Mold release film and method for producing molded product

By designing a mold release film with excellent characteristics, using the combination of a thermoplastic resin composition and a polyester resin, the problem of insufficient landfillability and mold release properties of the flexible printed circuit substrate is solved, and effective suppression of the adhesive is achieved The excellent performance of the molded film improves the quality and production efficiency of the molded product.

CN117425566BActive Publication Date: 2024-11-05SUMITOMO BAKELITE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280040308.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-09
Filing Date
2022-06-06
Publication Date
2024-11-05
Estimated Expiration
2042-06-06

AI Technical Summary

Technical Problem

The conventional release film has shortcomings in the landfillability and release properties of the recesses of the flexible printed circuit substrate, and it is difficult to effectively suppress the problems of elongation or fracture during infiltration and peeling of the adhesive.

Method used

The release film of the first release layer composed of the first thermoplastic resin composition and the buffer layer composed of the third thermoplastic resin composition is used to ensure that the complex shear elastic modulus under 80°C is 1.00 MPa or less. And the energy storage elastic modulus and loss shear elastic modulus under 150°C have a specific range. Combined with the combination of polyester resin and polyolefin resin, the thickness and surface roughness of the buffer layer and the release layer are designed. To achieve excellent landfill and mold release.

Benefits of technology

Effective landfill of the recesses of the flexible printed circuit board is achieved, which inhibits adhesive infiltration, and ensures the integrity of the molded film during the peeling process, avoids elongation and fracture, and improves the quality and production efficiency of the molded product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117425566B_ABST
    Figure CN117425566B_ABST
Patent Text Reader

Abstract

The release film (10) of the present invention comprises a first release layer (1) composed of a first thermoplastic resin composition and a buffer layer (3) composed of a third thermoplastic resin composition, wherein the complex shear modulus of the release film (10) at 80° C. is 1.00 MPa or less. Furthermore, the storage modulus of the buffer layer (3) at 150° C. is preferably 9.0 MPa or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a release film and a molded product. Background Art

[0002] In recent years, a release film is generally used when a cover film is bonded to a flexible circuit board with an exposed circuit by heat pressing via an adhesive layer provided on the cover film to form a flexible printed circuit board, that is, a laminate.

[0003] When forming a flexible printed circuit board using such a release film, in other words, a laminate of a flexible circuit board and a cover film, the release film is required to have two properties, namely, both embedding property and release property.

[0004] Specifically, a cover film is first laminated on a flexible circuit board to form a recessed portion on the flexible printed circuit board, but the release film is required to exhibit excellent filling properties for the recessed portion.

[0005] More specifically, the cover film is laminated on the flexible circuit board via the adhesive layer of the cover film. During the lamination, the release film is required to exhibit excellent filling properties for the recessed portion and suppress the adhesive from penetrating into the recessed portion.

[0006] Furthermore, after laminating the cover film on the flexible circuit board as described above, it is required to peel off the release film having excellent releasability from the formed flexible printed circuit board.

[0007] More specifically, when the release film is peeled from the formed flexible printed circuit board, the release film is required to exhibit excellent releasability to the flexible printed circuit board and suppress the occurrence of elongation and breakage in the flexible printed circuit board.

[0008] In order to obtain a release film having both the above two characteristics (embedding property and releasability), for example, Patent Document 1 proposes a release film having a polyester elastomer layer as a release layer and a polyester layer as a cushion layer.

[0009] In the release film, the release layer is arranged in contact with the flexible printed circuit board, and the release film fills the concave portion. Thus, the release film is given a filling property, but from the viewpoint of suppressing the penetration of the adhesive into the concave portion, it is actually required to develop a release film that exhibits a better filling property for the concave portion.

[0010] Such a problem also occurs in the case where a molded product having a recessed portion is manufactured using an object formed of a material containing a semi-cured thermosetting resin with a release film attached thereto and the thermosetting resin is cured in this state.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application Publication No. 2011-88351 Summary of the invention

[0014] Problem that the invention aims to solve

[0015] An object of the present invention is to provide a mold release film capable of exhibiting excellent filling properties in a recessed portion and a method for producing a molded product using the mold release film.

[0016] Means used to solve problems

[0017] Such an object is achieved by the present invention described in the following (1) to (14).

[0018] (1) A release film comprising a first release layer composed of a first thermoplastic resin composition and a cushion layer composed of a third thermoplastic resin composition, wherein:

[0019] The release film has a complex shear modulus of elasticity of 1.00 MPa or less at 80°C.

[0020] (2) The release film according to (1) above, wherein

[0021] The buffer layer has a storage elastic modulus of 9.0 MPa or more at 150°C.

[0022] (3) The release film according to (1) or (2) above, wherein

[0023] The release film has a storage shear modulus of 1.00 MPa or less at 80°C.

[0024] (4) The release film according to any one of (1) to (3) above, wherein

[0025] The loss shear modulus of the release film at 80° C. is 0.40 MPa or less.

[0026] (5) The release film according to any one of (1) to (4) above, wherein

[0027] The first release layer has a surface on the opposite side to the buffer layer and has a ten-point average roughness (Rz) of 0.5 μm or more and 3.6 μm or less.

[0028] (6) The release film according to any one of (1) to (5) above, wherein

[0029] The first release layer has a storage elastic modulus E' at 150° C. of 100 MPa or more.

[0030] (7) The release film according to any one of (1) to (6) above, wherein

[0031] The first thermoplastic resin composition contains a polyester-based resin as a main material.

[0032] (8) The release film according to any one of (1) to (7) above, wherein

[0033] The buffer layer has an average thickness of 60 μm or more and 200 μm or less.

[0034] (9) The release film according to any one of (1) to (8) above, wherein

[0035] The first release layer has an average thickness of 5 μm or more and 30 μm or less.

[0036] (10) The release film according to any one of (1) to (9) above, wherein

[0037] The third thermoplastic resin composition contains a plurality of thermoplastic resins, and the melting point of the thermoplastic resins is lower than 80°C.

[0038] (11) The release film according to the above (10), wherein

[0039] The third thermoplastic resin composition contains a polyester-based resin and a polyolefin-based resin as the thermoplastic resin.

