Polystyrene / cellulose acetate / titanium dioxide fiber with porous structure and preparation method thereof
Polystyrene/cellulose acetate/titanium dioxide fibers prepared by centrifugal spinning and using ultraviolet light to form a porous structure solve the problem of insufficient permeability of existing micro-nano fibers and achieve wider applications in membrane distillation, oil and water Separation and air filtration and other fields.
Patent Information
- Application Number
- CN202310395951.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-14
AI Technical Summary
The existing micro-nanofiber preparation methods are complicated and have insufficient permeability, which limits their application in fields such as membrane distillation, oil-water separation, and air filtration.
Polystyrene/cellulose acetate/titanium dioxide fibers were prepared using a centrifugal spinning method, and ultraviolet light irradiation was used to form a porous structure on the surface of the fiber to increase the specific surface area and porosity of the fiber.
It significantly improves the permeability of the fiber and broadens its application prospects in fields such as membrane distillation, oil-water separation, and air filtration.
Smart Images

Figure HDA0004177588590000011 
Figure HDA0004177588590000012 
Figure HDA0004177588590000013
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of micro-nano fibers and relates to a porous fiber, in particular to a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure and a preparation method thereof. Background Art
[0002] Semiconductor photocatalytic materials are an important component of photocatalytic materials and play an important role in the preparation of hydrogen, treatment of water pollution, oxidation and reduction of carbon dioxide and promotion of photochemical reactions. TiO2 has the advantages of being non-toxic, inexpensive, stable and having high photocatalytic activity, making it stand out among many metal oxides and becoming one of the most promising environmentally friendly catalysts.
[0003] Polystyrene (PS) is synthesized from styrene monomers through free radical polymerization. It has the advantages of easy molding and processing, low price, etc., and is widely used in electronics, packaging materials, filtration and daily necessities. PS is used to prepare various multi-level structured micro-nano fibers due to its good spinnability, but PS fibers are not easy to decompose and have a certain impact on the environment. Cellulose acetate (CA) is non-toxic and harmless and can be degraded and regenerated. It is feasible to prepare fiber materials with good biocompatibility by compounding CA and PS. The main methods for preparing micro-nano fibers include template synthesis, phase separation, self-assembly, electrospinning, etc. Among them, the most commonly used is electrospinning. The micro-nano fiber membrane prepared by it has a large specific surface area, a small fiber diameter, and a high porosity. However, due to the disadvantages of complex manufacturing process and limited use of raw materials, its application is subject to certain restrictions.
[0004] Centrifugal spinning is a method for preparing micro-nano fibers with industrial application prospects due to its high production efficiency, wide range of raw materials, and controllable bulkiness of fiber aggregates. The equipment structure of centrifugal spinning is simple, mainly consisting of a motor at the bottom, a collecting rod, and a spinning head. Its working principle is that the solvent evaporates under the action of centrifugal force, and the spinning solution is stretched into fibers.
[0005] The porous structure of micro-nano fibers can increase the nanopore volume and specific surface area of the fibers, making them have broader application prospects in adsorption, filtration, antibacterial carriers, etc. Therefore, it is necessary to provide a new method for preparing porous micro-nano fibers. Summary of the invention
[0006] The object of the present invention is to provide a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure. The porous fiber has a larger specific surface area and porosity than the original fiber, and can effectively improve the permeability of the fiber.
[0007] The technical solution adopted by the present invention to solve its technical problem is:
[0008] A method for preparing polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure, the method comprising the following steps:
[0009] S1, mixing titanium dioxide, polystyrene, cellulose acetate and solvent DMF, stirring and dissolving to obtain a uniformly dispersed spinning solution;
[0010] In the spinning solution, the mass percentage of titanium dioxide is 1-3wt%, the sum of the mass percentages of polystyrene and acetate fiber is 23-25wt%, wherein the acetate fiber accounts for 20-40% of the total weight of polystyrene and acetate fiber;
[0011] S2, using the spinning solution prepared in S1 to perform centrifugal spinning to obtain polystyrene / cellulose acetate / titanium dioxide fibers;
[0012] S3. Irradiate the prepared fiber under a 400W ultraviolet lamp for 4-10 hours to finally obtain a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure.
