A composite diaphragm for liquid carbonate-based electrolyte lithium metal battery and its preparation and application
By introducing a charge equalizer into the lithium metal battery separator to form a structure with lithium salt anions and lithium ions, the problem of insufficient affinity between the lithium metal battery separator and the carbonate-based electrolyte is solved, and the migration number of lithium ions is significantly increased. and battery cycle life, ensuring battery stability and safety.
Patent Information
- Application Number
- CN202310440371.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-23
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-04-23
AI Technical Summary
Existing lithium metal battery separators have poor affinity with carbonate-based electrolytes, resulting in low lithium ion migration numbers and weak lithium dendrite growth inhibition capabilities, affecting battery cycle life and safety.
A charge equalizer is introduced into the separator of a lithium metal battery to form a "charge equalizer-lithium salt anion-lithium ion" structure. The charge equalizer attracts the lithium salt anions in the electrolyte and improves the affinity between the separator and the electrolyte. Control the deposition morphology of lithium ions.
It significantly improves the migration number of lithium ions and battery cycle life, inhibits the growth of lithium dendrites, extends the service life of the battery, and improves the applicability of the separator for industrial production and the cycle stability of the battery.
Smart Images

Figure CN116706423B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium battery diaphragms, and in particular relates to a composite diaphragm for a liquid carbonate-based electrolyte lithium metal battery and a preparation method and application thereof. Background Art
[0002] Since the commercialization of lithium-ion batteries in the 1990s, they have become the only choice for power supply of consumer electronic products due to their advantages such as high energy density, high operating voltage, long cycle life and no memory effect. With the large-scale commercialization of electric vehicles, hybrid vehicles, energy storage and other fields, the use scenarios of lithium-ion batteries are constantly expanding and enriching. In the context of the layout of new energy vehicles in many countries, people have put forward higher requirements for the energy density, endurance and safety of lithium-ion batteries.
[0003] Lithium metal batteries use lithium metal instead of graphite in traditional lithium-ion batteries as the negative electrode of the battery, and store and release electricity by shuttling lithium ions between the positive and negative electrodes. Because the lithium metal negative electrode has an ultra-high theoretical specific capacity (3860mAh / g), an extremely low electrode potential (-3.04V, relative to the standard hydrogen electrode), and a low density (0.59g / cm 3 ) and other advantages, and has the potential to further improve the energy storage performance of batteries, and has therefore received extensive research and attention. However, problems such as lithium dendrite growth and rapid consumption of electrolyte in lithium metal batteries have restricted the pace of its commercialization.
[0004] In lithium metal batteries, the diaphragm is located between the positive electrode and the lithium metal negative electrode, which prevents the positive and negative electrodes from contacting and short-circuiting, and provides a channel for lithium ions to move between the positive and negative electrodes. At present, the most mainstream lithium-ion battery diaphragms are microporous films made of polyolefin materials, such as polypropylene (PP) and polyethylene (PE). Due to the poor affinity between this type of diaphragm and polar carbonate-based electrolyte solvents, this poor affinity hinders the migration of lithium ions and causes uneven lithium ion distribution, leading to the growth of lithium dendrites. In particular, for polyolefin diaphragms used in lithium metal batteries, the above problems can lead to serious lithium dendrite growth, excessive consumption of electrolyte, reduced battery cycle performance, and even piercing the diaphragm to cause a short circuit in the battery. It can be seen that the affinity between the diaphragm and the electrolyte can directly affect the transmission of lithium ions and the deposition morphology of lithium ions. Improving the affinity between the diaphragm and the electrolyte has great potential in regulating the growth of lithium dendrites.
[0005] In order to avoid the potential safety hazards of commercial diaphragms, many new materials with good affinity for electrolytes have been tried in the research of lithium metal battery diaphragms. However, the pore size of the new diaphragms is difficult to control, which brings limitations. Using materials with affinity for electrolytes to coat the surface of the diaphragm can increase the affinity between the diaphragm and the electrolyte. Constructing an ordered pore structure on the diaphragm can provide a uniform migration channel for lithium ions, which is conducive to the uniform deposition of lithium ions and prolongs the battery life. However, both methods are difficult to apply on a large scale. Therefore, it is particularly important to develop a functional diaphragm for lithium metal batteries from a new perspective based on the law of lithium ion electrodeposition. Summary of the invention
[0006] In order to overcome the defects of the above-mentioned prior art, the present invention provides a composite diaphragm for liquid carbonate-based electrolyte lithium metal batteries and its preparation and application, by introducing a charge uniformizer into the diaphragm substrate to attract lithium salt anions in the electrolyte to form a "charge uniformizer-lithium salt anion-lithium ion" structure, so as to uniformly regulate the deposition of lithium ions, significantly improve the deposition morphology of lithium ions, and ensure the cycle stability of lithium metal batteries.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] One of the purposes of the present invention is to provide a composite diaphragm for a liquid carbonate-based electrolyte lithium metal battery, wherein the composite diaphragm is prepared by coating a colloidal diaphragm dispersion made of a polyvinylidene fluoride-based polymer and a charge uniforming agent.
