Non-aqueous electrolyte and secondary battery

By using a variety of lithium salt combinations and non-aqueous electrolytes with specific additives in lithium-ion batteries, the electrolyte decomposition problem of lithium-ion batteries under high voltage and high temperature is solved, the cycle performance and thermal stability of the battery are improved, and the battery is extended improved battery life.

CN117199526BActive Publication Date: 2024-10-25ZHONGNENG RUIXIN (XIAMEN) ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311224641.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-21
Publication Date
2024-10-25
Estimated Expiration
2043-09-21

AI Technical Summary

Technical Problem

Existing lithium-ion batteries are prone to electrolyte decomposition at high voltages and temperatures, leading to safety hazards and battery performance degradation. Moreover, existing electrolytes are prone to oxidative decomposition when higher than 4.3V, producing by-products and affecting the stability of electrode materials. .

Method used

A non-aqueous electrolyte is used, including a variety of lithium salt combinations, additives such as 1,3-propanediol 3-cyanophenylborate, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ethers. , as well as mixed solvents with high pressure resistance and high ionic conductivity, form a synergistic effect, improve the stability and thermal stability of the electrolyte, and prevent side reactions and transition metal ion dissolution.

Benefits of technology

Under an operating voltage in the range of 3 to 5.4V, the cycle performance and thermal stability of the battery are improved, the cycle life of the battery is extended, and the utilization of electrode materials and the high-temperature storage performance of the battery are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117199526B_ABST
    Figure CN117199526B_ABST
Patent Text Reader

Abstract

The present invention provides a non-aqueous electrolyte and a secondary battery. The non-aqueous electrolyte comprises a mixed lithium salt, an additive and a mixed solvent; the additive comprises a first additive and a second additive; the first additive comprises a combination of 3-cyanophenylboronic acid-1,3-propylene glycol ester, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether. The non-aqueous electrolyte provided by the present invention has the advantages of a wide voltage range and good thermal stability. Under an operating voltage in the range of 3 to 5.4 V, the cycle performance of the assembled battery is improved, solving the problems of a series of side reactions such as electrolyte decomposition generated by the battery under high voltage in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrolyte materials, and in particular relates to a non-aqueous electrolyte and a secondary battery. Background Art

[0002] With the continuous development of the new energy industry, lithium-ion batteries are widely used in all aspects of daily life. However, every year there are cases of casualties and property losses caused by the combustion or even explosion of lithium-ion batteries. Therefore, while constantly pursuing its high energy density, the safety issue of lithium-ion batteries has always attracted much attention. This is also one of the battery performances that both R&D personnel and consumers attach great importance to.

[0003] After research, it was found that the thermal runaway phenomenon of some batteries was caused by destructive actions such as collisions, while the thermal runaway of other batteries may be caused by the long-term serious degradation of the batteries themselves under high temperature or high voltage, resulting in the accumulation of problems such as electrolyte decomposition and gas production, destruction of the positive / negative electrode structure, thickening of the SEI film, and increased impedance. In order to fundamentally ensure the safety performance of the battery cell, the selection of battery cell raw materials with high safety is one of the key links. In order to ensure that the battery cell has a high energy density, most of the existing technologies use positive electrode main materials with a higher charging and discharging platform, such as ternary positive electrode materials, binary positive electrode materials or lithium iron manganese phosphate materials, so the electrolyte needs to be adapted to have stable performance under high voltage and high temperature.

[0004] The electrolyte generally includes electrolyte salt, non-aqueous solvent and various functional additives. Among them, the prior art discloses that the widely used lithium salt is lithium hexafluorophosphate, and the solvent is a carbonate solvent. The above electrolyte system is prone to oxidative decomposition when the voltage is higher than 4.3V, and produces byproducts such as hydrogen fluoride, which makes the interface stability between the electrode material and the electrolyte poor, thereby causing the electrolyte to decompose and the transition metal ions in the positive electrode material to dissolve. At the same time, the lithium salt is continuously consumed, which reduces the electrical performance of the battery in the short term, and there are certain safety hazards in long-term use.