[0013] The present invention utilizes the catalytic effect of titanium dioxide under ultraviolet light to etch the fiber surface, and finally prepares porous polystyrene / cellulose acetate / titanium dioxide fibers. The porous fibers prepared by the present invention have a larger specific surface area and porosity than the original fibers, and can effectively improve the permeability of the fibers, broadening their applications in the fields of membrane distillation, oil-water separation, and air filtration.
[0014] Preferably, in the spinning solution of S1, the sum of the mass percentages of polystyrene and acetate fiber is 24 wt %, wherein acetate fiber accounts for 30% of the total weight of polystyrene and acetate fiber.
[0015] Preferably, in S1, the molar mass of polystyrene is Mw=260000 g / mol, and the molar mass of cellulose acetate is Mw=100000 g / mol.
[0016] Preferably, in S1, the mass percentage of titanium dioxide (P25) is 2 wt %.
[0017] Preferably, in the centrifugal spinning of S2, the centrifugal rotation speed is 10000 rpm, the aperture of the spinning nozzle is 0.4 mm, and the collecting distance is set to 12 cm.
[0018] Preferably, in S3, the ultraviolet light irradiation time is 8 hours, at which time the porous structure of the obtained material is most obvious, and the titanium dioxide-carrying fiber surface is evenly distributed.
[0019] Preferably, the stirring conditions of S1 are: stirring at 40° C. and 600 rpm for 24 h.
[0020] A polystyrene / cellulose acetate / titanium dioxide fiber prepared by the preparation method of the invention.
[0021] Preferably, the centrifugal spinning device mainly includes a spinning head, a collecting rod and a motor. The spinning head has a built-in liquid storage chamber, a nozzle is provided on the outside, and a liquid injection hole is provided on the top. The collecting rods are evenly distributed around the spinning head. The two blades below the spinning head generate upward air turbulence to make the fibers better distributed on the collecting rods. During spinning, the spinning solution is injected from the top, the motor is started, and the solvent evaporates under the action of centrifugal force, and the spinning solution is stretched into fibers. During the spinning process, the centrifugal spinning controllable preparation of the fiber can be achieved by adjusting the speed of the centrifuge (0-12000r / min) and the distance from the collecting rod to the spinning head (8-12cm).
[0022] Description of the principle of the present invention:
[0023] The present invention uses polystyrene and cellulose acetate as raw materials, titanium dioxide as added nanoparticles, and uses a centrifugal spinning method to prepare polystyrene / cellulose acetate / titanium dioxide fibers, and then irradiates the prepared fibers under 400W ultraviolet light to finally obtain fibers with a porous structure. Under irradiation with 400W ultraviolet light, titanium dioxide has a catalytic effect and produces an etching effect on cellulose acetate, resulting in a hole structure on the fiber surface.
