A perovskite solar film for vehicles and its preparation method

By fabricating perovskite solar cell films on flexible substrates and employing stabilizing crosslinking agents and flexible substrate pretreatment techniques, the limitations of rigid substrates in the automotive field for perovskite solar cells have been overcome, achieving flexible integration and efficient power supply, and improving mechanical stability and power generation efficiency.

CN117255598BActive Publication Date: 2026-11-17HUABI NEW ENERGY TECH (SUZHOU) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310857828.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-13
Publication Date
2026-11-17
Estimated Expiration
2043-07-13

AI Technical Summary

Technical Problem

The application of existing perovskite solar cells in the automotive field is limited by rigid substrates, which cannot effectively utilize the non-planar area of ​​the vehicle body. Furthermore, the process is complex, making it difficult to achieve flexible integration and efficient power supply.

Method used

The flexible substrate pretreatment technology is adopted. By setting grooves on the substrate surface and filling them with elastic material, combined with the preparation methods of conductive layer, electron transport layer, perovskite layer, hole transport layer and electrode layer, the stabilizing crosslinking agent 4-bromophenylmethyl iodide is added to enhance the stability and flexibility of perovskite.

Benefits of technology

It enables flexible application of perovskite solar car films, which can adapt to different curved surfaces, improve mechanical stability and power generation efficiency, and simplify the production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117255598B_ABST
    Figure CN117255598B_ABST
Patent Text Reader

Abstract

This invention relates to a perovskite solar car film and its preparation method, belonging to the field of solar car film technology. The preparation method includes the following steps: S1, forming grooves on the surface of a flexible substrate and filling the grooves with an elastic material to obtain a pretreated flexible substrate; S2, sputtering a conductive material onto the pretreated flexible substrate to form a conductive layer; S3, forming an electron transport layer on the conductive layer; S4, coating a perovskite precursor solution onto the electron transport layer to form a perovskite layer; the perovskite precursor solution contains perovskite material, 4-bromophenylmethylamine iodide, and a solvent; S5, sequentially forming a hole transport layer and an electrode layer on the perovskite layer to obtain the perovskite solar car film. The perovskite solar car film of this invention improves the stability of the perovskite substrate and the mechanical properties of the device substrate, making it promising for applications. It can cover the entire vehicle body, and the manufacturing process is simple, possessing practical application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solar car film technology, and particularly relates to a perovskite solar car film and its preparation method. Background Technology

[0002] Perovskite materials with crystalline structures are widely used in various fields due to their advantages such as high extinction coefficient, wide absorption range, long carrier diffusion distance, tunable bandgap, and bipolar transport. Common applications include building photovoltaic facades, small-area solar power screens for digital products, and solar-powered vehicle windows.

[0003] Currently, with global energy shortages, the automotive industry, as one of the main energy consumers, faces the challenge of achieving green and sustainable development. The application of perovskite solar cells in the automotive field is known; for example, patent CN 212047105U provides a car window with perovskite solar cells. However, its effective area is only suitable for glass windows, thus limiting its power generation efficiency. Furthermore, existing perovskite solar cells used in vehicle bodies are typically on rigid substrates, hindering the utilization of non-planar areas of the vehicle body, and their manufacturing process is complex. Therefore, how to integrate perovskite solar cells into the vehicle body to utilize solar energy for vehicle power and alleviate the consumption of traditional energy sources in automobiles has become a problem that needs to be solved. Summary of the Invention

[0004] The first objective of this invention is to provide a method for preparing a perovskite solar film for vehicles, comprising the following steps:

[0005] S1. A groove is formed on the surface of a flexible substrate, and an elastic material is filled into the groove to obtain a pretreated flexible substrate.

