Soldering flux and method for manufacturing electronic device
By combining rosin compounds and a variety of organic solvents in the flux, and through specific coating and heating treatment, the problem of temporary fixability of existing fluxes when process conditions changes is solved, and the manufacturing of electronic equipment is realized. Stable and efficient temporary fixing effect.
Patent Information
- Application Number
- CN202280020898.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-13
- Filing Date
- 2022-03-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-03-09
AI Technical Summary
Existing fluxes are inadequate in stability when temporarily fixing electronic components, especially when process conditions change, and their temporary fixing capabilities are not fully utilized.
Develop a flux containing rosin compounds and more than 2 organic solvents. Through specific coating and heating treatment steps, it ensures that its adhesion reaches more than 50gf and remains stable when process conditions change, and adopts low volatility. and highly volatile organic solvents to improve temporary fixation capacity.
The stable temporary fixation of preformed solder and electronic components in electronic equipment manufacturing is achieved, and good adhesion can be maintained for a long time, and the temporary fixation capability does not significantly decrease even when process conditions change.
Smart Images

Figure CN116981541B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a soldering flux and a method for manufacturing an electronic device. More specifically, the present invention relates to a soldering flux used in soldering and a method for manufacturing an electronic device using the soldering flux. Background Art
[0002] In soldering, generally, flux is used.
[0003] The flux is used in two forms: (i) a form in which solder powder and flux are pre-mixed to form a solder paste, and (ii) a form in which flux is first applied to an electrode and then a preformed solder is placed on the electrode coated with flux for soldering.
[0004] In a first sense, flux is an auxiliary agent used when soldering solder to electrodes or electronic components as soldering objects, but it is well known that flux is required to play roles (functions) other than auxiliary agents for soldering.
[0005] For example, Patent Document 1 describes that first, flux is applied to electrodes of a substrate or chip component, and then solder balls are temporarily fixed to the electrodes by the applied flux, etc. That is, in Patent Document 1, flux is used not only as an auxiliary agent for soldering, but also as a "temporary fixing material" for solder balls.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2003-51668. Summary of the invention
[0009] Problems to be solved by the invention
[0010] As described in Patent Document 1, it is considered that flux can be used not only as an auxiliary agent for soldering but also for "temporary fixing" of preform solder and electronic components. However, as far as the inventors know, conventional flux has not been studied / optimized for temporary fixing, and there is room for improvement.
[0011] In addition, the flux used for temporary fixing is required to exhibit stable temporary fixing properties even when process conditions vary during the manufacture of electronic devices. However, as far as the inventors know, this viewpoint has not been studied in the past, and there is room for improvement.
[0012] The present invention has been made in view of such circumstances.
[0013] One of the objects of the present invention is to provide a flux that can preferably temporarily fix a preform or an electronic component in the manufacture of an electronic device and that exhibits stable temporary fixation even when process conditions vary.
[0014] Another object of the present invention is to provide a method for manufacturing an electronic device which is practically useful, using flux for temporary fixation of preform solder or electronic components.
[0015] Means for solving problems
[0016] The present inventors have completed the invention provided below and solved the above-mentioned problems.
[0017] According to the present invention, the following soldering flux is provided.
[0018] A soldering flux comprising a rosin compound and two or more organic solvents and containing no solder alloy, and being applied to a substrate for use without containing any solder alloy, wherein the soldering flux has an adhesion T of 50 gf or more measured by the following step 1, and an adhesion T' of 50 gf or more measured by the following step 2.
[0019] [Step 1]
[0020] (1) A Ni-plated Al plate having a circular depression with a diameter of 7 mm and a depth of 0.2 mm provided on at least one surface thereof is coated with flux in an amount sufficient to fill the depression.
[0021] (2) The Al plate coated with the flux was heated at 100° C. for 1 minute.
[0022] (3) After the Al plate after the heat treatment was cooled to room temperature, the adhesion T of the flux present in the depression was measured using an adhesion tester under the conditions of a pressing time of 0.2 sec, a pressing pressure of 50 gf, an intrusion speed of 2.0 mm / sec, and a pulling speed of 10 mm / sec.
[0023] [Step 2]
[0024] The adhesive force T' was measured by the same procedure as in [Procedure 1] except that the conditions of the heat treatment in the above (2) were changed to 100°C for 3 minutes.
[0025] Furthermore, according to the present invention, the following method for manufacturing an electronic device is provided.
[0026] A method for manufacturing an electronic device, wherein the method for manufacturing an electronic device comprises: a coating process, in which the flux is coated on a substrate; a temporary fixing process, in which a preformed solder or an electronic component is temporarily fixed on the substrate coated with the flux; and a bonding process, in which the substrate is heated to bond the preformed solder or the electronic component to the substrate.
[0027] Effects of the Invention
[0028] According to the present invention, there is provided a soldering flux that can preferably temporarily fix a preform or an electronic component in the production of an electronic device and that exhibits stable temporary fixation properties even when process conditions vary.
[0029] Furthermore, according to the present invention, there is provided a method for manufacturing an electronic device which is practically useful, in which the flux is used for temporary fixing of preform solder or electronic components. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a diagram for explaining a method of manufacturing an electronic device.
[0031] Figure 2 It is a supplementary diagram for explaining the evaluation method in Examples.
[0032] Figure 3 This is an image of the state of the soldering flux of Example 5 applied on a glass substrate.
[0033] Figure 4 This is an image of a conventional soldering flux applied on a glass substrate. DETAILED DESCRIPTION
[0034] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings.
[0035] The drawings are for illustration purposes only, and the shapes, dimensional ratios, etc. of the components in the drawings do not necessarily correspond to the actual products.
[0036] In the present specification, the expression "X to Y" in the description of the numerical range means X or more and Y or less unless otherwise specified. For example, "1 to 5 mass %" means "1 mass % or more and 5 mass % or less".
[0037] The term "electronic device" in this specification is used to mean components, devices, final products, etc. that apply electronic engineering technology, including semiconductor chips, semiconductor elements, printed wiring boards, circuit display devices, information communication terminals, light-emitting diodes, physical batteries, chemical batteries, etc.
[0038] In this specification, the unit "gf" represents gram weight as a unit of force. 1gf = 9.8g·m / s 2 .
[0039] <Flux>
[0040] The soldering flux of the present embodiment contains a rosin compound and two or more organic solvents.
[0041] The flux of this embodiment is generally used for soldering.