[0040] (12) The release film according to any one of (1) to (11) above, wherein

[0041] The release film includes a second release layer composed of a second thermoplastic resin composition, and the second release layer is laminated on the side of the cushion layer opposite to the first release layer.

[0042] (13) The release film according to any one of (1) to (12) above, wherein

[0043] This release film is used to form a circuit.

[0044] (14) A method for manufacturing a molded article, comprising:

[0045] a step of arranging the release film according to any one of (1) to (13) above on the object so that the first release layer of the release film faces the object side; and

[0046] a step of heat-pressing the object provided with the release film,

[0047] In the step of arranging the release film, the surface of the object on the side where the release film is arranged is formed of a material containing a semi-cured thermosetting resin.

[0048] Effects of the Invention

[0049] According to the present invention, it is possible to produce a release film that exhibits excellent filling properties for recessed portions.

[0050] Therefore, when the release film is used for forming a flexible printed circuit board using, for example, a flexible circuit board and a cover film, the release film having excellent embedding properties can be embedded in the recessed portion formed in the flexible printed circuit board. Therefore, when the recessed portion is formed in the flexible printed circuit board, it is possible to reliably suppress or prevent the adhesive from penetrating from the adhesive layer of the cover film into the formed recessed portion. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 This is a longitudinal sectional view for explaining a method of manufacturing a flexible printed circuit board in a state where a plurality of layers are stacked.

[0052] Figure 2 It is a longitudinal cross-sectional view showing each step in a method for manufacturing a flexible printed circuit board in a multi-layered state.

[0053] Figure 3 It is a longitudinal sectional view which shows the embodiment of the release film of this invention.

[0054] Figure 4 It is a local magnification Figure 3 A partially enlarged longitudinal sectional view of the portion A of the release film shown. DETAILED DESCRIPTION

[0055] Hereinafter, the method for producing the release film and the molded article of the present invention will be described in detail based on the preferred embodiments shown in the drawings.

[0056] In addition, the following is an example of manufacturing a flexible printed circuit board into multiple layers using the release film of the present invention, that is, using the release film of the present invention to form a circuit. And before describing the method for manufacturing the release film and the molded article of the present invention, first, a method for manufacturing a flexible printed circuit board into multiple layers is described.

[0057] <Method for producing flexible printed circuit board>

[0058] Figure 1 This is a longitudinal sectional view for explaining a method of manufacturing a flexible printed circuit board in a state where a plurality of layers are stacked. Figure 2 It is a longitudinal cross-sectional view showing each step in a method for manufacturing a flexible printed circuit board in a multi-layered state. Figure 3 It is a longitudinal sectional view which shows the embodiment of the release film of this invention. Figure 4 It is a local magnification Figure 3 A partial enlarged longitudinal sectional view of the A portion of the release film shown in FIG. Figure 1 to Figure 4 The upper side in the figure is referred to as “up” or “above”, the lower side is referred to as “down” or “below”, the left side is referred to as “left”, and the right side is referred to as “right”.

[0059] In the present embodiment, a method for manufacturing a flexible printed circuit board 200 (hereinafter, sometimes referred to as "FPC200") in a multilayer structure includes: a first step of stacking a laminate in a multilayer structure, wherein the laminate is a state in which glass cloth 300A, release film 10A, FPC200, release film 10B, and glass cloth 300B, each in a sheet form, are stacked in this order; a second step of bonding a cover film 220 (hereinafter, sometimes referred to as "CL film 220") to a flexible circuit board 210 in FPC200 by heat pressing the laminate in the multilayer structure; and a third step of demolding the release film 10 (10A, 10B) from FPC200 to obtain FPC200 in which the CL film 220 is bonded to the flexible circuit board 210. In addition, the method for manufacturing a molded product of the present invention is applicable to the method for manufacturing FPC200.

[0060] Hereinafter, each step will be described in order.

[0061] (1st step)

[0062] First, a laminate is stacked into a plurality of layers, wherein the glass cloth 300A, the release film 10A, the FPC 200, the release film 10B, and the glass cloth 300B, which are each in a sheet form, are stacked in this order (see FIG. Figure 1 , Figure 2 (a). Hereinafter, a case where the above-mentioned laminate is laminated into two layers will be described.

[0063] (1-1) First, three flat-plate-shaped heat compression plates 521 are prepared and arranged so as to form two gaps in the thickness direction thereof.

[0064] (1-2) Next, the glass cloth 300A, the release film 10A, the FPC 200, the release film 10B, and the glass cloth 300B, which are each in the form of a sheet (film), are arranged in the two gaps in an overlapping state in this order from the upper side to the lower side. In addition, in this step (1-2), the FPC 200 arranged in the gap is in a stacked state by overlapping the flexible circuit substrate 210 and the CL film 220, but the flexible circuit substrate 210 and the CL film 220 are not bonded by the adhesive layer 222 of the CL film 220.

[0065] Therefore, if Figure 1 As shown, between the heating and pressing plates 521 , a laminated body in which the glass cloth 300A, the release film 10A, the FPC 200 , the release film 10B, and the glass cloth 300B are stacked in this order is stacked in two layers.

[0066] Moreover, this step (1-2) constitutes a step of disposing a mold release film on the object (FPC 200) in the method for producing a molded article of the present invention.

[0067] (Second step)

[0068] Next, by heat-pressing the laminated bodies stacked in multiple layers through the first step, the CL film 220 and the flexible circuit substrate 210 are bonded to each other in the FPC 200 (see FIG. Figure 1 , Figure 2 (b). ).

[0069] (2-1) First, the heating and compression bonding plates 521 are heated while the glass cloths 300 (300A, 300B) are in contact with the heating and compression bonding plates 521.

[0070] Thus, the laminated body in which the glass cloth 300A, the release film 10A, the FPC 200 , the release film 10B, and the glass cloth 300B are stacked is heated by heat transfer from the heating and pressing plate 521 .

[0071] In the present step (2-1), the temperature at which the laminated body, namely the FPC 200, is heated is not particularly limited, but is, for example, preferably 100° C. or higher and 250° C. or lower, and more preferably 150° C. or higher and 200° C. or lower.

