Anion resin-based nano-cerium-manganese oxide composite material and its preparation method and application
By loading nano-hydrated cerium oxide and manganese particles in anionic resin, the removal problem of As(III) is solved, the oxidation and adsorption of As(III) is achieved, the removal efficiency and material stability are improved, and the removal efficiency is simplified. Process flow, suitable for deep removal of trivalent arsenic from water bodies.
Patent Information
- Application Number
- CN202311216126.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-20
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-09-20
AI Technical Summary
The prior art is difficult to effectively remove As(III) in water, and As(III) is highly toxic and is more easily adsorbed after oxidation to As(V). There are excessive and operational problems with the addition of existing oxidants, and commonly used carriers such as activated carbon. The mechanical strength is insufficient and it is difficult to meet the long-term use requirements.
Develop an anionic resin-based nanocerium-manganese oxide composite material to achieve the oxidation and adsorption of As(III) by loading nanohydrated cerium oxide and nanohydrated manganese oxide particles in anion exchange resin, using Mn(IV) oxide As(III) is oxidized to As(V), and then adsorbed by Ce(IV) oxide, combining the three-dimensional network structure of the resin and anion exchange group to achieve deep removal of As(III).
The synchronous oxidation-adsorption removal of As(III) is achieved, which improves the removal efficiency of As(III), enhances the mechanical strength and stability of the material, simplifies the process flow, reduces equipment and management investment, and is acidic and The organic ligand can still be effectively removed in the presence of the ligand.
Smart Images

Figure CN117181202B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a nano composite material with adsorption function, a preparation method and application thereof, and in particular to an anion resin-based nano cerium-manganese oxide composite material, a preparation method and application thereof. Background Art
[0002] Arsenic in water environments is mainly inorganic As(III) and As(V). At present, common arsenic treatment technologies mainly include precipitation, flocculation, membrane filtration and adsorption. Among them, adsorption has attracted much attention due to its strong selectivity, low cost and simple operation. Ce(IV) oxide nanoparticles can form internal coordination complexes with arsenic through ligand exchange, thereby achieving specific adsorption of arsenic. It has been proven that they have strong adsorption affinity, large adsorption capacity and strong anti-interference ability. Compared with the commonly used Fe(III) oxide, Ce(IV) oxide has stronger acid stability and resistance to pollution by organic ligands (such as oxalic acid), which gives it a broader application prospect.
[0003] However, nanoparticles are too small to be used in engineering applications. Researchers usually load them into large-sized porous carriers to prepare composite nanomaterials. A large number of studies have shown that the adsorption method has a significant effect on As(V), but the removal effect on As(III) is not ideal. This is mainly because As(III) exists in the form of electrically neutral molecules (H3AsO3) in most water bodies, while As(V) exists as negatively charged anions (H2AsO4 - and HAsO4 2- ), the electrostatic force makes As(V) easier to be captured and removed by the adsorbent. At the same time, As(III), as the main form of arsenic in groundwater, is also more toxic, more than 60 times that of As(V). Therefore, in order to achieve deep purification of As(III), it needs to be oxidized to As(V).
[0004] Some researchers have achieved pre-oxidation of As(III) by adding chemical oxidants to water bodies. Commonly used oxidants include chlorine, ozone, chloramines, hydrogen peroxide and Mn(IV) oxide, but these oxidants have more or less some problems. Compared with the above oxidants, Mn(IV) oxide can not only effectively oxidize As(III), but also effectively control the formation of disinfection by-products. However, when used in the pre-oxidation process, it needs to be directly added to the water body, and there is inevitably the problem of excessive addition. In addition, powdered Mn(IV) oxide also faces practical problems such as difficult operation and needs to be loaded on a suitable carrier.