[0042] Generally, the soldering flux of this embodiment is not suitable for solder paste prepared by premixing solder powder and soldering flux. The soldering flux of this embodiment does not contain solder alloy, and is applied on a substrate (electrode, etc.) in a form without solder alloy separately from solder alloy.
[0043] The adhesive force T of the flux of the present embodiment measured by the following step 1 is 50 gf or more, preferably 50 to 500 gf, more preferably 50 to 300 gf, and even more preferably 70 to 200 gf.
[0044] [Step 1]
[0045] (1) A Ni-plated Al plate having a circular depression with a diameter of 7 mm and a depth of 0.2 mm on at least one surface was coated with flux in an amount sufficient to fill the depression.
[0046] (2) The Al plate coated with the flux was heated at 100° C. for 1 minute.
[0047] (3) After cooling the Al plate after the heat treatment to room temperature, the adhesion T of the flux present in the above-mentioned depression was measured using an adhesion tester under the conditions of a pressing time of 0.2 sec, a pressing pressure of 50 gf, an intrusion speed of 2.0 mm / sec, and a pulling speed of 10 mm / sec.
[0048] Furthermore, when the flux of the present embodiment is measured in the following step 2, the adhesive force T' is 50 gf or more, preferably 50 to 500 gf, more preferably 50 to 300 gf, and even more preferably 70 to 200 gf.
[0049] [Step 2]
[0050] The adhesive force T' was measured by the same procedure as in [Procedure 1] except that the conditions of the heat treatment in the above (2) were changed to 100°C for 3 minutes.
[0051] The flux applied to the electrode preferably maintains the ability to temporarily fix the preform solder, etc. (temporary fixing ability) for a certain period of time, so that the preform solder, electronic components (hereinafter referred to as "preform solder, etc.") can be "temporarily fixed" on the electrode using the flux.
[0052] Specifically, in the manufacture of electronic devices, in order to facilitate flow operations, a certain amount of time is usually left between applying flux to the electrode and temporarily fixing the preformed solder to the electrode. In addition, a certain amount of time is usually left between temporarily fixing the preformed solder to the electrode and performing subsequent processes such as welding. Preferably, the flux applied to the electrode maintains sufficient temporary fixing ability even after these times. In addition, since various conditions may change in the manufacture of electronic devices, it is preferred that the temporary fixing ability does not change much even if the conditions change.
[0053] The adhesive force of the rosin compound alone is not great, but by wetting it with an organic solvent, a greater adhesive force can be obtained. Therefore, by using the rosin compound and the organic solvent together, sufficient temporary fixing ability is exhibited. However, conventional fluxes have no idea of using them for temporary fixing of preform solders, etc. Therefore, as time passes, the solvent, which is the main liquid component in the flux, evaporates, and the rosin compound in the flux becomes dry and loses its viscosity, which tends to reduce the temporary fixing ability. In addition, conventional fluxes are not designed to take into account the changing conditions in the manufacture of electronic devices.
[0054] Therefore, the present inventors have repeatedly conducted various studies to develop a flux that has a small decrease in temporary fixing ability with the passage of time after coating and exhibits stable temporary fixing properties even when process conditions vary during electronic device manufacturing.
[0055] Through continuous exploration, it was found that the adhesive force of the applied flux after heating for a fixed time may be related to the ability to temporarily fix preform solder for a long time in the electronic equipment manufacturing process and the stable temporary fixation.
[0056] The present inventors have conducted further research based on the above findings. Specifically, a new soldering flux is prepared, wherein the adhesive force T measured in the above [Step 1] is 50 gf or more, and the adhesive force T' measured in the above [Step 2] is 50 gf or more. By using this new soldering flux, a preform solder or the like can be preferably temporarily fixed to an electrode in the electronic device manufacturing process.
[0057] A soldering flux having an adhesion force T of 50 gf or more as measured in the above [Step 1] and an adhesion force T' of 50 gf or more as measured in the above [Step 2] can be manufactured by mixing appropriate materials in an appropriate amount ratio. The details will be described below. For example, by using an appropriate amount of a low-volatile organic solvent as at least a part of the organic solvent, a soldering flux having an adhesion force T of 50 gf or more and an adhesion force T' of 50 gf or more can be manufactured. Moreover, by using such a soldering flux, it is possible to preferably temporarily fix a preform solder or the like.
[0058] Incidentally, in the present embodiment, the value of T' / T is preferably 0.5 to 5, more preferably 0.7 to 4, and further preferably 0.9 to 3. In particular, it is considered that a value of T' / T that is neither too large nor too small corresponds to stable temporary fixation even when process conditions vary. That is, in addition to designing the flux so that each value of T and T' reaches an appropriate value, by designing the flux so that the value of T' / T also reaches an appropriate value, particularly stable temporary fixation can be obtained.
[0059] Hereinafter, the soldering flux according to the present embodiment will be described in more detail.
[0060] (rosin compound)
[0061] The soldering flux of the present embodiment contains a rosin compound.
[0062] Examples of the rosin compound include, without particular limitation, known rosin compounds (rosin-based resins, etc.).
[0063] Specific examples of the rosin compound include raw material rosins such as gum rosin, wood rosin, and tall oil rosin.
[0064] In addition, the rosin compound may include derivatives obtained from the above-mentioned raw material rosin. As the derivatives, for example, purified rosin, hydrogenated rosin, disproportionated rosin, polymerized rosin, acid-modified rosin, phenol-modified rosin, α,β-unsaturated carboxylic acid modified products (acrylated rosin, maleated rosin, fumarated rosin, etc.) may also be mentioned.
[0065] Furthermore, there can be mentioned purified products, hydrogenated products and disproportionated products of polymerized rosin, purified products, hydrogenated products and disproportionated products of α,β-unsaturated carboxylic acid-modified products, and the like.
[0066] The soldering flux of the present embodiment may contain only one rosin compound, or may contain two or more rosin compounds.
[0067] The amount of the rosin compound based on the entire flux including the organic solvent (100 mass %) is, for example, 10 to 70 mass %, preferably 15 to 60 mass %, and more preferably 20 to 55 mass %.
[0068] (Organic Solvent)
[0069] The soldering flux of the present embodiment contains two or more kinds of organic solvents.
[0070] Preferred organic solvents include low-volatility organic solvents and high-volatility organic solvents described below.
