Mold release film and method for producing molded product

By using a multi-layer thermoplastic resin composition and a buffer layer structure in the mold release film, the problems of landfillability and mold release in the prior art are solved, and the efficient adhesive suppression on the flexible printed circuit substrate is achieved. Cracks during the ooze and peeling process are prevented, improving the quality of the molded product.

CN115515787BActive Publication Date: 2024-11-05SUMITOMO BAKELITE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180034332.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-12
Filing Date
2021-08-03
Publication Date
2024-11-05
Estimated Expiration
2041-08-03

AI Technical Summary

Technical Problem

The existing mold release films are difficult to have excellent landfillability and mold release properties, resulting in problems of adhesive leakage, crease and fracture on the flexible printed circuit board.

Method used

The release film using the first release layer and the buffer layer formed of the first thermoplastic resin composition has an average thickness of more than 12 μm and less than 38 μm, a storage modulus of more than 30 MPa, and satisfies a specific storage under 180°C. The modulus to thickness ratio is combined with a combination of poly4-methyl 1-pentene resin and other thermoplastic resins to form a multilayer structure to improve landfillability and mold release.

Benefits of technology

It achieves a balanced landfill and mold release property on the flexible printed circuit board, inhibits adhesive leakage, and prevents creases and breaks during the peeling process, thereby improving the quality of the molded product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115515787B_ABST
    Figure CN115515787B_ABST
Patent Text Reader

Abstract

The release film (10) of the present invention comprises a first release layer (1) formed of a first thermoplastic resin composition and a buffer layer (3), wherein the average thickness of the first release layer (1) is 12 μm or more and 38 μm or less, and the storage modulus E' of the release film (10) at 180°C is 30 MPa or more. Furthermore, the average thickness of the release film (10) is preferably 80 μm or more and 180 μm or less, and the average thickness of the buffer layer (3) is preferably 40 μm or more and 110 μm or less. Furthermore, in the first release layer (1), the ten-point average roughness Rz on the surface on the side opposite to the buffer layer (3) is preferably 3 μm or more and 20 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a release film and a molded product. Background Art

[0002] In recent years, when a coverlay film is bonded to a flexible circuit board with an exposed circuit by heat pressing via an adhesive layer provided in the coverlay film to form a flexible printed circuit board, that is, a laminate, a mold release film is generally used.

[0003] When forming a flexible printed circuit board using such a release film, in other words, a laminate of a flexible circuit board and a coverlay film, the release film is required to have two properties, namely, excellent embedding property and excellent release property.

[0004] Specifically, first, a coverlay film is laminated on a flexible circuit board to form a recessed portion in the flexible printed circuit board, but the release film is required to exhibit excellent filling properties for the recessed portion.

[0005] More specifically, the coverlay film is laminated on the flexible circuit board via the adhesive layer provided on the coverlay film. During the lamination, the release film is required to exhibit excellent filling properties for the recessed portion and suppress the oozing of the adhesive in the recessed portion.

[0006] Furthermore, after laminating the coverlay film on the flexible circuit board as described above, it is required to peel the release film from the formed flexible printed circuit board with excellent releasability.

[0007] More specifically, when the release film is peeled from the formed flexible printed circuit board, the release film is required to exhibit excellent releasability to the flexible printed circuit board and suppress the occurrence of creases and breaks in the flexible printed circuit board.

[0008] In order to provide a mold release film having excellent two properties (embedding property and mold release property) as described above, a mold release film having a polyester elastomer layer and a polyester layer is proposed, for example, in Patent Document 1. However, in the mold release film of this structure, it cannot be said that both excellent embedding property and excellent mold release property are achieved, and the fact is that a mold release film having a better balance of these two properties is required to be developed.

[0009] Such a problem also occurs in the case where a mold release film is attached to an object made of a material containing a semi-cured thermosetting resin, and the thermosetting resin is cured in this state to produce a molded product using the object.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: Japanese Patent Application Publication No. 2011-88351. Summary of the invention

[0013] Technical issues to be solved by the invention

[0014] An object of the present invention is to provide a mold release film capable of exhibiting both excellent embedding properties and excellent releasability in a balanced manner, and a method for producing a molded article using the mold release film.

[0015] Means for solving problems

[0016] Such objects are achieved by the present invention described in the following (1) to (13).

[0017] (1) A release film comprising a first release layer formed of a first thermoplastic resin composition and a buffer layer, wherein the first release layer has an average thickness of 12 μm to 38 μm, and the release film has a storage modulus E' of 30 MPa or more at 180°C.

[0018] (2) The release film according to the above (1), wherein the average thickness of the release film is 80 μm or more and 180 μm or less.

[0019] (3) The release film according to (1) or (2) above, wherein the average thickness of the buffer layer is 40 μm or more and 110 μm or less.

[0020] (4) The release film according to any one of (1) to (3) above, wherein the first release layer has a ten-point average roughness (Rz) of 3 μm or more and 20 μm or less on a surface opposite to the buffer layer.

[0021] (5) The release film according to any one of (1) to (4) above, wherein the first release layer has a storage modulus E′ of 60 MPa or more at 180° C.