[0005] At present, the development of arsenic removal materials with dual functions of oxidation and adsorption is a research trend. Patent ZL200610008135.8 discloses a method for preparing, using and regenerating an iron-manganese composite oxide / diatomaceous earth adsorbent. This method achieves the simultaneous oxidation and adsorption of As(III) to a certain extent, but the stability of Fe(III) oxide is insufficient, especially in an acidic environment and an environment containing a large amount of organic ligands (such as oxalic acid, etc.), where there is a risk of loss. Patent CN 109731548 B discloses an activated carbon / zirconium-manganese oxide composite material and its preparation method and application. This method uses activated carbon as a carrier to load Zr(IV)-Mn(IV) oxide. The prepared composite material has good results for the simultaneous oxidation and adsorption of As(III). However, using activated carbon as a carrier, on the one hand, its mechanical strength is difficult to meet the requirements of long-term use, and on the other hand, the activated carbon itself has no functional group and has no additional gain effect on the diffusion and adsorption of pollutants.
[0006] In summary, there is still an urgent need to develop As(III) removal materials that have both oxidation-adsorption dual functions and practical application prospects. Summary of the invention
[0007] Purpose of the invention: The purpose of the present invention is to provide an anion resin-based nano-cerium-manganese oxide composite material for removing As(III) that has both oxidation-adsorption dual functions and has practical application prospects;
[0008] The second object of the present invention is to provide a method for preparing the above-mentioned anionic resin-based nano-cerium-manganese oxide composite material;
[0009] The third object of the present invention is to provide the use of the above-mentioned anion resin-based nano-cerium-manganese oxide composite material in deep removal of trivalent arsenic from water.
[0010] Technical solution: The anion resin-based nano cerium-manganese oxide composite material of the present invention comprises an anion exchange resin, wherein the anion exchange resin matrix is polystyrene-divinylbenzene or polyacrylic acid, the functional group is a quaternary ammonium group or a tertiary amine group, and nano hydrated cerium oxide particles and nano hydrated manganese oxide particles are loaded in the pores of the matrix. The mass fraction of cerium in the composite material is 7-16%, and the mass fraction of manganese is 6-15%.
[0011] The preparation method of the above-mentioned anion resin-based nano-cerium-manganese oxide composite material comprises the following steps:
[0012] (1) dissolving a cerium salt in an aqueous solution of nitric acid to obtain a cerium solution, wherein cerium ions and nitrate ions in the cerium solution form cerium complex anions;
[0013] (2) adding anion exchange resin to the cerium solution, stirring, so that the cerium complex anion is adsorbed on the anion exchange resin, filtering, adding the product to an alkali solution and stirring, so that the cerium complex anion is converted into cerium oxide and precipitated in situ inside the anion exchange resin, filtering, washing to neutrality, and drying to obtain anion resin-based nano-cerium oxide composite material;
[0014] (3) Add the anion resin-based nano-cerium oxide composite material to the potassium permanganate solution and stir to make MO4 - The ions are adsorbed onto anion exchange resin, filtered, and the product is added to an ethanol / water solution and stirred to make MnO4 - It is reduced to MnO2 and precipitated in situ inside the anion exchange resin matrix and filtered;
[0015] (4) adding the material filtered in step (3) into a NaCl solution, stirring to transform, washing with water until neutral, and drying to obtain an anionic resin-based nano-cerium-manganese oxide composite material.
[0016] Wherein, in step (1), the mass fraction of the aqueous solution of nitric acid is 10-40%, and the mass fraction of cerium in the prepared cerium solution is 2-10%. The cerium complex anion is Ce(NO3) m 3-m (m=4, 5, 6) complex anion; the cerium salt is at least one of cerium sulfate, cerium chloride, cerium nitrate or ammonium cerium nitrate.
[0017] Wherein, in step (2), the mass ratio of the anion exchange resin to the cerium solution is 1:5-1:10; the anion exchange resin matrix is polystyrene-divinylbenzene or polyacrylic acid, the functional group is a quaternary ammonium group or a tertiary amine group, and the commercially available model of the anion exchange resin is at least one of D201, D301, 201×4, 201×7, 201×10, IRA400 or IRA900.
[0018] Wherein, in step (2), the mass fraction of the alkali solution is 5-30%, and the mass ratio of the anion exchange resin to the alkali solution is 1:1-1:5.
