Acid liquid thickener and preparation method thereof

By adding specific monomers to the acid liquid thickening agent for copolymerization, the insufficient performance of the acid liquid thickening agent in high temperature, high mineralization and shear environment was solved, and excellent shear resistance and temperature resistance were prepared. A thickener with salt resistance, suitable for deep acidification and transformation.

CN116693744BActive Publication Date: 2024-11-01SHANDONG NUOER BIOLOGICAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310839727.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-10
Publication Date
2024-11-01
Estimated Expiration
2043-07-10

AI Technical Summary

Technical Problem

The existing acid liquid thickening agents have poor temperature and salt resistance and poor shear resistance under high temperature, high mineralization and shear environments, which are difficult to meet the needs of deep acidification transformation.

Method used

Excellent resistance was prepared by mixing acrylamide, methacryloyloxyethyltrimethylammonium chloride, 3,4-dihydroxycinnamic acid, anti-salt monomer and rigid monomer in water and copolymerization reaction. Acid liquid thickening agent with shear, temperature and salt resistance.

Benefits of technology

The prepared acid liquid thickening agent has good water solubility, acid resistance and high temperature stability. It can maintain excellent thickening effect and shear recovery ability in high-mineralization brine, and is suitable for deep acidification transformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004891485630000101
    Figure GDA0004891485630000101
  • Figure GDA0004891485630000111
    Figure GDA0004891485630000111
Patent Text Reader

Abstract

The invention provides an acid liquid thickener and a preparation method thereof, and relates to the field of oil field technology. The method comprises: placing acrylamide, methacryloyloxyethyl trimethylammonium chloride, 3,4-dihydroxycinnamic acid, a salt-resistant monomer, and a rigid monomer in water and mixing them uniformly to obtain a mixed solution; adding an initiator to the mixed solution for copolymerization to obtain the acid liquid thickener. The acid liquid thickener prepared by the invention has excellent shear resistance, temperature resistance, and salt resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil fields, and in particular to an acid liquid thickener and a preparation method thereof. Background Art

[0002] Fracturing acidification transformation technology is one of the important technical means for major oil fields to achieve oil and gas well reservoir transformation, production increase and water well injection. It uses acid to remove the pollution of oil and gas well reservoirs to restore the permeability of underground reservoirs, thereby achieving the purpose of increasing production and injection. Deep acidification is mainly to prevent the loss of acid on the fracture surface, and the loss of acid on the fracture surface forms acid corrosion holes. Therefore, acid with considerable viscosity can effectively slow down its loss rate, thereby increasing the effective acid corrosion distance.

[0003] The polymer thickener added to the acid can effectively increase the viscosity of the acid system, thereby effectively reducing the diffusion rate of hydrogen ions to the surface of the reservoir rock, thereby reducing the acid loss and acid-rock reaction rate, increasing the effective action distance of the acid, and facilitating deep acidification in the deep fractures of the seepage rock.

[0004] With the advancement of oil exploration technology, the development of oil and gas resources continues to develop in depth, drilling is getting deeper and deeper, and the temperature of the reservoir that needs to be transformed is getting higher and higher. In order to match the fracturing transformation of high-temperature oil and gas reservoirs, higher requirements are placed on the temperature and shear resistance of thickeners. However, the current acid thickeners are greatly affected by high temperature, high mineralization, and shear. In actual applications, there are still problems such as poor temperature and salt resistance and poor shear resistance. Summary of the invention

[0005] The embodiment of the present invention provides an acid liquid thickener and a preparation method thereof. The acid liquid thickener has excellent shear resistance, temperature resistance and salt resistance.

[0006] In a first aspect, the present invention provides a method for preparing an acid liquid thickener, the preparation method comprising:

[0007] Acrylamide, methacryloyloxyethyl trimethylammonium chloride, 3,4-dihydroxycinnamic acid, salt-resistant monomer and rigid monomer are placed in water and mixed evenly to obtain a mixed solution; an initiator is added to the mixed solution to carry out copolymerization reaction to obtain the acid liquid thickener.