[0022] (6) The release film according to any one of (1) to (5) above, wherein, when the average thickness of the first release layer is set to T1 [μm] and the storage modulus E' of the first release layer at 180°C is set to E'1 [MPa], E'1 / T1 [MPa / μm] satisfies the relationship of 2.1<E'1 / T1<6.0.

[0023] (7) The release film according to any one of (1) to (6) above, wherein the first thermoplastic resin composition comprises a poly (4-methylpentene-1) resin.

[0024] (8) The release film according to any one of (1) to (7) above, wherein the cushion layer is formed of a third thermoplastic resin composition comprising a poly (4-methylpentene-1) resin and a polyolefin-based resin different from the poly (4-methylpentene-1) resin.

[0025] (9) The release film according to any one of (1) to (8) above, comprising a second release layer formed of a second thermoplastic resin composition laminated on the side of the buffer layer opposite to the first release layer.

[0026] (10) A release film according to any one of (1) to (9) above, wherein the release film having a width of 270 mm is pressed and adhered to a flexible circuit substrate having projections and depressions with a pitch of 50 μm, a width of 50 μm, and a height of 18 μm by a roll-to-roll press under the conditions of 180°C, 11 MPa, and 120 sec, and when the flexible circuit substrate and the release film are peeled off while being conveyed immediately after the pressurization, the limit peeling speed at which no wrinkles are observed on the release film becomes greater than 100 mm / sec.

[0027] (11) A release film according to any one of (1) to (10) above, wherein the release film having a width of 270 mm is pressed into a laminate formed by attaching a covering layer film (manufactured by Arisawa Manufacturing Co., Ltd., "CMA0525") to a flexible circuit substrate having projections and depressions with a pitch of 50 μm, a width of 50 μm, and a height of 18 μm under the conditions of 180°C, 11 MPa, and 120 s, and the adhesive layer possessed by the covering layer film is on the side of the flexible circuit substrate, and then, when one end of the release film is grasped and peeled off, the maximum amount of adhesive seepage in the recessed portion of the laminate as viewed from above becomes less than 100 μm.

[0028] (12) A release film according to any one of (1) to (11) above, wherein the release film is used by overlapping the surface of an object in such a manner that the surface on the first release layer side is in contact with the surface of the object formed by a material containing a semi-cured thermosetting resin.

[0029] (13) A method for manufacturing a molded product, characterized in that the method for manufacturing a molded product includes a step of arranging the release film on the object in such a manner that the first release layer of the release film described in any one of (1) to (12) above becomes the object side, and a step of heating and pressing the object on which the release film is arranged, and in the step of arranging the release film, the surface of the side of the object on which the release film is arranged is formed by a material containing a thermosetting resin in a semi-cured state.

[0030] Effects of the Invention

[0031] According to the present invention, it is possible to provide a release film that exhibits both excellent embedding properties and excellent releasability in a balanced manner.

[0032] Therefore, when the release film is used to form a flexible printed circuit board using a flexible circuit board and a coverlay film, for example, it is possible to reliably suppress or prevent the adhesive from seeping into the recessed portion formed in the flexible printed circuit board.

[0033] Furthermore, after the flexible printed circuit board is formed, when the release film is peeled off from the flexible printed circuit board, the occurrence of creases and breaks in the flexible printed circuit board can be reliably suppressed or prevented. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a side view showing the main part of a roll-to-roll pressing machine for manufacturing a flexible printed circuit board.

[0035] Figure 2 It means using Figure 1 2 is a longitudinal cross-sectional view of each step in a method for manufacturing a flexible printed circuit board using a roll-to-roll pressing machine shown in FIG.

[0036] Figure 3 It means using Figure 1 A longitudinal sectional view of a heating and pressing step in a method for manufacturing a flexible printed circuit board using a roll-to-roll pressing machine shown in FIG.

[0037] Figure 4 It is a longitudinal sectional view which shows the embodiment of the release film of this invention.

[0038] Figure 5 It is a local magnification Figure 4 A partially enlarged longitudinal sectional view of the portion A of the release film shown in FIG. DETAILED DESCRIPTION

[0039] Hereinafter, the method for producing the release film and the molded article of the present invention will be described in detail based on the preferred embodiments shown in the drawings.

[0040] In addition, the case of manufacturing a flexible printed circuit board using the release film of the present invention is described below as an example. And before describing the method for manufacturing the release film and the molded product of the present invention, first, a roll-to-roll press for manufacturing a flexible printed circuit board is described.

[0041] <Roll-to-roll press>

[0042] Figure 1 is a side view showing the main part of a roll-to-roll press for manufacturing a flexible printed circuit board, Figure 2 It means using Figure 1 A longitudinal cross-sectional view of each step in a method for manufacturing a flexible printed circuit board using a roll-to-roll press machine shown in FIG. Figure 3It means using Figure 1 A longitudinal cross-sectional view of the heating and pressing process in the method for manufacturing a flexible printed circuit board using a roll-to-roll pressing machine shown in FIG. Figure 1 to Figure 3 The upper side in the figure is referred to as “up” or “above”, the lower side is referred to as “down” or “below”, the left side is referred to as “left”, and the right side is referred to as “right”.