[0005] Based on the above phenomenon, it is urgent to propose an electrolyte system to improve the working performance of the battery under high voltage and high temperature. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a non-aqueous electrolyte and a secondary battery. The non-aqueous electrolyte provided by the present invention has the advantages of a wide voltage range and good thermal stability. Under an operating voltage range of 3 to 5.4V, the cycle performance of the assembled battery is improved, solving the problem of a series of side reactions such as electrolyte decomposition generated by the battery under a high voltage state greater than 4.3V in the prior art.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a non-aqueous electrolyte, the non-aqueous electrolyte comprising a mixed lithium salt, an additive and a mixed solvent;

[0009] The additives include a first additive and a second additive;

[0010] The first additive includes a combination of 1,3-propylene glycol 3-cyanophenylboronic acid ester, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether.

[0011] Firstly, the present invention adopts a combination of multiple lithium salts with synergistic effects, so that the performance of lithium hexafluorophosphate is more stable, which is beneficial to promote the formation of SEI film on the surface of positive and negative electrodes, and fully plays a role in reducing the internal impedance of the battery and improving the thermal stability of the electrolyte;

[0012] Secondly, the cyano group with high polarity in the structure of 3-cyanophenylboronic acid-1,3-propylene glycol ester can combine with the positive electrode surface to form a protective film, mask the active sites on the positive electrode surface, avoid direct contact between the electrode material and the electrolyte, and prevent the electrolyte from continuously reacting on the electrode surface, thereby inhibiting a series of side reactions and generating gas. It can also prevent the transition metal ions from dissolving and depositing on the negative electrode side, thereby extending the cycle life of the battery; N,N-dimethyl 4-fluorobenzenesulfonamide can be reduced on the negative electrode surface to form a stable and thin SEI film, thereby improving the high-temperature storage performance and low-temperature discharge capacity of the battery; fatty acid polyoxyethylene ether can reduce the surface tension of the system, which not only enhances the wettability and penetration rate of the electrolyte to the diaphragm, but also improves the wettability to the electrode material with a high specific surface area, reduces the contact resistance, and comprehensively improves the utilization rate of the active material and the cycle stability of the battery;

[0013] Finally, a mixed solvent with high voltage resistance and high ionic conductivity is used to further improve the stability and coulombic efficiency of the electrolyte.

[0014] Preferably, the mass ratio of 3-cyanophenylboronic acid-1,3-propylene glycol ester, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether in the first additive is (2-6):(2-6):(1.5-5), for example, it can be 2:2:1.5, 3:3:1.5, 4:4:1.5, 4.2:4.2:1.8, 4.5:4.5:2, 4.8:4:2.2, 4:4.8:2.5, 5:5:3, 5.2:4.5:3.5, 5.5:5:4, 6:5.5:5, 6:6:5, etc.

[0015] In the present invention, by adjusting the mass ratio of 3-cyanophenylboronic acid-1,3-propylene glycol ester, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether, the wettability and overall cycle performance of the battery pole piece are greatly improved. A too low mass ratio will lead to a deviation in the cycle performance, and vice versa, the pole piece wetting effect will be deviated.

[0016] Preferably, based on the total mass of the non-aqueous electrolyte as 100%, the mass percentage of the first additive is 1.9% to 3.8%, for example, it can be 1.9%, 2%, 2.2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.8%, etc.

[0017] Preferably, the second additive is a flame retardant additive.

[0018] Preferably, the flame retardant additive comprises trimethyl phosphate.

[0019] Preferably, based on the total mass of the non-aqueous electrolyte as 100%, the mass percentage of the second additive is 1.8% to 5.4%, preferably 2.9%, for example, it can be 1.8%, 2%, 2.2%, 2.5%, 2.8%, 2.9%, 3%, 3.2%, 3.5%, 3.7%, 3.8%, 4%, 4.2%, 4.5%, 4.8%, 5%, 5.2%, 5.4%, etc.

