A high-concentration high-entropy electrolyte, its preparation method, and a battery thereof.

By using a high-concentration, high-entropy electrolyte in sodium-carbon dioxide batteries, the problems of low electrolyte conductivity and poor stability are solved, improving battery performance and lifespan, and achieving high-efficiency electrochemical performance and long-term working capability.

CN117413406BActive Publication Date: 2026-11-17KUNMING UNIV OF SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380010847.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-05
Publication Date
2026-11-17
Estimated Expiration
2043-09-05

AI Technical Summary

Technical Problem

Existing sodium-carbon dioxide batteries have low electrolyte ionic conductivity, high viscosity, and a low electrochemical stability window, resulting in low battery energy density and solid discharge products clogging the catalyst layer, affecting battery performance and lifespan.

Method used

A high-concentration, high-entropy electrolyte is prepared by introducing multi-component solute salts into the electrolyte to improve its ionic conductivity, reduce its viscosity, and enhance its stability. The electrolyte includes a solvent and multiple solute salts with a concentration range of 20M-60M. The concentration of the first solute salt accounts for more than 50% of the total concentration, and the concentration of added salts is less than 50%.

Benefits of technology

It significantly improves the power density, discharge specific capacity, and cycle stability of sodium-carbon dioxide batteries, converts solid discharge products into liquid products, reduces electrode corrosion, and enhances the commercial potential of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117413406B_ABST
    Figure CN117413406B_ABST
Patent Text Reader

Abstract

This invention discloses a high-concentration high-entropy electrolyte, its preparation method, and a battery. The high-concentration high-entropy electrolyte has a high molar concentration and high disorder, comprising a solvent, a first solute salt, and added salts. The first solute salt is a solute salt with high solubility in the solvent, and the added salts are three or more solute salts. The molar concentration of the solute salts in the high-concentration high-entropy electrolyte ranges from 20M to 60M, the molar concentration of the first solute salt exceeds 20M, and the molar concentration of the first solute salt accounts for more than 50% of the molar concentration of the high-concentration high-entropy electrolyte. The sodium-carbon dioxide battery assembled with the high-concentration high-entropy electrolyte disclosed in this invention not only has a high power density but also excellent discharge specific capacity and rate performance. Furthermore, the battery exhibits good cycle stability, and the generation of liquid discharge product formic acid effectively avoids the blockage of the catalyst layer by solid discharge products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the design and manufacture of a high-concentration, high-entropy electrolyte and a battery. More specifically, this invention relates to a high-concentration, high-entropy electrolyte, its preparation method, and a battery. Background Technology

[0002] Global warming is leading to increased frequency and intensity of extreme weather and climate events, resulting in severe meteorological disasters. The massive emissions of carbon dioxide from the use of fossil fuels are a major cause of the greenhouse effect. Therefore, reducing carbon dioxide emissions and converting them into valuable chemical substances is an inevitable trend in today's society.

[0003] Metal-carbon dioxide batteries equipped with advanced carbon dioxide electrodes offer a promising strategy for carbon dioxide recycling and electrochemical energy conversion and storage. Among these, sodium-carbon dioxide batteries are particularly advantageous due to their abundant sodium resources and high energy density (1125 Wh / kg⁻¹). -1 Its advantages, such as [missing information], have attracted widespread attention. Therefore, conducting research related to the application of sodium-carbon dioxide batteries is of great significance for solving the energy crisis and mitigating the greenhouse effect.

[0004] However, the poor physicochemical properties of the electrolyte severely hinder the practical application of sodium-carbon dioxide batteries. First, current electrolytes have low ionic conductivity and high viscosity, which cannot meet the requirements for rapid sodium ion transport during charging and discharging. Second, the low electrochemical stability window of the electrolyte leads to low battery operating voltage, ultimately resulting in low energy density. Third, when using existing electrolytes, the discharge products are all solid products, namely sodium carbonate, sodium oxalate, or sodium bicarbonate. When the battery operates for extended periods, these solid discharge products can clog the catalyst layer, leading to battery failure. Therefore, researching new electrolytes to improve the electrochemical performance of sodium-carbon dioxide batteries and promote their application is of great significance. Summary of the Invention

[0005] This invention provides a high-performance, high-concentration, high-entropy electrolyte and its preparation method. Based on different sodium salt components and proportions, the most suitable sodium salt composition and concentration are optimized, and an electrolyte with high ionic conductivity, low viscosity, high stability, and high disorder is successfully prepared.

