A particle-reinforced high specific heat heat transfer alloy and preparation method thereof
By using Sn, Bi, Zn low-melting-point metal eutectic alloys and nanoparticle-enhanced high specific heat heat transfer alloys in the heat treatment of automobile leaf springs, the problems of low heat transfer efficiency and insufficient thermal stability of traditional coolants are solved and achieved. Efficient and safe cooling effect, suitable for smart manufacturing environments.
Patent Information
- Application Number
- CN202211706960.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-27
AI Technical Summary
The existing automobile leaf spring heat treatment quenching coolant has low heat transfer efficiency, insufficient thermal stability and high pipe corrosion, making it difficult to meet the needs of high-efficiency and high-quality production.
A eutectic alloy based on Sn, Bi, and Zn low-melting-point metal elements is used, and a nanoparticle reinforcement phase is added. A high-specific heat transfer alloy is prepared through powder metallurgy and secondary molding methods to increase its specific heat capacity and thermal conductivity.
It significantly improves the thermal conductivity and specific heat capacity of the heat transfer medium, reduces the volume of the cooling device, improves the utilization of the quenching pool, ensures high temperature stability and low cost, and avoids safety risks and pipeline corrosion.
Smart Images

Figure CN116179924B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of automobile leaf spring heat treatment quenching coolant, in particular to a particle-reinforced high specific heat heat transfer alloy and a preparation method thereof. Background Art
[0002] As the level of automation and intelligence in the automotive leaf spring manufacturing industry continues to improve, the efficiency of leaf spring production lines is getting higher and higher. During the heat treatment of leaf springs, especially during graded quenching, the temperature of the quenching liquid rises too quickly, which greatly affects the quenching quality of the leaf springs. The selection of high-efficiency, wide-temperature range heat transfer media is crucial to the production efficiency and quality stability of leaf spring products.
[0003] Among the different cooling media options, water or heat transfer oil is usually used to cool the heat treatment quenching liquid. However, due to the low heat transfer efficiency of water, the increase in pipeline pressure caused by easy evaporation, and the large size of the heat exchange device, it is often necessary to reduce production efficiency to meet the heat dissipation needs. Heat transfer oil has insufficient thermal stability and is prone to deterioration during long-term use, resulting in high production costs.
[0004] In order to meet the needs of large-scale and high-efficiency production, it is necessary to find a new ideal cooling medium with high heat transfer efficiency, high thermal stability and low pipeline corrosion. Summary of the invention
[0005] The purpose of the present invention is to overcome the above technical deficiencies, propose a particle-enhanced high specific heat heat transfer alloy and a preparation method thereof, and solve the technical problem that traditional cooling media in the prior art cannot take into account low cost, high heat transfer efficiency, high thermal stability and low pipeline corrosion.
[0006] In a first aspect, the present invention provides a particle-enhanced high specific heat transfer alloy, wherein the particle-enhanced high specific heat transfer alloy uses a eutectic alloy composed of low melting point metal elements such as Sn, Bi, and Zn as a matrix alloy, and uses nanoparticles as a reinforcing phase to regulate the specific heat capacity of the alloy.
[0007] In a second aspect, the present invention provides a method for preparing a particle-reinforced high specific heat heat transfer alloy, comprising the following steps:
[0008] The Sn ingot, the Bi ingot and the Zn pellets are mixed and smelted, and then cooled to obtain a matrix alloy;
[0009] The matrix alloy is made into powder, and then nanometer particles and water-soluble additives are added, mixed evenly, and then remelted and mixed, and after cooling, a particle-reinforced high specific heat heat transfer alloy is obtained.