[0019] Wherein, in step (3), the concentration of potassium permanganate in the solution is 0.01-0.05 mol / L.
[0020] Wherein, in step (3), the mass ratio of the anion resin-based nano-cerium oxide composite material to the potassium permanganate solution is 1:5-1:20.
[0021] Wherein, in step (3), the volume fraction of the ethanol / water solution is 40-60%.
[0022] Wherein, in step (4), the mass fraction of the NaCl solution is 3-10%, and the mass ratio of the filtered material to the NaCl solution is 1:1-1:5; the drying temperature is 50-70°C, preferably using a thermostatic oven for drying.
[0023] The "transformation" in step (4) is a technical term in the field of ion exchange resins. When the ion exchange resin is added to the alkaline solution, many hydroxide ions will be exchanged on the functional groups of the ion exchange resin, which will affect the pH of the water body during subsequent use. Therefore, the material needs to be added to the NaCl solution to transform the material from -OH type to -Cl type, that is, to use Cl - Put OH - The exchange is done to facilitate subsequent use, and this process is called transformation.
[0024] The above-mentioned anion resin-based nano-cerium-manganese oxide composite material is used for deep removal of trivalent arsenic from water bodies.
[0025] The method for deep removal of trivalent arsenic from water specifically comprises the following steps:
[0026] (1) Filtering wastewater containing trivalent arsenic to remove suspended particles and adjusting the pH of the filtrate to between 3.0 and 9.0;
[0027] (2) filling an adsorption tower with the anion resin-based nano-cerium-manganese oxide composite material and passing the filtrate in step (1) through the adsorption tower;
[0028] (3) When the arsenic concentration in the effluent reaches the leakage point, the adsorption is stopped, and the anion resin-based nano-cerium-manganese oxide composite material in the adsorption tower is desorbed and regenerated using a NaOH-NaCl mixed solution, and the composite material is recycled after regeneration.
[0029] Wherein, in step (1), the concentration of the wastewater containing trivalent arsenic is 100-500 μg / L.
[0030] Wherein, in step (2), the operating temperature of the adsorption tower is 5-40°C, and the speed at which the filtrate flows through the adsorption tower is 2-20BV / h.
[0031] Wherein, in step (3), the leakage point is an outlet water arsenic concentration of 10 μg / L. In the present invention, within the effective treatment capacity, the outlet water concentration is lower than 10 μg / L; the mass fractions of NaOH and NaCl in the NaOH-NaCl mixed solution are both 5-20%, the operating temperature is 40-60°C, and the flow rate is 0.5-2.0BV / h.
[0032] Beneficial effects: Compared with the prior art, the present invention achieves the following significant effects:
[0033] (1) The composite material of the present invention uses an anion exchange resin as a matrix and is loaded with cerium oxide and manganese oxide nanoparticles. In the process of removing As(III), Mn(IV) oxide nanoparticles first oxidize As(III) to As(V) which is less toxic and easier to adsorb, and then Ce(IV) oxide nanoparticles adsorb As(V), thereby achieving simultaneous oxidation-adsorption removal of As(III). Compared with Fe(III) oxide adsorption materials, Ce(IV) oxide has stronger chemical stability and has broader practical application prospects.
[0034] (2) The composite material of the present invention uses anion exchange resin as the matrix, and its three-dimensional network structure can effectively limit the loss of metal oxide nanoparticles, and the anion exchange groups on the resin can achieve pre-enrichment and enhanced diffusion of target pollutants through the Donnan membrane effect, and this enhanced effect on pollutant removal is not available in other carriers such as activated carbon and diatomaceous earth. At the same time, the anion exchange resin is a spherical particle with high mechanical strength, which can effectively reduce the pressure drop and is convenient for practical application;
[0035] (3) The present invention provides a method for deep removal of trivalent arsenic from water. The method uses the prepared composite material as the core, simplifies the oxidation and adsorption of As(III) into one process unit, simplifies the traditional two-stage arsenic removal process of pre-oxidation-adsorption, and greatly reduces the investment in site, equipment and management.