[0024] Compared with the prior art, the present invention has the following characteristics:
[0025] 1. The centrifugal spinning technology used in the present invention is simple to operate, has high yield, and controllable conditions during the reaction process;
[0026] 2. The present invention utilizes the photocatalytic etching effect of titanium dioxide under ultraviolet light on cellulose acetate to form a porous structure, and the degree of the porous structure is regulated by the irradiation time. The prepared porous fibers have a larger specific surface area and porosity than the original fibers, which can effectively improve the permeability of the fibers and broaden their applications in membrane distillation, oil-water separation, and air filtration. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a schematic diagram of a centrifugal spinning device used in the present invention;
[0028] Figure 2 These are scanning electron micrographs of polystyrene / cellulose acetate fibers prepared in Example 1 of the present invention at different mass ratios: (a) 6:4, (b) 7:3, (c) 8:2;
[0029] Figure 3 The scanning electron micrographs of polystyrene / cellulose acetate fibers at different weight percentages prepared in Example 2 of the present invention are: (a) 23 wt %, (b) 24 wt %, (c) 25 wt %;
[0030] Figure 4 The scanning electron micrographs of polystyrene / cellulose acetate / titanium dioxide fibers prepared in Example 3 of the present invention at different titanium dioxide mass percentages are (a) 1wt%, (b) 2wt%, and (c) 3wt%;
[0031] Figure 5 is a scanning electron microscope image of porous polystyrene / cellulose acetate / titanium dioxide fiber prepared in Example 4 of the present invention;
[0032] Figure 6 is a scanning electron microscope image of porous polystyrene / cellulose acetate / titanium dioxide fiber prepared in Example 5 of the present invention;
[0033] Figure 7 is a scanning electron microscope image of porous polystyrene / cellulose acetate / titanium dioxide fiber prepared in Example 6 of the present invention;
[0034] Figure 8 This is a scanning electron microscope image of the porous polystyrene / cellulose acetate / titanium dioxide fiber prepared in Example 7 of the present invention. DETAILED DESCRIPTION
[0035] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0036] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0037] The present invention is now further described in conjunction with specific examples. The following examples are only for explaining the present invention, but do not constitute a limitation of the present invention. The test samples and test processes used in the following examples include the following (if the specific experimental conditions are not indicated in the examples, they are usually in accordance with conventional conditions or the conditions recommended by the reagent company; the reagents, consumables, etc. used in the following examples, if not otherwise specified, can all be obtained from commercial channels).
[0038] The present invention adopts centrifugal spinning technology, uses polystyrene and cellulose acetate as carriers, and titanium dioxide as added nanoparticles to prepare micro-nano fibers, and uses ultraviolet irradiation to etch the fiber surface, and finally obtains porous polystyrene / cellulose acetate / titanium dioxide fibers. The porous structure of the polystyrene / cellulose acetate / titanium dioxide fibers can be controlled by adjusting the ultraviolet irradiation time.
[0039] Example 1 (Study on the mass ratio of polystyrene and cellulose acetate)
[0040] A method for preparing a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure, comprising the following steps:
[0041] (1) Polystyrene and cellulose acetate were weighed in a mass ratio of 6:4, 7:3, and 8:2, respectively (1.44 g, 0.96 g), (1.68 g, 0.72 g), and (1.92 g, 0.48 g), added to DMF, and stirred at 40°C and 600 rpm for 24 h. The sum of the mass percentages of polystyrene / cellulose acetate was 24 wt %, and the spinning solution was used.
[0042] (2) Adoption Figure 1 The spinning was carried out in a centrifugal spinning device, the speed of the centrifuge was set to 10000 r / min, the spinneret aperture of the spinning head was 0.4 mm, the distance of the collecting rod was 12 cm, 5 ml of the prepared spinning solution was added to the spinning head, and the polystyrene / cellulose acetate / titanium dioxide fiber was obtained by collecting the collecting rod. Figure 2 As shown in the figure, when the ratio of PS / CA is 6:4, the fiber thickness is uneven and there are droplets. The reason is that PS is a linear polymer, and CA is a cyclic polymer with more branches. As the content of CA increases, the viscosity of the solution decreases and the morphology is poor. When the ratio of PS / CA is 8:2, the fiber is thick and uneven. When the ratio of PS / CA is 7:3, the fiber thickness is uniform and the morphology is better.
[0043] Example 2 (Study on the sum of the mass percentages of polystyrene and acetate fiber in the spinning solution)
[0044] A method for preparing a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure, comprising the following steps:
[0045] (1) Polystyrene and cellulose acetate were weighed in a mass ratio of 7:3 (1.61 g, 0.69 g), (1.68 g, 0.72 g), and (1.75 g, 0.75 g), respectively, and added into DMF. The mixture was stirred at 40°C and 600 rpm for 24 h until the sum of the mass percentages of polystyrene / cellulose acetate was 23 wt%, 24 wt%, and 25 wt%, respectively, and the spinning solution was used as the spinning solution.