[0020] Preferably, the mixed lithium salt comprises a combination of lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, boric acid lithium salt and phosphate lithium salt.

[0021] Preferably, the borate lithium salt includes any one of lithium dioxalatoborate, lithium difluorooxalatoborate, lithium tetrafluoroborate or lithium dicyanooxalatoborate, or a combination of at least two thereof.

[0022] Preferably, the phosphate-based lithium salt includes any one of lithium difluorophosphate, lithium oxalate phosphate or lithium tetrafluorooxalate phosphate, or a combination of at least two thereof.

[0023] Preferably, the mass ratio of the lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, boric acid lithium salt and phosphate lithium salt is (0.3-0.4):(0.6-1.1):(0.2-0.5):(0.1-0.3), for example, it can be 0.3:0.6:0.2:0.1, 0.32:0.62:0.3:0.12, 0.35:0.7:0.4:0.15, 0.38:0.8:0.3:0.2, 0.4:1:0.4:0.22, 0.3:1.1:0.5:0.25, 0.4:1.1:0.3:0.3, etc.

[0024] In the present invention, by regulating the mass ratio of lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, boric acid lithium salt and phosphate lithium salt, the electrolyte has a higher ionic conductivity, which helps to form a stable and low-impedance SEI film during battery formation, and ultimately improves the battery cycle performance. Too low a mass ratio will weaken the comprehensive performance of the electrolyte, and vice versa.

[0025] Preferably, based on the total mass of the non-aqueous electrolyte being 100%, the mass percentage of the mixed lithium salt is 13% to 18%, for example, 13%, 14%, 15%, 16%, 17%, 18%, etc.

[0026] Preferably, the mixed solvent comprises a combination of a carbonate solvent, an ether solvent and a sulfone solvent.

[0027] In the present invention, the performance of ether solvents is stable, especially cyclic ether solvents can improve the conductivity of the system, and sulfone solvents can withstand high pressure and are not easy to decompose, which further improves the stability and coulombic efficiency of the electrolyte.

[0028] Preferably, the carbonate solvent includes any one of ethylene carbonate, propylene carbonate, ethylene carbonate or ethyl methyl carbonate, or a combination of at least two of them.

[0029] Preferably, the ether solvent includes diethylene glycol dimethyl ether and / or 2-methyltetrahydrofuran.

[0030] Preferably, the sulfone solvent includes any one of 3,3,3-trifluoropropyl methyl sulfone, cyclopentane or methyl ethyl sulfone, or a combination of at least two thereof.

[0031] Preferably, the mass ratio of the carbonate solvent, the ether solvent and the sulfone solvent in the mixed solvent is (1.4-5.7):1:(0.1-0.6), for example, it can be 1.4:1:0.1, 1.6:1:0.2, 1.8:1:0.3, 2:1:0.4, 2.5:1:0.5, 3:1:0.6, 4:1:0.2, 5:1:0.3, 5.7:1:0.4, etc.

[0032] In the present invention, the stability of the electrolyte is kept in an optimal state by regulating the mass ratio of the carbonate solvent, the ether solvent and the sulfone solvent. Too low a mass ratio will reduce its stability, and vice versa.

[0033] Preferably, based on the total mass of the non-aqueous electrolyte as 100%, the mass percentage of the mixed solvent is 72.8% to 78.6%, for example, it can be 72.8%, 73%, 73.5%, 74%, 74.5%, 75%, 75.5%, 76%, 76.5%, 77%, 77.5%, 78%, 78.6%, etc.

[0034] In a second aspect, the present invention provides a secondary battery, comprising a positive electrode, a negative electrode, an electrolyte and a separator, wherein the electrolyte comprises the non-aqueous electrolyte according to the first aspect.