[0036] (4) The method for removing trivalent arsenic of the present invention has the ability to remove As(III) in depth with high efficiency. In actual water bodies, even if there are other coexisting ions (SO4 2- , Cl - 、HCO3 - 、NO3 - Under the influence of factors such as atmospheric pressure, atmospheric pressure, etc., the As(III) concentration in water can still be reduced from 100-500μg / L to below 10μg / L in the range of 6000-12000BV; after adsorption saturation, the adsorbent material can be desorbed and regenerated by a NaOH-NaCl mixed solution (mass fraction is 5-20%), with a regeneration rate of more than 95%. The regenerated material can be recycled, thereby effectively reducing the cost of use.
[0037] (5) The present invention can be carried out at room temperature and pressure in a general container, is simple and easy to operate, and the metal oxide loading in the prepared composite material can reach more than 15wt% (calculated as metal), which is an economical and efficient preparation method. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1This is a scanning electron microscope-energy dispersive spectrometer (SEM-EDS) scanning image of the anion resin-based nano-cerium-manganese oxide composite material prepared in Example 1 of the present invention;
[0039] Figure 2 This is a transmission electron microscope (TEM) image of the anionic resin-based nano-cerium-manganese oxide composite material prepared in Example 1 of the present invention;
[0040] Figure 3 This is a graph showing the column test results after deep removal of trivalent arsenic from water according to Example 7 of the present invention;
[0041] Figure 4 This is a graph showing the desorption results of the material after deep removal of trivalent arsenic from water according to Example 7 of the present invention. DETAILED DESCRIPTION
[0042] The present invention is described in further detail below.
[0043] Example 1
[0044] A method for preparing an anionic resin-based nano-cerium-manganese oxide composite material comprises the following steps:
[0045] (1) dissolving 40 g of ammonium cerium nitrate in 250 mL of 20 wt% nitric acid solution, stirring at 180 rpm for 1 h, to prepare a cerium solution for standby use;
[0046] (2) 30 g of commercially available 201×4 resin was washed and dried, and then added to the solution prepared in step (1), and stirred at a speed of 180 rpm for 3 h to allow the cerium precursor to be introduced into the pores of the resin;
[0047] (3) The material after the cerium precursor is introduced in step (2) is drained, added to 50 mL of 5% (w / w) NaOH solution, stirred at 180 rpm, and reacted for 2 h, so that the introduced precursor can be in situ precipitated inside the resin; then the material is drained, washed with water to neutrality, and dried at 50° C. to obtain an anionic resin-based nano-cerium oxide composite material for use, waiting for further loading of manganese oxide;
[0048] (4) Dissolve 0.9875 g of potassium permanganate in 250 mL of water and stir evenly. The molar concentration of the resulting potassium permanganate solution is 0.025 mol / L.
[0049] (5) Add the material obtained in step (3) to the potassium permanganate solution prepared in step (4), stir at a speed of 180 rpm, and react for 4 hours to make MnO4 - The ions are adsorbed onto the resin matrix through the ion exchange effect of the anion resin.
[0050] (6) Adsorbing MnO4 in step (5) - The material was drained and added into 300 mL of 50% ethanol / water solution, stirred at 180 rpm and reacted for 4 h to make the MnO4 - It is reduced to MnO2 by ethanol and precipitated in situ inside the material.
[0051] (7) The material obtained in step (6) was added to 200 mL of 10 wt% NaCl solution and stirred at 180 rpm for 2 h, washed with water until neutral, and then dried in a thermostat at 50° C. to obtain an anionic resin-based nano-cerium-manganese oxide composite material.
[0052] The finished material is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 45% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 10.1% (w / w) and the manganese loading is 9.5% (w / w). The cross-section of the material is scanned by scanning electron microscopy-energy dispersive spectrometer (SEM-EDS), and the results show that the cerium loading in the finished material is 10.1% (w / w) and the manganese loading is 9.5% (w / w). Figure 1 , it can be seen that cerium and manganese are successfully loaded inside the material; through the characterization of the material by transmission electron microscopy (TEM), it can be seen that cerium-manganese oxide is evenly distributed inside the material in the form of nanoparticles. Figure 2 .