[0010] Compared with the prior art, the beneficial effects of the present invention include:
[0011] The present invention adopts a low melting point ternary eutectic alloy as a matrix, and adds nanoparticles to specifically improve the weakness of low specific heat capacity of the alloy material. The obtained composite heat transfer alloy has the advantages of high thermal conductivity, high specific heat capacity, high thermal stability, and no safety risks. The particle-reinforced high specific heat transfer alloy is used as a heat transfer medium, which can specifically improve the weakness of low specific heat capacity of the alloy material, conduct more heat, greatly reduce the volume of the cooling device, and improve the utilization rate of the quenching pool. The composite heat transfer alloy prepared by the present invention overcomes the shortcomings of the existing quenching liquid cooling medium, and has broad application prospects with the development of the intelligent manufacturing level of the leaf spring industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 The microscopic morphology image of the particle-reinforced high specific heat heat transfer alloy in Example 1;
[0013] Figure 2 The XRD pattern of the particle-reinforced high specific heat heat transfer alloy in Example 1;
[0014] Figure 3 The DSC spectrum of the particle-reinforced high specific heat heat transfer alloy in Example 1;
[0015] Figure 4 The thermal conductivity spectrum of the particle-reinforced high specific heat transfer alloy in Example 1;
[0016] Figure 5 The microscopic morphology image of the particle-reinforced high specific heat heat transfer alloy in Example 2;
[0017] Figure 6 The XRD pattern of the particle-reinforced high specific heat heat transfer alloy in Example 2;
[0018] Figure 7 The DSC spectrum of the particle-reinforced high specific heat heat transfer alloy in Example 2;
[0019] Figure 8 The thermal conductivity spectrum of the particle-reinforced high specific heat transfer alloy in Example 2;
[0020] Fig. 9 The microscopic morphology image of the particle-reinforced high specific heat heat transfer alloy in Example 3;
[0021] Fig.10 The XRD pattern of the particle-reinforced high specific heat heat transfer alloy in Example 3;
[0022] Fig.11 The DSC spectrum of the particle-reinforced high specific heat heat transfer alloy in Example 3;
[0023] Fig.12 This is the thermal conductivity spectrum of the particle-reinforced high specific heat transfer alloy in Example 3. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0025] In a first aspect, the present invention provides a particle-enhanced high specific heat transfer alloy, wherein the particle-enhanced high specific heat transfer alloy uses a eutectic alloy composed of low melting point metal elements such as Sn, Bi, and Zn as a matrix alloy, and uses nanoparticles as a reinforcing phase to regulate the specific heat capacity of the alloy.
[0026] In this embodiment, in the above-mentioned matrix alloy, the mass fraction of Sn is 46-48wt.%, the mass fraction of Bi is 49-52wt.%, and the mass fraction of Zn is 1-3wt.%.
[0027] In this embodiment, the nanoparticles are at least one of nano-samarium oxide particles, nano-tungsten carbide particles, and nano-nickel particles. Further, the mass fraction of the nanoparticles is 0.4-1wt.% of the high specific heat heat transfer alloy. If the amount of nanoparticles added is too low, no effect will be achieved. If the amount of nanoparticles added is too high, the nanoparticles will agglomerate, the particle size will increase significantly, and the enhancement effect will be reduced. Within this content range, the obtained particle-enhanced high specific heat heat transfer alloy has the best performance.
[0028] In the present embodiment, the purity of the alloy raw material is 99.9% or more, and the average particle size of the nanoparticles is 30 to 60 nm, and further 40 nm.
[0029] The particle-reinforced high specific heat transfer alloy obtained by the present invention has a specific heat capacity that is more than twice that of the base alloy, and a thermal conductivity of 47 W·m -1 ·K -1 above.
[0030] In a second aspect, the present invention provides a method for preparing a particle-reinforced high specific heat heat transfer alloy, comprising the following steps:
[0031] S1, mixing and smelting Sn ingots, Bi ingots and Zn pellets, and obtaining a matrix alloy after cooling;
[0032] S2. The above-mentioned base alloy is made into powder, and then nanoparticles and water-soluble additives are added, mixed evenly, and then remelted and mixed, and after cooling, a particle-reinforced high specific heat heat transfer alloy is obtained.