[0043] The roll-to-roll pressing machine 100 (RtoR pressing machine) includes: a conveying mechanism (not shown) for conveying a release film 10, a flexible printed circuit board 200 (hereinafter, sometimes referred to as "FPC") and glass cloths 300A and 300B; a heating and pressing mechanism 50 for bonding a flexible circuit board 210 and a covering layer film 220 (hereinafter, sometimes referred to as "CL film") provided by the FPC 200 by using the release film 10 to heat and press the CL film 220 onto the flexible circuit board 210; and a demolding mechanism 60 for demolding (peeling off) the release film 10 from the FPC 200 to which the CL film 220 is bonded.

[0044] In the conveying mechanism, the FPC 200, the release films 10A, 10B, and the glass cloths 300A, 300B respectively wound on different feed rollers are respectively conveyed along these length directions by the rotation of the tensioner (tension roller), and after being processed by the heating and pressing mechanism 50 and the demolding mechanism 60, they are wound on the winding rollers.

[0045] Each roller is made of a metal material such as stainless steel, etc. The rollers are arranged so that their rotation axes (central axes) face the same direction and are spaced apart from each other.

[0046] like Figure 1 As shown, the heating and pressing mechanism 50 has a heating and pressing portion 52 .

[0047] The heating and pressing section 52 has a pair of heating and pressing plates 521. The heating and pressing plates 521 are conveyed by a conveying mechanism and are opposite to the glass cloth 300A, the release film 10A, the FPC 200, the release film 10B, and the glass cloth 300B in an overlapping state, and one is arranged above and below each. Furthermore, when the glass cloth 300A, the release film 10A, the FPC 200, the release film 10B, and the glass cloth 300B in an overlapping state pass between the heating and pressing plates 521, the FPC 200 is heated and pressurized via the glass cloths 300A, 300B and the release films 10A, 10B by the heating and pressing plates 521. Therefore, in the FPC 200, the overlapping flexible circuit substrate 210 and the CL film 220 are bonded via the adhesive layer 222 of the CL film 220. In other words, the cover layer 221 and the flexible circuit board 210 are bonded via the adhesive layer 222. When the FPC 200 is heated and pressurized, that is, when the cover layer 221 and the flexible circuit board 210 are bonded via the adhesive layer 222, the release film 10 is embedded in the recess 223 formed in the cover layer 221. Therefore, the adhesive in the recess 223 from the adhesive layer 222 can be suppressed from leaking out (see Figure 2 (b)).

[0048] Before the heat and pressure bonding by the heat and pressure bonding plate 521 , the FPC 200 is in a stacked state by overlapping the flexible circuit substrate 210 and the CL film 220 , but the flexible circuit substrate 210 and the CL film 220 are not bonded by the adhesive layer 222 of the CL film 220 .

[0049] like Figure 1 As shown, the demolding mechanism 60 is arranged on the downstream side of the conveying direction relative to the heating and pressing mechanism 50. The demolding mechanism 60 is configured to separate the FPC200 from the demolding films 10A and B. As described above, in the heating and pressing section 52 provided in the heating and pressing mechanism 50, the demolding film 10 is embedded in the recess 223 formed in the covering layer 221, so that the demolding film 10 is bonded to the CL film 220 (FPC200). Thereafter, the roll-to-roll pressing machine 100 is configured to be able to peel (demold) the demolding film 10 from the CL film 220 (FPC200) through the action of the demolding mechanism 60 (refer to Figure 2 (c)).

[0050] The roll-to-roll press machine 100 described above can be used to manufacture a flexible printed circuit board 200 (FPC 200). Hereinafter, a method for manufacturing the FPC 200 using the roll-to-roll press machine will be described. In addition, the method for manufacturing a molded product of the present invention is applied to the method for manufacturing the FPC 200.

[0051] In the present embodiment, the manufacturing method of FPC200 includes: a first step of setting the glass cloth 300A, the release film 10A, the FPC200, the release film 10B and the glass cloth 300B, which are each in a sheet form, as a stacked body in a state of overlapping in sequence; a second step of heating and pressing the stacked body to bond the covering layer 221 (CL film 220) to the flexible circuit substrate 210 in the FPC200 via the adhesive layer 222; and a third step of demolding the release film 10 (10A, 10B) from the FPC200 to obtain the FPC200 with the CL film 220 bonded to the flexible circuit substrate 210.

[0052] Hereinafter, each of these steps will be described in sequence.

[0053] (First process)

[0054] First, the glass cloth 300A, the release film 10A, the FPC 200, the release film 10B, and the glass cloth 300B, which are each in a sheet form and are wound around a feed roller, are conveyed by a conveying mechanism to form a laminated body in a state where they are overlapped in this order (see FIG. Figure 1 , Figure 2 (a) Figure 3 ).