[0053] Example 2
[0054] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that 40 g of ammonium cerium nitrate in step (1) is replaced by 20 g of ammonium cerium nitrate.
[0055] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 45% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 7.0% (w / w) and 9.6% (w / w).
[0056] Example 3
[0057] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that 40 g of ammonium cerium nitrate in step (1) is replaced by 100 g of ammonium cerium nitrate.
[0058] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 45% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 16.0% (w / w) and 9.2% (w / w).
[0059] Example 4
[0060] The preparation method of the anion resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that the 20 wt % nitric acid solution in step (1) is replaced by a 10 wt % nitric acid solution.
[0061] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 44% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 8.2% (w / w) and 9.9% (w / w).
[0062] Example 5
[0063] The preparation method of the anion resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that the 20 wt % nitric acid solution in step (1) is replaced by a 40 wt % nitric acid solution.
[0064] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 47% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 10.9% (w / w) and 9.3% (w / w).
[0065] Example 6
[0066] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that 30 g of the commercially available 201×4 resin in step (2) is replaced by 60 g of the commercially available 201×4 resin.
[0067] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 44% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 7.9% (w / w) and 7.3% (w / w).
[0068] Example 7
[0069] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that 50 mL of 5% (w / w) NaOH in step (3) is replaced by 200 mL of 30% (w / w) NaOH.
[0070] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 45% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 10.3% (w / w) and 9.3% (w / w).
[0071] Example 8
[0072] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that 0.9875 g of potassium permanganate in step (4) is replaced by 1.975 g of potassium permanganate.
[0073] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 44% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 9.9% (w / w) and 15% (w / w).
[0074] Example 9
[0075] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that 0.9875 g of potassium permanganate in step (4) is replaced by 0.395 g of potassium permanganate.
[0076] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 45% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 10.4% (w / w) and 6% (w / w).
[0077] Example 10
[0078] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that 0.9875 g of potassium permanganate in step (4) is dissolved in 250 mL of water instead of 0.5925 g of potassium permanganate in 150 mL of water.
[0079] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 46% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 10.1% (w / w) and 8.2% (w / w).
[0080] Embodiment 11
[0081] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that 0.9875 g of potassium permanganate is dissolved in 250 mL of water in step (4) instead of 2.37 g of potassium permanganate being dissolved in 600 mL of water.
[0082] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 44% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 9.9% (w / w) and 10.1% (w / w).
[0083] Example 12
[0084] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that the 200 mL 10 wt % NaCl solution in step (7) is replaced by 200 mL 3 wt % NaCl solution.
[0085] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 45% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 9.9% (w / w) and 9.6% (w / w).
[0086] Examples 2 to 12 demonstrate that the cerium and manganese loadings of the composite material can be regulated by changing the raw material dosage.
[0087] Example 13
[0088] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that 40 g of ammonium cerium nitrate in step (1) is replaced by 30 g of cerium nitrate.
[0089] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 45% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 12.1% (w / w) and 9.4% (w / w).
[0090] Embodiment 14
[0091] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that 40 g of ammonium cerium nitrate in step (1) is replaced by 20 g of cerium chloride.
[0092] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 44% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 10.9% (w / w) and 9.5% (w / w).
[0093] Example 13 and Example 14 demonstrate that in the present invention, different cerium salts can be used as raw materials and good loading effects can be achieved.
[0094] Embodiment 15
[0095] The preparation method of the anion resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that the 201×4 resin in step (2) is replaced by D201 resin, which is a macroporous strong base anion exchange resin with a skeleton of polystyrene-divinylbenzene and a functional group of quaternary ammonium group.
[0096] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 45% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 10.9% (w / w) and 10.1% (w / w).
[0097] Example 16
[0098] The preparation method of the anion resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that the 201×4 resin in step (2) is replaced by D301 resin, which is a macroporous weak base anion exchange resin with a skeleton of polystyrene-divinylbenzene and a functional group of tertiary amine.