[0008] Preferably, the salt-resistant monomer comprises a sulfonic acid group, a benzene ring and a carbon-carbon double bond, and the benzene ring carries a sulfonic acid group.

[0009] Preferably, the rigid monomer comprises a benzene ring and a single heterocyclic ring.

[0010] Preferably, the salt-resistant monomer is 4,4'-diaminostilbene-2,2'-disulfonic acid or 4,4'-dihydrazinostilbene-2,2'-disulfonic acid.

[0011] Preferably, the rigid monomer is 4-acrylamidebenzo-15-crown-5 or styryl boric acid diethanolamine ester.

[0012] Preferably, the weight proportions of the components for preparing the acid liquid thickener are as follows: 90-110 parts of acrylamide, 360-440 parts of methacryloyloxyethyltrimethylammonium chloride, 20-30 parts of 3,4-dihydroxycinnamic acid, 8-15 parts of salt-resistant monomer, 6-10 parts of rigid monomer, 395-516 parts of water and 0.02-0.036 parts of initiator.

[0013] Preferably, the initiation temperature of the copolymerization reaction is 0-5°C, and the reaction time is 3-5h.

[0014] Preferably, the preparation method further comprises:

[0015] The pH of the mixed solution is adjusted to 3-4.

[0016] More preferably, a pH adjuster is used to adjust the pH of the mixed solution.

[0017] Preferably, the pH adjuster is at least one of adipic acid, aminosulfonic acid and citric acid.

[0018] Preferably, the preparation method further comprises:

[0019] After nitrogen is introduced into the mixed solution, the initiator is added to carry out copolymerization reaction.

[0020] More preferably, the nitrogen is introduced for 30 to 50 minutes.

[0021] Preferably, the initiator is an azo initiator and a redox initiator including an oxidant and a reductant.

[0022] Preferably, the mass ratio of the azo initiator, the oxidant and the reducing agent is (0.01-0.02):(0.005-0.008):(0.005-0.008).

[0023] More preferably, the azo initiator is at least one of VA-044 initiator, azobisisobutyronitrile, and V-50 initiator.

[0024] More preferably, the oxidant is at least one of sodium persulfate, potassium persulfate, and ammonium persulfate;

[0025] The reducing agent is at least one of sodium sulfite, sodium bisulfite, sodium pyrosulfite and ammonium ferrous sulfate.

[0026] In a second aspect, the present invention provides an acid liquid thickener prepared by any preparation method described in the first aspect.

[0027] Compared with the prior art, the present invention has at least the following beneficial effects:

[0028] The acid liquid thickener prepared by the present invention includes hydrogen ion insensitive groups: cationic groups and hydroxyl groups, so that the prepared thickener has acid resistance and is suitable for acid liquid thickener. The hydroxyl group is introduced by adding 3,4-dihydroxycinnamic acid, and the hydroxyl group is a strong hydrophilic group, so that the polymer has good solubility in water; at the same time, the benzene ring is introduced to increase the strength of the molecular chain, and improve the shear resistance and temperature resistance of the acid liquid thickener.

[0029] In the present invention, in the preparation of the acid liquid thickener, due to the addition of salt-resistant monomers and rigid monomers, the acid liquid thickener molecular chain carries large groups such as benzene rings and single heterocycles, which improves the rigidity of the molecular chain and further enhances its shear resistance; at the same time, the benzene ring and the single heterocycle have hydrophobic properties, and the association of the hydrophobic group can occur within the molecule or between molecules, that is, intramolecular association and intermolecular association. Through the interlaced association of the hydrophobic groups, a spatial network structure is formed, and the polymer molecular chain produces hydrophobic association micro-regions. The spatial network structure formed between molecules achieves a viscosity-increasing effect, so that the rigidity of the polymer molecular chain and the hydrophobic association jointly improve the thermal stability of the polymer; in addition, the association also makes the thickener have excellent shear resistance, shear dilution and shear recovery ability. In addition, the benzene ring of the salt-resistant monomer also carries two sulfonic acid groups, which are salt-resistant and hydrolysis-resistant groups, which improve the salt resistance of the polymer. At the same time, the sulfonic acid group is also a hydrophilic group, which ensures the solubility of the polymer. The acid liquid thickener prepared by the present invention comprises an amide group, a cationic group and a hydroxyl group, and these groups are hydrophilic groups, so that the acid liquid thickener has good water solubility in water. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0031] The present invention provides a method for preparing an acid liquid thickener, the preparation method comprising:

[0032] Acrylamide, methacryloyloxyethyl trimethylammonium chloride, 3,4-dihydroxycinnamic acid, salt-resistant monomer and rigid monomer are placed in water and mixed evenly to obtain a mixed solution; an initiator is added to the mixed solution to carry out copolymerization reaction to obtain the acid liquid thickener.

[0033] The present invention prepares a cationic polyacrylamide acid thickener through copolymerization, and has excellent thickening effect, excellent shear resistance, temperature resistance and salt resistance. By adding 3,4-dihydroxycinnamic acid to introduce hydroxyl groups, the hydroxyl groups are strong hydrophilic groups, so that the acid thickener polymer has good solubility in water; and the hydroxyl groups are hydrogen ion insensitive groups, have good acid resistance, and improve the acid resistance of the polymer; at the same time, the benzene ring is introduced to increase the strength of the molecular chain, and improve the shear resistance and temperature resistance of the acid thickener.

[0034] According to some preferred embodiments, the salt-resistant monomer comprises a sulfonic acid group, a benzene ring and a carbon-carbon double bond, and the benzene ring carries a sulfonic acid group.

[0035] According to some preferred embodiments, the rigid monomer comprises a benzene ring and a single heterocyclic ring.

[0036] In the present invention, due to the addition of salt-resistant monomers and rigid monomers, the acid liquid thickener molecular chain carries large groups such as benzene rings and single heterocycles, which improves the rigidity of the molecular chain and further enhances its shear resistance; at the same time, the benzene ring and the single heterocycle have hydrophobic properties, and the association of hydrophobic groups can occur within the molecule or between molecules, that is, intramolecular association and intermolecular association. The hydrophobic groups are intertwined with each other to form a spatial network structure, and the polymer molecular chain produces hydrophobic association micro-regions. The spatial network structure formed between molecules achieves a viscosity-increasing effect. In this way, the rigidity of the polymer molecular chain and the hydrophobic association jointly improve the thermal stability of the polymer; in addition, the association also makes the thickener have excellent shear resistance, shear thinning and shear recovery capabilities.

[0037] In the present invention, the benzene ring of the salt-resistant monomer also carries a sulfonic acid group, which is a salt-resistant and hydrolysis-resistant group, improving the salt-resistant property of the polymer, and the sulfonic acid group is also a hydrophilic group, ensuring the solubility of the polymer. At the same time, the acid liquid thickener includes an amide group, a cationic group, and a hydroxyl group, which are hydrophilic groups, so that the acid liquid thickener has good water solubility in water.

[0038] According to some preferred embodiments, the salt-resistant monomer is 4,4'-diaminostilbene-2,2'-disulfonic acid or 4,4'-dihydrazinostilbene-2,2'-disulfonic acid.

[0039] According to some preferred embodiments, the rigid monomer is 4-acrylamidebenzo-15-crown-5 or styryl boric acid diethanolamine ester.

[0040] In the present invention, the benzene ring of the salt-resistant monomer carries two sulfonic acid groups, which further improves the salt-resistant property of the acid liquid thickener and the solubility of the acid liquid thickener in water or salt water.