[0033] In this embodiment, the smelting tools need to be dried before smelting. Specifically, the smelting furnace is heated to 300°C, and the graphite crucible and the metal mold are placed therein and kept warm for 10 to 20 minutes. In order to prevent the alloy solution from adhering to the inner wall of the crucible due to impurities in the crucible and the mold, affecting the composition and properties of the alloy, a layer of release agent needs to be applied to the inner wall of the crucible before the graphite crucible is placed in the pit furnace for preheating. At the same time, applying a release agent to the inner wall of the mold is also convenient for removing the alloy sample.
[0034] In this embodiment, the smelting process includes: adding a weighed Sn ingot to a lead-free tin furnace, heating it to 250-270°C, keeping it warm for 20-40 minutes, adding a weighed Bi ingot after the Sn ingot is melted, adjusting the heating temperature to 400-450°C after the Bi ingot is melted, adding Zn particles and keeping them warm until they are completely melted, adjusting the heating temperature to 400-420°C, and keeping them warm for 20-40 minutes. In this process, tools are needed to stir the alloy melt evenly. At the same time, in order to prevent the alloy from reacting with air during the melting process, activated carbon powder is used to cover the surface of the liquid metal. After the liquid alloy is mixed evenly, the activated carbon powder covering the surface of the liquid metal in the crucible is cleaned with a skimmer.
[0035] In this embodiment, after the smelting process is completed, the molten metal is quickly poured into the mold, and after it is naturally cooled to room temperature, the alloy ingot is taken out to obtain the matrix alloy.
[0036] In this embodiment, the base alloy is made into powder using a ball mill.
[0037] In this embodiment, the water-soluble additive is a composite organic liquid material having the ability to remove oxidation on the metal surface, wherein succinic acid accounts for 1.5-2wt.%, adipic acid accounts for 1.0-1.5wt.%, salicylic acid accounts for 0.5-1wt.%, and the balance is ethanol. Further, the mass fraction of the water-soluble additive is 18-20wt.% of the composite alloy powder (matrix alloy + nanoparticles).
[0038] In this embodiment, the remelting temperature is 140 to 160°C, the holding time is 10 to 20 minutes, and the remelting is carried out under an inert atmosphere (such as nitrogen, argon, etc.). If the remelting temperature is too low, the alloy cannot be melted, and the effect of uniform composition cannot be achieved; if the remelting temperature is too high, it may cause the alloying of nano Ni particles, reduce the proportion of Ni in the form of single-phase second-phase particles, and affect the strengthening effect. In addition, excessively high temperatures have adverse effects on energy consumption, labor, production costs, etc. At the same time, in this process, in order to reduce the oxidation of the alloy, the melting furnace cover needs to be covered during the smelting process, and an argon protective atmosphere needs to be added.
[0039] In this embodiment, the number of remelting is 2 to 3 times. After one remelting is completed, the material is cooled to room temperature, and after it is completely solidified, it is remelted once more before casting to ensure that the composition of the material is uniform.
[0040] Examples 1 to 3
[0041] Embodiments 1 to 3 provide a method for preparing a particle-reinforced high specific heat heat transfer alloy, comprising the following steps:
[0042] (1) All smelting tools must be dried before smelting. First, heat the smelting furnace to 300°C, put the graphite crucible and metal mold into it, and keep it warm for 10 minutes. In order to prevent the alloy solution from adhering to the inner wall of the crucible due to impurities in the crucible and mold, affecting the composition and properties of the alloy, a layer of release agent must be applied to the inner wall of the crucible before the graphite crucible is placed in the pit furnace for preheating. At the same time, applying a release agent on the inner wall of the mold is also convenient for removing the alloy sample.