[0099] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 45% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 10.6% (w / w) and 9.7% (w / w).
[0100] Example 15 and Example 16 demonstrate that in the present invention, different anion exchange resins can be used as carriers, and good loading effects can be achieved.
[0101] Embodiment 17
[0102] The preparation method of the anionic resin-based nano-cerium-manganese oxide composite material is similar to that of Example 1, except that 40 g of ammonium cerium nitrate in step (1) is replaced by 160 g of ammonium cerium nitrate, and 250 mL of 20 wt% nitric acid solution is replaced by 1000 mL of 20 wt% nitric acid solution; 20 g of 201×4 resin in step (B) is replaced by 80 g of 201×4 resin; 50 mL of 10% (w / w) NaOH solution in step (3) is replaced by 200 mL of 10% (w / w) NaOH solution; 0.9875 g of potassium permanganate dissolved in 250 mL of water in step (4) is replaced by 3.95 g of potassium permanganate dissolved in 1 L of water; 300 mL of 50% ethanol / water solution in step (6) is replaced by 1.2 L of 50% ethanol / water solution; 200 mL of 10 wt% NaCl solution in step (7) is replaced by 800 mL of 10 wt% NaCl solution; 10wt% NaCl solution.
[0103] The composite material prepared in this embodiment is spherical, with a diameter of 0.6-0.8 mm and a moisture content of 45% (v / v). After drying, the cerium loading in the finished material is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) to be 9.8% (w / w) and 9.4% (w / w).
[0104] This embodiment proves that in the present invention, the increase in output can be achieved by proportionally amplifying the material dosage, and the load effect remains unchanged.
[0105] Embodiment 18
[0106] A method for deep removal of trivalent arsenic from water, characterized in that it comprises the following steps:
[0107] (1) Prepare wastewater containing trivalent arsenic, with a trivalent arsenic concentration of 200 μg / L and SO4 2- , Cl - 、HCO3 - 、NO3 - The concentrations were 100 mg / L, 100 mg / L, 100 mg / L, and 5 mg / L, respectively. After filtration, the raw water pH was adjusted to 7.0;
[0108] (2) filling an adsorption tower with the composite material prepared in Example 1, and passing the arsenic-containing wastewater prepared in step (1) through the adsorption tower at a temperature of 20° C. at a flow rate of 10 BV / h;
[0109] (3) When the arsenic concentration in the outlet water reaches the leakage point of 10 μg / L, the adsorption is stopped and a NaOH-NaCl mixed solution with a mass fraction of 5% is passed through the adsorption tower to regenerate the material by adsorption. The temperature is controlled at 50°C and the flow rate is 1 BV / h.
[0110] In this embodiment, the arsenic concentration of the effluent can be reduced to below 10 μg / L, and the treatment capacity is about 9150 BV. Figure 3 , and more than 95% of arsenic can be desorbed using only 7BV of desorption solution. Figure 4 .
[0111] Embodiment 19
[0112] The method for deep removal of trivalent arsenic from water is similar to that of Example 18, except that the NaOH-NaCl mixed solution with a mass fraction of 5% in step (3) is replaced by a NaOH-NaCl mixed solution with a mass fraction of 10%.
[0113] In this embodiment, the arsenic concentration of the effluent can be reduced to below 10 μg / L, the treatment capacity is about 8700 BV, and more than 95% of the arsenic can be desorbed using only 5 BV of desorption liquid.
[0114] This example demonstrates that in the present invention, the desorption efficiency can be increased by increasing the concentration of the desorption solution.
[0115] Embodiment 20
[0116] The method for deeply removing trivalent arsenic from water is similar to that in Example 18, except that the concentration of trivalent arsenic in step (1) is replaced from 200 μg / L to 100 μg / L.
[0117] In this embodiment, the arsenic concentration of the effluent can be reduced to below 10 μg / L, the processing capacity is about 11900 BV, and more than 95% of the arsenic can be desorbed using only 9 BV of desorption liquid.