[0055] In addition, the method of stacking the components (films) into a laminate is not particularly limited. For example, the components can be stacked while being pressed by a roller, or can be stacked while being pressed by a press. In addition, the order of stacking the components can also be arbitrary. For example, all components can be stacked at the same time, or the cover layer film 220 and the flexible circuit substrate 210 can be stacked in advance, and then other components can be stacked at the same time.

[0056] Then, by forming the laminated body in the first step, a step of disposing the release film 10 on the object (FPC 200 ) in the method for producing a molded article of the present invention is constituted.

[0057] (Second process)

[0058] Next, the laminated body formed by stacking the glass cloth 300A, the release film 10A, the FPC 200, the release film 10B, and the glass cloth 300B in this order is heated and pressed by the heating and pressing mechanism 50 (heating and pressing section 52), thereby bonding the cover layer 221 (CL film 220) to the flexible circuit substrate 210 via the adhesive layer 222 in the FPC 200 (heating and pressing step, see Figure 1 , Figure 2 (b) Figure 3 ).

[0059] In the heat pressing step, the temperature at which the FPC 200 is heated is not particularly limited, but is, for example, preferably 100° C. or higher and 250° C. or lower, and more preferably 150° C. or higher and 200° C. or lower.

[0060] Furthermore, in the heating and pressing step, the pressure at which the FPC 200 is pressed is not particularly limited, but is preferably set to 1 MPa or more and 14 MPa or less, and more preferably set to 5 MPa or more and 14 MPa or less.

[0061] Furthermore, the conveying speed of the stacked body is not particularly limited, but is preferably 40 mm / sec to 400 mm / sec, and more preferably 200 mm / sec to 350 mm / sec.

[0062] In addition, the heating and pressing step constitutes a step of heating and pressing the object (FPC200) provided with the release film 10 in the method for manufacturing the molded product of the present invention. And, in the case where the covering layer 221 (insulating layer) is composed of a material containing a semi-cured thermosetting resin, the covering layer 221 constitutes the surface of the side of the object (FPC200) on which the release film 10 is provided. And, using the release film 10, the surface of the first release layer 1 side is overlapped with the surface of the covering layer 221 in such a manner that the surface is in contact with the surface of the covering layer 221, so that the shape of the covering layer 221 formed with the recess 223 can be maintained by the release film 10, and the thermosetting resin can be cured. Thus, the covering layer 221 (molded product) can be molded on the flexible circuit substrate 210 with excellent precision. And, in the present embodiment, a method of heating by heating and pressing is shown, but it is not necessarily limited to this method, for example, heating can be performed by infrared rays, and heating can also be performed by a heating roller.

[0063] (Third process)

[0064] Next, in the demolding mechanism 60, the demolding films 10 (10A, 10B) are demolded from the FPC 200. That is, the demolding films 10A and 10B are peeled off from the bonded body of the cover layer film 220 and the flexible circuit substrate 210. Thus, the FPC 200 (refer to FIG. 2 ) in which the CL film 220 is bonded to the flexible circuit substrate 210 is obtained. Figure 1 , Figure 2 (c) Figure 3 ).

[0065] In addition, the demolding mechanism 60 is not particularly limited. For example, it can be a structure in which a vacuum device is set on the outside to perform vacuum suction to achieve peeling, or it can be a structure in which air is sent between the joint body and the release films 10A, 10B to achieve peeling, or it can be a structure in which a rod is clamped between the joint body and the release films 10A, 10B to achieve peeling.

[0066] Thereafter, the bonded body of the coverlay film 220 and the flexible circuit board 210 , the glass cloth 300A, the release film 10A, the release film 10B, and the glass cloth 300B are wound up by respective take-up rolls.

[0067] By winding in this way, the FPC 200 in which the flexible circuit board 210 and the CL film 220 are bonded to each other via the adhesive layer 222 provided in the CL film 220 can be continuously obtained in a state of being wound on a take-up roll.

[0068] As described above, by applying the method for manufacturing the flexible printed circuit board 200 using the roll-to-roll pressing machine 100 using the release film 10 , the flexible printed circuit board 200 can be manufactured continuously.

[0069] Furthermore, the release film of the present invention can be used as the release film 10 used in the roll-to-roll press machine 100. That is, as the release film 10, a release film is used, which is characterized by having a first release layer formed of a first thermoplastic resin composition and a buffer layer, the average thickness of the first release layer is 12 μm or more and 38 μm or less, and the storage modulus E' of the entire release film layer at 180° C. is 30 MPa or more.

[0070] The mold release film 10 has such a structure, and thereby can be a mold release film that exhibits both excellent embedding properties and excellent mold release properties in a balanced manner.

[0071] Therefore, as described above, when a release film is used to form FPC200 using flexible circuit board 210 and CL film 220, in the second step, it is possible to reliably suppress or prevent the adhesive from adhesive layer 222 from seeping into recess 223 formed in FPC200.

[0072] Furthermore, after forming the FPC 200 in which the flexible circuit substrate 210 and the CL film 220 are bonded via the adhesive layer 222 of the CL film 220 , when the release film 10 is peeled off from the FPC 200 in the third step, creases and breaks in the FPC 200 can be reliably suppressed or prevented.