[0035] Preferably, the material of the positive electrode includes lithium nickel cobalt manganese oxide.

[0036] Preferably, the material of the negative electrode includes graphite.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] The present invention provides a non-aqueous electrolyte. Firstly, by using a combination of multiple lithium salts with synergistic effects, the performance of lithium hexafluorophosphate is more stable, which is beneficial to promote the formation of SEI film on the surface of positive and negative electrodes, and fully plays a role in reducing the internal impedance of the battery and improving the thermal stability of the electrolyte.

[0039] Secondly, the cyano group with high polarity in the structure of 3-cyanophenylboronic acid-1,3-propylene glycol ester can combine with the positive electrode surface to form a protective film, mask the active sites on the positive electrode surface, avoid direct contact between the electrode material and the electrolyte, and prevent the electrolyte from continuously reacting on the electrode surface, thereby inhibiting a series of side reactions and generating gas. It can also prevent the transition metal ions from dissolving and depositing on the negative electrode side, thereby extending the cycle life of the battery; N,N-dimethyl 4-fluorobenzenesulfonamide can be reduced on the negative electrode surface to form a stable and thin SEI film, thereby improving the high-temperature storage performance and low-temperature discharge capacity of the battery; fatty acid polyoxyethylene ether can reduce the surface tension of the system, which not only enhances the wettability and penetration rate of the electrolyte to the diaphragm, but also improves the wettability to the electrode material with a high specific surface area, reduces the contact resistance, and comprehensively improves the utilization rate of the active material and the cycle stability of the battery;

[0040] Finally, a mixed solvent with high voltage resistance and high ionic conductivity is used to further improve the stability and coulombic efficiency of the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 Normal temperature cycle performance diagram of the battery provided for Application Examples 1-3, Comparative Application Examples 1-3 and Comparative Application Example 6;

[0042] Figure 2 High temperature cycle performance diagram of the batteries provided for Application Examples 1-3, Comparative Application Examples 1-3 and Comparative Application Example 6. DETAILED DESCRIPTION

[0043] The technical solution of the present invention is further described below by combining the accompanying drawings and specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0044] Example 1

[0045] This embodiment provides a non-aqueous electrolyte and a preparation method thereof, which comprises the following steps:

[0046] In a glove box filled with inert gas and with water and oxygen contents less than 0.1 ppm, the mixed lithium salt is stirred until fully dissolved in the mixed solvent, and then the first additive and the second additive are added and stirred to obtain a non-aqueous electrolyte. Taking the total mass of the non-aqueous electrolyte as 100%, the composition of the mixed lithium salt is a combination of lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium bis(oxalate)borate and lithium difluorophosphate in a mass ratio of 0.35:0.82:0.23:0.23, and the mass percentage of the mixed lithium salt is 17.5wt.%; the composition of the mixed solvent is a combination of ethylene carbonate, ethyl methyl carbonate, diethylene glycol dimethyl ether and cyclopentane sulfone in a mass ratio of 1.7:3.9:1:0.3, and the mass percentage of the mixed solvent is 77.6wt.%; the composition of the first additive is a combination of 3-cyanophenylboronic acid-1,3-propylene glycol ester, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether in a mass ratio of 4:4:2, and the mass percentage of the first additive is 2.0wt.%; the second additive is trimethyl phosphate, and the mass percentage is 2.9.wt.%.

[0047] Example 2

[0048] The difference between this embodiment and embodiment 1 is that the composition of the first additive is a combination of 3-cyanophenylboronic acid-1,3-propylene glycol ester, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether in a mass ratio of 3.5:4.5:2, and the rest is the same as embodiment 1.

[0049] Example 3

[0050] The difference between this embodiment and embodiment 1 is that the composition of the first additive is a combination of 3-cyanophenylboronic acid-1,3-propylene glycol ester, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether in a mass ratio of 4.5:3.5:2, and the rest is the same as embodiment 1.