[0006] S2. Sputter conductive material onto the pretreated flexible substrate described in S1 to form a conductive layer;

[0007] S3. Coat the conductive layer described in S2 with an electron transport material to form an electron transport layer;

[0008] S4. A perovskite precursor solution is coated onto the electron transport layer described in S3 to form a perovskite layer; the perovskite precursor solution contains perovskite material, a stabilizing crosslinking agent, and a solvent; the perovskite material is ABX3 type perovskite, and the A-site cation is selected from methylammonium ion CH3NH3. + (MA + ), formamidinium ion HC(NH2)2 + (FA + ), Cesium ions Cs + and rubidium ion Rb + One or more of the following; the B-site cation is selected from lead ion Pb. 2+ Tin ions (Sn)2+ and germanium ions Ge 2+ One or more of the following; the X-position anion is selected from iodide ions (I0). - Bromide ions (Br) - and chloride ions Cl - One or more of the following; the stabilizing crosslinking agent is selected from 4-bromobenzyl iodide (4-BBAI);

[0009] S5. A hole transport layer and an electrode layer are sequentially formed on the perovskite layer described in S4 to obtain the perovskite solar car film.

[0010] In one embodiment of the present invention, in S1, the material of the flexible substrate is selected from one or more of polyethylene terephthalate (PET), polyimide (PI), and polyethylene naphthalate (PEN); the elastic material is selected from polyurethane and / or polydimethylsiloxane (PDMS).

[0011] In one embodiment of the present invention, in S1, the thickness of the flexible substrate is 50μm-125μm.

[0012] In one embodiment of the present invention, in S1, the width of the groove is 20μm-50μm and the depth is less than the thickness of the flexible substrate.

[0013] In one embodiment of the present invention, in S1, the shape of the groove is selected from straight lines and / or wavy lines.

[0014] In one embodiment of the present invention, in S1, the groove is formed by laser scribing and / or mechanical scribing.

[0015] In one embodiment of the present invention, in S1, the width and depth of the filling groove of the elastic material are adjusted, and it can be fully covered or applied in spots.

[0016] In one embodiment of the present invention, in S2, the conductive material is selected from indium tin oxide (ITO) and / or fluorine-doped SnO2 (FTO).

[0017] In one embodiment of the present invention, in S3, the electron transport material is selected from TiO2, SnO2, ZnO, and C. 60 PCBM, ICBA, or CPTA; the thickness of the electron transport layer is 20nm-30nm.

[0018] In one embodiment of the present invention, in S4, the concentration of perovskite material in the perovskite precursor solution is 0.8 mol / L-1.2 mol / L, and the concentration of the stabilizing crosslinking agent is 5 mol / L-20 mol / L.

[0019] In one embodiment of the present invention, in S4, the solvent is selected from one or more of 2-mercaptoethanol (2-ME), γ-butyrolactone (γ-GBL), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and N-methylpyrrolidone (NMP).

[0020] Furthermore, the solvent is selected from N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO).

[0021] In one embodiment of the present invention, in S5, the material of the hole transport layer is selected from CuI, CuSCN, and NiO. x The hole transport layer is one or more of PEDOT:PSS, Spiro-MeOTAD, PTAA, and P3HT; the thickness of the hole transport layer is 40nm-50nm.

[0022] In one embodiment of the present invention, in S5, the material of the electrode layer is selected from gold, silver or aluminum; the thickness of the electrode layer is 80nm-100nm.

[0023] A second objective of this invention is to provide a perovskite solar car film prepared by the method described above.

[0024] The technical solution of the present invention has the following advantages compared with the prior art:

[0025] (1) The perovskite precursor solution prepared in this invention contains a stabilizing crosslinking agent, 4-bromophenylmethyl iodide (4-BBAI), which introduces halogen anions bromine and iodine. These anions can coordinate with the B-site cations in the perovskite, acting as an anchoring agent and forming a 2D structure on the perovskite interface. This 3D / 2D structure increases the stability of the functional layer. In addition, the introduced cation NH3... + It can inhibit the migration and decomposition of organic amine cations in perovskite materials containing organic amine cations, effectively improving the stability of perovskite materials.