[0073] Hereinafter, a release film 10 to which the release film of the present invention is applied will be described. In addition, the case where the release film 10 is composed of a laminated body in which the first release layer 1, the buffer layer 3, and the second release layer 2 are laminated in this order will be described below.

[0074] <Release film 10>

[0075] Figure 4 is a longitudinal sectional view showing an embodiment of the release film of the present invention, Figure 5 It is a local magnification Figure 4In the following description, for the sake of convenience, Figure 4 , Figure 5 The upper side in the figure is referred to as “upper”, and the lower side is referred to as “lower”.

[0076] like Figure 4 As shown, in this embodiment, the release film 10 is sequentially stacked with a first release layer 1, a buffer layer 3 and a second release layer 2, and is used by overlapping the CL film 220 in such a way that the surface of the first release layer 1 side is in contact with the CL film 220 of the FPC 200.

[0077] Hereinafter, each layer constituting the release film 10 will be described.

[0078] <First release layer 1>

[0079] First, the first mold release layer 1 will be described. The first mold release layer 1 is laminated on one surface side of the buffer layer 3 .

[0080] The first release layer 1 has flexibility. In the aforementioned method for manufacturing a flexible printed circuit board 200 based on a roll-to-roll press machine 100 using the release film 10, the release film 10 overlaps with the CL film 220 of the FPC 200 so that the first release layer 1 is in contact with the CL film 220. In addition, the first release layer 1 is a layer that is pressed into the second step of the manufacturing method by following the shape of the recess 223 formed by the flexible circuit board 210 and the CL film 220 when it is bonded to the overlapping flexible circuit board 210 and the CL film 220 via the adhesive layer 222. Thus, the first release layer 1 functions as a protective (buffer) material for preventing the release film 10 from breaking. Furthermore, the first release layer 1 has a function as a contact layer for exerting the excellent release property of the release film 10 from the CL film 220 (FPC 200) in the third step.

[0081] The first mold release layer 1 is composed of a first thermoplastic resin composition. The first thermoplastic resin composition is not particularly limited as long as it is a composition that can set the storage modulus E' of the mold release film 10 at 180°C to 30 MPa or more, but preferably contains poly-4-methyl-1-pentene resin (polymethylpentene; TPX (registered trademark)) as a main component. As a result, the storage modulus E' can be set to 30 MPa or more relatively easily, and the above-mentioned function can be reliably imparted to the first mold release layer 1.

[0082] Therefore, as described above, when the release film 10 is used to form the FPC 200 using the flexible circuit board 210 and the CL film 220 , in the second step, the adhesive from the adhesive layer 222 can be reliably suppressed or prevented from seeping into the recess 223 formed in the FPC 200 .

[0083] Furthermore, after forming the FPC 200 in which the flexible circuit substrate 210 and the CL film 220 are bonded via the adhesive layer 222 of the CL film 220 , when the release film 10 is peeled off from the FPC 200 in the third step, creases and breaks in the FPC 200 can be reliably suppressed or prevented.

[0084] Furthermore, the melt flow rate (MFR) of the poly 4-methyl-1-pentene resin measured at 260°C and a load of 5.0 kg is preferably 5 g / 10 min or more and 250 g / 10 min or less, more preferably 30 g / 10 min or more and 200 g / 10 min or less, and still more preferably 40 g / 10 min or more and 160 g / 10 min or less. Thus, the effect obtained by using the poly 4-methyl-1-pentene resin can be more significantly exerted.

[0085] In addition, the first thermoplastic resin composition may contain a resin material other than the poly-4-methyl-1-pentene resin. Examples of the resin material include polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyolefin resins other than poly-4-methyl-1-pentene such as polyethylene and polypropylene; and polystyrene resins such as syndiotactic polystyrene. One of these resins or a combination of two or more thereof may be used.

[0086] Furthermore, the first thermoplastic resin composition may contain at least one of inorganic particles and organic particles in addition to the poly-4-methyl-1-pentene resin. By including the above particles in the first thermoplastic resin composition, especially when an air knife film forming method is used, such as Figure 5 As shown, the first release layer 1 having a concavo-convex shape on the surface of the first release layer 1 on the side opposite to the buffer layer 3 can be formed.

[0087] The inorganic particles are not particularly limited, but for example, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whiskers, boron nitride, crystalline silica, amorphous silica, antimony oxide, E glass, D glass, S glass, etc. can be mentioned. One of these or a combination of two or more can be used.

[0088] Furthermore, the organic particles are not particularly limited, but examples thereof include polystyrene particles, acrylic particles, polyimide particles, polyester particles, silicone particles, polypropylene particles, polyethylene particles, fluororesin particles, and core-shell particles, and one of these particles or a combination of two or more thereof may be used.

[0089] Furthermore, the average particle size of the inorganic particles and the organic particles is preferably 3 μm to 20 μm, more preferably 5 μm to 20 μm. This ensures that the uneven shape can be formed on the surface of the first release layer 1 opposite to the buffer layer 3 .