[0118] Embodiment 21
[0119] The method for deeply removing trivalent arsenic from water is similar to that in Example 18, except that the concentration of trivalent arsenic in step (1) is replaced from 200 μg / L to 500 μg / L.
[0120] In this embodiment, the arsenic concentration of the effluent can be reduced to below 10 μg / L, the treatment capacity is about 6100 BV, and more than 95% of the arsenic can be desorbed using only 12 BV of desorption liquid.
[0121] Example 20 and Example 21 demonstrate that in the present invention, the As(III) concentration in the raw water has a good effect in the range of 100-500 μg / L.
[0122] Embodiment 22
[0123] The method for deep removal of trivalent arsenic from water is similar to that in Example 18, except that the SO4 in step (1) is replaced by 2- , Cl - 、HCO3 - 、NO3- The concentrations were changed from 100 mg / L, 100 mg / L, 100 mg / L, and 5 mg / L to 200 mg / L, 200 mg / L, 200 mg / L, and 10 mg / L respectively.
[0124] In this embodiment, the arsenic concentration of the effluent can be reduced to below 10 μg / L, the treatment capacity is about 8600 BV, and more than 95% of the arsenic can be desorbed using only 10 BV of desorption liquid.
[0125] This example proves that the method for deep removal of trivalent arsenic from water bodies proposed by the present invention is less affected by coexisting ions in the water bodies and has good application prospects.
[0126] Embodiment 23
[0127] The method for deep removal of trivalent arsenic from water is similar to that in Example 18, except that the pH of the raw water in step (1) is adjusted from 7.0 to 3.0.
[0128] In this embodiment, the arsenic concentration of the effluent can be reduced to below 10 μg / L, the treatment capacity is about 9100 BV, and more than 95% of the arsenic can be desorbed using only 12 BV of desorption liquid.
[0129] Embodiment 24
[0130] The method for deep removal of trivalent arsenic from water is similar to that in Example 18, except that the pH of the raw water in step (1) is adjusted from 7.0 to 9.0.
[0131] In this embodiment, the arsenic concentration of the effluent can be reduced to below 10 μg / L, the treatment capacity is about 8400 BV, and more than 95% of the arsenic can be desorbed using only 8 BV of desorption liquid.
[0132] Example 23 and Example 24 demonstrate that the method for deep removal of trivalent arsenic from water bodies proposed in the present invention has a wide pH applicable range and can produce a good removal effect on As(III) regardless of whether it is in an acidic, neutral or weakly alkaline environment.
[0133] Embodiment 25
[0134] The method for deep removal of trivalent arsenic from water is similar to that of Example 18, except that the trivalent arsenic-containing wastewater prepared in step (1) is replaced with groundwater from a certain place in Shanxi Province, with a total arsenic content of 200-250 μg / L, of which As(III) accounts for about 70-80%. In addition to arsenic, the wastewater also contains Ca 2+ Mg 2+ Isocations and SO4 2- , Cl - 、HCO3 - 、NO3 -Isoanions, raw water pH is 7.5-8.5, TOC is about 1.8mg / L.
[0135] In this embodiment, the arsenic concentration of the effluent can be reduced to below 10 μg / L, the treatment capacity is about 8400 BV, and more than 95% of the arsenic can be desorbed using only 13 BV of desorption liquid.
[0136] Embodiment 26
[0137] The method for deep removal of trivalent arsenic from water is similar to that of Example 18, except that the prepared trivalent arsenic-containing wastewater in step (1) is replaced with contaminated surface water from a certain place in Henan Province, with a total arsenic content of 300-500 μg / L, of which As(III) accounts for about 40-50%. In addition to arsenic, the wastewater also contains Ca 2+ Mg 2+ Cations and SO4 2- , Cl - 、HCO3 - 、NO3 - Isoanions, raw water pH is 6.0-7.0, TOC is about 3.5mg / L.
[0138] In this embodiment, the arsenic concentration of the effluent can be reduced to below 10 μg / L, the treatment capacity is about 7800 BV, and more than 95% of the arsenic can be desorbed using only 16 BV of desorption liquid.