[0041] According to some preferred embodiments, the weight parts of the components for preparing the acid liquid thickener are as follows: 90-110 parts of acrylamide (for example, 90 parts, 91 parts, 95 parts, 100 parts, 105 parts, 108 parts or 110 parts), 360-440 parts of methacryloyloxyethyl trimethyl ammonium chloride (for example, 360 parts, 365 parts, 370 parts, 375 parts, 380 parts, 385 parts, 390 parts, 395 parts, 400 parts, 405 parts, 410 parts, 415 parts, 420 parts, 425 parts, 430 parts, 435 parts or 440 parts), 20-30 parts of 3,4-dihydroxycinnamic acid (for example, 20 parts, 22 parts, 24 parts, 25 parts, 26 parts, 28 parts or 30 parts) ), 8-15 parts of salt-resistant monomer (for example, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts), 6-10 parts of rigid monomer (for example, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts or 10 parts), 395-516 parts of water (for example, 395 parts, 400 parts, 410 parts, 420 parts, 450 parts, 480 parts, 500 parts, 505 parts, 510 parts or 516 parts) and 0.02-0.036 parts of initiator (for example, 0.02 parts, 0.03 parts, 0.05 parts, 0.1 parts, 0.15 parts, 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts or 0.036 parts).

[0042] In the present invention, it has been experimentally confirmed that when the dosage of other components remains unchanged, 3,4-dihydroxycinnamic acid is limited to 20-30 parts. If the dosage of 3,4-dihydroxycinnamic acid is too little, the acid resistance of the prepared thickener cannot meet the requirements; if the dosage of 3,4-dihydroxycinnamic acid is too much, the molecular weight of the prepared acid liquid thickener will be greatly reduced due to the introduction of too many benzene rings, affecting its performance in acid fracturing. When the dosage of other components remains unchanged, the salt-resistant monomer is limited to 8-15 parts. If the dosage of the salt-resistant monomer is too little, the prepared acid liquid thickener has poor salt resistance and poor shear resistance; if the dosage of the salt-resistant monomer is too much, the solubility of the prepared acid liquid thickener is poor, and the molecular weight will also be greatly reduced, affecting its performance in acid fracturing. When the dosage of other components remains unchanged, the rigid monomer is limited to 6 to 10 parts. If the dosage of the rigid monomer is too small, the prepared acid liquid thickener will have poor shear resistance and thermal stability; if the dosage of the rigid monomer is too large, the solubility of the prepared acid liquid thickener will deteriorate and the molecular weight will be greatly reduced, affecting its performance in acid fracturing.

[0043] According to some preferred embodiments, the initiation temperature of the copolymerization reaction is 0-5°C (for example, it can be 0°C, 0.5°C, 1°C, 1.5°C, 2°C, 2.5°C, 3°C, 3.5°C, 4°C, 4.5°C or 5°C), and the reaction time is 3-5h (for example, it can be 3h, 3.5h, 4h, 4.5h or 5h).

[0044] According to some preferred embodiments, the preparation method further comprises: adjusting the pH of the mixed solution to 3-4 (for example, 3, 3.2, 3.4, 3.5, 3.6, 3.8 or 4).

[0045] In the present invention, it has been experimentally confirmed that the pH of the mixed solution is adjusted to 3-4, so that the acidity and alkalinity of the reaction medium can be prevented from affecting the decomposition rate of the initiator and the polymerization degree of the acid liquid thickener can be ensured.

[0046] According to some more preferred embodiments, a pH adjuster is used to adjust the pH of the mixed solution.

[0047] According to some preferred embodiments, the pH adjuster is at least one of adipic acid, aminosulfonic acid, and citric acid.

[0048] It should be noted that at least one is any one or a mixture of any several in any proportion.

[0049] According to some more preferred embodiments, the preparation method further comprises:

[0050] After nitrogen is introduced into the mixed solution, the initiator is added to carry out copolymerization reaction.

[0051] According to some more preferred embodiments, the time for introducing nitrogen is 30 to 50 min (for example, 30 min, 35 min, 40 min, 45 min or 50 min).

[0052] In the present invention, since oxygen, as an inhibitor, will affect the polymerization reaction of polyacrylamide, nitrogen needs to be introduced to remove oxygen to ensure that the polymerization reaction proceeds normally.