[0071] The difference in volatility between low-volatile organic solvents and high-volatile organic solvents is relative. Specifically, when the vapor pressure of the low-volatile organic solvent at 20°C is pL, and the vapor pressure of the high-volatile organic solvent at 20°C is pH, pL<pH, and the value of pH-pL is preferably 5 Pa or more, more preferably 6 Pa or more, and further preferably 7 Pa or more. There is no particular limitation on the upper limit of the value of pH-pL, and the upper limit of the value of pH-pL is generally 10000 Pa, specifically about 5000 Pa.
[0072] By using a rosin compound and a low-volatile organic solvent together, after the flux is applied to the electrode, the applied flux is likely to maintain a "sticky" state for a long time. That is, by using a low-volatile organic solvent, it is easy to produce a flux with an adhesive force T of 50 gf or more. In addition, by applying such a flux to the electrode, a preform solder or the like can be preferably temporarily fixed to the electrode.
[0073] In addition, by using a high-volatile organic solvent in addition to a low-volatile organic solvent, the viscosity of the flux is reduced compared to a flux containing only a low-volatile organic solvent, and the coating property of the flux when applied to the electrode can be improved. That is, by using a low-volatile organic solvent and a high-volatile organic solvent together, it is possible to achieve both good coating property when applying the flux to the electrode and maintenance of appropriate adhesion after the flux is applied.
[0074] Furthermore, by using a highly volatile organic solvent, the viscosity of the flux can be easily adjusted to a level that allows easy application of the flux without changing the temporary fixability that is ultimately intended.
[0075] From the viewpoint of the appropriate adhesive force after the application of the flux, it is preferred to appropriately adjust the amount of the rosin compound and the amount of the low-volatile organic solvent. Specifically, the ratio of the low-volatile organic solvent to the total amount (100% by mass) of the rosin compound and the low-volatile organic solvent is preferably 5 to 50% by mass, more preferably 5 to 40% by mass, and further preferably 10 to 30% by mass.
[0076] Examples of low-volatile organic solvents include one or more of MTEM (tetraethylene glycol dimethyl ether), HeDG (diethylene glycol monohexyl ether), TOTM (tri(2-ethylhexyl) trimellitate), DBDG (diethylene glycol dibutyl ether), PhG (ethylene glycol monophenyl ether), and EHDG (2-[2-[(2-ethylhexyl)oxy]ethoxy]ethanol).
[0077] As the low-volatile organic solvent, an ether solvent or an alcohol solvent is preferred from the viewpoints of easy availability of a high-purity product and compatibility with the rosin compound.
[0078] Examples of highly volatile organic solvents include one or more of MB (3-methoxy-1-butanol), MBA (3-methoxybutyl acetate), PNB (1-butoxy-2-propanol), IPA (isopropyl alcohol), EDG (diethylene glycol monoethyl ether), MFDG (dipropylene glycol monomethyl ether), and MFG (propylene glycol monomethyl ether).
[0079] As the highly volatile organic solvent, an ether solvent or an alcohol solvent is preferred from the viewpoints of easy availability of a high-purity product and compatibility with the rosin compound.
[0080] It should be noted that "low volatility" and "high volatility" are relative concepts. Sometimes the low volatility organic solvents exemplified above can also become high volatility organic solvents, or vice versa. In short, no matter what amount ratio of solvent is used, as long as the adhesive force T measured by [Step 1] is 50 gf or more, and the adhesive force T' measured by [Step 2] is 50 gf or more.
[0081] However, from the viewpoints of the availability of solvents, the ease of preparation, the operability, etc., the vapor pressure pL of the low-volatile organic solvent at 20°C is preferably 5 Pa or less, more preferably 0.1 to 5 Pa, and even more preferably 0.5 to 5 Pa. In addition, the vapor pressure pH of the high-volatile organic solvent at 20°C is preferably greater than 6 Pa, more preferably 10 Pa or more, even more preferably 15 to 10,000 Pa, and even more preferably 15 to 5,000 Pa.
[0082] By the way, when the flux contains three or more organic solvents, the following describes whether each organic solvent belongs to a low-volatility organic solvent or a high-volatility organic solvent, and describes how to judge the pH-pL value in this case.
[0083] (i) First, solvents with a vapor pressure of more than 5 Pa at 20° C. are identified as high-volatility organic solvents, and solvents with a vapor pressure of less than 5 Pa are identified as low-volatility organic solvents.
[0084] (ii) The vapor pressure difference is calculated for all combinations of the high-volatility organic solvent and the low-volatility organic solvent identified in (i) above, and the pH-pL value is considered to be 5 Pa or more only when all the calculated values are 5 Pa or more.
[0085] For example, when the flux contains three organic solvents (organic solvents 1, 2 and 3) having a vapor pressure greater than 5 Pa at 20°C and one low-volatility organic solvent (organic solvent 4) having a vapor pressure of less than 5 Pa at 20°C, when the three respective vapor pressure differences of organic solvent 1-organic solvent 4, organic solvent 2-organic solvent 4, and organic solvent 1-organic solvent 4 are all greater than 5 Pa, the pH-pL value is deemed to be greater than 5 Pa.
[0086] The amount of the organic solvent based on the entire flux (100 mass %) is, for example, 30 to 95 mass %, preferably 30 to 90 mass %, and more preferably 30 to 80 mass %.
[0087] In addition, when the organic solvent contains a low-volatile organic solvent and a high-volatile organic solvent, their ratio by mass ratio is, for example, low-volatile organic solvent: high-volatile organic solvent = 5:95 to 95:5, preferably low-volatile organic solvent: high-volatile organic solvent = 10:90 to 90:10, and more preferably low-volatile organic solvent: high-volatile organic solvent = 20:80 to 80:20.
[0088] (Viscosity of flux)
[0089] From the viewpoint of coating properties of the flux on the electrode, it is preferable to appropriately adjust the viscosity of the flux of this embodiment. The viscosity can be adjusted by changing the type and amount ratio of the low-volatile organic solvent and the high-volatile organic solvent.
[0090] As an example, the viscosity of the flux of the present embodiment measured using a B-type viscometer at 20° C., a rotation speed of 12 rpm, and a rotor M2 is preferably 2500 mPa·s or less. The lower limit is, for example, 250 mPa·s or more.
[0091] As another example, the viscosity of the flux of the present embodiment measured using a Brookfield viscometer at 20° C., 30 rpm, and rotor L / Adp is preferably 20 mPa·s or less. The lower limit is, for example, 2 mPa·s or more.