[0090] In the first release layer 1 having the concavo-convex shape on the surface, the ten-point average roughness (Rz) on the surface is preferably 3 μm or more and 20 μm or less, more preferably 5 μm or more and 17 μm or less, and further preferably 7 μm or more and 17 μm or less. Thus, the first release layer 1 can be more reliably given the aforementioned function. In addition, in the second step, when the first release layer 1 is pressed into the concave portion 223 formed in the FPC 200, the concavo-convex shape can be reliably suppressed or prevented from being transferred to the surface of the flexible circuit substrate 210 and the CL film 220. In addition, the ten-point average roughness (Rz) can be measured in accordance with JIS B 0601-1994.

[0091] The storage modulus E'1 of the first release layer 1 having such a structure at 180°C is preferably 60 MPa or more, more preferably 65 MPa or more and 150 MPa or less, further preferably 68 MPa or more and 150 MPa or less, and particularly preferably 70 MPa or more and 100 MPa or less. Thus, by setting the storage modulus E'1 of the first release layer 1 at 180°C as described above, the storage modulus E't of the release film 10 at 180°C can be set to 30 MPa or more relatively easily.

[0092] In addition, the storage modulus E'1 of the first release layer 1 at 180°C can be obtained as follows: in accordance with JIS K7244-4, a first release layer 1 with a width of 4 mm and a length of 20 mm is prepared, and a dynamic viscoelasticity measuring device (manufactured by SII NanoTechnology Inc., "DMS6100") is used to measure the first release layer 1 under the conditions of tensile mode, a frequency of 1 Hz, and a heating rate of 5°C / min.

[0093] Furthermore, in the present invention, the average thickness T1 of the first release layer 1 is set to be 12 μm or more and 38 μm or less, preferably 14 μm or more and 36 μm or less, and more preferably 25 μm or more and 36 μm or less. Thus, the first release layer 1 can be more reliably provided with the aforementioned function, and the storage modulus E' of the release film 10 at 180° C. can be reliably set to be 30 MPa or more.

[0094] Furthermore, when the average thickness of the first release layer 1 is set to T1 [μm] and the storage modulus E' of the first release layer 1 at 180°C is set to E'1 [MPa], E'1 / T1 [MPa / μm] preferably satisfies the relationship of 2.1 < E'1 / T1 < 6.0, more preferably satisfies the relationship of 2.2 < E'1 / T1 < 5.0, and further preferably satisfies the relationship of 2.2 < E'1 / T1 < 2.9. Thus, the effect obtained by setting the storage modulus E' and the average thickness of the first release layer 1 as described above can be more significantly exerted.

[0095] As described above, when the surface of the first release layer 1 opposite to the buffer layer 3 has an uneven shape, the thickness of the first release layer 1 is measured at a position including the convexities in the convexities and at a position including the concaveities in the concave portions.

[0096] Furthermore, the first thermoplastic resin composition constituting the first release layer 1 may contain additives such as a crystal nucleating agent, an antioxidant, a slip agent, an anti-adhesive agent, an antistatic agent, a colorant, and a stabilizer in addition to the aforementioned resin material, inorganic particles, and organic particles.

[0097] In addition, when the first thermoplastic resin composition contains a crystal nucleus agent, the crystallinity of polymethylpentene can be increased, and as a result, the storage modulus E′ can be set to 30 MPa or more relatively easily.

[0098] In this case, the content of the crystal nucleating agent in the first thermoplastic resin composition is preferably 0.1% by weight or more and 2.0% by weight or less, and more preferably 0.3% by weight or more and 0.8% by weight or less.

[0099] <Buffer layer 3>

[0100] Next, the buffer layer 3 will be described. The buffer layer 3 is provided as an intermediate layer between the first release layer 1 and the second release layer 2 .

[0101] The buffer layer 3 has excellent followability. As described above, in the manufacturing method of the flexible printed circuit board 200 based on the roll-to-roll pressing machine 100 using the release film 10, the release film 10 overlaps with the CL film 220 of the FPC 200 so that the first release layer 1 is in contact with the CL film 220. In addition, the buffer layer 3 is a layer that is pressed into the first release layer 1 in a manner that follows the shape of the recess 223 formed by the flexible circuit board 210 and the CL film 220 when it is bonded to the overlapping flexible circuit board 210 and the CL film 220 via the adhesive layer 222 in the second step of the manufacturing method, and has a function as a buffer. In addition, by having the buffer layer 3 on the release film 10, the CL film 220 can be pressed against the flexible circuit board 210 with uniform pressure through the release film 10.

[0102] The buffer layer 3 is composed of a third thermoplastic resin composition. The third thermoplastic resin composition is not particularly limited as long as it can impart excellent conformability to the buffer layer 3. For example, it preferably contains poly-4-methyl-1-pentene resin (polymethylpentene; TPX (registered trademark)) and a polyolefin resin different from the poly-4-methyl-1-pentene resin. Thus, the buffer layer 3 can be imparted with excellent conformability, and the buffer layer 3 can exhibit excellent adhesion to the first release layer 1 and the second release layer 2.