[0072] The time for heating the laminate is not particularly limited, but is preferably 40 seconds to 5000 seconds, more preferably 200 seconds to 4000 seconds. Thus, the glass cloth 300A, the release film 10A, the FPC 200, the release film 10B, and the glass cloth 300B in the laminate can be heated almost uniformly.

[0073] (2-2) Also, almost simultaneously with the heating of the heating and pressing plate 521 in the aforementioned step (2-1), the heating and pressing plate 521 located on the upper side and the heating and pressing plate 521 located on the lower side are brought closer together in their thickness direction (press forming method).

[0074] As a result, in the laminated body in which the glass cloth 300A, the release film 10A, the FPC 200, the release film 10B, and the glass cloth 300B are respectively arranged in the two gaps formed between the three heating and pressing plates 521, the FPC 200 is pressurized via the glass cloths 300A, 300B and the release films 10A, 10B (refer to Figure 1 , Figure 2 (b)).

[0075] Thus, since the FPC 200 is heated and pressurized at the same time, in the FPC 200, the overlapping flexible circuit substrate 210 and the CL film 220 are bonded via the adhesive layer 222 provided on the CL film 220. In other words, the cover layer 221 and the flexible circuit substrate 210 are bonded via the adhesive layer 222. Furthermore, when the FPC 200 is heated / pressurized, that is, when the cover layer 221 and the flexible circuit substrate 210 are bonded via the adhesive layer 222, the release film 10 is embedded in the recess 223 formed in the cover layer 221. Therefore, it is possible to suppress the adhesive from the adhesive layer 222 from penetrating into the recess 223 (refer to Figure 2 (b)).

[0076] In the present step (2-2), the pressure at which the FPC 200 is pressurized is not particularly limited, but is preferably set to 0.1 MPa to 20.0 MPa, and more preferably set to 0.5 MPa to 15.0 MPa.

[0077] The time for pressurizing the FPC 200 is not particularly limited, but is preferably set to 20 sec to 5000 sec, and more preferably set to 100 sec to 4000 sec.

[0078] By setting the pressure and time for pressurizing the FPC 200 within the above ranges, the coverlay 221 and the flexible circuit board 210 can be reliably bonded to each other via the adhesive layer 222 .

[0079] In addition, this step (2-2) constitutes a step of hot pressing the object (FPC200) provided with the release film 10 in the method for manufacturing the molded product of the present invention. And, in the case where the cover layer 221 is composed of a material containing a semi-cured thermosetting resin, the cover layer 221 constitutes the surface of the object (FPC200) on the side where the release film 10 is provided. In addition, the release film 10 is used in a manner that the surface of the first release layer 1 side described later is in contact with the surface of the cover layer 221, so that the shape of the cover layer 221 formed with the recessed portion 223 can be maintained by the release film 10, and the thermosetting resin can be cured, so that the cover layer 221 (molded product) can be molded on the flexible circuit substrate 210 with excellent accuracy.

[0080] Furthermore, in the above, the heating of the FPC 200 in the aforementioned step (2-1) and the pressurization of the FPC 200 in the present step (2-2) are preferably performed almost simultaneously as described above, but they can also be performed in the order of the step (2-1) and the step (2-2). However, by performing the step (2-1) and the step (2-2) almost simultaneously, it is possible to shorten the second step and further shorten the time required for manufacturing the FPC 200.

[0081] (Step 3; Step (3))

[0082] Next, the release film 10 (10A, 10B) is released from the FPC 200 to obtain the FPC 200 in which the CL film 220 is bonded to the flexible circuit board 210 (see FIG. Figure 2 (c). ).

[0083] The method for releasing the release film 10 from the FPC 200 is not particularly limited, and a method of, for example, grasping one end of the release film by hand and then peeling it in a direction of 90° to 180° is preferably used.

[0084] When excellent releasability is exhibited between the heat-compression bonding plate 521 and the release film 10 when the release film 10 is peeled from the FPC 200 , the arrangement of the glass cloth 300 between the heat-compression bonding plate 521 and the release film 10 may be omitted.

[0085] Through the above steps, a method for manufacturing the flexible printed circuit board 200 using the release film 10 is constructed.

[0086] Furthermore, the release film of the present invention is used as the release film 10 suitable for manufacturing the flexible printed circuit board 200. That is, as the release film 10, the following release film is used: the first release layer 1 composed of the first thermoplastic resin composition, the buffer layer 3 composed of the third thermoplastic resin composition, and the second release layer 2 composed of the second thermoplastic resin composition are stacked in this order, and the complex shear elastic modulus of the release film 10 at 80°C is 1.00 MPa or less.

[0087] Here, as described above, in the method of manufacturing the flexible printed circuit board 200 using the release film 10 , it is required to achieve both the filling property of the release film 10 in the recessed portion 223 and the releasability from the flexible printed circuit board 200 .

[0088] However, particularly when considering the filling property of the release film 10 for the recess 223 formed in the flexible printed circuit substrate 200, from the perspective of suppressing the penetration of the adhesive originating from the adhesive layer 222 into the recess 223, it is actually required to develop a release film 10 that has better filling property for the recess 223 in the aforementioned step (2-2).

[0089] In response to this actual situation, in the present invention, a mold release film having a complex shear modulus of 1.00 MPa or less at 80° C. is selected as the mold release film 10. As a result, the mold release film 10 exhibits a more excellent filling property for the recess 223 formed in the flexible printed circuit board 200, thereby suppressing the adhesive from the adhesive layer 222 from penetrating into the recess 223.

[0090] Hereinafter, a release film 10 to which the release film of the present invention is applied will be described.

[0091] <Release film 10>

[0092] like Figure 3 As shown, in this embodiment, the release film 10 is composed of a laminated body in which the first release layer 1, the buffer layer 3 and the second release layer 2 are laminated in this order, and is overlapped and used in a manner in which the surface on the first release layer 1 side contacts the CL film 220 provided in the FPC 200.