[0053] According to some more preferred embodiments, the preparation method of the acid liquid thickener specifically includes: adding acrylamide, methacryloyloxyethyltrimethylammonium chloride, 3,4-dihydroxycinnamic acid, a salt-resistant monomer, and a rigid monomer into water and mixing them evenly to obtain a mixed solution; using a pH regulator to adjust the pH of the mixed solution to 3-4, adding the mixed solution to a reactor and passing nitrogen for 30-50 minutes, and then adding an initiator to initiate a copolymerization reaction at 0-5°C to obtain a colloidal acid liquid thickener.

[0054] It should be noted that in application, the acid liquid thickener in the colloidal state obtained by the present invention needs to be granulated, dried, ground, sieved and then packaged, which is more convenient for storage and transportation and can further reduce transportation costs.

[0055] According to some preferred embodiments, the initiator is an azo initiator and a redox initiator comprising an oxidant and a reductant.

[0056] According to some preferred embodiments, the mass ratio of the azo initiator, the oxidant and the reducing agent is (0.01-0.02):(0.005-0.008):(0.005-0.008).

[0057] According to some more preferred embodiments, the azo initiator is at least one of VA-044 initiator, azobisisobutyronitrile, and V-50 initiator.

[0058] According to some more preferred embodiments, the oxidant is at least one of sodium persulfate, potassium persulfate, and ammonium persulfate;

[0059] The reducing agent is at least one of sodium sulfite, sodium bisulfite, sodium pyrosulfite and ammonium ferrous sulfate.

[0060] In the present invention, the composite initiator can increase the temperature of the reaction system by utilizing the heat released by the redox initiator when initiating the polymerization reaction at low temperature, thereby causing the azo initiator to decompose and generate free radicals to continuously initiate the polymerization reaction, thereby reducing energy consumption and increasing the copolymerization reaction conversion rate and the molecular weight of the polymer.

[0061] In the present invention, water is used as the reaction medium of the polymerization reaction, which not only has low cost, but also can eliminate the impact of organic solvents on environmental pollution, the preparation process is simple, and the reaction exothermicity does not require heating. In addition, the environment of the reaction medium is neutral, the preparation process is environmentally friendly, pollution-free, low in energy consumption, the product is non-toxic and non-corrosive, and no secondary pollution is generated, which is in line with the development direction of green environmental protection chemical additives.

[0062] In the present invention, by limiting the number of components used in the acid liquid thickener, the dissolution time of the dry powder acid liquid thickener obtained after granulation and drying in water or brine does not exceed 30 minutes. In the actual field application process, the time utilization rate is improved and the production cost is reduced.

[0063] The present invention also provides an acid liquid thickener, which is prepared by the preparation method provided by the present invention.

[0064] In order to more clearly illustrate the technical solution and advantages of the present invention, an acid liquid thickener and a preparation method thereof are described in detail below through several embodiments.

[0065] In the following examples, the masses of acrylamide, methacryloyloxyethyltrimethylammonium chloride, 3,4-dihydroxycinnamic acid, salt-resistant monomer, rigid monomer, water and initiator are expressed in parts by weight.

[0066] Example 1

[0067] 90 parts of acrylamide, 360 parts of methacryloyloxyethyl trimethylammonium chloride, 20 parts of 3,4-dihydroxycinnamic acid, 8 parts of 4,4'-diaminostilbene-2,2'-disulfonic acid, 6 parts of 4-acrylamidebenzo-15-crown-5, and 516 parts of deionized water were added into a beaker and mixed evenly, and then the pH value of the solution was adjusted to 3.0 with adipic acid; after the temperature of the solution system was cooled to 0°C, all of it was poured into a reactor, and nitrogen was introduced for deoxygenation for 30 minutes, and then 0.01 parts of VA-044 initiator, 0.008 parts of sodium persulfate, and 0.005 parts of sodium bisulfite were added, and nitrogen was continued to be introduced for 10 minutes, and then the beaker was sealed and reacted for 4.5 hours. After the reaction was completed, an acid thickener was obtained.