[0051] Example 4

[0052] The difference between this embodiment and embodiment 1 is that the composition of the first additive is a combination of 3-cyanophenylboronic acid-1,3-propylene glycol ester, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether in a mass ratio of 5:3:2, and the rest is the same as embodiment 1.

[0053] Example 5

[0054] The difference between this embodiment and embodiment 1 is that the composition of the first additive is a combination of 3-cyanophenylboronic acid-1,3-propylene glycol ester, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether in a mass ratio of 3:5:2, and the rest is the same as embodiment 1.

[0055] Example 6

[0056] The difference between this embodiment and embodiment 1 is that the composition of the mixed lithium salt is a combination of lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium bis(oxalatoborate) and lithium difluorophosphate in a mass ratio of 0.34:0.8:0.21:0.29, and the rest is the same as embodiment 1.

[0057] Example 7

[0058] The difference between this embodiment and embodiment 1 is that the composition of the mixed lithium salt is a combination of lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, lithium bis(oxalatoborate) and lithium difluorophosphate in a mass ratio of 0.36:0.9:0.32:0.19, and the rest is the same as embodiment 1.

[0059] Example 8

[0060] The difference between this embodiment and embodiment 1 is that the composition of the mixed solvent is a combination of ethylene carbonate, ethyl methyl carbonate, diethylene glycol dimethyl ether and cyclopentane sulfone in a mass ratio of 1.5:2.9:1:0.45, and the rest is the same as embodiment 1.

[0061] Comparative Example 1

[0062] The difference between this comparative example and Example 1 is that the composition of the first additive is a combination of 3-cyanophenylboronic acid-1,3-propylene glycol ester and N,N-dimethyl 4-fluorobenzenesulfonamide in a mass ratio of 1:1, and the rest is the same as Example 1.

[0063] Comparative Example 2

[0064] The difference between this comparative example and Example 1 is that the composition of the first additive is a combination of 3-cyanophenylboronic acid-1,3-propylene glycol ester and fatty acid polyoxyethylene ether in a mass ratio of 8:2, and the rest is the same as Example 1.

[0065] Comparative Example 3

[0066] The difference between this comparative example and Example 1 is that the composition of the first additive is a combination of N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether in a mass ratio of 8:2, and the rest is the same as Example 1.

[0067] Comparative Example 4

[0068] The difference between this comparative example and Example 1 is that the first additive is 3-cyanophenylboronic acid-1,3-propylene glycol ester, and the rest is the same as Example 1.

[0069] Comparative Example 5

[0070] The difference between this comparative example and Example 1 is that the first additive is N,N-dimethyl 4-fluorobenzenesulfonamide, and the rest is the same as Example 1.

[0071] Comparative Example 6

[0072] The difference between this comparative example and Example 1 is that the first additive is fatty acid polyoxyethylene ether, and the rest is the same as Example 1.

[0073] Comparative Example 7

[0074] The difference between this comparative example and Example 1 is that the first additive is replaced with an equal content of trimethyl phosphate, and the rest is the same as Example 1.

[0075] Comparative Example 8

[0076] The difference between this comparative example and Example 1 is that the mixed lithium salt is replaced with lithium hexafluorophosphate of the same content, and the rest is the same as Example 1.

[0077] Application Examples 1 to 8 and Comparative Application Examples 1 to 8

[0078] The non-aqueous electrolytes provided in Examples 1 to 8 and Comparative Examples 1 to 8 are used to prepare lithium-ion batteries, and the preparation method is as follows:

[0079] The non-aqueous electrolyte, artificial graphite negative electrode and nickel cobalt lithium manganese oxide positive electrode were assembled into a soft-pack battery cell with a capacity of 6Ah.