[0043] (2) According to the proportion in Table 1, add the weighed Sn ingot into the lead-free tin furnace and heat it to 250-270℃ to melt, and keep it warm for 30 minutes. After the Sn ingot is melted, add the weighed Bi ingot. After the Bi ingot is melted, adjust the heating temperature to 400-450℃, add Zn particles and keep warm until it is completely melted. Use tools to stir the alloy melt evenly. At the same time, in order to prevent the alloy from reacting with air during the melting process, cover the surface of the liquid metal with activated carbon powder. Adjust the heating temperature to 400-420℃ and keep it warm for 30 minutes.
[0044] (3) After the liquid alloy is evenly mixed, use a skimmer to clean the activated carbon powder covering the surface of the liquid metal in the crucible. Then quickly pour the molten metal into a cylindrical metal mold, wait for it to cool naturally to room temperature, take out the alloy ingot, and the preparation of the matrix alloy is completed.
[0045] (4) The base alloy is made into powder by a ball mill, and the base alloy powder and nanoparticles are mixed according to the alloy design composition according to the proportion in Table 1, and a water-soluble co-solvent accounting for 18 wt.% of the total mass of the composite alloy powder is added (succinic acid accounts for 1.5 wt.%, adipic acid accounts for 1.2 wt.%, salicylic acid accounts for 0.7 wt.%, and the balance is ethanol). The paste-like composite powder is stirred for 30 minutes until it is fully mixed, and then the composite alloy powder is placed in a vacuum melting furnace with a set temperature of 150°C for remelting and mixing. In order to reduce the oxidation of the alloy, the melting furnace cover needs to be covered during the melting process, and an argon protective atmosphere is added. After keeping warm for ten minutes, it is cooled to room temperature. After complete solidification, it is remelted once and then cast to ensure that the composition of the material is uniform.
[0046] Table 1 Designed values of alloy composition of particle-reinforced high specific heat transfer alloys obtained in Examples 1 to 3
[0047]
[0048] (In Table 1, the sum of the various components of the matrix alloy is 99.5%, and the nanoparticles account for 0.5% of the total mass of the composite alloy powder (matrix alloy + nanoparticles))
[0049] Table 2 Alloy composition measurement values of particle-reinforced high specific heat transfer alloys obtained in Examples 1 to 3
[0050]
[0051] (In Table 2, the sum of the components of the particle-reinforced high specific heat heat transfer alloy is 100%).
[0052] See also Figures 1 to 12 The particle-reinforced high specific heat heat transfer alloy prepared by the present invention has a Cp of 12 Jg -1 K -1 Above, thermal conductivity is 47W·m -1 ·K -1 above.
[0053] Compared with the prior art, the beneficial effects of the present invention include:
[0054] (1) The particle-enhanced high specific heat transfer alloy of the present invention uses a ternary eutectic alloy as a matrix, and adds nanoparticles to control the specific heat capacity of the alloy, thereby greatly improving the heat transfer efficiency of the heat transfer medium and saving energy costs.
[0055] (2) The particle-reinforced high specific heat transfer alloy of the present invention has the characteristics of high specific heat capacity and high heat transfer efficiency compared with heat transfer media such as water, heat-conducting oil and liquid metal. Due to its high density and thermal conductivity, the cooling medium per unit volume can conduct more heat, and the volume of the cooling device is also greatly reduced, thereby improving the utilization rate of the quenching pool.
[0056] (3) The particle-enhanced high specific heat heat transfer alloy of the present invention adopts powder metallurgy and secondary molding to add nanoparticles into the matrix alloy to form an independent second heat-conducting phase. The raw materials are cheap, the operation method is simple, the degree of alloying is high during the preparation process, the metal oxidation is less, and the heat transfer effect per unit volume is better.
[0057] (4) The particle-reinforced high specific heat heat transfer alloy of the present invention has good high temperature stability and can be used for a long time without deterioration. The volume change before and after the phase change is small, and pipeline leakage is not likely to occur. It is safe and risk-free.
[0058] (5) The process of the present invention is simple, easy to operate, and low-cost. There is no need to modify the existing production line equipment, and it can effectively improve the efficiency of heat treatment of large quantities of leaf springs and improve the economic benefits of the enterprise.
