Electrolytes and their lithium-ion batteries

By introducing additives with P=S or P=O structures into the electrolyte of lithium-ion batteries, a stable interfacial film is formed, which solves the problem of oxidation and decomposition of high-nickel ternary materials under high voltage and improves the high-temperature storage and cycle performance of the battery.

CN116315107BActive Publication Date: 2026-11-17ZHUHAI SMOOTHWAY ELECTRONICS MATERIALS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310527758.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2026-11-17
Estimated Expiration
2043-05-11

AI Technical Summary

Technical Problem

High-nickel ternary lithium-ion batteries suffer from severe oxidation and decomposition on the cathode surface under high voltage and high temperature conditions, which accelerates the oxidation and decomposition of the electrolyte, affecting the battery's thermal stability and cycle performance.

Method used

Additives containing P=S or P=O structures are used to form a stable interface film, reduce the internal resistance of the battery, and improve the high-temperature storage and cycle performance of lithium-ion batteries.

Benefits of technology

By leveraging the low oxidation and reduction potentials of P=S or P=O bonds, they participate in the formation of CEI and SEI, thereby improving the interfacial film stability of lithium-ion batteries, reducing internal resistance, and enhancing the battery's high-temperature storage and cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116315107B_ABST
    Figure CN116315107B_ABST
Patent Text Reader

Abstract

This invention provides an electrolyte and a lithium-ion battery thereof. The electrolyte comprises a lithium salt, an organic solvent, and additives. The additives include compound A of structural formula I, II, or III, wherein R1-R2 are each independently selected from halogens, substituted or unsubstituted C1-C6 hydrocarbon groups; R3-R4 are selected from substituted or unsubstituted C1-C6 hydrocarbon groups; R5 is selected from trimethylsilyl, substituted or unsubstituted C1-C6 hydrocarbon groups; X is selected from S; Y is selected from O; Z is selected from O or S; and M is selected from an alkali metal element. Because the additives in the electrolyte of this invention have P=S or P=O structures, these two structures can form a stable interfacial film at the interface. This film has good lithium-ion conductivity, thus the lithium-ion battery of this invention exhibits superior high-temperature cycling and low-temperature discharge performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, and more particularly to an electrolyte and a lithium-ion battery thereof. Background Technology

[0002] High-nickel ternary materials, as cathode materials for lithium-ion batteries, possess characteristics such as high operating voltage, low cost, and environmental friendliness with low toxicity. Their energy density is also higher than traditional cathode materials such as LiCoO2, Li2Mn2O4, and LiFePO4. With increasing nickel content and decreasing cobalt content, the energy density of ternary materials gradually increases, and the unit cost decreases, but their thermal stability and cycle performance are inferior to low-nickel ternary materials. Conventional carbonate electrolytes will oxidize and decompose on the surface of the battery cathode at a high voltage of 4.4V. Especially under high temperature conditions, this oxidation and decomposition of the electrolyte is accelerated, simultaneously promoting the deterioration of the cathode material.

[0003] Therefore, there is an urgent need to develop an electrolyte that can reduce the oxidative decomposition of the cathode surface to protect the cathode material, extend its service life, and thus achieve excellent performance of lithium-ion batteries. Summary of the Invention

[0004] One of the objectives of this invention is to provide an electrolyte that can reduce the surface activity of the positive electrode and inhibit the oxidative decomposition of the electrolyte, thereby reducing the internal resistance of the battery and effectively improving the high-temperature storage and cycle performance of lithium-ion batteries.

[0005] The second objective of this invention is to provide a lithium-ion battery that effectively improves the high-temperature storage performance, cycle performance, and low-temperature discharge performance of the lithium-ion battery by using the above-mentioned electrolyte.

[0006] To achieve the above objectives, the present invention provides an electrolyte comprising a lithium salt, an organic solvent, and an additive, wherein the additive comprises compound A, such as structural formula I, structural formula II, or structural formula III.