[0026] (2) The perovskite solar car film of the present invention uses a pre-treated flexible substrate, which gives the flexible substrate a tensile-resistant structure. That is, lines are scribed on the flexible substrate to form grooves with a depth less than the substrate thickness, and the grooves are filled with elastic material. When the car film is applied to the car, it will be stretched. The grooves and the elastic material in the grooves can buffer some of the stress to adapt to different curved surfaces. At this time, due to the presence of the tensile-resistant structure in the flexible substrate, the mechanical properties of the car film are relatively stable. After testing, the pre-treated substrate can withstand a 3% stretch, and the device does not suffer serious damage when stretched by external force. The device efficiency remains basically stable, which to a certain extent solves the problem of poor mechanical stability of flexible car films during actual application.

[0027] (3) The perovskite solar car film of the present invention improves the stability of the perovskite body and the mechanical properties of the device substrate, making the perovskite solar car film have great application prospects. It can cover the entire vehicle body, and the production process is simple and has practical application value. Attached Figure Description

[0028] To make the content of this invention easier to understand, the invention will be further described in detail below with reference to specific embodiments and accompanying drawings, wherein:

[0029] Figure 1 The structural formula of 4-bromophenylmethyl iodide (4-BBAI) in the embodiments of the present invention is shown below;

[0030] Figure 2 This is a SEM characterization image of the perovskite layer based on Example 1 of the present invention;

[0031] Figure 3 This is a SEM characterization image of the perovskite layer under tensile conditions based on Example 1 of the present invention;

[0032] Figure 4 This is a SEM characterization image of the perovskite layer under tensile conditions based on Comparative Example 1.

[0033] Figure 5 This is a SEM characterization image of the perovskite layer under tensile conditions based on Comparative Example 2. Detailed Implementation

[0034] To address the aforementioned technical problems, this invention provides a perovskite solar car film and its preparation method. The perovskite solar car film has a semi-transparent appearance. When sunlight enters the perovskite layer from the electrode layer, photogenerated carriers are generated. Electrons and holes are transported to the conductive layer and the electrode layer, respectively. Finally, a photocurrent is generated through the circuit connecting the conductive layer and the electrode layer, thereby powering the vehicle body.

[0035] The first objective of this invention is to provide a method for preparing a perovskite solar film for vehicles, comprising the following steps:

[0036] S1. A groove is formed on the surface of a flexible substrate, and an elastic material is filled into the groove to obtain a pretreated flexible substrate.

[0037] S2. Sputter conductive material onto the pretreated flexible substrate described in S1 to form a conductive layer;

[0038] S3. Coat the conductive layer described in S2 with an electron transport material to form an electron transport layer;

[0039] S4. A perovskite precursor solution is coated onto the electron transport layer described in S3 to form a perovskite layer; the perovskite precursor solution contains perovskite material, a stabilizing crosslinking agent, and a solvent; the perovskite material is ABX3 type perovskite, and the A-site cation is selected from methylammonium ion CH3NH3. + (MA + ), formamidinium ion HC(NH2)2 + (FA + ), Cesium ions Cs + and rubidium ion Rb + One or more of the following; the B-site cation is selected from lead ion Pb. 2+ Tin ions (Sn) 2+ and germanium ions Ge 2+ One or more of the following; the X-position anion is selected from iodide ions (I0). - Bromide ions (Br) - and chloride ions Cl - One or more of the following; the stabilizing crosslinking agent is selected from 4-bromobenzyl iodide (4-BBAI);

[0040] S5. A hole transport layer and an electrode layer are sequentially formed on the perovskite layer described in S4 to obtain the perovskite solar car film.

[0041] In one embodiment of the present invention, in S1, the material of the flexible substrate is selected from one or more of polyethylene terephthalate (PET), polyimide (PI), and polyethylene naphthalate (PEN); the elastic material is selected from polyurethane and / or polydimethylsiloxane (PDMS).

[0042] Furthermore, in S1, the material of the flexible substrate is selected from polyethylene terephthalate (PET).

[0043] In one embodiment of the present invention, in S1, the thickness of the flexible substrate is 50μm-125μm.