[0093] As the release film 10 , as described above, in the present invention, a release film having a complex shear modulus of 1.00 MPa or less at 80° C. is selected. Thereby, a release film 10 having a more excellent followability can be obtained.

[0094] The release film 10 has a better followability, and thus the buffer layer 3 is a layer that is pressed into the first release layer 1 in such a way that the first release layer 1 follows the shape of the concave portion 223 formed by the flexible circuit substrate 210 and the CL film 220 when the overlapping flexible circuit substrate 210 and the CL film 220 are bonded via the adhesive layer 222 in the aforementioned step (2-2) of the flexible printed circuit substrate 200 using the release film 10, and plays a role as a buffer. In addition, since the release film 10 has the buffer layer 3, the CL film 220 can be pressed against the flexible circuit substrate 210 with a uniform pressure through the release film 10.

[0095] As described above, particularly when the heating of FPC200 in the aforementioned step (2-1) and the pressurization of FPC200 in the aforementioned step (2-2) are performed almost simultaneously, the heating of FPC200 in the aforementioned step (2-1) has a lower responsiveness than the pressurization of FPC200 in the aforementioned step (2-2). That is, when the heating and pressurization of FPC200 are performed almost simultaneously, it takes a long time for FPC200 to reach the target heating temperature, compared to the fact that the target pressure can be applied to FPC200 relatively early.

[0096] Therefore, before the FPC 200 is heated under the target heating temperature condition, the target pressure is applied to the FPC 200. Therefore, considering the heating temperature of the FPC 200 in the aforementioned step (2-1), even if the elastic modulus of the release film 10 is set within the range of 100° C. or more and 250° C. or less as the preferred temperature range of the heating temperature, the release film 10 having excellent embedding properties cannot be embedded in the recess 223, and it has been impossible to sufficiently suppress the adhesive from the adhesive layer 222 from penetrating into the recess 223.

[0097] In contrast, in the present invention, the heating temperature of FPC 200 has not reached the target temperature when the target pressure is applied to FPC 200, and the complex shear modulus of the release film 10 at 80° C. is set to 1.00 MPa or less as described above. Therefore, the release film 10 can more surely function as the release film 10 and can be embedded in the recess 223 with the release film 10 having excellent embedding properties. Therefore, the adhesive from the adhesive layer 222 can be surely suppressed or prevented from penetrating into the recess 223.

[0098] Hereinafter, each layer constituting the release film 10 will be described.

[0099] <Buffer layer 3>

[0100] First, the buffer layer 3 will be described. The buffer layer 3 is disposed as an intermediate layer between the first release layer 1 and the second release layer 2 .

[0101] The cushion layer 3 is composed of a third thermoplastic resin composition. In order to impart the aforementioned function to the release film 10, that is, to set the complex shear modulus of the release film 10 at 80°C to be below the aforementioned upper limit, the third thermoplastic resin composition preferably contains a plurality of thermoplastic resins.

[0102] As a combination of multiple thermoplastic resins, for example, there can be mentioned a combination of a polyester resin and a polyolefin resin, a combination of polyolefin resins, and a combination of a polyamide resin and a polyolefin resin, among which, by selecting a combination of a polyester resin and a polyolefin resin, it is relatively easy to set the complex shear modulus of the release film 10 at 80°C to below the aforementioned upper limit value.

[0103] As polyester resin, there is no particular limitation, for example, polyethylene terephthalate (PET), polycyclohexane terephthalate (PCT), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polycyclohexane dimethanol terephthalate, polytrimethylene terephthalate, etc., can be cited, and one of these or a combination of two or more can be used. In addition, when two or more of these are used in combination, the polyester resin can be a mixture of these or a copolymer. Among these, the polyester resin is particularly preferably polybutylene terephthalate. Thus, the buffer layer 3 can be given excellent tracking properties for the recess 223. In addition, when the first thermoplastic resin composition constituting the first release layer 1 contains polybutylene terephthalate, the buffer layer 3 exerts excellent adhesion to the first release layer 1.

[0104] Furthermore, as polyolefin resin, there is no particular limitation, for example, polyethylene such as low-density polyethylene, high-density polyethylene, polypropylene and other α-olefin polymers, copolymers of ethylene and hexene, copolymers of ethylene and octene, copolymers of α-olefin and (meth) acrylic acid ester, copolymers of ethylene and vinyl acetate, α-olefin copolymers such as copolymers of ethylene and (meth) acrylic acid, etc., which have ethylene, propylene, butene, pentene, hexene, octene, etc. as polymer components, can be cited, and one of these or a combination of two or more can be used. Among these, at least one of the copolymers of ethylene and vinyl acetate (ethylene vinyl acetate copolymer) and the copolymers of ethylene and (meth) acrylic acid (ethylene (meth) acrylic acid copolymer) is preferred. Thus, the buffer layer 3 can be given excellent tracking properties for the recess 223.

[0105] In the case of a combination of a polyester resin and a polyolefin resin, the content of the polyester resin in the third thermoplastic resin composition is preferably 5 wt % or more, more preferably 8 wt % or more and 20 wt % or less. This can provide the release film 10 with excellent followability to the recessed portion 223 .

[0106] The melting point of the thermoplastic resin contained in the third thermoplastic resin composition is preferably lower than 80° C., more preferably 40° C. to lower than 80° C. This makes it relatively easy to set the complex shear modulus of the release film 10 at 80° C. to the upper limit.

[0107] Furthermore, the third thermoplastic resin composition constituting the buffer layer 3 may contain additives such as a crystal nucleating agent, an antioxidant, a slip agent, an anti-blocking agent, an antistatic agent, a colorant, and a stabilizer in addition to the aforementioned resin material.

[0108] The storage elastic modulus E' of the buffer layer 3 at 150°C is preferably 9.0 MPa or more, more preferably 10 MPa or more and 50 MPa or less, and further preferably 10 MPa or more and 25 MPa or less. The storage elastic modulus E' of the buffer layer 3 at 150°C is set as described above, so that when the release film 10 in the aforementioned step (2-2) is buried in the recess 223, a portion of the buffer layer 3 is exposed from the edge of the release film 10, and adhesion to the FPC 200 can be reliably suppressed or prevented. Therefore, contamination of the FPC 200 can be reliably suppressed or prevented. In addition, the release film 10 that clamps the edge of the release film 10 in the aforementioned step (3) can be easily peeled off.