[0007]

[0008]

[0009] Among them, R1-R2 are each independently selected from halogens, substituted or unsubstituted C1-C6 hydrocarbon groups; R3-R4 are each independently selected from substituted or unsubstituted C1-C6 hydrocarbon groups; R5 is selected from trimethylsilyl, substituted or unsubstituted C1-C6 hydrocarbon groups; X is selected from S; Y is selected from O; Z is selected from O or S; M is selected from alkali metal elements.

[0010] Compared with existing technologies, the additives of this invention have P=S or P=O structures, which can form stable interfacial films. Because P=S or P=O bonds have low oxidation and reduction potentials, they readily participate in the formation of CEI and SEI. Phosphorus-, oxygen-, and sulfur-containing CEI or SEI exhibit relatively superior lithium-ion conductivity, thus reducing the battery's internal resistance. Simultaneously, they possess good structural stability, preventing lithium-ion channel collapse during cycling, thereby improving cycle and low-temperature performance. The introduction of R-based side-chain structures further enhances SEI stability.

[0011] Preferably, R1-R2 are each independently selected from halogens, substituted or unsubstituted C1-C3 alkyl groups; R3-R4 are each independently selected from substituted or unsubstituted C1-C3 hydrocarbon groups; R5 is selected from substituted or unsubstituted C1-C3 alkyl groups or trimethylsilyl groups; and M is selected from Li, Na or Cs.

[0012] Preferably, R1-R2 are each independently selected from F and trifluoromethyl; R3-R4 are selected from trifluoromethyl; and R5 is selected from methyl, isopropyl, or trimethylsilyl. By introducing elements such as F and Si into the side chains of structural formula I or structural formula II, the composition of the electrode / electrolyte interface film is enriched, the structural stability of the interface film is further improved, and thus the storage performance of the lithium-ion battery is improved.

[0013] Preferably, compound A is selected from at least one of the following compounds.

[0014]

[0015]

[0016] The synthetic route for compound 1 is as follows:

[0017]

[0018] The synthetic route for compound 2 is as follows:

[0019]

[0020] The synthetic route for compound 3 is as follows:

[0021]

[0022] The synthetic route for compound 4 is as follows:

[0023]

[0024] The synthetic route for compound 5 is as follows:

[0025]

[0026] The specific synthesis methods of compounds 1-5 are the same as those in the prior art, and will not be described again in this invention.

[0027] Preferably, the mass of compound A accounts for 0.1%-5.0% of the total mass of the electrolyte, specifically but not limited to 0.1%, 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, and 5%.

[0028] Preferably, the lithium salt is one or more of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium methanesulfonate (LiCH3SO3), lithium trifluoromethanesulfonate (LiCF3SO3), lithium dioxalate borate (C4BLiO8), lithium difluorooxalate borate (C2BF2LiO4), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalate) phosphate (LiDFBP), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0029] Preferably, the concentration of the lithium salt is 0.5M-1.5M, specifically but not limited to 0.5M, 0.8M, 1.0M, 1.1M, 1.2M, 1.3M, 1.4M, and 1.5M.

[0030] Preferably, the organic solvent is one or more of chain carbonates, cyclic carbonates, carboxylic acid esters, ether compounds, and heterocyclic compounds. Specifically, the organic solvent is selected from at least one of ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), butyl acetate (n-BA), γ-butyrolactone (GBL), propyl propionate (n-PP), ethyl propionate (EP), and ethyl butyrate (EB).

[0031] Preferably, the electrolyte further includes an additive, which includes one or more of vinylene carbonate (VC), vinylene carbonate (VEC), fluoroethylene carbonate (FEC), vinyl sulfite (ES), 1,3-propanesulfonate lactone (PS), and vinyl sulfate (DTD). The additive used accounts for 0.1-5% of the total mass of the electrolyte.

[0032] A second aspect of the present invention also provides a lithium-ion battery, including a positive electrode and a negative electrode, and further including the electrolyte described above.