[0044] Further, in S1, the thickness of the flexible substrate is 50μm, 55μm, 60μm, 65μm, μm, 70μm, 75μm, 80μm, 85μm, 90μm, 95μm, 100μm, 105μm, 110μm, μm, 115μm, 120μm, 125μm, or any thickness between any two values.

[0045] In one embodiment of the present invention, in S1, the width of the groove is 20μm-50μm and the depth is less than the thickness of the flexible substrate.

[0046] In one embodiment of the present invention, in S1, the shape of the groove is selected from straight lines and / or wavy lines.

[0047] In one embodiment of the present invention, in S1, the groove is formed by laser scribing and / or mechanical scribing.

[0048] In one embodiment of the present invention, in S1, the width and depth of the filling groove of the elastic material are adjusted, and it can be fully covered or applied in spots.

[0049] In one embodiment of the present invention, in S2, the conductive material is selected from indium tin oxide (ITO) and / or fluorine-doped SnO2 (FTO).

[0050] Furthermore, in S2, the conductive material is selected from fluorine-doped SnO2 (FTO).

[0051] In one embodiment of the present invention, in S3, the electron transport material is selected from TiO2, SnO2, ZnO, and C. 60 PCBM, ICBA, or CPTA; the thickness of the electron transport layer is 20nm-30nm.

[0052] In one embodiment of the present invention, in S4, the concentration of perovskite material in the perovskite precursor solution is 0.8 mol / L-1.2 mol / L, and the concentration of the stabilizing crosslinking agent is 5 mol / L-20 mol / L.

[0053] In one embodiment of the present invention, in S4, the solvent is selected from one or more of 2-mercaptoethanol (2-ME), γ-butyrolactone (γ-GBL), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and N-methylpyrrolidone (NMP).

[0054] Furthermore, the solvent is selected from N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO).

[0055] In one embodiment of the present invention, in S5, the material of the hole transport layer is selected from CuI, CuSCN, and NiO. x The hole transport layer is one or more of PEDOT:PSS, Spiro-MeOTAD, PTAA, and P3HT; the thickness of the hole transport layer is 40nm-50nm.

[0056] In one embodiment of the present invention, in S5, the material of the electrode layer is selected from gold, silver or aluminum; the thickness of the electrode layer is 80nm-100nm.

[0057] A second objective of this invention is to provide a perovskite solar car film prepared by the method described above.

[0058] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand and implement the present invention. However, the embodiments described are not intended to limit the present invention.

[0059] In this invention, unless otherwise stated, the main equipment used in the embodiments is a roll-to-roll device.

[0060] Example 1

[0061] The perovskite solar cell film for vehicles and its preparation method of the present invention specifically include the following steps:

[0062] S1. Preparation of perovskite precursor solution:

[0063] S11. Weigh out a mixed solution of FAI and PbI2 dissolved in DMF and DMSO (volume ratio 4:1), stir overnight at 65°C to obtain a mixed solution;

[0064] S12. Weigh out CsI and dissolve it in DMSO. Stir at 70°C for about 2.5 hours to obtain a CsI solution.

[0065] S13. Add an equal volume of CsI solution to the mixed solution to obtain a perovskite solution, wherein the perovskite system is CsI. 0.05 FA 0.95 The concentration of PbI3 and perovskite is 0.8 mol / L;

[0066] S14, Add to perovskite solution Figure 1 The stabilizing crosslinking agent 4-bromophenylmethyl iodide shown was mixed to obtain a perovskite precursor solution, wherein the concentration of 4-bromophenylmethyl iodide was 8 mol / L.

[0067] S2. Pretreatment of flexible substrate:

[0068] S21. A straight groove is drawn on a flexible polyethylene terephthalate (PET) substrate with a thickness of about 125 μm using laser scribing. The groove has a width of about 45 μm and a depth of about 50 μm.

[0069] S22. Fill the groove with polyurethane elastic material to complete the pretreatment of the flexible substrate.

[0070] S3. Sputter conductive material FTO onto a pretreated flexible substrate to form a conductive layer;

[0071] S4. Coat the conductive layer with a deionized aqueous dispersion of FTO, anneal and dry at 150°C for 25 min to form an electron transport layer with a thickness of about 25 nm.