[0006] The present invention also provides a sodium-carbon dioxide battery based on the high-concentration, high-entropy electrolyte, and improves the battery’s rate, capacity, power density, cycle life and other electrochemical performance by using the electrolyte.

[0007] This invention provides a high-concentration, high-entropy electrolyte. By introducing multiple component solute salts (both inorganic and organic salts) into the electrolyte, the concentration of solute salts in the electrolyte is increased, and the disorder of salt anions or cations in the electrolyte is further enhanced. The high-concentration, high-entropy electrolyte includes a solvent, a first solute salt, and additive salts. The first solute salt is a solute salt with high solubility in the solvent, and the additive salts are three or more solute salts. The molar concentration of the solute salts in the high-concentration, high-entropy electrolyte ranges from 20M to 60M, the molar concentration of the first solute salt exceeds 20M, and the molar concentration of the first solute salt accounts for more than 50% of the molar concentration of the high-concentration, high-entropy electrolyte.

[0008] Furthermore, the sum of the molar concentrations of the added salts is less than 50% of the molar concentration of the high-concentration, high-entropy electrolyte, and the addition ratio of the added salts is calculated based on the solubility of the solute salts in the solvent.

[0009] Further, the solvent is an organic solvent or an inorganic solvent; the organic solvent is at least one of aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, alcohols, ethers, esters, ketones, glycol derivatives, and acetonitrile, pyridine, phenol, etc.; the inorganic solvent is at least one of acidic solvents, basic solvents, amphoteric solvents, and inert solvents.

[0010] Furthermore, the solute salt includes organic or inorganic salts. Specifically, the solute salt includes lithium trifluoride (LiOTf), sodium trifluoride (NaOTf), magnesium bis(trifluoromethanesulfonyl)imide (Mg(TFSI)2), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium nitrate (LiNO3), sodium nitrate (NaNO3), sodium bis(fluorosulfonyl)imide (NaFSI), lithium bis(fluorosulfonyl)imide (LiFSI), sodium perchlorate (NaClO4), lithium perchlorate (LiClO4), sodium chloride (NaCl), lithium chloride (LiCl), zinc chloride (ZnCl2), sodium iodide (NaI), etc.; the solvent is water (distilled water or deionized water).

[0011] This invention also provides a method for preparing a high-concentration, high-entropy electrolyte, comprising the following steps:

[0012] S1. Select a solute salt with high solubility as the first solute salt, weigh a certain amount of the first solute salt and dissolve it in the solvent to obtain an electrolyte with a certain molar concentration, heat it to 60℃, and obtain a basic high-concentration electrolyte.

[0013] S2. Select three or more solute salts as added salts, calculate and weigh the required added salts according to the preset molar concentration, add them to the basic high-concentration electrolyte obtained in step S1, and heat to 60°C to ensure that all solute salts are completely dissolved to obtain a mixed high-concentration electrolyte.

[0014] S3. Place the mixed high-concentration electrolyte obtained in S2 into an ultrasonic instrument and sonicate for 5-30 minutes to ensure that all components in the solution are completely mixed. Cool the solution to room temperature to obtain a high-concentration high-entropy electrolyte.

[0015] Furthermore, the molar concentration of the solute salt in the high-concentration high-entropy electrolyte is in the range of 20M-60M, the molar concentration of the first solute salt exceeds 20M, and the molar concentration of the first solute salt accounts for more than 50% of the total molar concentration of the high-concentration high-entropy electrolyte; the sum of the molar concentrations of the added salts is less than 50% of the total molar concentration of the high-concentration high-entropy electrolyte.

[0016] On the other hand, the present invention also provides a sodium-carbon dioxide battery comprising the high-concentration high-entropy electrolyte, wherein the high-concentration high-entropy electrolyte replaces the traditional positive electrode electrolyte (saturated sodium chloride solution, "salt-in-water" electrolyte, seawater electrolyte, etc.) to obtain a sodium-carbon dioxide battery based on the high-concentration high-entropy electrolyte.