[0009] It is further defined that the polyvinylidene fluoride-based polymer is one or a mixture of any proportion of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluoroethylene, and polyvinylidene fluoride-chlorotrifluoroethylene.
[0010] It is further defined that the molecular weight of the polyvinylidene fluoride based polymer is 500,000-1.5 million.
[0011] It is further defined that the charge uniformizer is one or a mixture of any ratio of octadecyl dimethyl hydroxyethyl quaternary ammonium nitrate, sodium α-pyrrolidone-5 carboxylate, and dodecylamine polyoxyethylene ether.
[0012] It is further defined that the mass ratio of the charge uniformizer to the polyvinylidene fluoride based polymer is (5-50):100.
[0013] The second object of the present invention is to provide a method for preparing a composite diaphragm for a liquid carbonate-based electrolyte lithium metal battery, the preparation method being carried out according to the following steps:
[0014] Step 1: Disperse the charge uniformity agent in an organic solvent and stir magnetically for 1-3 hours at room temperature to obtain a dispersion;
[0015] Step 2: Add the polyvinylidene fluoride-based polymer to the dispersion of step 1, and stir magnetically at 50-70° C. for 0.5-1 h to obtain a colloidal dispersion;
[0016] Step 3: Add deionized water dropwise to the colloidal dispersion of step 2, stir magnetically at 50-70° C. for 0.5-1 h, and cool to room temperature to obtain a colloidal diaphragm dispersion;
[0017] Step 4: Scrape the colloidal diaphragm dispersion prepared in step 3 onto the substrate and dry it at room temperature to obtain a composite diaphragm.
[0018] It is further defined that the organic solvent in step 1 is one or a mixture of any ratio of acetone, N-methylpyrrolidone, N-N-dimethylformamide, and N-N-dimethylacetamide.
[0019] Furthermore, in step 1, the magnetic stirring speed is 500-1500 rpm.
[0020] It is further defined that the mass ratio of the polyvinylidene fluoride based polymer in step 2 to the charge uniforming agent in step 1 is 100:(5-50).
[0021] It is further defined that the mass ratio of the polyvinylidene fluoride based polymer in step 2 to the organic solvent in step 1 is 1:(6-10).
[0022] Furthermore, in step 2, the magnetic stirring speed is 500-1500 rpm.
[0023] It is further defined that the mass ratio of the deionized water in step 3 to the organic solvent in step 1 is (3-5):100.
[0024] Furthermore, in step 3, the magnetic stirring speed is 500-1500 rpm.
[0025] A third object of the present invention is to provide an application of a composite diaphragm in a lithium metal battery with a liquid carbonate-based electrolyte.
[0026] Compared with the prior art, the present invention has the following significant effects:
[0027] (1) The present invention aims to solve the technical problems that the existing polyolefin separators have poor affinity with electrolytes, low lithium ion migration numbers, and weak ability to inhibit lithium dendrite growth. The present invention provides a composite separator for lithium metal batteries that inhibits dendrite growth. The separator introduces cationic sites into the separator to improve the electrolyte affinity of the separator to inhibit lithium dendrite growth. The separator improves the lithium ion migration number and battery cycle life. The composite separator proposed by the present invention not only ensures the original wettability of the separator, but also improves the lithium ion transmission capacity of the separator.
[0028] (2) The present invention also provides a simple method for preparing a composite diaphragm for lithium metal batteries that inhibits dendrite growth, which is suitable for industrial production and can prepare a composite diaphragm with consistent morphology and controllable porosity, which can meet the application requirements of the diaphragm in the field of lithium metal batteries.