[0092] As another example, the viscosity of the flux of the present embodiment measured using a Brookfield viscometer at 20° C., 30 rpm, and rotor M2 is preferably 1000 mPa·s or less. The lower limit is, for example, 100 mPa·s or more.
[0093] (In order to perform appropriate viscosity measurement, it is important to select measurement conditions, particularly rotation speed and rotor. Therefore, the preferred ranges of viscosity under three different measurement conditions are described above.)
[0094] By optimizing the viscosity, good coating properties can be obtained and good temporary fixation can be obtained after coating.
[0095] (Other added ingredients)
[0096] The soldering flux of this embodiment may contain one or more additive components such as organic acid, amine, surfactant, halide (organic halogen compound, amine hydrohalide), or may not contain any additive components (the content may be 0%). These additive components serve as activators to improve solderability.
[0097] Examples of the organic acid include glutaric acid, adipic acid, azelaic acid, eicosanedioic acid, citric acid, glycolic acid, succinic acid, salicylic acid, diglycolic acid, dipyridinecarboxylic acid, dibutylaniline diglycolic acid, suberic acid, sebacic acid, thioglycolic acid, terephthalic acid, dodecanedioic acid, p-hydroxyphenylacetic acid, phenylsuccinic acid, phthalic acid, fumaric acid, maleic acid, malonic acid, lauric acid, benzoic acid, tartaric acid, tris(2-carboxyethyl)isocyanurate, glycine, 1,3-cyclohexanedicarboxylic acid, 2,2-bis(hydroxymethyl)propionic acid, 2,2-bis(hydroxymethyl)butyric acid, 2,3-dihydroxybenzoic acid, 2,4-diethylglutaric acid, 2-quinolinecarboxylic acid, 3-hydroxybenzoic acid, malic acid, p-anisic acid, stearic acid, 12-hydroxystearic acid, oleic acid, linoleic acid, and linolenic acid.
[0098] Examples of the organic acid include dimer acid, trimer acid, hydrogenated dimer acid, which is a hydrogenated product of hydrogenated dimer acid, and hydrogenated trimer acid, which is a hydrogenated product of hydrogenated trimer acid.
[0099] For example, there can be mentioned a dimer acid as a reaction product of oleic acid and linoleic acid, a trimer acid as a reaction product of oleic acid and linoleic acid, a dimer acid as a reaction product of acrylic acid, a trimer acid as a reaction product of acrylic acid, a dimer acid as a reaction product of methacrylic acid, a trimer acid as a reaction product of methacrylic acid, a dimer acid as a reaction product of acrylic acid and methacrylic acid, a trimer acid as a reaction product of acrylic acid and methacrylic acid, a dimer acid as a reaction product of oleic acid, a trimer acid as a reaction product of oleic acid, a dimer acid as a reaction product of linoleic acid, a trimer acid as a reaction product of linolenic acid, a dimer acid as a reaction product of linolenic acid, a trimer acid as a reaction product of linolenic acid, a dimer acid as a reaction product of acrylic acid and oleic acid, a trimer acid as a reaction product of acrylic acid and linoleic acid, and a dimer acid as a reaction product of acrylic acid and oleic acid. trimer acid as a reaction product of olefinic acid and linoleic acid, dimer acid as a reaction product of acrylic acid and linolenic acid, trimer acid as a reaction product of acrylic acid and linolenic acid, dimer acid as a reaction product of methacrylic acid and oleic acid, trimer acid as a reaction product of methacrylic acid and oleic acid, dimer acid as a reaction product of methacrylic acid and linoleic acid, trimer acid as a reaction product of methacrylic acid and linoleic acid, dimer acid as a reaction product of methacrylic acid and linoleic acid, trimer acid as a reaction product of methacrylic acid and linolenic acid, dimer acid as a reaction product of oleic acid and linolenic acid, trimer acid as a reaction product of linoleic acid and linolenic acid, dimer acid as a reaction product of linoleic acid and linolenic acid, trimer acid as a reaction product of linoleic acid and linolenic acid, hydrogenated dimer acid as a hydrogenated product of the above dimer acids, hydrogenated trimer acid as a hydrogenated product of the above trimer acids, etc.
[0100] When an organic acid is used, only one kind of organic acid may be used, or two or more kinds of organic acids may be used in combination.
[0101] When an organic acid is used, its amount is, for example, greater than 0 mass % and 10 mass % or less, preferably 0.01 to 10 mass %, and more preferably 0.05 to 5 mass %, based on the entire flux including the organic solvent (100 mass %).
[0102] Examples of the amine include monoethanolamine, diphenylguanidine, xylylguanidine, ethylamine, triethylamine, cyclohexylamine, ethylenediamine, triethylenetetramine, 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole trimellitate, 2,4-diamino-6-[2'- methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, 2-phenylimidazoline , 2,4-diamino-6-vinyl-s-triazine, 2,4-diamino-6-vinyl-s-triazine isocyanuric acid adduct, 2,4-diamino-6-methacryloyloxyethyl-s-triazine, epoxy-imidazole adduct, 2-methylbenzimidazole, 2-octylbenzimidazole, 2-pentylbenzimidazole, 2-(1-ethylpentyl)benzimidazole, 2-nonylbenzimidazole, 2-(4-thiazolyl)benzimidazole, benzimidazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-pentylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-octylbenzene 1-[(2-ethylhexyl)aminomethyl]benzotriazole, carboxybenzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]methylbenzotriazole, 2,2'-[[(methyl-1H-benzotriazol-1-yl)methyl]imino]bisethanol, 1-(1',2'-dicarboxyethyl)benzotriazole, 1-(2,3-dicarboxypropyl)benzotriazole, 1-[(2-ethylhexylamino)methyl]benzotriazole, 2,6-bis[(1H-benzotriazol-1-yl)methyl]-4-methylphenol, 5-methylbenzotriazole, 5-phenyltetrazolyl, etc.
[0103] When an amine is used, only one type of amine may be used, or two or more types of amines may be used in combination.
[0104] When an amine is used, its amount is, for example, greater than 0 mass % and 10 mass % or less, preferably 0.01 to 10 mass %, and more preferably 0.05 to 5 mass %, based on the entire flux including the organic solvent (100 mass %).
[0105] Examples of the organic halogen compound include trans-2,3-dibromo-2-butene-1,4-diol, triallyl isocyanurate hexabromide, 1-bromo-2-butanol, 1-bromo-2-propanol, 3-bromo-1-propanol, 3-bromo-1,2-propanediol, 1,4-dibromo-2-butanol, 1,3-dibromo-2-propanol, 2,3-dibromo-1-propanol, 2,3-dibromo-1,4-butanediol, 2,3-dibromo-1,4-butanediol, 2,3-dibromo-2-butene-1,4-diol, tris(2,3-dibromopropyl)isocyanurate, and chlorendic anhydride.