[0033] Preferably, the positive electrode comprises a nickel-cobalt-manganese oxide material, specifically, the nickel-cobalt-manganese oxide material is a high-nickel-cobalt-manganese oxide LiNi. x Co y Mn (1-x-y) Mz O2, where 0.6≤x<0.9, x+y≤1, 0≤z<0.08, and M is any one of Al, Mg, Zr, and Ti. Detailed Implementation

[0034] To better illustrate the purpose, technical solution, and beneficial effects of this invention, the invention will be further described below with reference to specific embodiments. It should be noted that the methods described below are further explanations of this invention and should not be construed as limiting it.

[0035] The present invention will be described in detail below. In the present invention, a lithium-ion battery includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode comprises a high-nickel cobalt-manganese oxide (LiNi). x Co y Mn (1-x-y) M z O2, wherein 0.6≤x<0.9, x+y≤1, M is one of Al, Mg, Zr, Ti, 0≤z<0.08, preferably x=0.6, y=0.2, M is Zr, z=0.03. The negative electrode is a carbon negative electrode material, a silicon negative electrode material, or a silicon-carbon negative electrode material, preferably a silicon-carbon negative electrode material (10% Si). The electrolyte includes lithium salt, organic solvent, additives, and auxiliaries, with additives accounting for 0.1%-5.0% of the total electrolyte mass. The auxiliaries are one or more of vinylene carbonate (VC), vinylene carbonate (VEC), fluoroethylene carbonate (FEC), vinyl sulfite (ES), 1,3-propanesulfonate lactone (PS), and vinyl sulfate (DTD), with auxiliaries accounting for 0.1%-5% of the total electrolyte mass. The lithium salt is one or more selected from lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium methanesulfonate (LiCH3SO3), lithium trifluoromethanesulfonate (LiCF3SO3), lithium dioxalatoborate (C4BLiO8), lithium difluorooxalatoborate (C2BF2LiO4), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalato)phosphate (LiDFBP), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), wherein the concentration of the lithium salt is 0.5M-1.5M. The organic solvent is selected from one or more selected from ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), propylene carbonate (PC), butyl acetate (n-BA), γ-butyrolactone (GBL), propyl propionate (n-PP), ethyl propionate (EP), and ethyl butyrate (EB).

[0036] Example 1

[0037] Electrolyte preparation:

[0038] In a nitrogen-filled glove box (O2 < 1 ppm, H2O < 1 ppm), ethyl propionate (EP), dimethyl carbonate (DMC), and diethyl carbonate (DEC) were mixed thoroughly in a mass ratio of 1:1:1 to obtain a mixed solvent, which was then used as an organic solvent. Additives and auxiliaries were added to obtain a mixed solution. The mixed solution was sealed and packaged and frozen in a freezer (-4°C) for 2 hours. After being removed, lithium hexafluorophosphate (LiPF6) was slowly added to the mixed solution in a nitrogen-filled glove box (O2 < 1 ppm, H2O < 1 ppm). After thorough mixing, the electrolyte was prepared.

[0039] Preparation of positive electrode:

[0040] Ternary material LiNi 0.6 Co 0.2 Mn 0.2 Zr 0.03 O2, conductive agent SuperP, binder PVDF, and carbon nanotubes (CNTs) were mixed uniformly at a mass ratio of 97.5:1.5:1:1 to prepare a lithium-ion battery positive electrode slurry of a certain viscosity. This slurry was then coated onto aluminum foil used for current collectors, with a coating weight of 324 g / m². 2 After drying at 85℃, the material is cold-pressed; then it is trimmed, cut into pieces, and slit. After slitting, it is dried at 85℃ for 4 hours under vacuum conditions, and then the tabs are welded to produce a lithium-ion battery positive electrode sheet that meets the requirements.

[0041] Preparation of negative electrode:

[0042] Artificial graphite and silicon are mixed at a mass ratio of 90:10, and then mixed with conductive agent SuperP, thickener CMC, and binder SBR (styrene-butadiene rubber latex) at a mass ratio of 95:1.5:1.0:2.5 to form a slurry. After being mixed evenly, the slurry is coated on both sides of copper foil, dried, and rolled to obtain a negative electrode sheet, thus producing a lithium-ion battery negative electrode sheet that meets the requirements.