[0080] Test conditions

[0081] The soft-pack cells provided in Application Examples 1 to 8 and Comparative Application Examples 1 to 8 were tested, and the cells after cycling were fully charged and disassembled. The testing method is as follows:

[0082] (1) Room temperature 1C cycle performance test: 1C constant current and constant voltage charging to 4.5V, cut-off current is 0.05C, 1C constant current discharge to 3.0V, and calculate its capacity retention rate after 250 cycles;

[0083] (2) 55°C high temperature cycle test: 1C constant current and constant voltage charging to 4.5V, cut-off current is 0.05C, 1C constant current discharge to 3.0V, and calculate its capacity retention rate after 250 cycles.

[0084] The test results are shown in Table 1:

[0085] Table 1

[0086]

[0087] It can be seen from Table 1 that by comparing Comparative Application Example 1, Comparative Application Example 4, Comparative Application Example 5 and Comparative Application Example 7 with other groups containing fatty acid polyoxyethylene ether, under the same infiltration process, the electrodes of other groups containing fatty acid polyoxyethylene ether are fully charged and disassembled without black spots, and the electrode wettability is significantly better.

[0088] It can be seen from Table 1 that the cycle performance of comparative application example 6 (containing only fatty acid polyoxyethylene ether) is extremely low, and obvious lithium precipitation of the electrode occurs. The cycle performance of comparative application example 7 (without the first additive) is the worst, and lithium precipitation and black spots appear on the electrode at the same time. By comparing application example 8 with application example 1, it can be seen that the cycle performance of the battery cell composed of the electrolyte containing only one lithium salt, lithium hexafluorophosphate, is greatly reduced. By comparing the cycle performance of application examples 6 to 8 with application example 1, it can be seen that the lithium salt and solvent ratios in application example 1 are all within the optimal ratio range, and too high or too low lithium salt content and solvent ratio in the electrolyte are not beneficial to the cycle performance.

[0089] According to the capacity retention rate after high temperature cycling of Comparative Application Examples 4 to 6 in Table 1, it can be seen that the addition of either of the two auxiliary additives, 3-cyanophenylboronic acid-1,3-propylene glycol ester and N,N-dimethyl 4-fluorobenzenesulfonamide, will greatly improve the high voltage and high temperature cycling performance of the battery cell, among which 3-cyanophenylboronic acid-1,3-propylene glycol ester has a greater impact. According to the capacity retention rate after high temperature cycling of Application Examples 1 to 5 in Table 1, reference Figure 2 It can be seen that the battery cell made from the formula of Application Example 1 has a stable cycle curve at 250 cycles, with the smallest slope and the highest capacity retention rate, that is, the high-voltage and high-temperature cycle performance of the battery cell is best improved when the ratio of the two additives is equal. Figure 1 From Table 1, it can be seen that when the mass ratio of fatty acid polyoxyethylene ether in the first additive remains unchanged, when the ratio of the two auxiliary additives, 3-cyanophenylboronic acid-1,3-propylene glycol ester and N,N-dimethyl 4-fluorobenzenesulfonamide, is within the preferred range of (3.5-4.5):(3.5-4.5), the room temperature cycle performance of the battery cell is significantly improved, and the closer the ratio of the two is, the higher the capacity retention rate of the battery cell is when the number of cycles is the same, and the better the cycle performance is.

[0090] The above application examples and comparative application examples well demonstrate the beneficial effects of the present invention on improving the electrical properties of the battery cell and the battery cell interface. The raw materials and contents of the electrolyte formula of the present invention, the type and content of the first additive, the type and content of the mixed lithium salt, and the type and content of the mixed solvent can exert a good synergistic effect, so that the thermal stability of the electrolyte under a high voltage state greater than 4.3V can be specifically improved, thereby achieving the effect of the present invention.