[0029] (3) In the diaphragm preparation method of the present invention, during the lithium ion deposition process, the charge uniformizer in the diaphragm attracts the anions in the electrolyte to form a lithium-philic surface, adjusts the distribution of lithium ions, makes the distribution and migration of lithium ions more uniform, inhibits the growth of lithium dendrites, and can ensure the stability of the battery during long-term cycles, prevent premature battery failure, and extend the cycle life of lithium metal batteries.
[0030] (4) The application effect of the diaphragm of the present invention in lithium metal batteries is good. The discharge capacity retention rate of the lithium iron phosphate positive electrode lithium metal battery is 96.9% after 800 cycles at a 1C rate, and the discharge capacity retention rate is 93.4% after 1000 cycles at a 2C rate. Its cycle stability is significantly improved compared with commercial battery diaphragms and battery capacity retention rates in domestic and foreign research. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a scanning electron microscope morphology image of the surface of the composite diaphragm prepared in Example 2;
[0032] Figure 2 The scanning electron microscope morphology and element distribution diagram of the cross section of the composite diaphragm prepared in Example 2; a-SEM, b-EDS;
[0033] Figure 3 A comparison chart of the lithium ion migration numbers of the separators of Comparative Examples 1-2 and Example 2;
[0034] Figure 4 It is a comparative diagram of wettability characterization of the diaphragms of Comparative Examples 1-2 and Example 2;
[0035] Figure 5 This is a scanning electron microscope morphology of the lithium metal negative electrode of the lithium iron phosphate / lithium metal battery using the separator of Comparative Example 1 after 200 cycles at a 2C rate;
[0036] Figure 6 This is a scanning electron microscope morphology of the lithium metal negative electrode of the lithium iron phosphate / lithium metal battery using the separator of Comparative Example 2 after 200 cycles at a 2C rate;
[0037] Figure 7 This is a scanning electron microscope morphology of the lithium metal negative electrode of the lithium iron phosphate / lithium metal battery using the composite separator of Example 2 after 200 cycles at a 2C rate;
[0038] Figure 8It is a comparison chart of the cycle performance of the separators of Comparative Examples 1-2 and Example 2 at a 1C rate;
[0039] Fig. 9 The cycle performance of the membranes of Comparative Examples 1-2 and Example 2 at a 2C rate;
[0040] Wherein, pp is the commercial polypropylene membrane Celgard2500 of Comparative Example 1, PVDF-HFP is the pure polyvinylidene fluoride-hexafluoropropylene membrane of Comparative Example 2, and PVDF-HFP / SN is the composite membrane of Example 2. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0042] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.
[0043] The terms "comprising," "including," "having," "containing," or any other variations thereof, as used in the following examples, are intended to cover a non-exclusive inclusion. For example, a composition, step, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent to such composition, step, method, article, or apparatus.
[0044] When equivalent, concentration or other value or parameter is represented by the range limited by range, preferred range or a series of upper preferred value and lower preferred value, this should be understood as specifically disclosing all ranges formed by any pairing of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether the scope is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the scope is intended to include its end value and all integers and fractions within the scope. In the present application specification and claims, range limitation can be combined and / or interchanged, if these ranges are not otherwise stated, include all sub-ranges contained therein.
[0045] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.
[0046] Embodiment 1:
[0047] The preparation method of the composite diaphragm for liquid lithium metal battery based on polar carbonate-based electrolyte of this embodiment is carried out according to the following steps:
[0048] Step 1: Disperse 0.035 g of octadecane dimethyl hydroxyethyl quaternary ammonium nitrate in 5.6 g of acetone, and stir magnetically at 1000 rpm for 2 h at room temperature to obtain a dispersion;
[0049] Step 2: Add 0.7 g of polyvinylidene fluoride-hexafluoropropylene (molecular weight 600,000) to the dispersion obtained in step 1, and stir magnetically at 55° C. and 1000 rpm for 0.5 h to obtain a colloidal dispersion;
[0050] Step 3: 0.18 g of deionized water was added dropwise to the colloidal dispersion obtained in step 2, and the mixture was magnetically stirred at 1000 rpm for 0.5 h at 55° C., and cooled to room temperature to obtain a colloidal diaphragm dispersion;
[0051] Step 4: Scrape the colloidal diaphragm dispersion obtained in step 3 onto a glass substrate and dry it at room temperature to obtain a composite diaphragm with a thickness of 15 μm.