[0106] Amine hydrohalides are compounds formed by reacting amines with hydrogen halides.
[0107] As the amine of the amine hydrohalide, the above-mentioned amines can be used, and ethylamine, cyclohexylamine, ethylenediamine, triethylamine, diphenylguanidine, xylylguanidine, methylimidazole, 2-ethyl-4-methylimidazole, etc. can be mentioned. As the hydrogen halide, chlorine, bromine, iodine, fluorine hydride (hydrogen chloride, hydrogen bromide, hydrogen iodide, hydrogen fluoride) can be mentioned. In addition, amine hydrohalide can be replaced with borofluoride or included with amine hydrohalide, and as the borofluoride, fluoroboric acid, etc. can be mentioned.
[0108] Examples of the amine hydrohalide salt include aniline hydrochloride, cyclohexylamine hydrochloride, aniline hydrobromide, diphenylguanidine hydrobromide, xylylguanidine hydrobromide, and ethylamine hydrobromide.
[0109] When a halide is used, only one type of halide may be used, or two or more types of halide may be used in combination.
[0110] When a halide is used, its amount is, for example, greater than 0 mass % and 10 mass % or less, preferably 0.01 to 10 mass %, and more preferably 0.05 to 5 mass %, based on the entire flux including the organic solvent (100 mass %).
[0111] As the surfactant, there are various surfactants such as cationic, anionic, amphoteric, and nonionic surfactants, and any surfactant can be used as long as the temporary fixation property is not excessively impaired.
[0112] As an example of a preferred surfactant, a fluorine-based surfactant can be cited. Examples of fluorine-based surfactants include the "Surflon" series manufactured by AGC Seimi Chemical Co., Ltd. (AGC), the "Fluorad" series manufactured by 3M, and the "Megaface" series manufactured by DIC.
[0113] Another example of a preferred surfactant is an acrylic surfactant. Examples of acrylic surfactants include the "Polyflow" series manufactured by Kyoeisha Chemical Co., Ltd.
[0114] Another example of a preferred surfactant is a polyether surfactant. Examples of the polyether surfactant include the "Newcol" series manufactured by Nippon Emulsifier Co., Ltd.
[0115] When a surfactant is used, only one type of surfactant may be used, or two or more types of surfactants may be used in combination.
[0116] When a surfactant is used, its amount is, for example, greater than 0 mass % and 5 mass % or less, preferably 0.01 to 3 mass %, and more preferably 0.05 to 2 mass %, based on the entire flux including the organic solvent (100 mass %).
[0117] <How to use flux / Method for manufacturing electronic devices>
[0118] Electronic devices can be manufactured using the soldering flux of this embodiment.
[0119] For example, an electronic device can be manufactured by a series of steps including: a coating step of coating the above-mentioned flux on an electrode; a temporary fixing step of temporarily fixing a preformed solder or an electronic component on the above-mentioned electrode coated with the flux; and a bonding step of heating the above-mentioned electrode and bonding the preformed solder or the electronic component to the above-mentioned electrode.
[0120] The above-mentioned steps and other optional steps will be described with reference to the drawings.
[0121] (Coating process( Figure 1 (a) Figure 1 (b))
[0122] In the coating step, for example, the flux is coated on at least the electrodes of the substrate 1 (electrodes not shown) provided with electrodes, thereby forming a coating film 3 of the flux.
[0123] As the substrate 1, a printed wiring board or the like can be cited. The material constituting the electrode may be any material as long as it can be bonded with solder. The electrode is usually made of copper or a copper alloy.
[0124] The electrodes may be plated with solder in advance. In this case, in the temporary fixing step described later, the electronic components are temporarily fixed instead of the preform solder.
[0125] The flux coating 3 only needs to be provided at least on the electrode portion of the substrate 1. Alternatively, the flux coating 3 may be provided on both the electrode portion and other portions of the substrate 1. In short, the flux only needs to be applied to the portion where the preform solder or electronic component is to be temporarily fixed in the temporary fixing process. Figure 1 In (b), a flux coating film 3 is provided on the entire one surface of the substrate 1 .
[0126] As long as the preform solder or the electronic component is temporarily fixed sufficiently strongly in the temporary fixing step, there is no particular limitation on the thickness of the flux coating film 3. The thickness of the flux coating film 3 is typically 1 to 300 nm, preferably 5 to 250 μm.
[0127] The method for forming the flux coating 3 is not particularly limited. Typically, the flux coating 3 can be formed by a spin coating method, a spray method, a printing method such as screen printing, a slit coating method, or the like. The flux coating 3 may also be formed using a brush. In addition, a spray fluxer, a foaming fluxer, or the like may also be used.
[0128] It is preferred that the organic solvent is appropriately dried after the flux is applied to the substrate. That is, it is preferred that a drying step is provided between the application step and the temporary fixing step. It is preferred that a part of the organic solvent in the applied flux, specifically the highly volatile organic solvent, is dried in the drying step.
[0129] The drying process may be performed at room temperature or by heating. In addition, the drying of the organic solvent in the flux may be accelerated by reducing the pressure. When heating, the heating conditions may be set to, for example, 40 to 100° C. for about 1 to 20 minutes.
[0130] (Temporary Fixing Process( Figure 1 (c))
[0131] In the temporary fixing step, the solder preform or the electronic component 5 is placed on the substrate (electrode) coated with flux and temporarily fixed.
[0132] When the preform solder is temporarily fixed, there is no particular limitation on its shape, size, etc., and it can be appropriately selected according to the shape and size of the electrode on the substrate. The shape of the preform solder can also be, for example, a strip, square, disc, washer, chip, ring, column, sphere or wire. In addition, there is no particular limitation on the alloy composition of the preform solder, as long as the appropriate alloy composition is selected according to various purposes.
[0133] When temporarily fixing electronic components, it is preferred to solder the electronic components in advance or attach them to the electronic components in advance. However, when solder is plated on the substrate (electrode) in advance, it is not necessary to solder or attach the solder to the electronic components in advance.
[0134] (Joining process)
[0135] In the bonding step, the substrate (electrode) is heated to bond the preform or the electronic component 5 to the electrode. The bonding step can be performed by melting the solder using a reflow furnace, for example.