[0109] In addition, the storage elastic modulus E' of the buffer layer 3 at 150°C can be obtained, for example, as follows: according to JIS K7244-4, a buffer layer 3 with a width of 4 mm and a length of 20 mm is prepared, and measured using a dynamic viscoelasticity measuring device (manufactured by Hitachi High-Tech Science Corporation, "DMA7100") in a tensile mode, a frequency of 1 Hz, and a heating rate of 5°C / min.

[0110] The average thickness Tk of the buffer layer 3 is preferably 60 μm to 200 μm, more preferably 70 μm to 180 μm. This can more significantly exert the effect obtained by setting the complex shear modulus of the release film 10 at 80° C. to the upper limit value or less.

[0111] <First release layer 1>

[0112] Next, the first release layer 1 will be described. The first release layer 1 is laminated on one surface side of the buffer layer 3 .

[0113] The first release layer 1 has flexibility, and in the aforementioned method for manufacturing a flexible printed circuit board 200 using the release film 10, the release film 10 is overlapped in such a manner that the first release layer 1 contacts the CL film 220 of the FPC 200. Then, in the aforementioned step (2-2) of the manufacturing method, the first release layer 1 is a layer that is pressed in following the shape of the recess 223 formed by the flexible circuit board 210 and the CL film 220 when the overlapped flexible circuit board 210 and the CL film 220 are bonded via the adhesive layer 222, and functions as a protective (buffer) material for preventing the release film 10 from breaking. In addition, the first release layer 1 has a function as a contact layer for exerting the excellent releasability of the release film 10 from the CL film 220 (FPC 200) in the aforementioned step (3).

[0114] Therefore, in the aforementioned step (2-2), it is possible to reliably suppress or prevent the adhesive from the adhesive layer 222 from penetrating into the recess 223 formed in the FPC 200. Furthermore, after forming the FPC 200 in which the flexible circuit substrate 210 and the CL film 220 are bonded via the adhesive layer 222 provided on the CL film 220 in the aforementioned step (2-2), when the release film 10 is peeled off from the FPC 200 in the aforementioned step (3), it is possible to reliably suppress or prevent the elongation and breakage in the FPC 200. Furthermore, in the case where the third thermoplastic resin composition constituting the buffer layer 3 contains a polyester resin, the first release layer 1 can exhibit excellent adhesion to the buffer layer 3.

[0115] The first release layer 1 is composed of a first thermoplastic resin composition. The first thermoplastic resin composition is preferably composed of a composition capable of setting the storage elastic modulus E' of the first release layer 1 at 150°C to 100 MPa or more, and preferably mainly contains a polyester resin. As a result, it is relatively easy to set the storage elastic modulus E' to 100 MPa or more, and the first release layer 1 can be reliably given the above-mentioned function. In addition, it is relatively easy to give the release film 10 the above-mentioned function, that is, it is relatively easy to set the complex shear elastic modulus of the release film 10 at 80°C to below the above-mentioned upper limit.

[0116] Furthermore, the polyester resin is not particularly limited, and for example, the same resin as that mentioned in the third thermoplastic resin composition can be used, and polybutylene terephthalate (PBT) is particularly preferred. Thus, the effect obtained by using the polyester resin can be more significantly exerted. Furthermore, when the third thermoplastic resin composition constituting the buffer layer 3 contains polybutylene terephthalate, the first release layer 1 can be prepared to have excellent adhesion to the buffer layer 3.

[0117] In addition, when the first thermoplastic resin composition is mainly composed of a polyester resin, it may contain a thermoplastic resin other than the polyester resin. Examples of the thermoplastic resin include polyolefin resins such as polyethylene, polypropylene, and poly-4-methylpentene-1, and polystyrene resins such as syndiotactic polystyrene. These resins may be used alone or in combination of two or more.

[0118] Furthermore, the first thermoplastic resin composition may contain at least one of inorganic particles and organic particles in addition to the aforementioned thermoplastic resin.

[0119] The inorganic particles are not particularly limited, and examples thereof include aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whiskers, boron nitride, crystalline silica, amorphous silica, antimony oxide, E glass, D glass, S glass, etc., and one of them or a combination of two or more thereof can be used.

[0120] The organic particles are not particularly limited, and examples thereof include polystyrene particles, acrylic particles, polyimide particles, polyester particles, silicone particles, polypropylene particles, polyethylene particles, fluororesin particles, and core-shell particles. One of these particles or a combination of two or more thereof may be used.

[0121] In addition, the average particle size of the inorganic particles and the organic particles is preferably 3 μm or more and 20 μm or less, and more preferably 5 μm or more and 20 μm or less. Thus, when the first thermoplastic resin composition contains at least one of the inorganic particles and the organic particles, the surface roughness of the surface of the first release layer 1 on the side opposite to the buffer layer 3 can be set relatively easily within the range described below.

[0122] When the first release layer 1 has a concavo-convex shape on its surface, the ten-point average roughness (Rz) of the surface is preferably 0.5 μm or more and 3.6 μm or less, and more preferably 1.0 μm or more and 3.5 μm or less. Thus, when the release film 10 is released from the FPC 200 (flexible circuit board 210), the release can be performed with excellent release properties. In addition, the ten-point average roughness (Rz) can be measured in accordance with JIS B0601-1994.

[0123] The storage elastic modulus E′ of the first release layer 1 having such a structure at 150° C. is preferably 100 MPa or more, more preferably 100 MPa or more and 1000 MPa or less, and particularly preferably 100 MPa or more and 200 MPa or less. Thus, the above-mentioned function can be reliably imparted to the first release layer 1 .

[0124] The storage elastic modulus E' of the first release layer 1 at 150°C can be obtained as follows: in accordance with JIS K7244-4, a first release layer 1 having a width of 4 mm and a length of 20 mm is prepared, and measured using a viscoelasticity measuring apparatus (manufactured by Hitachi High-Tech Sciences, Inc., "DMA7100") in a tensile mode, a frequency of 1 Hz, and a heating rate of 5°C / min.