[0046] (2) Adoption Figure 1 The spinning was carried out in a centrifugal spinning device, the speed of the centrifuge was set to 10000 r / min, the spinneret aperture of the spinning head was 0.4 mm, the distance of the collecting rod was 12 cm, 5 ml of the prepared spinning solution was added to the spinning head, and the polystyrene / cellulose acetate / titanium dioxide fiber was obtained by collecting the collecting rod. Figure 3 As shown in the figure, when the sum of the mass percentages of polystyrene / cellulose acetate is 23wt%, the fiber morphology is poor, the entanglement between the molecular chains is restricted, the spinning is uneven and droplets are generated. When the sum of the mass percentages of polystyrene / cellulose acetate is 25wt%, the prepared fibers are uneven, the viscosity of the solution is large, and the spinning amount is also small. When the sum of the mass percentages of polystyrene / cellulose acetate is 24wt%, the prepared fibers are uniform in thickness and have a good morphology.
[0047] Example 3 (Study on the amount of titanium dioxide used)
[0048] A method for preparing a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure, comprising the following steps:
[0049] (1) Weigh 0.1 g, 0.2 g, and 0.3 g of titanium dioxide, respectively, and add them to DMF. Weigh 1.68 g and 0.72 g of polystyrene and cellulose acetate, respectively, in a mass ratio of 7:3. Add the two to three mixed solutions, respectively, and stir at 40°C and 600 rpm for 24 h. The sum of the mass percentages of polystyrene / cellulose acetate is 24 wt%, and the mass percentages of titanium dioxide are 1 wt%, 2 wt%, and 3 wt%, respectively, which are used as spinning solutions.
[0050] (2) Adoption Figure 1 The spinning was carried out in a centrifugal spinning device, the speed of the centrifuge was set to 10000 r / min, the spinneret aperture of the spinning head was 0.4 mm, the distance of the collecting rod was 12 cm, 5 ml of the prepared spinning solution was added to the spinning head, and the polystyrene / cellulose acetate / titanium dioxide fiber was obtained by collecting the collecting rod. Figure 4As shown in the figure, when the mass fraction of titanium dioxide is 1wt%, there are fewer titanium dioxide particles distributed on the fiber surface. When the mass fraction of titanium dioxide is 2wt%, the content of titanium dioxide particles on the fiber surface increases and is evenly distributed. When the mass fraction of titanium dioxide is 3wt%, the content of titanium dioxide particles on the fiber surface is too much and is unevenly distributed and agglomerates.
[0051] Example 4 (Investigation of irradiation time)
[0052] A method for preparing a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure, comprising the following steps:
[0053] (1) Weigh 0.2 g of titanium dioxide and add it to 7.4 g of DMF. Weigh 1.68 g of polystyrene and 0.72 g of cellulose acetate in a mass ratio of 7:3, respectively. Add the two to the mixed solution, and stir at 40°C and 600 rpm for 24 h. The sum of the mass percentages of polystyrene / cellulose acetate is 24 wt%, and the mass percentage of titanium dioxide is 2 wt%. This is used as the spinning solution.
[0054] (2) Adoption Figure 1 The spinning was carried out using a centrifugal spinning device, with the centrifuge speed set to 10000 r / min, the spinneret aperture of the spinning head to 0.4 mm, the collecting rod distance to 12 cm, 5 ml of the prepared spinning solution was added to the spinning head, and the polystyrene / cellulose acetate / titanium dioxide fiber was obtained by receiving it through the collecting rod.
[0055] (3) The prepared polystyrene / cellulose acetate / titanium dioxide fiber was placed under 400 W ultraviolet light for 4 h to obtain a polystyrene / cellulose acetate / titanium dioxide fiber with a less porous structure, whose surface structure is as follows: Figure 5 As shown, the porous structure of the fiber surface is not obvious at this time.
[0056] Example 5 (Investigation of irradiation time)
[0057] A method for preparing a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure, comprising the following steps:
[0058] Steps (1) and (2) are the same as those in Example 4 (1) and (2). (3) The prepared polystyrene / cellulose acetate / titanium dioxide fiber is placed under 400W ultraviolet light for 6 hours. The surface structure of the polystyrene / cellulose acetate / titanium dioxide fiber is as follows: Figure 6 As shown, the porous structure of the fiber surface increases but is still not obvious.