[0017] Compared with existing technologies, this invention provides a sodium-carbon dioxide battery based on a high-concentration, high-entropy electrolyte. The high-concentration, high-entropy electrolyte comprises a high-concentration base electrolyte and added salts. This electrolyte exhibits higher ionic conductivity, lower viscosity, higher stability, and higher disorder than conventional electrolytes. Furthermore, it possesses higher carbon dioxide solubility and weaker solvation effects. Using this high-concentration, high-entropy electrolyte can effectively improve the power density and discharge specific capacity of sodium-carbon dioxide batteries, and also address the poor rate performance of batteries based on conventional electrolytes. Simultaneously, this electrolyte can convert the solid discharge products of sodium-carbon dioxide batteries based on conventional electrolytes into liquid discharge products, which is beneficial for improving the battery's cycle stability and increasing the utilization rate of the metallic sodium anode. In addition, this electrolyte can effectively reduce electrolyte corrosion of the electrodes, thereby improving battery performance and having significant implications for the commercialization of sodium-carbon dioxide batteries. Attached Figure Description

[0018] Figure 1 This is a schematic diagram of a method for preparing a high-concentration, high-entropy electrolyte according to an embodiment of the present invention.

[0019] Figure 2 This is a schematic diagram of the structure of the sodium-carbon dioxide battery provided in an embodiment of the present invention.

[0020] Figure 3 This is a sodium nuclear magnetic resonance spectrum of a high-concentration, high-entropy electrolyte and a conventional electrolyte provided in one embodiment of the present invention.

[0021] Figure 4 This is a power density curve of a sodium-carbon dioxide battery based on a high-concentration high-entropy electrolyte and a traditional electrolyte, provided by an embodiment of the present invention.

[0022] Figure 5 This is a rate curve of a sodium-carbon dioxide battery based on a high-concentration high-entropy electrolyte and a traditional electrolyte, provided by an embodiment of the present invention.

[0023] Figure 6 This is a discharge specific capacity curve of a sodium-carbon dioxide battery based on a high-concentration high-entropy electrolyte and a traditional electrolyte, provided by an embodiment of the present invention.

[0024] Figure 7 This is a photograph of the sodium metal anode of a battery after discharge, based on a conventional electrolyte and a high-concentration high-entropy electrolyte, according to an embodiment of the present invention.

[0025] Figure 8 This is a cycle curve diagram of a sodium-carbon dioxide battery based on a high-concentration high-entropy electrolyte and a conventional electrolyte, provided by an embodiment of the present invention.

[0026] Figure 9 This is a Raman characterization diagram of the discharge products of a sodium-carbon dioxide battery based on a conventional electrolyte, provided in one embodiment of the present invention.

[0027] Figure 10 This is a hydrogen nuclear magnetic resonance spectrum of sodium-carbon dioxide battery products based on a high-concentration, high-entropy electrolyte, provided in one embodiment of the present invention. Detailed Implementation

[0028] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0029] Please see Figure 1 , Figure 1 This is a schematic flowchart of a method for preparing a high-concentration, high-entropy electrolyte according to an embodiment of the present invention. The specific preparation steps of the method for preparing the high-concentration, high-entropy electrolyte according to the embodiment of the present invention are as follows:

[0030] S1. Select a solute salt with high solubility as the first solute salt, weigh a certain amount of the first solute salt and dissolve it in the solvent to obtain an electrolyte with a certain molar concentration, heat it to 60°C, and obtain a basic high-concentration electrolyte.

[0031] S2. Select three or more solute salts as additive salts, calculate and weigh the required additive salts according to the preset molar concentration, add them to the basic high-concentration electrolyte obtained in step S1, and heat to 60°C to ensure that all solute salts are completely dissolved to obtain a mixed high-concentration electrolyte.

[0032] S3. Place the mixed high-concentration electrolyte obtained in S2 into an ultrasonic instrument and sonicate for 5-30 minutes to ensure that all components in the solution are completely mixed. Cool the solution to room temperature to obtain a high-concentration high-entropy electrolyte.

[0033] It is understood that high solubility refers to the mass (solid and liquid) or volume of solute that dissolves after reaching saturation. In this embodiment, it refers to the mass of solute that dissolves after the solute salt reaches saturation in the solvent.

[0034] In the high-concentration high-entropy electrolyte prepared according to the method described above, the molar concentration of the solute salt is in the range of 20M-60M, the molar concentration of the first solute salt exceeds 20M, and the molar concentration of the first solute salt accounts for more than 50% of the total molar concentration of the high-concentration high-entropy electrolyte; the sum of the molar concentrations of the added salts is less than 50% of the total molar concentration of the high-concentration high-entropy electrolyte.