[0043] The fabrication of lithium-ion batteries:

[0044] The positive electrode, negative electrode, and separator prepared according to the above process are stacked to form a lithium-ion battery with a thickness of 4.7 mm, a width of 55 mm, and a length of 60 mm. The battery is then vacuum-baked at 75°C for 10 hours and injected with the above-mentioned electrolyte. After standing for 24 hours, it is charged to 4.45V with a constant current of 0.1C (180 mA), and then charged at a constant voltage of 4.45V until the current drops to 0.05C (90 mA). It is then discharged to 3.0V at 0.2C (180 mA), and this charge-discharge cycle is repeated twice. Finally, the battery is charged to 3.8V at 0.2C (180 mA) to complete the fabrication of the lithium-ion battery.

[0045] The composition of the electrolytes in Examples 1-28 and Comparative Examples 1-8 is shown in Table 1. The preparation processes of the electrolytes, positive electrode sheets, negative electrode sheets, and lithium-ion batteries in Examples 2-28 and Comparative Examples 1-8 are the same as those in Example 1.

[0046] Table 1: Composition of the electrolytes in the examples and comparative examples

[0047]

[0048]

[0049]

[0050] The lithium-ion batteries prepared in Examples 1-28 and Comparative Examples 1-8 were tested for high-temperature storage, cycle performance and low-temperature discharge performance under the following conditions, and the results are shown in Table 2.

[0051] Room temperature cycle test: Under room temperature (25℃) conditions, the lithium-ion battery is charged and discharged once at 1.0C / 1.0C (battery discharge capacity is C0), with an upper limit voltage of 4.4V. Then, under room temperature conditions, it is charged and discharged for 500 cycles at 1.0C / 1.0C (battery discharge capacity is C1), and the capacity retention rate is calculated.

[0052] Capacity retention rate = (C1 / C0) * 100%

[0053] High-temperature cycling test: Under high temperature (45℃) conditions, the lithium-ion battery is charged and discharged once at 1.0C / 1.0C (battery discharge capacity is C0), with an upper limit voltage of 4.4V. Then, it is charged and discharged for 500 cycles at 1.0C / 1.0C under normal temperature conditions (battery discharge capacity is C1), and the capacity retention rate is calculated.

[0054] Capacity retention rate = (C1 / C0) * 100%

[0055] High-temperature storage test: Under normal temperature (25℃) conditions, the lithium-ion battery was charged and discharged once at 0.3C / 0.3C (the battery discharge capacity was recorded as C0), with an upper limit voltage of 4.4V; the battery was placed in a 60℃ oven for 15 days, then removed and placed in a 25℃ environment for 0.3C discharge, with the discharge capacity recorded as C1; then the lithium-ion battery was charged and discharged once at 0.3C / 0.3C (the battery discharge capacity was recorded as C2), and the capacity retention rate and capacity recovery rate were calculated.

[0056] Capacity retention rate = (C1 / C0) * 100%

[0057] Capacity recovery rate = (C2 / C0) * 100%

[0058] Low-temperature discharge test: Under normal temperature (25℃) conditions, the lithium-ion battery was charged and discharged once at 0.3C / 0.3C (the battery discharge capacity was recorded as C0), with an upper limit voltage of 4.4V; then the battery was charged to 4.4V under constant current and constant voltage conditions at 0.5C, and the battery was placed in a -20℃ oven for 4 hours. The battery was then discharged at 0.3C at -20℃ (the discharge capacity was recorded as C1), with a cutoff voltage of 3.0V. The low-temperature discharge rate was then calculated.

[0059] Low-temperature discharge rate = (C1 / C0) * 100%

[0060] Table 2: Performance Test Results of Lithium-ion Batteries

[0061]

[0062]

[0063] As shown in Table 2, compared to Comparative Examples 1-4, Examples 1-28 exhibit significantly improved low-temperature discharge performance, cycle performance, and high-temperature storage performance of lithium-ion batteries after using the additives of the present invention. This may be due to the lower oxidation and reduction potentials of P=S or P=O bonds, which readily participate in the formation of CEI and SEI. Phosphorus-, oxygen-, and sulfur-containing CEI or SEIs possess relatively superior lithium-ion conductivity, thus reducing the battery's internal resistance. Furthermore, they exhibit good structural stability, preventing the collapse of lithium-ion channels during cycling, thereby improving cycle and low-temperature performance. The introduction of the R-based side chain structure further enhances the stability of the SEI.