Claims
1. An anionic resin-based nano-cerium-manganese oxide composite material, characterized in that: The composite material comprises an anion exchange resin, wherein the matrix of the anion exchange resin is polystyrene-divinylbenzene or polyacrylic acid, the functional group is a quaternary ammonium group or a tertiary amine group, and nano-hydrated cerium oxide particles and nano-hydrated manganese oxide particles are loaded in the pores of the matrix, and the mass fraction of cerium in the composite material is 7-16%, and the mass fraction of manganese is 6-15%; The preparation method of the anion resin-based nano cerium-manganese oxide composite material comprises the following steps: (1) dissolving a cerium salt in an aqueous solution of nitric acid to obtain a cerium solution, wherein cerium ions and nitrate ions in the cerium solution form cerium complex anions; the mass fraction of the aqueous solution of nitric acid is 10-40%, and the mass fraction of cerium in the obtained cerium solution is 2-10%; (2) adding anion exchange resin to the cerium solution, stirring, so that the cerium complex anion is adsorbed on the anion exchange resin, filtering, adding the product to an alkali solution and stirring, so that the cerium complex anion is converted into cerium oxide and precipitated in situ inside the anion exchange resin, filtering, washing to neutrality, and drying to obtain anion resin-based nano-cerium oxide composite material; (3) Add the anion resin-based nano-cerium oxide composite material to the potassium permanganate solution and stir to make MnO4 - The ions are adsorbed onto anion exchange resin, filtered, and the product is added to an ethanol / water solution and stirred to make MnO4 - It is reduced to MnO2 and precipitated in situ inside the anion exchange resin matrix and filtered; (4) Add the filtered material in step (3) into a NaCl solution, stir to transform, wash with water until neutral, and dry to obtain an anionic resin-based nano-cerium-manganese oxide composite material.
2. The anionic resin-based nano-cerium-manganese oxide composite material according to claim 1, characterized in that: In step (2), the mass ratio of the anion exchange resin to the cerium solution is 1:5-1:
10.
3. The anionic resin-based nano-cerium-manganese oxide composite material according to claim 1, characterized in that: In step (2), the mass fraction of the alkali solution is 5-30%, and the mass ratio of the anion exchange resin to the alkali solution is 1:1-1:
5.
4. The anion resin-based nano-cerium-manganese oxide composite material according to claim 1, characterized in that: In step (3), the concentration of potassium permanganate in the solution is 0.01-0.05 mol / L.
5. The anionic resin-based nano-cerium-manganese oxide composite material according to claim 1, characterized in that: In step (3), the mass ratio of the anion resin-based nano-cerium oxide composite material to the potassium permanganate solution is 1:5-1:
20.
6. The anion resin-based nano-cerium-manganese oxide composite material according to claim 1, characterized in that: In step (4), the mass fraction of the NaCl solution is 3-10%; the mass ratio of the filtered material to the NaCl solution is 1:1-1:
5.
7. Use of the anion resin-based nano-cerium-manganese oxide composite material according to claim 1 in deep removal of trivalent arsenic from water.
8. The use of the anion resin-based nano-cerium-manganese oxide composite material in deep removal of trivalent arsenic from water according to claim 7, characterized in that: The following steps are involved: (1) Filter wastewater containing trivalent arsenic, remove suspended particles, and adjust the pH of the filtrate to between 3.0 and 9.0; (2) filling an adsorption tower with the anionic resin-based nano-cerium-manganese oxide composite material of claim 1, and passing the filtrate in step (1) through the adsorption tower; (3) When the arsenic concentration in the effluent reaches the leakage point, the adsorption is stopped, and the anion resin-based nano-cerium-manganese oxide composite material in the adsorption tower is desorbed and regenerated using a NaOH-NaCl mixed solution, and the regenerated material is recycled.
Citation Information
Cited By
Novel resin-based filtering material as well as preparation method and application thereof
CN119912024A
A resin-based filter material, its preparation method and application
CN119912024B