[0125] The average thickness T1 of the first release layer 1 is preferably 5 μm to 30 μm, more preferably 6 μm to 25 μm. Thus, the average thickness of the first release layer 1 is set within an appropriate range, so that the above-mentioned function can be more reliably imparted to the first release layer 1.

[0126] As described above, when the surface of the first release layer 1 opposite to the buffer layer 3 has an uneven shape, the thickness of the first release layer 1 is measured at a position including the convexities in the convexities and at a position including the concaveities in the concave portions.

[0127] Furthermore, the first thermoplastic resin composition constituting the first mold release layer 1 may contain the same additives as those mentioned above for the third thermoplastic resin composition in addition to the above-mentioned resin material, inorganic particles, and organic particles.

[0128] <Second release layer 2>

[0129] Next, the second mold release layer 2 will be described. The second mold release layer 2 is laminated on the other surface side of the buffer layer 3, that is, on the surface side of the buffer layer 3 opposite to the first mold release layer 1.

[0130] The second release layer 2 has flexibility and in the aforementioned method for manufacturing a flexible printed circuit board 200 using the release film 10, the release film 10 is overlapped in such a manner that the first release layer 1 contacts the CL film 220 of the FPC 200, and then, in the aforementioned step (2-2) of the manufacturing method, when the overlapped flexible circuit board 210 and the CL film 220 are bonded via the adhesive layer 222, the second release layer 2 functions as a layer that transmits the force from the heating and pressing plate 521 to the buffer layer 3. In addition, the second release layer 2 has a function as a contact layer for achieving excellent releasability between the glass cloth 300 and the release film 10 in the aforementioned step (3).

[0131] The second mold release layer 2 is composed of a second thermoplastic resin composition, and the second thermoplastic resin composition is preferably selected to be a resin that can set the storage elastic modulus E' of the second mold release layer 2 at 150°C to 100 MPa or more. Specifically, it is preferably mainly composed of a polyester resin, as in the first thermoplastic resin composition. As a result, the storage elastic modulus E' can be set to 100 MPa or more relatively easily, and the aforementioned function can be reliably imparted to the second mold release layer 2. In addition, the aforementioned function can be imparted to the mold release film 10 relatively easily, that is, the complex shear elastic modulus of the mold release film 10 at 80°C can be set to be less than the aforementioned upper limit relatively easily.

[0132] Furthermore, the polyester resin is not particularly limited, and for example, the same resin as that mentioned in the third thermoplastic resin composition can be used, and polybutylene terephthalate (PBT) is particularly preferred. Thus, the effect obtained by using the polyester resin can be more significantly exerted.

[0133] When the second thermoplastic resin composition is mainly composed of a polyester resin, it may contain a thermoplastic resin other than the polyester resin. As the thermoplastic resin, the same resins as those mentioned in the first thermoplastic resin composition can be used.

[0134] Furthermore, the second thermoplastic resin composition may contain at least one of inorganic particles and organic particles in addition to the aforementioned thermoplastic resin.

[0135] The inorganic particles and the organic particles are not particularly limited, and the same particles as those exemplified in the first thermoplastic resin composition can be used.

[0136] The storage elastic modulus E′ of the second release layer 2 having such a structure at 150° C. is preferably 100 MPa or more, more preferably 100 MPa or more and 1000 MPa or less. Thus, the above-mentioned function can be reliably imparted to the second release layer 2 .

[0137] Furthermore, the average thickness T2 of the second mold release layer 2 is preferably 5 μm or more and 30 μm or less, and more preferably 6 μm or more and 25 μm or less. This allows the second mold release layer 2 to more reliably be provided with the above-mentioned function.

[0138] Furthermore, the second thermoplastic resin composition constituting the second mold release layer 2 may contain the same additives as those mentioned above for the third thermoplastic resin composition in addition to the above-mentioned resin material, inorganic particles, and organic particles.

[0139] Furthermore, in the first release layer 1 and the second release layer 2, the first thermoplastic resin composition and the second thermoplastic resin composition may be the same or different, but are preferably the same or of the same nature from the viewpoint of substitution. In addition, in the first release layer 1 and the second release layer 2, the average thickness thereof may be the same or different.

[0140] In the release film 10 having the structure of the laminated first release layer 1, the buffer layer 3, and the second release layer 2, the average thickness Tt is preferably 90 μm or more and 250 μm or less, and more preferably 100 μm or more and 220 μm or less. Thus, the effect obtained by setting the complex shear modulus of the release film 10 at 80° C. to below the upper limit can be more reliably exerted.

[0141] Here, as described above, the complex shear modulus of the release film 10 at 80° C. may be 1.00 MPa or less, preferably 0.65 MPa or less. By setting the complex shear modulus of the release film 10 at 80° C. as described above, the adhesive from the adhesive layer 222 can be more reliably suppressed or prevented from penetrating into the recess 223 .

[0142] Furthermore, the storage shear modulus of the release film 10 at 80°C is preferably 1.00 MPa or less, and more preferably 0.60 MPa or less. Furthermore, the loss shear modulus of the release film 10 at 80°C is preferably 0.40 MPa or less, and more preferably 0.25 MPa or less. By setting the storage shear modulus and the loss shear modulus of the release film 10 at 80°C as described above, the adhesive from the adhesive layer 222 can be more reliably suppressed or prevented from penetrating into the recess 223.

[0143] The complex shear modulus, storage shear modulus and loss shear modulus of the release film 10 under 80°C conditions can be obtained as follows: for example, a release film 10 having an overall disc shape with a diameter of 8 mm, i.e., a circular shape when viewed from above, is prepared, and measured using a viscoelasticity measuring device (manufactured by Anton Paar GmbH, "MCR102") at a frequency of 10 Hz, a strain of 0.1%, and a heating rate of 4°C / min.