[0035] Specifically, the molar concentration of the solute salt can be 20M, 25M, 30M, 35M, 40M, 45M, 50M, 55M, or 60M, as long as it is within the range of 20M-60M. The molar concentration of the first solute salt exceeds 20M, meaning the molar concentration of the first solute salt can be 20M, 25M, 30M, 35M, 40M, 45M, 50M, 55M, or 60M, etc.; when the molar concentration of the high-concentration high-entropy electrolyte is 50M, then the molar concentration of the first solute salt is at least 25M; when the molar concentration of the high-concentration high-entropy electrolyte is 60M, then the molar concentration of the first solute salt is at least 30M, meaning the molar concentration of the first solute salt... The molar concentration accounts for more than 50% of the total molar concentration of the high-concentration high-entropy electrolyte. It can be understood that when the molar concentration of the first solute salt accounts for more than 50% of the total molar concentration of the high-concentration high-entropy electrolyte, the sum of the molar concentrations of the added salts is less than 50% of the total molar concentration of the high-concentration high-entropy electrolyte. That is, when the molar concentration of the high-concentration high-entropy electrolyte is 50M, the molar concentration of the first solute salt is at least 25M, and the sum of the molar concentrations of the added salts is less than 25M.

[0036] In steps S1 and S2, the mass of the first solute salt and the added salt to be added are calculated based on the preset concentration of the high-concentration high-entropy electrolyte and the concentration of the first solute salt. Then, the required mass of the first solute salt and the added salt are weighed to prepare a solution with the corresponding molar concentration in steps S1 and S2.

[0037] In this embodiment, the solute salt includes organic or inorganic salts. Specifically, the solute salt includes lithium trifluoride (LiOTf), sodium trifluoride (NaOTf), magnesium bis(trifluoromethanesulfonyl)imide (Mg(TFSI)2), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium nitrate (LiNO3), sodium nitrate (NaNO3), sodium bis(fluorosulfonyl)imide (NaFSI), lithium bis(fluorosulfonyl)imide (LiFSI), sodium perchlorate (NaClO4), lithium perchlorate (LiClO4), sodium chloride (NaCl), lithium chloride (LiCl), zinc chloride (ZnCl2), and sodium iodide (NaI), etc. Specifically, the first solute salt is one of sodium fluorosulfonyl imide (NaFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and zinc chloride (ZnCl2); the added salt is at least three of lithium nitrate (LiNO3), sodium nitrate (NaNO3), sodium perchlorate (NaClO4), lithium perchlorate (LiClO4), sodium chloride (NaCl), lithium chloride (LiCl), and sodium iodide (NaI). It is understood that the added salt can be three of the aforementioned solute salts, or four, five, six, or even more.

[0038] The solvent described in this embodiment of the invention can be an organic solvent, selected from at least one of aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, alcohols, ethers, esters, ketones, glycol derivatives, and acetonitrile, pyridine, phenol, etc.; or it can be an inorganic solvent, selected from at least one of acidic solvents, basic solvents, amphoteric solvents, and inert solvents. In this embodiment, the solvent used is water and / or deionized water.

[0039] In some embodiments, the high-concentration high-entropy electrolyte is prepared by using a salt with high solubility in water as the first solute, such as NaFSI, LiFSI, LiTFSI, ZnCl2, etc., and then selecting three or more salts as additives, dissolving them in deionized water at a certain molar concentration to obtain the high-concentration high-entropy electrolyte. The additive salts are LiNO3, NaNO3, NaClO4, LiClO4, NaCl, LiCl, NaI, etc. This high-concentration high-entropy electrolyte obtained using multiple salts has lower viscosity, higher ionic conductivity, a wider electrochemical stability window, and greater stability than traditional electrolytes. Furthermore, this electrolyte has a higher carbon dioxide dissolving capacity than traditional electrolytes. Most importantly, this high-concentration high-entropy electrolyte exhibits lower solvation than traditional electrolytes.

[0040] The high-concentration high-entropy electrolyte prepared by the method described in this embodiment of the invention has high ionic conductivity, low viscosity, high stability, and high disorder; at the same time, it also has high carbon dioxide dissolving capacity and weak solvation effect.