[0068] Example 2

[0069] 95 parts of acrylamide, 370 parts of methacryloyloxyethyl trimethylammonium chloride, 22 parts of 3,4-dihydroxycinnamic acid, 9 parts of 4,4'-diaminostilbene-2,2'-disulfonic acid, 7 parts of 4-acrylamidebenzo-15-crown-5, and 497 parts of deionized water were added into a beaker and mixed evenly, and then the pH value of the solution was adjusted to 3.5 with aminosulfonic acid; after the temperature of the solution system was cooled to 2°C, all of it was poured into a reactor, and nitrogen was introduced for deoxygenation for 30 minutes, and then 0.015 parts of azobisisobutyronitrile, 0.008 parts of potassium persulfate, 0.005 parts of sodium bisulfite, and 0.002 parts of ammonium ferrous sulfate were added, and nitrogen was continued to be introduced for 10 minutes, and then the beaker was sealed and reacted for 4 hours. After the reaction was completed, an acid thickener was obtained.

[0070] Example 3

[0071] 100 parts of acrylamide, 380 parts of methacryloyloxyethyl trimethylammonium chloride, 25 parts of 3,4-dihydroxycinnamic acid, 10 parts of 4,4'-diaminostilbene-2,2'-disulfonic acid, 8 parts of 4-acrylamidebenzo-15-crown-5, and 477 parts of deionized water were added into a beaker and mixed evenly, and then the pH value of the solution was adjusted to 3.7 with citric acid; after the temperature of the solution system was cooled to 3°C, all of it was poured into a reactor, and nitrogen was introduced for deoxygenation for 30 minutes, and then 0.012 parts of V-50 initiator, 0.007 parts of ammonium persulfate, and 0.005 parts of sodium pyrosulfite were added, and nitrogen was continued to be introduced for 10 minutes, and then the beaker was sealed and reacted for 3.5 hours. After the reaction was completed, an acid thickener was obtained.

[0072] Example 4

[0073] 110 parts of acrylamide, 440 parts of methacryloyloxyethyl trimethylammonium chloride, 30 parts of 3,4-dihydroxycinnamic acid, 15 parts of 4,4'-dihydrazinostilbene-2,2'-disulfonic acid, 10 parts of styryl boric acid diethanolamine ester, and 395 parts of deionized water were added into a beaker and mixed evenly, and then the pH value of the solution was adjusted to 4.0 with citric acid; after the temperature of the solution system was cooled to 0°C, all of it was poured into a reactor, and nitrogen was introduced for deoxygenation for 30 minutes, and then 0.01 parts of VA-044 initiator, 0.008 parts of ammonium persulfate, and 0.007 parts of sodium sulfite were added, and nitrogen was continued to be introduced for 10 minutes, and then the beaker was sealed and reacted for 3.0 hours. After the reaction was completed, an acid thickener was obtained.

[0074] Example 5

[0075] 105 parts of acrylamide, 400 parts of methacryloyloxyethyl trimethylammonium chloride, 26 parts of 3,4-dihydroxycinnamic acid, 13 parts of 4,4'-dihydrazinostilbene-2,2'-disulfonic acid, 6 parts of 4-acrylamidebenzo-15-crown-5, and 450 parts of deionized water were added into a beaker and mixed evenly, and then the pH value of the solution was adjusted to 3.1 with aminosulfonic acid; after the temperature of the solution system was cooled to 5°C, all of it was poured into a reactor, and nitrogen was introduced for deoxygenation for 30 minutes, and then 0.011 parts of V50 initiator, 0.006 parts of sodium persulfate, and 0.005 parts of sodium pyrosulfite were added, and nitrogen was continued to be introduced for 10 minutes, and then the beaker was sealed and reacted for 3.5 hours. After the reaction was completed, an acid thickener was obtained.