[0059] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A particle-reinforced high specific heat heat transfer alloy, characterized in that: The particle-enhanced high specific heat transfer alloy uses a eutectic alloy composed of Sn, Bi, and Zn low melting point metal elements as a matrix alloy, and uses nanoparticles as a reinforcing phase to regulate the specific heat capacity of the alloy. The particle-enhanced high specific heat transfer alloy has a Cp of more than 12 J / (g·K) and a thermal conductivity of more than 47 W / (m·K); wherein, In the matrix alloy, the mass fraction of Sn is 46-48 wt.%, the mass fraction of Bi is 49-52 wt.%, and the mass fraction of Zn is 1-3 wt.%; The mass fraction of the nanoparticles is 0.4-1 wt.% of the total mass of the high specific heat heat transfer alloy; The particle-enhanced high specific heat heat transfer alloy is obtained by the following steps: Sn ingots, Bi ingots, and Zn particles are mixed and smelted, and a matrix alloy is obtained after cooling; the matrix alloy is made into a powder, and then nanoparticles and a water-soluble additive are added, mixed evenly, and then remelted and mixed, and a particle-enhanced high specific heat heat transfer alloy is obtained after cooling; the water-soluble additive is: 1.5-2 wt.%, succinic acid, 1.0-1.5 wt.%, adipic acid, 0.5-1 wt.%, and the balance is ethanol.
2. The particle-reinforced high specific heat heat transfer alloy according to claim 1, characterized in that: The nanoparticles are at least one of nano-samarium oxide particles, nano-tungsten carbide particles, and nano-nickel particles.
3. The particle-reinforced high specific heat heat transfer alloy according to claim 1, characterized in that: The purity of the alloy raw material is above 99.9%, and the average particle size of the nanoparticles is 30-60 nm.
4. A method for preparing a particle-reinforced high specific heat heat transfer alloy as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: The Sn ingot, the Bi ingot and the Zn pellets are mixed and smelted, and then cooled to obtain a matrix alloy; The base alloy is made into powder, and then nanoparticles and water-soluble additives are added, mixed evenly, and then remelted and mixed, and after cooling, a particle-reinforced high specific heat heat transfer alloy is obtained; Wherein, the water-soluble auxiliary agent is: succinic acid 1.5-2 wt.%, adipic acid 1.0-1.5 wt.%, salicylic acid 0.5-1 wt.%, and the balance is ethanol.
5. The method for preparing the particle-reinforced high specific heat heat transfer alloy according to claim 4, characterized in that: The smelting process includes: adding a weighed Sn ingot into a lead-free tin furnace, heating it to 250-270°C, keeping it warm for 20-40 minutes, adding a weighed Bi ingot after the Sn ingot is melted, adjusting the heating temperature to 400-450°C after the Bi ingot is melted, adding Zn particles and keeping them warm until they are completely melted, adjusting the heating temperature to 400-420°C, and keeping them warm for 20-40 minutes.
6. The method for preparing the particle-reinforced high specific heat heat transfer alloy according to claim 4, characterized in that: The mass fraction of the water-soluble additive is 18-20 wt.% of the composite alloy powder.
7. The method for preparing the particle-reinforced high specific heat heat transfer alloy according to claim 4, characterized in that: The remelting temperature is 140-160° C., the holding time is 10-20 min, the remelting is carried out under an inert atmosphere, and the number of remelting is 2-3 times.
Citation Information
Patent Citations
Low-melting-point phase change energy storage alloy with high heat conductivity, preparation process and application
CN106282734A
Preparation process of low melting point alloy thermal interface material
CN111235459A
Nano porous copper liquid metal composite thermal interface material and preparation method thereof
CN113201660A
High Transverse Thermal Conductivity Fiber Reinforced Polymeric Composites
US20120153216A1
Micro / nano particle reinforced composite solder and preparation method therefor
US20200001406A1