[0072] S5. Coat the perovskite precursor solution on the electron transport layer, anneal and dry at 110℃ for 15 min to form a perovskite layer.

[0073] S6. A Spiro-MeOTAD hole transport layer with a thickness of approximately 45 nm is formed on the perovskite layer;

[0074] S7. An Ag electrode layer with a thickness of approximately 90 nm is formed on the hole transport layer to obtain a perovskite solar car film.

[0075] Example 2

[0076] The perovskite solar cell film for vehicles and its preparation method of the present invention specifically include the following steps:

[0077] S1. Preparation of perovskite precursor solution:

[0078] S11. Weigh out a mixed solution of FAI and PbI2 dissolved in DMF and DMSO (volume ratio 4:1), stir overnight at 65°C to obtain a mixed solution;

[0079] S12. Weigh out CsI and dissolve it in DMSO. Stir at 70°C for about 2.5 hours to obtain a CsI solution.

[0080] S13. Add an equal volume of CsI solution to the mixed solution to obtain a perovskite solution, wherein the perovskite system is CsI. 0.05 FA 0.95 The concentration of PbI3 and perovskite is 0.8 mol / L;

[0081] S14, Add to perovskite solution Figure 1 The stabilizing crosslinking agent 4-bromophenylmethyl iodide shown was mixed to obtain a perovskite precursor solution, wherein the concentration of 4-bromophenylmethyl iodide was 5 mol / L.

[0082] S2. Pretreatment of flexible substrate:

[0083] S21. A straight groove is drawn on a flexible polyethylene terephthalate (PET) substrate with a thickness of about 125 μm using laser scribing. The groove has a width of about 45 μm and a depth of about 50 μm.

[0084] S22. Fill the groove with polyurethane elastic material to complete the pretreatment of the flexible substrate.

[0085] S3. Sputter conductive material FTO onto a pretreated flexible substrate to form a conductive layer;

[0086] S4. Coat the conductive layer with a deionized aqueous dispersion of FTO, anneal and dry at 150°C for 25 min to form an electron transport layer with a thickness of about 25 nm.

[0087] S5. Coat the perovskite precursor solution on the electron transport layer, anneal and dry at 110℃ for 15 min to form a perovskite layer.

[0088] S6. A Spiro-MeOTAD hole transport layer with a thickness of approximately 45 nm is formed on the perovskite layer;

[0089] S7. An Ag electrode layer with a thickness of approximately 90 nm is formed on the hole transport layer to obtain a perovskite solar car film.

[0090] Comparative Example 1 is basically the same as Example 1, except that no stabilizing crosslinking agent is added to the perovskite precursor solution.

[0091] S1. Preparation of perovskite solution:

[0092] S11. Weigh out a mixed solution of FAI and PbI2 dissolved in DMF and DMSO (volume ratio 4:1), stir overnight at 65°C to obtain a mixed solution;

[0093] S12. Weigh out CsI and dissolve it in DMSO. Stir at 70°C for about 2.5 hours to obtain a CsI solution.

[0094] S13. Add an equal volume of CsI solution to the mixed solution to obtain a perovskite solution, wherein the perovskite system is CsI. 0.05 FA 0.95 The concentration of PbI3 and perovskite is 0.8 mol / L;

[0095] S2. Pretreatment of flexible substrate:

[0096] S21. A straight groove is drawn on a flexible polyethylene terephthalate (PET) substrate with a thickness of about 125 μm using laser scribing. The groove has a width of about 45 μm and a depth of about 50 μm.

[0097] S22. Fill the groove with polyurethane elastic material to complete the pretreatment of the flexible substrate.

[0098] S3. Sputter conductive material FTO onto a pretreated flexible substrate to form a conductive layer;

[0099] S4. Coat the conductive layer with a deionized aqueous dispersion of FTO, anneal and dry at 150°C for 25 min to form an electron transport layer with a thickness of about 25 nm.