[0076] Example 6

[0077] 93 parts of acrylamide, 395 parts of methacryloyloxyethyl trimethylammonium chloride, 23 parts of 3,4-dihydroxycinnamic acid, 11 parts of 4,4'-diaminostilbene-2,2'-disulfonic acid, 9 parts of styryl boric acid diethanolamine ester, and 469 parts of deionized water were added into a beaker and mixed evenly, and then the pH value of the solution was adjusted to 3.3 with adipic acid; after the temperature of the solution system was cooled to 1°C, all of it was poured into a reactor, and nitrogen was introduced for deoxygenation for 30 minutes, and then 0.013 parts of azobisisobutyronitrile, 0.007 parts of potassium persulfate, 0.004 parts of sodium bisulfite, and 0.002 parts of ammonium ferrous sulfate were added, and nitrogen was continued to be introduced for 10 minutes, and then the beaker was sealed and reacted for 4.5 hours. After the reaction was completed, an acid thickener was obtained.

[0078] Comparative Example 1

[0079] 100 parts of acrylamide, 400 parts of methacryloyloxyethyltrimethylammonium chloride and 500 parts of deionized water were added into a beaker and mixed evenly, and then the pH value of the solution was adjusted to 4.0 with citric acid; after the temperature of the solution system was cooled to 5°C, all of it was poured into a reactor, and nitrogen was introduced for deoxygenation for 30 minutes, and then 0.011 parts of V50 initiator, 0.008 parts of sodium persulfate, and 0.005 parts of sodium pyrosulfite were added, and nitrogen was continued to be introduced for 10 minutes, and then the beaker was sealed and reacted for 3.5 hours. After the reaction was completed, an acid thickener was obtained.

[0080] Comparative Example 2

[0081] Comparative Example 2 is substantially the same as Example 6, except that: 3,4-dihydroxycinnamic acid is not added, and 23 parts of deionized water are added instead, that is, a total of 492 parts of deionized water are added.

[0082] Comparative Example 3

[0083] Comparative Example 3 is substantially the same as Example 6, except that: 4,4'-diaminostilbene-2,2'-disulfonic acid is not added, and 11 parts of deionized water are added instead, that is, a total of 480 parts of deionized water are added.

[0084] Comparative Example 4

[0085] Comparative Example 4 is substantially the same as Example 6, except that 9 parts of deionized water are added instead of styryl boric acid diethanolamine ester, i.e., a total of 478 parts of deionized water.

[0086] Comparative Example 5

[0087] Comparative Example 5 is substantially the same as Example 6, except that: 3,4-dihydroxycinnamic acid and 4,4'-diaminostilbene-2,2'-disulfonic acid are not added, and 34 parts of deionized water are added instead, that is, a total of 503 parts of deionized water are added.

[0088] Comparative Example 6

[0089] Comparative Example 6 is substantially the same as Example 6, except that 40 parts of 3,4-dihydroxycinnamic acid are added and 17 parts of deionized water are added less, that is, a total of 452 parts of deionized water are added.

[0090] Comparative Example 7

[0091] Comparative Example 7 is substantially the same as Example 6, except that 20 parts of 4,4'-diaminostilbene-2,2'-disulfonic acid are added, and 9 parts of deionized water are added less, that is, a total of 460 parts of deionized water are added.

[0092] The acid liquid thickener obtained in Examples 1 to 6 and the colloidal acid liquid thickener obtained in Comparative Examples 1 to 7 were granulated, dried, ground, and sieved (the mesh size was 250 μm) to obtain acid liquid thickener particles. The acid liquid thickener particles were used as samples to perform tests on apparent viscosity, shear resistance, apparent viscosity after shearing, and temperature resistance. The test results are shown in Table 1.

[0093] Preparation of thickened acid: prepare a hydrochloric acid solution containing 20% ​​by mass with saline having a mineralization degree of 100,000 mg / L and a calcium and magnesium ion content of 2000 mg / L; weigh 3.00 g of the sample, slowly add it to 497.00 g of the above hydrochloric acid solution while stirring with a magnetic stirrer (the adding time is less than 10 s), stir until there is no insoluble matter and the mixture is homogeneous, then stop stirring and cover the mixture, place it in a constant temperature water bath at 25°C for 30 min to allow it to fully swell, and prepare the thickened acid; the mass fraction of the sample in the thickened acid is 6‰.