[0041] On the other hand, embodiments of the present invention also provide a sodium-carbon dioxide battery comprising the aforementioned high-concentration, high-entropy electrolyte. For example... Figure 2 As shown, Figure 2 This is a schematic diagram of a sodium-carbon dioxide battery provided in an embodiment of the present invention. The sodium-carbon dioxide battery includes a negative electrode A, a solid electrolyte membrane B, and a positive electrode C. The negative electrode A includes a metallic sodium negative electrode A1 and a negative electrolyte A2, and the positive electrode C includes a positive electrolyte C1 and a catalyst layer C2. In this embodiment, the metallic sodium negative electrode A1, the negative electrolyte A2, the solid electrolyte membrane B, and the catalyst layer C2 are the same as those in conventional sodium-carbon dioxide batteries. However, the positive electrolyte C1 differs from that in conventional sodium-carbon dioxide batteries; the positive electrolyte C1 is a high-concentration, high-entropy electrolyte prepared by the method described in this embodiment.

[0042] Specifically, the sodium metal anode A1 is a sodium metal sheet with a purity exceeding 99.7%, a thickness of 1 mm, and a diameter of 10 mm; the anode electrolyte A2 is an ester electrolyte of 1 mol / L NaClO4 / [(EC+DMC)(1:1)+1 vol% FEC], where 1:1 is a volume ratio; and the solid electrolyte membrane B is Na3Zr2Si2PO4. 12The fast ion conductor has a NASICON structure, and the solid electrolyte has a thickness of 10 mm and a diameter of 16 mm. The catalyst layer C2 is formed by pressing carbon paper with a catalyst support and nickel foam. The carbon paper with the catalyst support has a diameter of 10 mm and a thickness of 0.5 mm. The carbon paper with the catalyst support is prepared by coating a slurry formed by dispersing the catalyst in a mixed solution onto hydrophilic carbon paper. The catalyst is a 5% Ru / C catalyst, and the mixed solution is a mixed solution of alcohol:water:binder with a volume ratio of 8:1.5:0.5. The binder is a 5% PVDF aqueous solution. The nickel foam has a thickness of 1 mm and a diameter of 10 mm.

[0043] In some embodiments, when a high-concentration, high-entropy electrolyte is used instead of a traditional electrolyte in the positive electrode electrolyte C1 of a sodium-carbon dioxide battery, the lower viscosity of the high-concentration, high-entropy electrolyte can significantly improve the battery's power density. Its higher ionic conductivity and lower solvation effect are beneficial for improving the battery's rate performance. A wider electrochemical stability window and greater stability contribute to improved battery cycle performance, and its higher carbon dioxide solubility helps increase the battery's discharge specific capacity. Furthermore, the unique solvation structure of the high-concentration, high-entropy electrolyte can selectively generate the liquid product formic acid. The formation of this liquid product is less likely to clog the catalytic active sites of the catalyst layer, allowing the battery to operate for extended periods, thereby improving the utilization rate of the negative electrode.

[0044] Example 1:

[0045] like Figure 3As shown, this embodiment presents the NMR sodium spectra of a high-concentration high-entropy electrolyte prepared according to the aforementioned preparation method and a conventional electrolyte. The high-concentration high-entropy electrolyte is prepared by dissolving four solute salts (20M NaFSI, 5M NaClO4, 5M NaCl, and 5M NaNO3) in deionized water. The conventional electrolyte is obtained by dissolving 35M NaFSI in deionized water. NMR processing of the two electrolytes revealed that, in the NMR sodium spectra, compared to the conventional electrolyte, the chemical shift of the sodium ion characteristic peak in the high-concentration high-entropy electrolyte gradually shifts to a lower field, indicating a reduced solvation effect around sodium ions. This is beneficial for sodium ion extraction during battery operation and facilitates rapid sodium ion transfer. In this embodiment, two sodium-carbon dioxide batteries are provided for comparative experiments. The two sodium-carbon dioxide batteries, from the negative electrode portion A to the positive electrode portion C, sequentially include a metallic sodium negative electrode A1, a negative electrode electrolyte A2, a solid electrolyte membrane B, a positive electrode electrolyte C1, and a catalyst layer C2. In this embodiment, the negative electrode A1 is a sodium metal sheet with a thickness of 1 mm and a diameter of 10 mm; the negative electrode electrolyte A2 is 1 mol / L NaClO4 / [(EC+DMC)(1:1)+1 vol% FEC]; the solid electrolyte membrane B is a NASICON type fast ion conductor with a thickness of 1 mm and a diameter of 16 mm; the positive electrode electrolyte of one sodium-carbon dioxide battery is the high-concentration high-entropy electrolyte mentioned above in this embodiment, that is, the high-concentration high-entropy electrolyte is prepared by dissolving 20 M NaFSI, 5 M NaClO4, 5 M NaCl, and 5 M NaNO3 four solute salts in deionized water; the positive electrode electrolyte of another sodium-carbon dioxide battery is the conventional electrolyte mentioned above in this embodiment, that is, the conventional electrolyte is 35 M The catalyst layer is obtained by dissolving NaFSI in deionized water; the catalyst layer is formed by pressing carbon paper with catalyst support and nickel foam. The carbon paper with catalyst support is a porous hydrophilic carbon paper with a diameter of 10 mm and a thickness of 0.5 mm. The catalyst is 5% Ru / C. The nickel foam has a thickness of 1 mm and a diameter of 10 mm.