[0052] Embodiment 2:
[0053] The preparation method of the composite diaphragm for liquid lithium metal battery based on polar carbonate-based electrolyte of this embodiment is carried out according to the following steps:
[0054] Step 1: Disperse 0.07 g of octadecane dimethyl hydroxyethyl quaternary ammonium nitrate in 5.56 g of acetone, and stir magnetically at 1000 rpm for 2 h at room temperature to obtain a dispersion;
[0055] Step 2: Add 0.7 g of polyvinylidene fluoride-hexafluoropropylene (molecular weight 600,000) to the dispersion obtained in step 1, and stir magnetically at 55° C. and 1000 rpm for 0.5 h to obtain a colloidal dispersion;
[0056] Step 3: 0.18 g of deionized water was added dropwise to the colloidal dispersion obtained in step 2, and the mixture was magnetically stirred at 1000 rpm for 0.5 h at 55° C., and cooled to room temperature to obtain a colloidal diaphragm dispersion;
[0057] Step 4: Scrape the colloidal diaphragm dispersion obtained in step 3 onto a glass substrate and dry it at room temperature to obtain a composite diaphragm with a thickness of 15 μm, abbreviated as PVDF-HFP / SN.
[0058] Embodiment 3:
[0059] The preparation method of the composite diaphragm for liquid lithium metal battery based on polar carbonate-based electrolyte of this embodiment is carried out according to the following steps:
[0060] Step 1: Disperse 0.14 g of octadecane dimethyl hydroxyethyl quaternary ammonium nitrate in 5.6 g of acetone, and stir magnetically at 1000 rpm for 2 h at room temperature to obtain a dispersion;
[0061] Step 2: Add 0.7 g of polyvinylidene fluoride-hexafluoropropylene (molecular weight 600,000) to the dispersion obtained in step 1, and stir magnetically at 55° C. and 1000 rpm for 0.5 h to obtain a colloidal dispersion;
[0062] Step 3: 0.18 g of deionized water was added dropwise to the colloidal dispersion obtained in step 2, and the mixture was magnetically stirred at 1000 rpm for 0.5 h at 55° C., and cooled to room temperature to obtain a colloidal diaphragm dispersion;
[0063] Step 4: Scrape the colloidal diaphragm dispersion obtained in step 3 onto a glass substrate and dry it at room temperature to obtain a composite diaphragm with a thickness of 15 μm.
[0064] Comparative Example 1: Commercial polypropylene diaphragm Celgard 2500, abbreviated as PP.
[0065] Comparative Example 2: This embodiment provides a polyvinylidene fluoride-hexafluoropropylene diaphragm, and the preparation method thereof is as follows:
[0066] Step 1, dissolving 0.7 g of polyvinylidene fluoride-hexafluoropropylene in 5.6 g of acetone, and magnetically stirring at 55° C. and 1000 rpm for 30 min to obtain a transparent colloidal solution;
[0067] Step 2: 0.18 g of deionized water was added dropwise to the transparent colloidal solution obtained in step 1, and magnetic stirring was performed at 55° C. and 1000 rpm for 0.5 h, and the solution was cooled to room temperature to obtain a colloidal diaphragm dispersion;
[0068] Step 3: Scrape the colloidal membrane dispersion obtained in step 2 onto a glass substrate and dry it at room temperature to obtain a pure polyvinylidene fluoride-hexafluoropropylene membrane with a thickness of 15 μm, abbreviated as PVDF-HFP.
[0069] Application examples:
[0070] The diaphragms of Examples 1-3 and Comparative Examples 1-2 were assembled in a liquid lithium-ion battery, wherein the positive electrode was lithium iron phosphate, the negative electrode was lithium foil, the electrolyte was a mixed solution containing 1 mol / L LiPF6, and the solvent was a mixture of ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate in a volume ratio of 1:1:1.
[0071] Testing: The electrochemical performance of the battery is tested at room temperature.
[0072] Experiment 1: The SEM morphology of the composite membrane surface of Example 2 is as follows: Figure 1 The SEM morphology and element distribution of the cross section are shown in Figure 2 As shown, it can be seen that the N and O elements are evenly distributed in the PVDF-HFP / SN composite membrane, and the charge uniformizer is fully mixed with PVDF-HFP.
[0073] Test 2: Characterize the lithium ion migration number of lithium batteries in the corresponding use case, and the results are shown in Figure 3 As shown in Table 1, the lithium ion migration number of the PVDF-HFP / SN composite membrane is significantly improved.