[0094] Determination of apparent viscosity: The thickened acid was transferred to the sample cup of a six-speed rotary viscometer and -1 The apparent viscosity η0 at 25°C was tested under shear rate, mPa·s;

[0095] Test of apparent viscosity under shear and temperature resistance: transfer the thickened acid to the rheometer sample tank and set the shear rate of the rheometer to 170s -1 , temperature is 120℃, and the apparent viscosity η1, mPa·s after shearing for 2h is tested.

[0096] Viscosity retention rate K: K = η1 / η0×100%, %.

[0097] Table 1

[0098]

[0099]

[0100] It can be seen from the data in Table 1 that the acid liquid thickener prepared by the present invention has excellent salt resistance and high temperature shear resistance. In the hydrochloric acid solution configured with high mineralization brine, it has strong acid resistance and viscosity increasing ability; and the acid liquid thickener with a mass fraction of 6‰ has a viscosity increasing ability of 170s -1 The viscosity reaches above 60mPa·s under the shear rate, and has a certain shear resistance; after shearing for 2 hours at a high temperature of 120°C, there is no stratification or precipitation, the high temperature stability is good, and the viscosity retention rate can reach above 90%.

[0101] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention. The parts not described in detail in the present invention are well-known technologies of those skilled in the art.

Claims

1. A method for preparing an acid liquid thickener, characterized in that: The preparation method comprises: acrylamide, methacryloyloxyethyl trimethylammonium chloride, 3,4-dihydroxycinnamic acid, salt-resistant monomer, and rigid monomer are placed in water and mixed evenly to obtain a mixed solution; an initiator is added to the mixed solution to carry out a copolymerization reaction to obtain the acid liquid thickener; The salt-resistant monomer is 4,4'-diaminostilbene-2,2'-disulfonic acid or 4,4'-dihydrazinostilbene-2,2'-disulfonic acid; The rigid monomer is 4-acrylamide benzo-15-crown-5 or styryl boric acid diethanolamine ester; The weight proportions of the components for preparing the acid liquid thickener are as follows: 90-110 parts of acrylamide, 360-440 parts of methacryloyloxyethyl trimethyl ammonium chloride, 20-30 parts of 3,4-dihydroxycinnamic acid, 8-15 parts of salt-resistant monomer, 6-10 parts of rigid monomer, 395-516 parts of water and 0.02-0.036 parts of initiator.

2. The preparation method according to claim 1, characterized in that: The initiation temperature of the copolymerization reaction is 0-5°C, and the reaction time is 3-5h.

3. The preparation method according to claim 1, characterized in that: Also includes: The pH of the mixed solution is adjusted to 3-4.

4. The preparation method according to claim 1, characterized in that: Also includes: The pH of the mixed solution is adjusted using a pH adjuster.

5. The preparation method according to claim 4, characterized in that: The pH adjuster is at least one of adipic acid, aminosulfonic acid and citric acid.

6. The preparation method according to claim 1, characterized in that: Also includes: After nitrogen is introduced into the mixed solution, the initiator is added to carry out copolymerization reaction.

7. The preparation method according to claim 6, characterized in that: Also includes: The nitrogen gas is introduced for 30 to 50 minutes.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The initiator is an azo initiator and a redox initiator including an oxidant and a reductant.

9. The preparation method according to claim 8, characterized in that: The mass ratio of the azo initiator, the oxidant and the reducing agent is (0.01-0.02):(0.005-0.008):(0.005-0.008).

10. The preparation method according to claim 8, characterized in that: The azo initiator is at least one of VA-044 initiator, azobisisobutyronitrile and V-50 initiator.

11. The preparation method according to claim 8, characterized in that: The oxidant is at least one of sodium persulfate, potassium persulfate and ammonium persulfate.

12. The preparation method according to claim 8, characterized in that: The reducing agent is at least one of sodium sulfite, sodium bisulfite, sodium pyrosulfite and ammonium ferrous sulfate.

13. An acid liquid thickener, characterized in that: The method is prepared by any one of claims 1 to 12.