[0046] The two sodium-carbon dioxide batteries assembled in this embodiment were subjected to performance tests under constant temperature (30°C) and pure CO2 conditions, and their power density curves are shown below. Figure 4 As shown, the magnification curve is as follows Figure 5 As shown, when the positive electrode electrolyte is the high-concentration, high-entropy electrolyte, the maximum power density of the sodium-carbon dioxide battery is 5.85 mW / cm³. 2 When the positive electrode electrolyte is a conventional electrolyte, the maximum power density of the sodium-carbon dioxide battery is 2.26 mW / cm³. 2 .from Figure 5It can be seen that when the positive electrode electrolyte is a high-concentration, high-entropy electrolyte, the rate performance of the sodium-carbon dioxide battery is significantly better than when the positive electrode electrolyte is a conventional electrolyte; furthermore, when the current density increases to 2 mA / cm², the rate performance is significantly better. 2 At that time, sodium-carbon dioxide batteries using conventional electrolytes could no longer function properly, while sodium-carbon dioxide batteries using high-concentration, high-entropy electrolytes still exhibited excellent charge-discharge performance. Therefore, in this embodiment, the performance of the sodium-carbon dioxide battery using the aforementioned high-concentration, high-entropy electrolyte as the positive electrode electrolyte is better than that of the sodium-carbon dioxide battery using conventional electrolytes as the positive electrode electrolyte.

[0047] Example 2:

[0048] In this embodiment, two sodium-carbon dioxide batteries are provided for comparative experiments. The two sodium-carbon dioxide batteries, from the negative electrode portion A to the positive electrode portion C, sequentially include a metallic sodium negative electrode A1, a negative electrode electrolyte A2, a solid electrolyte membrane B, a positive electrode electrolyte C1, and a catalyst layer C2. The negative electrode A1 is a sodium metal sheet with a thickness of 1 mm and a diameter of 10 mm; the negative electrode electrolyte A2 is 1 mol / L NaClO4 / [(EC+DMC)(1:1)+1 vol% FEC]; the solid electrolyte membrane B is a NASICON type fast ion conductor with a thickness of 1 mm and a diameter of 16 mm; in one sodium-carbon dioxide battery, the positive electrode electrolyte is a high-concentration high-entropy electrolyte, which is prepared by dissolving five solute salts (27 M NaFSI, 2 M NaClO4, 2 M NaCl, 2 M NaNO3, and 2 M NaI) in deionized water according to the above preparation method; in another sodium-carbon dioxide battery, the positive electrode electrolyte is a conventional electrolyte, which is 18 M NaClO4 / [(EC+DMC)(1:1)+1 vol% FEC]; The catalyst layer is prepared by dissolving NaClO4 in deionized water according to the above preparation method; the catalyst layer is formed by pressing carbon paper with catalyst support and nickel foam, the carbon paper with catalyst support is porous hydrophilic carbon paper with a diameter of 10 mm and a thickness of 0.5 mm, the catalyst is 5% Ru / C, and the nickel foam has a thickness of 1 mm and a diameter of 10 mm.

[0049] The two sodium-carbon dioxide batteries assembled in this embodiment were subjected to performance tests under constant temperature (30°C) and pure CO2 conditions. Their discharge specific capacity curves are shown below. Figure 6 As shown, when the positive electrode electrolyte is a high-concentration, high-entropy electrolyte, the discharge specific capacity of the sodium-carbon dioxide battery is 44.85 mAh / cm³. 2 When the positive electrode electrolyte is a conventional electrolyte, the discharge specific capacity of the sodium-carbon dioxide battery is 10.67 mAh / cm³. 2 In addition, such as Figure 7As shown, when the positive electrode electrolyte is a conventional electrolyte, the residual amount of metallic sodium in the negative electrode of the sodium-carbon dioxide battery is significantly lower than that when the positive electrode electrolyte is a high-concentration, high-entropy electrolyte, which significantly improves the utilization rate of metallic sodium in the negative electrode. Therefore, the performance of the sodium-carbon dioxide battery using the high-concentration, high-entropy electrolyte as the positive electrode electrolyte in this embodiment is better than that of the sodium-carbon dioxide battery using a conventional electrolyte as the positive electrode electrolyte.