[0136] In the manufacture of industrial electronic equipment, it is sometimes necessary to transport substrates between processes. In this embodiment, electronic components are unlikely to shift between the temporary fixing process and the bonding process, so even if electrodes (substrates) are transported between the temporary fixing process and the bonding process, welding with good positional accuracy can be performed.
[0137] After the flux having an adhesion T of 50 gf or more measured as in [Step 1] is applied to the substrate, it maintains the temporary fixing ability of the preform solder etc. for a certain degree of long time (even after a certain degree of long time after application, it still shows a large adhesion). This property is a preferred property in the manufacture of industrial electronic equipment. This is because, in order to facilitate flow operations in the manufacture of electronic equipment, a certain degree of time is mostly left between the time when the flux etc. is applied to the substrate and the time when the preform solder etc. is temporarily fixed to the substrate.
[0138] In addition, the soldering flux having an adhesive force T of 50 gf or more measured as in [Step 2] has a less change in temporary fixing ability even when conditions (such as temperature and time) vary in each process. This property is a preferred property in the manufacture of electronic devices involving varying conditions.
[0139] (Time between each process)
[0140] It should be noted that the time between each process is supplemented.
[0141] The time between the coating step and the temporary fixing step is, for example, 30 seconds to 200 minutes, specifically, 1 minute to 120 minutes. In this embodiment, by using a flux having an adhesive force T of 50 gf or more and an adhesive force T' of 50 gf or more, even if the time between the coating step and the temporary fixing step is long to a certain extent, the preform solder etc. can be temporarily fixed sufficiently firmly.
[0142] In addition, the time between the temporary fixing process and the joining process is, for example, 30 seconds to 60 minutes, specifically, 1 minute to 30 minutes. In this embodiment, by using a flux having an adhesive force T of 50 gf or more and an adhesive force T' of 50 gf or more, even if the time between the temporary fixing process and the joining process is long to a certain extent, the preform solder etc. can be kept temporarily fixed sufficiently firmly.
[0143] The embodiments of the present invention are described above, but these are examples of the present invention, and various configurations other than the above can be adopted. In addition, the present invention is not limited to the above embodiments, and modifications and improvements within the scope of achieving the purpose of the present invention are also included in the present invention.
[0144] Example
[0145] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. However, the present invention is not limited to the Examples.
[0146] <Preparation of flux>
[0147] The components shown in the following tables were uniformly mixed to prepare fluxes of Examples 1 to 6 and Comparative Examples 1 to 5. Each component was purchased commercially available on the market and used.
[0148] In each table, the unit of the blending amount is mass %.
[0149] Table 1
[0150] Example 1 Amount Polymerized rosin 14.4 Hydrogenated rosin 21.6 HeDG (Diethylene glycol monohexyl ether) 9 IPA (Isopropyl Alcohol) 55
[0151] Table 2
[0152] Example 2 Amount Modified polymerized rosin 21 Hydrogenated acid modified rosin 20 Hydrogenated rosin 20 MTEM (Tetraethylene glycol dimethyl ether) 12 Acrylic acid surfactant 1 MFDG (Dipropylene glycol monomethyl ether) 26
[0153] Table 3
[0154] Example 3 Amount Modified polymerized rosin 43.1 Hydrogenated acid modified rosin 4.85 Glutaric acid 4.75 MTEM (Tetraethylene glycol dimethyl ether) 18.5 MIPA (monoisopropanolamine) 1.8 PNB (1-Butoxy-2-propanol) 26 Megaface F-477 (fluorinated surfactant) 0.5 Surflon S-611 (fluorinated surfactant) 0.5
[0155] Table 4
[0156] Example 4 Amount Modified polymerized rosin 15.4 Hydrogenated acid modified rosin 11.35 Hydrogenated rosin 25.8 Glutaric acid 5.3 MTEM (Tetraethylene glycol dimethyl ether) 15.3 MIPA (monoisopropanolamine) 1.85 MB(3-methoxy-1-butanol) 24 Fluorinated surfactants 0.5 Fluorinated surfactants 0.5
[0157] Table 5
[0158] Example 5 Amount Modified polymerized rosin 15 Hydrogenated acid modified rosin 11.05 Hydrogenated rosin 25.1 Glutaric acid 2.35 MTEM (Tetraethylene glycol dimethyl ether) 14.8 NP-300(amine polyether polyol) 4.7 EDG (Diethylene glycol monoethyl ether) 26 Fluorinated surfactants 0.5 Fluorinated surfactants 0.5
[0159] Table 6
[0160] Example 6 Amount Modified polymerized rosin 15.2 Hydrogenated acid modified rosin 11.1 Hydrogenated rosin 25.7 Glutaric acid 5 MTEM (Tetraethylene glycol dimethyl ether) 20 MIPA (monoisopropanolamine) 2.1 MB(3-methoxy-1-butanol) 9.4 MFDG (Dipropylene glycol monomethyl ether) 10.5 Fluorinated surfactants 0.5 Fluorinated surfactants 0.5
[0161] Table 7
[0162] Comparative Example 1 Comparative Example 2 Comparative Example 3 Polymerized rosin 18 17.46 7.2 Hydrogenated rosin 27 26.19 10.8 HeDG (Diethylene glycol monohexyl ether) 0 1.35 27 IPA (Isopropyl Alcohol) 55 55 55
[0163] Table 8
[0164] Comparative Example 4 Polymerized rosin 18 Hydrogenated rosin 27 MTEM (Tetraethylene glycol dimethyl ether) 5 HeDG (Diethylene glycol monohexyl ether) 50
[0165] Table 9
[0166] Comparative Example 5 Comparative Example 6 Polymerized rosin 12 20 Hydrogenated rosin 20 25 Sebacic acid 1 Diethylene glycol monobutyl ether 4 5 Polyethylene glycol monooleate 1 Acrylic acid surfactant 1 IPA (Isopropyl Alcohol) 62 49
[0167] In addition, for reference, the vapor pressures of the organic solvents used in Examples and Comparative Examples at 20° C. are shown in the following table.