[0074] Test 3: Test of membrane liquid absorption rate: Weigh the mass of the membrane, then soak the membrane in the electrolyte for 40 minutes, weigh the mass of the membrane before and after soaking in the electrolyte, and the liquid absorption rate is obtained by (mass after soaking - initial mass) / initial mass. The results are shown in Table 1. It can be seen that the liquid absorption rate of the composite membrane is improved compared with the pure PVDF-HFP membrane by adding the charge uniformizer.
[0075] Experiment 4: Contact angle test was performed on the diaphragms in Examples 1-3 and Comparative Examples 1-2. The results are shown in Figure 4 From Table 1, it can be seen that the affinity of PVDF-HFP / SN composite membrane to electrolyte is much higher than that of commercial PP membrane.
[0076] Experiment 5: Scanning electron microscope morphology of the lithium metal negative electrode of the battery using the separator of Comparative Examples 1-2 and Example 2 after 200 cycles at 2C rate, as shown in FIG. Figure 5-7 As shown in the figure, it can be seen that the lithium metal negative electrode using the PVDF-HFP / SN composite separator has a very dense deposition morphology, proving that the separator has the effect of inhibiting dendrite growth.
[0077] Test 6: At room temperature (25°C), 1C (1C = 170mAg -1 ) and the cycle performance under 2C were tested, and the results are shown in Figure 8-9 As shown in Table 1, the separator composed of the charge uniformizer and PVDF-HFP can improve the cycle life and capacity retention rate of the battery, and the battery cycle performance using the composite separator of Example 2 of the present invention is more excellent.
[0078] Table 1 Diaphragm and battery performance test data
[0079] Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 Lithium ion migration number 0.4 0.45 0.52 0.63 0.62 Wettability (contact angle) (°) 44.5 23.5 22.8 22.2 22.6 Electrolyte absorption rate 110 220 230 235 238 Capacity retention rate of LFP / Li battery after 800 cycles at 25℃ / 1C 0 0 75.4% 96.9% 62.7% Capacity retention rate of LFP / Li battery after 1000 cycles at 25℃ / 2C 0 0 68.8% 93.4% 53.5%
[0080] The above are only preferred specific embodiments of the present invention, which are all different implementations based on the overall concept of the present invention, and the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a composite diaphragm for a liquid carbonate-based electrolyte lithium metal battery, characterized in that: The invention is prepared by coating a colloidal diaphragm dispersion made of a polyvinylidene fluoride polymer and a charge uniformizer; the charge uniformizer is octadecane dimethyl hydroxyethyl quaternary ammonium nitrate; The preparation method is carried out according to the following steps: Step 1: Disperse the charge uniformity agent in an organic solvent and stir magnetically for 1-3 hours at room temperature to obtain a dispersion; Step 2: Add the polyvinylidene fluoride-based polymer to the dispersion of step 1, and stir magnetically at 50-70° C. for 0.5-1 h to obtain a colloidal dispersion; Step 3: Add deionized water dropwise to the colloidal dispersion of step 2, stir magnetically at 50-70° C. for 0.5-1 h, and cool to room temperature to obtain a colloidal diaphragm dispersion; Step 4: Scrape the colloidal diaphragm dispersion prepared in step 3 onto the substrate and dry it at room temperature to obtain a composite diaphragm.
2. The method according to claim 1, characterized in that The polyvinylidene fluoride-based polymer is one or a mixture of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluoroethylene, and polyvinylidene fluoride-chlorotrifluoroethylene.
3. The method according to claim 2, characterized in that The molecular weight of polyvinylidene fluoride based polymer is 500,000-1.5 million.
4. The method according to claim 1, characterized in that: The mass ratio of the charge uniformizer to the polyvinylidene fluoride based polymer is (5-50):
100.
5. The method according to claim 1, characterized in that In step 1, the organic solvent is a mixture of one or more of acetone, N-methylpyrrolidone, N-dimethylformamide, and N-dimethylacetamide, and the magnetic stirring speed is 500-1500 rpm.
6. The method according to claim 1, characterized in that The mass ratio of the polyvinylidene fluoride based polymer in step 2 to the organic solvent in step 1 is 1:(6-10), and the magnetic stirring speed is 500-1500 rpm.
7. The method according to claim 1, characterized in that The mass ratio of deionized water in step 3 to the organic solvent in step 1 is (3-5):100, and the magnetic stirring speed is 500-1500 rpm.
8. Use of the composite diaphragm prepared by the method according to any one of claims 1 to 7 in a lithium metal battery with a liquid carbonate-based electrolyte.