[0103] The content of the poly 4-methylpentene-1 resin in the third thermoplastic resin composition is preferably 20% by weight or more, more preferably 20% by weight or more and 50% by weight or less. This can more significantly exert the effects obtained by setting the composition containing the poly 4-methylpentene-1 resin and the polyolefin-based resin.

[0104] Furthermore, the melt flow rate (MFR) of the poly 4-methyl-1-pentene resin measured at 260°C and 5.0 kg load is preferably 5 g / 10 min or more and 250 g / 10 min or less, more preferably 15 g / 10 min or more and 200 g / 10 min or less, and further preferably 20 g / 10 min or more and 150 g / 10 min or less. Thus, in the second step, the buffer layer 3 can be more reliably given a function as a press-in layer that presses the first release layer 1 in such a manner that the first release layer 1 follows the shape of the recess 223 formed by the flexible circuit substrate 210 and the CL film 220.

[0105] Furthermore, the polyolefin resin other than the poly-4-methyl-1-pentene resin contained in the third thermoplastic resin composition is not particularly limited, and examples thereof include α-olefin polymers such as polyethylene and polypropylene; α-olefin copolymers having ethylene, propylene, butene, pentene, hexene, methylpentene, etc. as polymer components, and the like. One of these or a combination of two or more thereof can be used.

[0106] Furthermore, the average thickness Tk of the buffer layer 3 is preferably 40 μm to 110 μm, more preferably 50 μm to 100 μm, and further preferably 60 μm to 85 μm. Thus, the buffer layer 3 can be more reliably provided with the aforementioned function, and the storage modulus E' of the release film 10 at 180° C. can be reliably set to 30 MPa or more.

[0107] In addition, the third thermoplastic resin composition constituting the buffer layer 3 may contain the same additives as those mentioned in the first thermoplastic resin composition in addition to the aforementioned resin material.

[0108] <Second release layer 2>

[0109] Next, the second mold release layer 2 will be described. The second mold release layer 2 is laminated on the other surface side of the buffer layer 3, that is, on the side of the buffer layer 3 opposite to the first mold release layer 1.

[0110] The second release layer 2 has flexibility. As described above, in the manufacturing method of the flexible printed circuit board 200 based on the roll-to-roll pressing machine 100 using the release film 10, the release film 10 is overlapped with the CL film 220 of the FPC 200 so that the first release layer 1 is in contact with the CL film 220. In addition, the second release layer 2 functions as a layer that transmits the force from the heating and pressing plate 521 to the buffer layer 3 when it is bonded to the overlapping flexible circuit board 210 and the CL film 220 via the adhesive layer 222 in the second step of the manufacturing method. Furthermore, the second release layer 2 has a function as a contact layer for achieving excellent releasability between the glass cloth 300A, 300B and the release film 10 in the third step.

[0111] The second mold release layer 2 is formed of a second thermoplastic resin composition. The second thermoplastic resin composition is not particularly limited as long as it is a composition that can set the storage modulus E' of the mold release film 10 at 180°C to 30 MPa or more. However, like the first thermoplastic resin composition, it preferably contains poly-4-methyl-1-pentene resin (polymethylpentene; TPX (registered trademark)) as a main component. Thus, the storage modulus E' can be set to 30 MPa or more relatively easily, and the above-mentioned function can be reliably imparted to the second mold release layer 2.

[0112] Furthermore, the melt flow rate (MFR) of the poly 4-methyl-1-pentene resin measured at 260°C and a load of 5.0 kg is preferably 5 g / 10 min or more and 250 g / 10 min or less, more preferably 30 g / 10 min or more and 200 g / 10 min or less, and still more preferably 40 g / 10 min or more and 160 g / 10 min or less. Thus, the effect obtained by using the poly 4-methyl-1-pentene resin can be more significantly exerted.

[0113] The second thermoplastic resin composition may contain a resin material other than the poly-4-methylpentene-1 resin, and as the resin material, the same resin material as exemplified in the first thermoplastic resin composition can be used.

[0114] Furthermore, the second thermoplastic resin composition may contain at least one of inorganic particles and organic particles in addition to the poly-4-methyl-1-pentene resin. By including the above particles in the second thermoplastic resin composition, especially when an air knife film forming method is used, such as Figure 5 As shown, the second release layer 2 having a concavo-convex shape on the surface of the second release layer 2 on the side opposite to the buffer layer 3 can be formed.

[0115] The inorganic particles and organic particles are not particularly limited, but the same particles as those mentioned in the first thermoplastic resin composition can be used.

[0116] The average particle size of the inorganic particles and the organic particles is preferably 3 μm to 20 μm, more preferably 5 μm to 20 μm. This ensures that the uneven shape can be formed on the surface of the second release layer 2 opposite to the buffer layer 3 .