[0144] In addition, in the present embodiment, the release film 10 is composed of a laminate in which the first release layer 1, the buffer layer 3 and the second release layer 2 are stacked in this order, but is not limited to this structure. For example, it can be composed of a laminate having an intermediate layer such as an adhesive layer arranged between the first release layer 1 and the buffer layer 3 and between the second release layer 2 and the buffer layer 3.

[0145] Furthermore, if the release film 10 can maintain excellent releasability between the glass cloth 300 and the release film 10 in the above step (3), the second release layer 2 in contact with the glass cloth 300 may be omitted.

[0146] As mentioned above, although the manufacturing method of the mold release film and the molded article of this invention was demonstrated, this invention is not limited to these.

[0147] For example, in the aforementioned embodiment, the release film of the present invention is applied to a press molding method for manufacturing a flexible printed circuit substrate arranged between heating and cooling plates by stacking two layers, but the number of stacked flexible printed circuit substrates is not limited to two layers, and can be one layer or three or more layers.

[0148] Furthermore, although the release film of the present invention is suitable for use in a case where a flexible printed circuit substrate arranged between heating and cooling plates is pressurized using a press molding method, it is not limited to this. The pressurization of the flexible printed circuit substrate can be implemented, for example, using a roll-to-roll press machine, and can also be implemented using a vacuum pressure molding method.

[0149] [Example]

[0150] Hereinafter, the present invention will be described in detail based on Examples, but the present invention is not limited thereto.

[0151] 1. Preparation of raw materials

[0152] As raw materials for producing the release film, the following materials were prepared respectively.

[0153] Thermoplastic resin material

[0154] Low-density polyethylene (LDPE, manufactured by Ube-Maruzen Polyethlene Co., Ltd., "R300")

[0155] Ethylene vinyl acetate copolymer (EVA, manufactured by DOW-MITSUIPOLY CHEMICALS CO., LTD., "P1403")

[0156] Ethylene vinyl acetate copolymer (EVA, manufactured by DOW-MITSUIPOLYCHEMICALS CO., LTD., "EV360")

[0157] Ethylene vinyl acetate copolymer (EVA, manufactured by DOW-MITSUIPOLY CHEMICALS CO., LTD., "V5274")

[0158] Ethylene methyl methacrylate copolymer (EMMA, manufactured by Sumitomo Chemical Co., Ltd., "WH102")

[0159] Ethylene methyl acrylate copolymer (EMA, manufactured by SK Chemicals Co., Ltd., "29MA03")

[0160] Ethylene methyl acrylate copolymer (EMA, manufactured by Japan Polyethylene Corporation, "EB050S")

[0161] Polybutylene terephthalate (PBT, manufactured by Changchun Petrochemical Company, "1100-630S")

[0162] Copolymer polybutylene terephthalate (PBT, manufactured by Mitsubishi Engineering-Plastics Corporation, “5505S”)

[0163] Polypropylene (PP, manufactured by Sumitomo Chemical Co., Ltd., "FH1016")

[0164] Adhesive polyolefin (AD, manufactured by Mitsubishi Chemical Corporation, "F515A")

[0165] 2. Production of release film

[0166] <Example 1>

[0167] First, as the first thermoplastic resin composition and the second thermoplastic resin composition, a composition composed of 70 parts by weight of polybutylene terephthalate (PBT, 1100-630S) and 30 parts by weight of copolymerized polybutylene terephthalate (PBT, 5505S) was prepared, respectively. And as the third thermoplastic resin composition, a composition composed of 40 parts by weight of ethylene vinyl acetate copolymer (EVA, EV360), 35 parts by weight of ethylene methyl methacrylate copolymer (EMMA, WH102), 10 parts by weight of polybutylene terephthalate (PBT, 1100-630S) and 15 parts by weight of polypropylene (PP, FH1016) was prepared.

[0168] Next, the first thermoplastic resin composition was used to form a film by an extrusion T-die method, thereby obtaining the first mold release layer 1 .

[0169] Next, the first release layer 1 was sequentially subjected to extrusion T-die film formation using the third thermoplastic resin composition and the second thermoplastic resin composition, thereby forming a laminate having the buffer layer 3 and the second release layer 2 laminated in this order on the first release layer 1, thereby obtaining a release film 10 of Example 1.

[0170] In the obtained release film 10 , the first release layer 1 had an average thickness T1 of 15 μm, the buffer layer 3 had an average thickness Tk of 80 μm, and the second release layer 2 had an average thickness T2 of 15 μm.

[0171] In addition, for the release film 10, the complex shear modulus, storage shear modulus and loss shear modulus at 80°C were measured using a viscoelasticity measuring device (manufactured by Anton Paar, "Product No. MCR102") at a frequency of 10 Hz, a strain of 0.1% and a heating rate of 4°C / min. The results were 0.63 MPa, 0.59 MPa and 0.21 MPa, respectively.

[0172] The storage elastic modulus E' of the first release layer 1 and the buffer layer 3 were measured at 150°C using a dynamic viscoelasticity measuring device ("DMA7100" manufactured by Hitachi High-Tech Sciences, Inc.) in a tensile mode at a frequency of 1 Hz and a heating rate of 5°C / min. The results were 180 MPa and 16 MPa, respectively.

[0173] The ten-point average roughness (Rz) of the surface of the first release layer 1 exposed on the side opposite to the buffer layer 3 was measured using a surface roughness measuring device (“SURFTST SJ-210” manufactured by Mitutoyo Corporation) and was found to be 2.7 μm.

[0174] <Example 2, Comparative Examples 1 to 4>

[0175] As the first thermoplastic resin composition, the second thermoplastic resin composition, and the third thermoplastic resin composition, the compositions shown in Table 1 were used, and the first release layer 1, the buffer layer 3, and the second release layer 2 having average thicknesses shown in Table 1 were formed. In the same manner as in Example 1, release films 10 having complex shear moduli at 80° C. as shown in Table 1 were obtained for Example 2 and Comparative Examples 1 to 4.

[0176] 3. Evaluation

[0177] The following evaluations were performed on the release films 10 of the respective Examples and Comparative Examples.