[0059] Embodiment 6 (best embodiment)
[0060] A method for preparing a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure, comprising the following steps:
[0061] Steps (1) and (2) are the same as those in Example 4 (1) and (2).
[0062] Step (3), placing the prepared polystyrene / cellulose acetate / titanium dioxide fiber under 400W ultraviolet light for 8 hours, the surface structure of the polystyrene / cellulose acetate / titanium dioxide fiber is as follows: Figure 7 As shown, the porous structure of the fiber surface is obvious and the titanium dioxide is evenly distributed.
[0063] Example 7 (Investigation of irradiation time)
[0064] A method for preparing a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure, comprising the following steps:
[0065] Steps (1) and (2) are the same as those in Example 4 (1) and (2). (3) The prepared polystyrene / cellulose acetate / titanium dioxide fiber is placed under 400W ultraviolet light for 10 hours. The surface structure of the polystyrene / cellulose acetate / titanium dioxide fiber is as follows: Figure 8 As shown, with the increase of UV irradiation time, the etching effect of titanium dioxide on cellulose acetate increases, resulting in increased exposure of titanium dioxide and agglomeration, and the porous structure is also reduced.
[0066] The above embodiment adjusts the degree of the porous structure of the fiber by adjusting the length of time for which the fiber is irradiated with ultraviolet light. As the ultraviolet light irradiation time increases from 4 hours to 10 hours, the porous structure of the fiber becomes gradually more obvious.
[0067] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0068] The above is a detailed introduction to a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure and a preparation method thereof provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a porous polystyrene / cellulose acetate / titanium dioxide fiber, characterized in that The method comprises the following steps: S1, mixing titanium dioxide, polystyrene, cellulose acetate and solvent DMF, stirring and dissolving to obtain a uniformly dispersed spinning solution; In the spinning solution, the mass percentage of titanium dioxide is 1-3wt%, the sum of the mass percentages of polystyrene and cellulose acetate is 23-25wt%, wherein cellulose acetate accounts for 20-40wt% of the total weight of polystyrene and cellulose acetate; S2, using the spinning solution prepared in S1 to perform centrifugal spinning to obtain polystyrene / cellulose acetate / titanium dioxide fibers; S3. Irradiate the prepared fiber under a 400W ultraviolet lamp for 4-10 hours to finally obtain a polystyrene / cellulose acetate / titanium dioxide fiber with a porous structure.
2. The preparation method according to claim 1, characterized in that: In the spinning solution of S1, the sum of the mass percentages of polystyrene and cellulose acetate is 24 wt %, of which cellulose acetate accounts for 30% of the total weight of polystyrene and cellulose acetate.
3. The preparation method according to claim 1, characterized in that: In S1, the molar mass of polystyrene is Mw = 260000 g / mol, and the molar mass of cellulose acetate is Mw = 100000 g / mol.
4. The preparation method according to claim 1, characterized in that: In S1, the mass percentage of titanium dioxide is 2 wt %.
5. The preparation method according to claim 1, characterized in that: In the centrifugal spinning of S2, the centrifugal rotation speed was 10000 rpm, the aperture of the spinning nozzle was 0.4 mm, and the collection distance was set to 12 cm.
6. The preparation method according to claim 1, characterized in that: In S3, the UV irradiation time is 8 h, at which time the porous structure of the obtained material is most obvious, and titanium dioxide is evenly distributed on the fiber surface.
7. The preparation method according to claim 1, characterized in that: The stirring conditions of S1 were: stirring at 40°C and 600 rpm for 24 h.
8. A polystyrene / cellulose acetate / titanium dioxide fiber prepared by the preparation method according to claim 1.
Citation Information
Patent Citations
Preparation method, product and application of antibacterial porous fiber with orientation pore structure
CN110512300A
Process for production of monosaccharide and process for production of ethanol both utilizing cellulose-based substance
US20100167368A1
Cited By
Preparation method of super-porous polymer fiber
CN121407244A