[0091] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A non-aqueous electrolyte, characterized in that: The non-aqueous electrolyte comprises a mixed lithium salt, an additive and a mixed solvent; The additives include a first additive and a second additive; The first additive includes a combination of 3-cyanophenylboronic acid-1,3-propylene glycol ester, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether; The mass ratio of 3-cyanophenylboronic acid-1,3-propylene glycol ester, N,N-dimethyl 4-fluorobenzenesulfonamide and fatty acid polyoxyethylene ether in the first additive is (2-6):(2-6):(1.5-5); Based on the total mass of the non-aqueous electrolyte being 100%, the mass percentage of the first additive is 1.9% to 3.8%.

2. The non-aqueous electrolyte according to claim 1, characterized in that The second additive is a flame retardant additive.

3. The non-aqueous electrolyte according to claim 2, characterized in that The flame retardant additive includes trimethyl phosphate.

4. The non-aqueous electrolyte according to claim 1, characterized in that Based on the total mass of the non-aqueous electrolyte being 100%, the mass percentage of the second additive is 1.8% to 5.4%.

5. The non-aqueous electrolyte according to claim 4, characterized in that Based on the total mass of the non-aqueous electrolyte being 100%, the mass percentage of the second additive is 2.9%.

6. The non-aqueous electrolyte according to claim 1, characterized in that The mixed lithium salt includes a combination of lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, boric acid lithium salt and phosphate lithium salt.

7. The non-aqueous electrolyte according to claim 6, characterized in that The boric acid lithium salt includes any one of lithium dioxalatoborate, lithium difluorooxalatoborate, lithium tetrafluoroborate or lithium dicyanooxalatoborate or a combination of at least two thereof.

8. The non-aqueous electrolyte according to claim 6, characterized in that The phosphate lithium salt includes any one of lithium difluorophosphate, lithium oxalate phosphate, or lithium tetrafluorooxalate phosphate, or a combination of at least two thereof.

9. The non-aqueous electrolyte according to claim 6, characterized in that The mass ratio of the lithium bis(fluorosulfonyl)imide, lithium hexafluorophosphate, boric acid lithium salt and phosphate lithium salt is (0.3-0.4):(0.6-1.1):(0.2-0.5):(0.1-0.3).

10. The non-aqueous electrolyte according to claim 1, characterized in that Taking the total mass of the non-aqueous electrolyte as 100%, the mass percentage of the mixed lithium salt is 13% to 18%.

11. The non-aqueous electrolyte according to claim 1, characterized in that The mixed solvent includes a combination of a carbonate solvent, an ether solvent and a sulfone solvent.

12. The non-aqueous electrolyte according to claim 11, characterized in that The carbonate solvent includes any one of ethylene carbonate, propylene carbonate, ethylene carbonate or ethyl methyl carbonate, or a combination of at least two thereof.

13. The non-aqueous electrolyte according to claim 11, characterized in that The ether solvent includes diethylene glycol dimethyl ether and / or 2-methyltetrahydrofuran.

14. The non-aqueous electrolyte according to claim 11, characterized in that The sulfone solvent includes any one of 3,3,3-trifluoropropyl methyl sulfone, cyclopentane or methyl ethyl sulfone, or a combination of at least two thereof.

15. The non-aqueous electrolyte according to claim 11, characterized in that The mass ratio of the carbonate solvent, the ether solvent and the sulfone solvent in the mixed solvent is (1.4-5.7):1:(0.1-0.6).

16. The non-aqueous electrolyte according to claim 1, characterized in that Taking the total mass of the non-aqueous electrolyte as 100%, the mass percentage of the mixed solvent is 72.8% to 78.6%.

17. A secondary battery, characterized in that: The secondary battery comprises a positive electrode, a negative electrode, an electrolyte and a separator, wherein the electrolyte comprises the nonaqueous electrolyte according to any one of claims 1 to 16.

18. The secondary battery according to claim 17, characterized in that: The material of the positive electrode includes lithium nickel cobalt manganese oxide.

19. The secondary battery according to claim 17, characterized in that: The material of the negative electrode includes graphite.