[0178] 3-1. Filling properties of release film

[0179] The release film 10 of each embodiment and each comparative example was set to have a width of 270 mm. Furthermore, a FPC 200 (laminated body) having a concave-convex shape with a pitch of 50 μm, a width of 50 μm, and a height of 18 μm was formed by attaching a cover film 220 (made by Arisawa Manufacturing Co., Ltd., Japan, “CMA0525”) to a flexible circuit substrate 210 with an adhesive layer 222 of the cover film 220 as the side of the flexible circuit substrate 210, and then the release film 10 was pressed into the following conditions at 180° C., 3 MPa, and 15 minutes. Figure 1Then, in a state where the laminate of FPC200 and release film 10 is set, the laminate is cut (sheared) in the thickness direction, and then the release film 10 is peeled off by holding one end of the release film 10. The maximum amount of adhesive infiltration in the concave portion of FPC200 when peeling off by holding one end of the release film 10 in a plan view is measured and evaluated according to the following criteria.

[0180] [Evaluation criteria]

[0181] A: The maximum penetration is less than 55mm.

[0182] B: The maximum penetration amount is 55 or more and less than 65 mm.

[0183] C: The maximum penetration amount is 65 or more.

[0184] 3-2. Release properties of release film

[0185] The release film 10 of each embodiment and each comparative example was set to a width of 270 mm, and was set to be an FPC 200 (laminated body) having a concave-convex shape with a pitch of 50 μm, a width of 50 μm, and a height of 18 μm, formed by attaching a cover film 220 (manufactured by Arisawa Manufacturing Co., Ltd., Japan, "CMA0525") on a flexible circuit substrate 210 so that the adhesive layer 222 of the cover film 220 was on the side of the flexible circuit substrate 210. Then, the release film 10 was pressed into the FPC 200 (laminated body) at 180° C., 3 MPa, and 15 minutes. Figure 1 Then, the release film 10 was peeled off by holding one end of the release film 10 and evaluating the ease of peeling (mold release property) according to the following criteria.

[0186] [Evaluation criteria]

[0187] A: When the release film was peeled off, it was peelable.

[0188] B: When the release film was peeled off, the cushion layers were fused to each other and were difficult to peel off.

[0189] 3-3. Summary

[0190] Table 1 shows the evaluation results obtained in 3-1. embedding property of release film and 3-2. release property of release film.

[0191]

[0192] As shown in Table 1, the following results are shown. In each example, the complex shear modulus of the release film 10 at 80° C. was set to 1.00 MPa or less, and as a result, the penetration of the adhesive into the recessed portion 223 was suppressed.

[0193] On the other hand, in each comparative example, since the complex shear modulus of the release film 10 at 80° C. could not be set to 1.00 MPa or less, it was clearly confirmed that the adhesive penetrated into the recessed portion 223 .

[0194] Description of Reference Numerals

[0195] 1 first release layer;

[0196] 2 second release layer;

[0197] 3. Buffer layer;

[0198] 10 release film;

[0199] 10A release film;

[0200] 10B release film;

[0201] 200 Flexible printed circuit board (FPC);

[0202] 210 flexible circuit substrate;

[0203] 220 covering film (CL film);

[0204] 221 overlay;

[0205] 222 adhesive layer;

[0206] 223 recess;

[0207] 300 glass cloth;

[0208] 300A glass cloth;

[0209] 300B glass cloth;

[0210] 521 Heating and pressing plate;

[0211] T1 average thickness of the first release layer;

[0212] T2 average thickness of the second release layer;

[0213] Tk is the average thickness of the buffer layer;

[0214] Tt Average thickness of release film.

[0215] Industrial Applicability

[0216] According to the present invention, a mold release film having excellent filling properties for a concave portion can be produced. Therefore, when the mold release film is used to form a flexible printed circuit board formed by using, for example, a flexible circuit board and a cover film, the mold release film having excellent filling properties can be filled in the concave portion formed in the flexible printed circuit board. Therefore, when a concave portion is formed on the flexible printed circuit board, it is possible to reliably suppress or prevent the adhesive from penetrating into the formed concave portion from the adhesive layer of the cover film. Therefore, the present invention has industrial applicability.

Claims

1. A release film comprising a first release layer composed of a first thermoplastic resin composition and a buffer layer composed of a third thermoplastic resin composition, wherein: The first thermoplastic resin composition contains a polyester resin as a main material, The third thermoplastic resin composition contains a polyester resin and a polyolefin resin. The complex shear elastic modulus of the release film at 80° C. is less than 1.00 MPa, The storage elastic modulus E' of the first release layer at 150° C. is 100 MPa or more, The buffer layer has a storage elastic modulus of 9.0 MPa or more at 150°C.

2. The release film according to claim 1, wherein The release film has a storage shear modulus of elasticity of 1.00 MPa or less at 80° C.

3. The release film according to claim 1 or 2, wherein The release film has a loss shear modulus of elasticity of 0.40 MPa or less at 80°C.

4. The release film according to claim 1 or 2, wherein The first release layer has a surface on the opposite side to the buffer layer and has a ten-point average roughness Rz of 0.5 μm or more and 3.6 μm or less.

5. The release film according to claim 1 or 2, wherein The buffer layer has an average thickness of 60 μm or more and 200 μm or less.

6. The release film according to claim 1 or 2, wherein The first release layer has an average thickness of 5 μm or more and 30 μm or less.

7. The release film according to claim 1 or 2, wherein The third thermoplastic resin composition contains a plurality of thermoplastic resins, and a portion of the plurality of thermoplastic resins has a melting point of less than 80°C.

8. The release film according to claim 1 or 2, wherein The release film includes a second release layer composed of a second thermoplastic resin composition, and the second release layer is laminated on the side of the cushion layer opposite to the first release layer.

9. The release film according to claim 1 or 2, wherein The release film is used to form a circuit.

10. A method for manufacturing a molded product, characterized in that: include: A step of arranging the release film according to any one of claims 1 to 9 on the object so that the first release layer of the release film faces the object side; as well as a step of heat-pressing the object provided with the release film, In the step of arranging the release film, the surface of the object on the side where the release film is arranged is formed of a material containing a semi-cured thermosetting resin.