[0050] Example 3:

[0051] In this embodiment, two sodium-carbon dioxide batteries are provided for comparative experiments. From the negative electrode portion A to the positive electrode portion C, both sodium-carbon dioxide batteries sequentially include a metallic sodium negative electrode A1, a negative electrolyte A2, a solid electrolyte membrane B, a positive electrolyte C1, and a catalyst layer C2. The metallic negative electrode A1 is a metallic sodium sheet with a thickness of 1 mm and a diameter of 10 mm. The negative electrolyte A2 is 1 mol / L NaClO4 / [(EC+DMC)(1:1)+1 vol% FEC]. The solid electrolyte membrane B is a NASICON-type fast ion conductor with a thickness of 1 mm and a diameter of 16 mm. The positive electrolyte of one sodium-carbon dioxide battery is a high-concentration, high-entropy electrolyte, which is composed of 23 M NaFSI, 3 M NaClO4, 3 M NaCl, 3 M NaNO3, and 3 M NaI. Five solute salts were dissolved in deionized water and prepared according to the above preparation method; the positive electrode electrolyte of another sodium-carbon dioxide battery is a conventional electrolyte, which is a saturated sodium chloride solution; the catalyst layer is made of carbon paper with a catalyst supported and nickel foam pressed together, the carbon paper with the catalyst supported is a porous hydrophilic carbon paper with a diameter of 10 mm and a thickness of 0.5 mm, the catalyst is 5% Ru / C, and the nickel foam has a thickness of 1 mm and a diameter of 10 mm.

[0052] The two sodium-carbon dioxide batteries assembled in this embodiment were subjected to performance testing under constant temperature (30°C) and pure CO2 conditions, and their cycle curves are shown below. Figure 8 As shown, when the positive electrode electrolyte is a high-concentration, high-entropy electrolyte, the sodium-carbon dioxide battery achieves a cycle life of up to 374 cycles; while when the positive electrode electrolyte is a conventional electrolyte, the cycle life of the sodium-carbon dioxide battery reaches up to 108 cycles. Therefore, the sodium-carbon dioxide battery using the high-concentration, high-entropy electrolyte as the positive electrode electrolyte in this embodiment exhibits better performance than the sodium-carbon dioxide battery using a conventional electrolyte as the positive electrode electrolyte.

[0053] Example 4:

[0054] In this embodiment, two sodium-carbon dioxide batteries are provided for comparative experiments. From the negative electrode portion A to the positive electrode portion C, both sodium-carbon dioxide batteries sequentially include a metallic sodium negative electrode A1, a negative electrolyte A2, a solid electrolyte membrane B, a positive electrolyte C1, and a catalyst layer C2. The metallic negative electrode A1 is a metallic sodium sheet with a thickness of 1 mm and a diameter of 10 mm. The negative electrolyte A2 is 1 mol / L NaClO4 / [(EC+DMC)(1:1)+1 vol% FEC]. The solid electrolyte membrane B is a NASICON-type fast ion conductor with a thickness of 1 mm and a diameter of 16 mm. The positive electrolyte of one sodium-carbon dioxide battery is a high-concentration, high-entropy electrolyte, consisting of 20 M NaFSI, 4 M NaClO4, 4 M NaCl, 4 M NaNO3, and 3 M NaI. Five solute salts were dissolved in deionized water and prepared according to the above preparation method; the positive electrode electrolyte of another sodium-carbon dioxide battery is a conventional electrolyte, which is a saturated sodium perchlorate solution; the catalyst layer is made of carbon paper with catalyst supported and nickel foam pressed together, the carbon paper with catalyst supported is a porous hydrophilic carbon paper with a diameter of 10 mm and a thickness of 0.5 mm, the catalyst is 5% Ru / C, and the nickel foam has a thickness of 1 mm and a diameter of 10 mm.