[0100] S5. Coat the electron transport layer with perovskite solution, anneal and dry at 110°C for 15 min to form a perovskite layer.

[0101] S6. A Spiro-MeOTAD hole transport layer with a thickness of approximately 45 nm is formed on the perovskite layer;

[0102] S7. An Ag electrode layer with a thickness of approximately 90 nm is formed on the hole transport layer to obtain a perovskite solar car film.

[0103] Comparative Example 2 is basically the same as Comparative Example 1, except that the flexible substrate is not pretreated.

[0104] S1. Preparation of perovskite solution:

[0105] S11. Weigh out a mixed solution of FAI and PbI2 dissolved in DMF and DMSO (volume ratio 4:1), stir overnight at 65°C to obtain a mixed solution;

[0106] S12. Weigh out CsI and dissolve it in DMSO. Stir at 70°C for about 2.5 hours to obtain a CsI solution.

[0107] S13. Add an equal volume of CsI solution to the mixed solution to obtain a perovskite solution, wherein the perovskite system is CsI. 0.05 FA 0.95 The concentration of PbI3 and perovskite is 0.8 mol / L;

[0108] S2. Sputter conductive material FTO onto a flexible polyethylene terephthalate (PET) substrate with a thickness of approximately 125 μm to form a conductive layer;

[0109] S3. Coat the conductive layer with a deionized aqueous dispersion of FTO, anneal and dry at 150°C for 25 min to form an electron transport layer with a thickness of about 25 nm.

[0110] S4. Coat the electron transport layer with perovskite solution, anneal and dry at 110℃ for 15 min to form a perovskite layer.

[0111] S5. A Spiro-MeOTAD hole transport layer with a thickness of approximately 45 nm is formed on the perovskite layer;

[0112] S6. An Ag electrode layer with a thickness of approximately 90 nm is formed on the hole transport layer to obtain a perovskite solar car film.

[0113] Test Example 1

[0114] The perovskite layer was characterized by SEM based on Example 1, and the results are as follows: Figure 2 As shown. From Figure 2 It can be seen that, due to the addition of the stabilizing crosslinking agent 4-bromophenylmethyl iodide (4-BBAI) to the perovskite precursor solution, a 2D structure is formed on the perovskite interface, which combines with the 3D structure of the perovskite. This 3D / 2D structure increases the stability of the functional layer. When used as a car cover, the perovskite layer can remain unbroken under certain stretching.

[0115] Test Example 2

[0116] Based on Example 1 and Comparative Examples 1-2, the prepared perovskite layers were stretched by 3%, and the perovskite layers under the stretching condition were characterized by SEM. The results are as follows. Figure 3-5 As shown. From Figure 3-5 It can be seen that the tensile properties of the perovskite film are significantly improved after the addition of 4-bromophenylmethylamine iodide (4-BBAI) compared to the sample without 4-BBAI, and no cracks appear. This is because the addition of 4-BBAI introduces halide anions bromine and iodine, which can coordinate with lead ions in the perovskite and act as anchors, forming a 2D structure at the perovskite interface. This 2D structure combines with the 3D perovskite structure, and this 3D / 2D structure increases the stability of the functional layer. In addition, the introduced cation NH3... + It can inhibit the migration and decomposition of organic amine cations in perovskite materials containing organic amine cations, effectively improving the stability of perovskite materials.

[0117] Test Example 3

[0118] Based on Example 1 and Comparative Examples 1-2, the electrical properties of the perovskite solar car film before and after stretching were tested, and the results are shown in Table 1:

[0119] Table 1

[0120]