[0168] Table 10
[0169] Vapor pressure (20℃) Pa MTEM (Tetraethylene glycol dimethyl ether) 1 HeDG (Diethylene glycol monohexyl ether) 1.333 MFDG (Dipropylene glycol monomethyl ether) 7.999 MB(3-methoxy-1-butanol) 17 PNB (1-Butoxy-2-propanol) 80 IPA (Isopropyl Alcohol) 4400 EDG (Diethylene glycol monoethyl ether) 13.3 Diethylene glycol monobutyl ether (butyl carbitol) 3
[0170] <Physical property measurement>
[0171] (Measurement of Adhesion Force T)
[0172] The adhesion T of each flux was measured according to (1) to (3) of the above-mentioned [Step 1].
[0173] Supplementary information is recorded for (1) to (3) of [Step 1].
[0174] As the Ni-plated Al plate, a plate having at least five circular depressions with a diameter of 7 mm and a depth of 0.2 mm was used. The adhesive force was measured at each of the five depressions, and the average value thereof was used as the adhesive force T.
[0175] (1) Coating method: Apply a slightly larger amount of flux to the concave surface, then slide the spatula while it is in contact with the board to remove excess flux. 3 (π is the ratio of a circumference of a circle) amount of flux enters the depression.
[0176] Adhesion was measured in accordance with JIS Z 3284-3 using an adhesion tester (model: TK-1) manufactured by Malcom, with a constant pressure intrusion method under the conditions of a pressing time of 0.2 sec, a pressing pressure of 50 gf, an intrusion speed of 2.0 mm / sec, and a pull-off speed of 10 mm / sec. The material of the probe of the adhesion tester was SUS (stainless steel) and the diameter was 5.1 mm.
[0177] The adhesive force was measured under the conditions of 25° C. and 50% RH.
[0178] (Measurement of Adhesion Force T')
[0179] The "heat treatment at 100° C. for 1 minute" in (2) of [Step 1] was changed to "heat treatment at 100° C. for 3 minutes", and the adhesive force T' was measured.
[0180] (Viscosity measurement)
[0181] The viscosity of the flux of each example and comparative example was measured under the following conditions using a B-type viscometer (model: TVB-15) manufactured by Toki Sangyo Co., Ltd.
[0182] Example 1, Comparative Examples 1, 2, and 5: Rotation speed: 30 rpm, rotor: L / Adp (No. 19).
[0183] Comparative Examples 3 and 4: Rotation speed: 60 rpm, rotor: L / Adp (No. 19).
[0184] Example 2: Rotation speed: 12 rpm, rotor: M2 (No. 21).
[0185] Examples 3, 4, 5, and 6: Rotation speed: 30 rpm, rotor: M2 (No. 21)
[0186] <Performance Evaluation>
[0187] (Temporary fixation and coating properties of preform solder (solder particles))
[0188] The evaluation was performed by the following steps.
[0189] (1) Apply 75 ± 15 mg of flux using a brush to the entire surface of a copper plate measuring 50 mm long, 50 mm wide, and 0.3 mm thick.
[0190] (2) The copper plate coated with the flux in (1) was heated on a hot plate at 50° C. for 10 minutes (thereby volatilizing the highly volatile organic solvent in the flux).
[0191] (3) After cooling to room temperature, five solder particles (2 mm long x 2 mm wide, 100 μm thick, composition: 3.0 mass % Sn-1.0 mass % Ag-balance Pb) were gently placed on the flux-coated surface of the copper plate using tweezers.
[0192] (4) After 1 minute, if Figure 2 As shown in FIG. 1 , a vertical copper plate is dropped from a height of 150 mm and impacted. The drop is repeated three times. The direction of the copper plate when the copper plate is dropped is "vertical" (see also Figure 2 ).
[0193] (5) After (4), the deviation of the particles on the copper plate was confirmed. The temporary fixation was considered "good" if the positions of all five particles were not deviated and remained temporarily fixed even after three drops, and the temporary fixation was considered "poor" if even one of the five particles was deviated or fell off during the "first to third drops".
[0194] (6) In the above (1), the case where there was no particular problem with the brush and the flux could be applied sufficiently uniformly was regarded as "good" in terms of coating properties.
[0195] (Temporary fixity stability against process changes)
[0196] In the evaluation of temporary fixation in the above (1) to (5), the temporary fixation of the preform solder (solder particles) was evaluated by replacing "heating on a 50°C hot plate for 10 minutes" in (2) with "heating on a 50°C hot plate for 30 minutes".
[0197] If the temporary fixation properties are good in both "heating on a 50°C hot plate for 10 minutes" and "heating on a 50°C hot plate for 30 minutes", it can be said that the evaluated flux exhibits stable temporary fixation properties even when process conditions vary in the manufacture of electronic devices.
[0198] (Weldability)
[0199] Evaluation was performed by the method described in 8.3.1.1 of JIS Z 3197: 2012. However, the conditions were changed from those described in JIS in that a copper plate (not oxidized) was used as a test piece.
[0200] A spread rate of 50% or more was determined to be good.
[0201] Various information is shown in Tables 10 and 11.
[0202] Incidentally, the soldering flux of Example 6 contains three kinds of organic solvents. Therefore, according to the above procedure, the vapor pressure difference was calculated by all combinations of high-volatility organic solvents and low-volatility organic solvents. And the calculated values are recorded in Table 11.
[0203] Table 11
[0204]
[0205] Table 12
[0206]
[0207] As shown in Table 11, by using the fluxes of Examples 1 to 6 whose adhesion T measured by step 1 is 50 gf or more and whose adhesion T' measured by step 2 is 50 gf or more, the solder particles can be temporarily fixed to the copper plate (electrode) well. In addition, the fluxes of Examples 1 to 6 show stable temporary fixation to process changes in electronic device manufacturing. Furthermore, the evaluation results of the solderability of the fluxes of Examples 1 to 6 are good.
[0208] It should be noted that the fluxes of Examples 1 to 6 had good coating properties.
[0209] On the other hand, as shown in Table 12, even when the fluxes of Comparative Examples 1 to 6 were used, in which the adhesion T measured in step 1 was less than 50 gf and / or the adhesion T' measured in step 2 was less than 50 gf, the solder particles could not be temporarily fixed to the copper plate (electrode) sufficiently firmly. In particular, as shown in Comparative Examples 5 and 6, even when the adhesion T measured in step 1 was 50 gf or more and the adhesion T' measured in step 2 was less than 50 gf, the evaluation results of the stability of the temporary fixity with respect to the process variation were not satisfactory.
[0210] <Additional evaluation: Uniform coating by spin coating>
[0211] For the soldering flux of Example 5, the following evaluation was additionally performed in order to demonstrate that the soldering flux can be applied sufficiently uniformly not only by brush application but also by spin coating.