[0055] The two sodium-carbon dioxide batteries assembled in this embodiment were subjected to a complete discharge test under constant temperature of 30°C and pure CO2 conditions. Figure 9 As shown, Raman spectroscopy was used to detect the catalyst layer after battery discharge. The results showed that when the positive electrode electrolyte was a conventional electrolyte, the discharge product was Na₂CO₃. Figure 10 As shown, nuclear magnetic resonance hydrogen spectroscopy was used to detect the electrolyte after battery discharge. It was found that when the positive electrode electrolyte was a high-concentration, high-entropy electrolyte, the discharge product of the battery was liquid formic acid. Therefore, in this embodiment, the sodium-carbon dioxide battery using the high-concentration, high-entropy electrolyte as the positive electrode electrolyte produces formic acid as the discharge product. As a liquid, formic acid will not clog the catalyst layer and cause battery failure, thus ensuring the performance of the sodium-carbon dioxide battery using the high-concentration, high-entropy electrolyte.

[0056] Although the invention has been described above in conjunction with exemplary embodiments, those skilled in the art will understand that various modifications and changes can be made to the exemplary embodiments of the invention without departing from the spirit and scope defined by the claims.

Claims

1. A high-concentration, high-entropy electrolyte, characterized in that, The high-concentration, high-entropy electrolyte includes a solvent, A first solute salt and an added salt, wherein the first solute salt is a solute salt with high solubility in the solvent, and the added salt comprises three or more solute salts; the total molar concentration of the first solute salt and the added salts in the high-concentration high-entropy electrolyte ranges from 20 M to 60 M, the molar concentration of the first solute salt exceeds 20 M, and the molar concentration of the first solute salt accounts for more than 50% of the molar concentration of the high-concentration high-entropy electrolyte; Wherein, the first solute salt is sodium fluorosulfonamide (NaFSI); the added salt is at least three of lithium nitrate (LiNO3), sodium nitrate (NaNO3), sodium perchlorate (NaClO4), sodium chloride (NaCl), and sodium iodide (NaI); and the solvent is water.

2. The high-concentration, high-entropy electrolyte according to claim 1, characterized in that, The sum of the molar concentrations of the added salts is less than 50% of the molar concentration of the high-concentration, high-entropy electrolyte, and the proportion of added salts is calculated based on the solubility of the solute salts in the solvent.

3. A method for preparing a high-concentration, high-entropy electrolyte, characterized in that, Includes the following steps: S1, Select a solute salt with high solubility as the first solute salt, calculate and weigh the required mass of the first solute salt according to the preset molar concentration, dissolve it in a solvent, heat it, and obtain a basic high-concentration electrolyte; S2, select three or more solute salts as added salts, calculate and weigh the required added salts according to the preset molar concentration, dissolve them in the basic high-concentration electrolyte in step S1, heat them to completely dissolve the added salts, and obtain a mixed high-concentration electrolyte; S3, the mixed high-concentration electrolyte from step S2 is ultrasonically treated in an ultrasonic instrument to ensure that all components in the mixed high-concentration electrolyte are completely mixed, and then cooled to room temperature to obtain a high-concentration high-entropy electrolyte; Wherein, the total molar concentration range of the first solute salt and the added salt in the high-concentration high-entropy electrolyte is 20 M-60 M, the molar concentration of the first solute salt exceeds 20 M, and the molar concentration of the first solute salt accounts for more than 50% of the molar concentration of the high-concentration high-entropy electrolyte. The first solute salt is sodium fluorosulfonamide (NaFSI); the added salt is at least three of lithium nitrate (LiNO3), sodium nitrate (NaNO3), sodium perchlorate (NaClO4), sodium chloride (NaCl), and sodium iodide (NaI); and the solvent is water.

4. A sodium-carbon dioxide battery, characterized in that, The sodium-carbon dioxide battery comprises, in sequence, a sodium metal anode, a negative electrode electrolyte, a solid electrolyte membrane, a positive electrode electrolyte, and a catalyst layer; the sodium metal anode is a sodium metal sheet, and the negative electrode electrolyte is an ester electrolyte of 1 mol / L NaClO4 / [(EC+DMC)(1:1)+1 vol% FEC], where 1:1 is a volume ratio; the solid electrolyte membrane is Na3Zr2Si2PO4. 12 The fast ion conductor has a NASICON structure; the positive electrode electrolyte is a high-concentration high-entropy electrolyte prepared according to any one of claims 1-2 or according to the preparation method of the high-concentration high-entropy electrolyte according to claim 3; the catalyst layer is made of carbon paper with a catalyst supported and nickel foam pressed together, and the catalyst is a 5% Ru / C catalyst.

Citation Information