[0121] As shown in Table 1, the PCE of all devices decreased after stretching by 3%. However, due to the addition of 4-bromophenylmethylamine iodide (4-BBAI) and pretreatment of the flexible substrate, the devices did not suffer severe damage during external stretching, and the device efficiency remained basically stable. In contrast, the performance of devices without substrate pretreatment and those with the addition of 4-BBAI showed a more significant decline. This is because the addition of 4-BBAI introduces halide anions bromine and iodine, which can coordinate with lead ions in the perovskite, acting as an anchor and forming a 2D structure at the perovskite interface. This 2D structure combines with the 3D perovskite structure, increasing the stability of the functional layer. Additionally, the introduced cation NH3... + It can inhibit the migration and decomposition of organic amine cations in perovskite materials containing organic amine cations, effectively improving the stability of perovskite materials; on the other hand, the flexible substrate has been pretreated, which also buffers some of the tensile stress. When the film is stretched by external force, the grooves and the elastic material in the grooves can buffer some of the stress to adapt to different tensile forces. At this time, due to the presence of the tensile-resistant structure in the flexible substrate, the film is relatively stable.

[0122] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for preparing a perovskite solar film for vehicles, characterized in that, Includes the following steps, S1. A groove is formed on the surface of a flexible substrate, and an elastic material is filled into the groove to obtain a pretreated flexible substrate. S2. Sputter conductive material onto the pretreated flexible substrate described in S1 to form a conductive layer; S3. Coat the conductive layer described in S2 with an electron transport material to form an electron transport layer; S4. A perovskite precursor solution is coated onto the electron transport layer described in S3 to form a perovskite layer; the perovskite precursor solution comprises a perovskite material, a stabilizing crosslinking agent, and a solvent; the perovskite material is ABX3 type perovskite, the A-site cation is selected from one or more of methylammonium ion, formamidinium ion, cesium ion, and rubidium ion; the B-site cation is selected from one or more of lead ion, tin ion, and germanium ion; the X-site anion is selected from one or more of iodide ion, bromide ion, and chloride ion; the stabilizing crosslinking agent is selected from 4-bromophenylmethylamine iodide. S5. A hole transport layer and an electrode layer are sequentially formed on the perovskite layer described in S4 to obtain the perovskite solar car film.

2. The method for preparing the perovskite solar film for vehicles according to claim 1, characterized in that, In S1, the material of the flexible substrate is selected from one or more of polyethylene terephthalate, polyimide and polyethylene naphthalate; the elastic material is selected from polyurethane and / or polydimethylsiloxane.

3. The method for preparing the perovskite solar film for vehicles according to claim 1, characterized in that, In S1, the thickness of the flexible substrate is 50μm-125μm.

4. The method for preparing the perovskite solar film for vehicles according to claim 1, characterized in that, In S1, the width of the groove is 20μm-50μm, and the depth is less than the thickness of the flexible substrate.

5. The method for preparing the perovskite solar film for vehicles according to claim 1, characterized in that, In S2, the conductive material is selected from indium tin oxide and / or fluorine-doped SnO2.

6. The method for preparing the perovskite solar film for vehicles according to claim 1, characterized in that, In S3, the electron transport material is selected from Ti02, Sn02, ZnO, C 60 , PCBM, ICBA or CPTA; the thickness of the electron transport layer is 20 nm-30 nm.

7. The method for preparing the perovskite solar film for vehicles according to claim 1, characterized in that, In S4, the concentration of perovskite material in the perovskite precursor solution is 0.8 mol / L-1.2 mol / L, and the concentration of the stabilizing crosslinking agent is 5 mol / L-20 mol / L.

8. The method for preparing the perovskite solar film for vehicles according to claim 1, characterized in that, In S5, the material of the hole transport layer is selected from CuI, CuSCN, and NiO. x One or more of PEDOT:PSS, Spiro-MeOTAD, PTAA, and P3HT; the thickness of the hole transport layer is 40nm-50nm.

9. The method for preparing the perovskite solar film for vehicles according to claim 1, characterized in that, In S5, the material of the electrode layer is selected from gold, silver or aluminum; the thickness of the electrode layer is 80nm-100nm.

10. A perovskite solar car film prepared by the method of any one of claims 1-9.

Citation Information

Patent Citations

  • Two-dimensional and three-dimensional perovskite heterojunction resistive random access memory and preparation method thereof

    CN111244275A

  • Red perovskite light emitting diode based on mixed halogen and preparation method thereof

    CN111916571A