[0212] A glass substrate made of glass, having a size of 50 mm×50 mm and a thickness of 0.7 mm was prepared, and the flux of Example 6 was applied to one surface of the glass substrate using a spin coater: ACT-400AII manufactured by ACTIVE Co., Ltd. under the following spin coating conditions.
[0213] Spin coating conditions: 300 rpm for 3 sec, then 3000 rpm for 30 sec.
[0214] The glass substrate coated with the solder flux was heated for 20 minutes on a 40°C hot plate (thereby volatilizing the highly volatile organic solvent in the solder flux). Then, it was cooled to room temperature. The uniformity of the solder flux coating film formed on the glass substrate was observed using an optical microscope at a magnification of 500 times.
[0215] As a result of the observation, the coating film was sufficiently uniform, and no significant unevenness or unevenness in film thickness was observed.
[0216] For reference, a photograph of the coating film obtained by the above spin coating is shown in Figure 3A photograph of a coating film obtained by spin-coating a conventional soldering flux which was not intended for temporary fixing purposes on a glass substrate is shown in Figure 4 .and Figure 4 Compared to the coating film shown (obviously non-uniform), Figure 3 The coating film shown is extremely uniform.
[0217] <Reference method>
[0218] In this specification, the description will be mainly about the flux having an adhesion T of 50 gf or more measured in step 1 and an adhesion T′ of 50 gf or more measured in step 2.
[0219] On the other hand, if stable temporary fixation with respect to changes in process conditions in the manufacture of electronic devices is not necessarily considered, it is considered that as long as the adhesion T measured by at least step 1 is 50 gf or more (preform solder and electronic components can be preferably temporarily fixed). The flux in this case is described as follows.
[0220] “A soldering flux comprising a rosin compound and two or more organic solvents and containing no solder alloy and applied to a substrate for use in a form containing no solder alloy, wherein the soldering flux has an adhesion force T of 50 gf or more measured by the following step 1.
[0221] [Step 1]
[0222] (1) A Ni-plated Al plate having a circular depression with a diameter of 7 mm and a depth of 0.2 mm provided on at least one surface thereof is coated with flux in an amount sufficient to fill the depression.
[0223] (2) The Al plate coated with the flux was heated at 100° C. for 1 minute.
[0224] (3) After cooling the Al plate after the heat treatment to room temperature, the adhesion T of the flux present in the depression was measured using an adhesion tester under the conditions of a pressing time of 0.2 sec, a pressing pressure of 50 gf, an intrusion speed of 2.0 mm / sec, and a pulling speed of 10 mm / sec.
[0225] This application claims priority based on Japanese patent application No. 2021-040415 filed on March 12, 2021, Japanese patent application No. 2021-040416 filed on March 12, 2021, and Japanese patent application No. 2021-201425 filed on December 13, 2021, and all disclosed contents are incorporated herein.
[0226] Description of Reference Numerals
[0227] 1: Substrate; 3: Flux coating; 5: Preformed solder or electronic components.
Claims
1. A soldering flux comprising a rosin compound and two or more organic solvents and containing no solder alloy, and being applied on a substrate in a form containing no solder alloy to temporarily fix a preform solder or an electronic component on the substrate, in, The organic solvent at least comprises a low-volatility organic solvent having a vapor pressure of pL at 20°C and a high-volatility organic solvent having a vapor pressure of pH at 20°C, pL<pH, and the value of pH-pL is above 5 Pa. The pL of the low-volatility organic solvent is 0.1 to 5 Pa, The highly volatile organic solvent is one or more of 3-methoxy-1-butanol, 3-methoxy butyl acetate, 1-butoxy-2-propanol, isopropanol, diethylene glycol monoethyl ether, dipropylene glycol monomethyl ether, and propylene glycol monomethyl ether. The ratio of the low-volatile organic solvent to the total of the rosin compound and the low-volatile organic solvent is 5 to 50% by mass. The adhesion T of the flux measured by the following step 1 is 70 to 300 gf. The adhesion T' of the flux measured by the following step 2 is 70 to 300 gf. The value of T' / T is 0.9~3, [Step 1] (1) A Ni-plated Al plate having a circular depression with a diameter of 7 mm and a depth of 0.2 mm on at least one surface is coated with flux in an amount sufficient to fill the depression. (2) The Al plate coated with solder flux was heated at 100° C. for 1 minute. (3) After the Al plate after the heat treatment is cooled to room temperature, the adhesion T of the flux present in the depression is measured using an adhesion tester under the conditions of a pressing time of 0.2 sec, a pressing pressure of 50 gf, an intrusion speed of 2.0 mm / sec, and a pulling speed of 10 mm / sec. [Step 2] The adhesive force T' was measured by the same procedure as in [Procedure 1] except that the conditions of the heat treatment in the above (2) were changed to 100°C for 3 minutes.
2. The soldering flux according to claim 1, in, The soldering flux also contains an organic acid.
3. The soldering flux according to claim 1 or 2, in, The soldering flux further contains an amine compound.
4. The soldering flux according to claim 1 or 2, in, The soldering flux further contains a surfactant.
5. The soldering flux according to claim 1 or 2, in, The soldering flux further contains at least one halide selected from the group consisting of organic halogen compounds and amine hydrohalide salts.
6. The soldering flux according to claim 1 or 2, in, The viscosity measured using a B-type viscometer at 20° C., a rotation speed of 12 rpm, and a rotor M2 was 2500 mPa·s or less.
7. A method for manufacturing an electronic device, in, The manufacturing method of the electronic device comprises: A coating step of coating the soldering flux according to any one of claims 1 to 6 on a substrate; a temporary fixing step of temporarily fixing a solder preform or an electronic component on the substrate coated with the solder flux; and The step of bonding is to heat the substrate to bond the solder preform or the electronic component to the substrate.
8. The method for manufacturing an electronic device according to claim 7, in, The thickness of the flux coating film provided on the substrate is 5 to 250 μm.
9. The method for manufacturing an electronic device according to claim 7 or 8, in, The coating step is performed by one or more methods including spin coating, spraying, printing, slit coating, or brushing.
Citation Information
Patent Citations
Method and apparatus for manufacturing electronic component
JP2003051668A
Flux for solder paste, solder paste, and solder joined body
CN107000133A
Flux for fast-heating method, and solder paste for fast-heating method
CN107107277A
Solder wire soldering flux capable of reducing splashing and preparation method thereof
CN111906472A
Flux
JP1996213746A