[0064] Comparing the data from Comparative Example 5 with Examples 1-13, Comparative Examples 6-7 with Examples 14-17, and Comparative Example 8 with Examples 18-28, it can be seen that the performance of Examples 1-28 of the present invention is significantly improved. This may be because the P=S ratio and the side chain structure enrich the elemental composition of the interface, and elements such as F and S can form a thin and dense SEI, significantly improving the protection of the electrode. At the same time, the spatial structure of the side chains can further support the structural stability of the SEI pores, and the cycle and low-temperature performance of the battery are further improved.

[0065] A comparison of Examples 1-9 and Examples 18-26 shows that adding additives to the additives of the present invention results in better cycle performance and high-temperature storage performance; adding additives other than VC significantly enhances low-temperature discharge performance; a comparison of Examples 14-18 shows that when a VC / FEC mixed additive is used in the electrolyte, the lithium-ion battery of the present invention exhibits better cycle performance and high-temperature storage performance.

[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A lithium-ion battery, comprising a positive electrode, a negative electrode, and an electrolyte, characterized in that, The charging cutoff voltage is 4.4V, and the positive electrode comprises a nickel-cobalt-manganese oxide material, wherein the nickel-cobalt-manganese oxide material is a high-nickel-cobalt-manganese oxide LiNi. x Co y Mn (1-x-y) M z O2, wherein 0.6≤x<0.9, x+y≤1, 0≤z<0.08, and M is any one of Al, Mg, Zr, and Ti; the electrolyte comprises lithium salt, organic solvent, additives, and auxiliaries; the auxiliaries are selected from vinylene carbonate and fluorovinyl carbonate; and the additives include compound A, such as structural formula I or structural formula III. R1-R2 are each independently selected from halogens, substituted or unsubstituted C1-C3 alkyl groups; R5 is selected from substituted or unsubstituted C1-C3 alkyl groups or trimethylsilyl groups; X is selected from S, Z is selected from S; M is selected from Li, Na or Cs.

2. The lithium-ion battery according to claim 1, characterized in that, Compound A is selected from at least one of compound 1, compound 2, compound 3, compound 4, compound 6, compound 7, and compound 8. 。 3. The lithium-ion battery according to claim 1, characterized in that, The mass of compound A used accounts for 0.1%-5% of the total mass of the electrolyte.

4. The lithium-ion battery according to claim 1, characterized in that, The lithium salt is one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium methanesulfonate, lithium trifluoromethanesulfonate, lithium dioxalate borate, lithium difluorooxalate borate, lithium difluorophosphate, lithium difluorobis(oxalate) phosphate, lithium difluorosulfonylimide, and lithium di(trifluoromethanesulfonylimide).

5. The lithium-ion battery according to claim 4, characterized in that, The concentration of the lithium salt is 0.5M-1.5M.

6. The lithium-ion battery according to claim 1, characterized in that, The organic solvent is one or more of chain carbonates, cyclic carbonates, carboxylic acid esters, ether compounds, and heterocyclic compounds.

Citation Information

Patent Citations

  • Composition for addition to electrolyte solutions containing silyl group-containing compound, electrolyte solution for nonaqueous electricity storage devices containing said composition, and lithium ion secondary battery containing said electrolyte solution

    CN105745779A

  • Non-aqueous electrolyte, non-aqueous electrolyte secondary battery and manufacturing method for the non-aqueous electrolyte secondary battery

    CN113054254A

  • Preparation method of lithium bis (trifluoromethyl) phosphate

    CN114685559A

  • P / S bond-containing sulfur phosphate electrolyte additive, non-aqueous electrolyte containing additive and lithium ion battery

    CN115498259A