the exhaust system of a gasoline engine installed on a table. In addition, an O2 sensor was installed downstream of the catalyst. The air-fuel ratio A / F of the mixed gas supplied to the engine oscillated between rich combustion and lean combustion in a rectangular manner. The sum of the oxygen release amount and the oxygen absorption amount at this time was accumulated to calculate OSC. The results are shown in Figure 4 .

[0079] <NO x Evaluation of purification capacity>

[0080] The exhaust gas purification catalysts of the embodiments, comparative examples and reference examples were installed in the exhaust system of the engine rig, and the combustion state of the engine was controlled according to the theoretical air-fuel ratio. The temperature of the gas flowing into the catalyst was raised from 200°C to 500°C at a heating rate of 10°C / min using a heat exchanger. The intake air volume of the engine was set to 25g / sec. The gas components of the gas flowing into the catalyst and the gas flowing out of the catalyst during the heating process were analyzed, and the gas composition that could reduce 50% of NO x Temperature of component purification (NO x 50% purification temperature of ingredients: T50-NO x The results are shown in Figure 5 .

[0081] like Figure 4 As shown in the results, when a cordierite substrate (i.e., a substrate different from a Si-SiC substrate) is used, the smaller the average particle size of the barium component, the higher the high-temperature durability of the oxygen storage capacity. This is because the smaller the average particle size of the barium component, the higher the degree of dispersion of the barium component, and the higher the effect of suppressing the poisoning of the platinum group catalyst by HC.

[0082] In contrast, when a Si-SiC substrate is used, it can be seen that the high-temperature durability of the oxygen storage capacity is different. Specifically, the high-temperature durability of the oxygen storage capacity is high when the average particle size of the barium component is within the range of 100 nm to 350 nm. This is because when a Si-SiC substrate is used, the average particle size of the barium component is significantly increased, which can reduce the contact between Ba contained in the catalyst layer and Si contained in the substrate; in addition, by setting the average particle size within an appropriate range, the Ba element can be dispersed in the catalyst layer together with the platinum group catalyst.

[0083] In addition, according to Figure 5 The results showed that when the cordierite substrate was used, the smaller the average particle size of the barium component, the higher the NO x The higher the purification performance.

[0084] In contrast, when the Si-SiC substrate is used, the NO x Especially when the average particle size is less than 100nm, due to the degradation of OSC materials, NO x The purification performance is significantly reduced. This is because when the average particle size of the barium component is too small, the Si-SiC substrate is damaged, and the electrical conductivity and thermal uniformity of the substrate deteriorate.

[0085] As can be seen from the above, the exhaust gas purification catalyst disclosed herein is excellent in high temperature durability of oxygen storage capacity despite the use of a Si-SiC composite material for the substrate and a barium component for the catalyst layer.

[0086] Although the specific examples of the present invention have been described in detail above, these are merely illustrative and do not limit the scope of the claims. The technology described in the scope of the claims includes various modifications and changes of the specific examples described above.

Claims

1. A catalyst for exhaust gas purification, It is characterized in that having a substrate and a catalyst layer in contact with the substrate, The substrate contains a silicon-silicon carbide composite material, The catalyst layer contains a platinum group catalyst, a barium component and an oxygen storage material. The barium component is at least one selected from barium and barium compounds, The barium component is present at least on the surface of the oxygen storage material. The average particle size of the barium component is not less than 100 nm and not more than 350 nm.

2. The exhaust gas purification catalyst according to claim 1, It is characterized in that The average particle size of the barium component is not less than 100 nm and not more than 200 nm.

3. The exhaust gas purification catalyst according to claim 1, It is characterized in that The platinum group catalyst is Pd.

4. The exhaust gas purification catalyst according to any one of claims 1 to 3, It is characterized in that The exhaust gas purifying catalyst further includes an electrode, and the exhaust gas purifying catalyst is an electrically heated catalyst.

Citation Information

Patent Citations

  • A spilt for shallow structure

    JP1985052250B2

  • Electric heating type catalyst device

    JP2004351292A

  • Honeycomb catalyst, and apparatus for cleaning exhaust

    JP2011194323A

  • Filter device and laser device

    JP2020134758A

  • Alumina material containing barium sulfate and exhaust gas purifying catalyst using same

    CN104066507A