[0117] In the second release layer 2 having the concavo-convex shape on the surface, the ten-point average roughness (Rz) on the surface is preferably 3 μm or more and 20 μm or less, more preferably 5 μm or more and 17 μm or less, and further preferably 7 μm or more and 17 μm or less. Thus, the above-mentioned function can be more reliably imparted to the second release layer 2. In addition, the ten-point average roughness (Rz) can be measured in accordance with JIS B 0601-1994.

[0118] The storage modulus E'2 of the second release layer 2 having such a structure at 180°C is preferably 60 MPa or more, more preferably 65 MPa or more and 150 MPa or less, further preferably 68 MPa or more and 150 MPa or less, and particularly preferably 70 MPa or more and 100 MPa or less. Thus, by setting the storage modulus E' of the second release layer 2 at 180°C as described above, the storage modulus E' of the release film 10 at 180°C can be set to 30 MPa or more relatively easily.

[0119] Furthermore, the average thickness T2 of the second release layer 2 is preferably 12 μm to 38 μm, more preferably 14 μm to 36 μm, and further preferably 25 μm to 36 μm. Thus, the second release layer 2 can be more reliably provided with the aforementioned function, and the storage modulus E' of the release film 10 at 180° C. can be reliably set to 30 MPa or more.

[0120] The second thermoplastic resin composition constituting the second mold release layer 2 may contain the same additives as those mentioned above for the first thermoplastic resin composition in addition to the aforementioned resin material, inorganic particles, and organic particles.

[0121] Furthermore, in the first release layer 1 and the second release layer 2, the first thermoplastic resin composition and the second thermoplastic resin composition may be the same or different, but are preferably the same or of the same nature from the viewpoint of substitution. Furthermore, in the first release layer 1 and the second release layer 2, the average thickness thereof may be the same or different.

[0122] Here, in the present invention, the average thickness T1 of the first release layer 1 included in the release film 10 is set to 12 μm or more and 38 μm or less, and the storage modulus E′t of the release film 10 at 180° C. is set to 30 MPa or more.

[0123] As described above, when the release film 10 is used to form the FPC 200 using the flexible circuit substrate 210 and the CL film 220, the average thickness of the first release layer 1 pressed into the recess 223 formed in the FPC 200 in the second step is set within the range, and further, the storage modulus E' of the release film 10 as a whole at 180°C is set to be above the lower limit value, thereby enabling the release film 10 to be obtained that exhibits both excellent embedding properties and excellent release properties in a balanced manner.

[0124] Therefore, as described above, when the release film 10 is used to form the FPC 200 using the flexible circuit board 210 and the CL film 220 , in the second step, the adhesive from the adhesive layer 222 can be reliably suppressed or prevented from seeping into the recess 223 formed in the FPC 200 .

[0125] Specifically, under the conditions of 180°C, 11 MPa, and 120 sec, a release film 10 with a width of 270 mm is pressed into a laminate formed by attaching a covering layer film 220 (manufactured by Arisawa Manufacturing Co., Ltd., Japan, "CMA0525") to a flexible circuit substrate 210 having a concave-convex pattern (circuit) with a pitch of 50 μm, a width of 50 μm, and a height of 18 μm, and the adhesive layer 222 possessed by the covering layer film 220 is on the flexible circuit substrate 210 side. When one end of the release film 10 is subsequently grasped and peeled off, the maximum amount of adhesive seepage in the concave portion of the laminate when viewed from above is preferably set to less than 100 μm, and more preferably set to less than 85 μm.

[0126] Furthermore, after forming the FPC 200 in which the flexible circuit substrate 210 and the CL film 220 are bonded via the adhesive layer 222 of the CL film 220 , when the release film 10 is peeled off from the FPC 200 in the third step, creases and breaks in the FPC 200 can be reliably suppressed or prevented.

[0127] Specifically, under the conditions of 180°C, 11 MPa, and 120 seconds, a release film 10 with a width of 270 mm is pressurized and attached to a flexible circuit substrate 210 having projections and depressions (circuits) with a pitch of 50 μm, a width of 50 μm, and a height of 18 μm by a roll-to-roll press machine 100. When the flexible circuit substrate 210 and the release film 10 are peeled off while being conveyed immediately after the pressurization, the limiting peeling speed at which no wrinkles are observed on the release film 10 can be preferably set to 100 mm / second or more, more preferably to 150 mm / second or more, further preferably to 190 mm / second or more, and particularly preferably to 250 mm / second or more.

[0128] As described above, since the maximum oozing amount is set to be equal to or less than the upper limit value and the limiting peeling rate is set to be equal to or more than the lower limit value, it can be said that the release film 10 is a release film that exhibits both excellent embedding properties and release properties in a balanced manner.

[0129] The storage modulus E't of the release film 10 at 180°C may be 30 MPa or more, but is preferably 30 MPa or more and 150 MPa or less. This can provide a release film 10 that exhibits both excellent embedding properties and excellent release properties in a more balanced manner.

[0130] In addition, the storage modulus E't of the release film 10 at 180°C can be obtained as follows: in accordance with JIS K7244-4, a release film 10 with a width of 4 mm and a length of 20 mm is prepared, and a dynamic viscoelasticity measuring device (manufactured by SII NanoTechnology Inc., "DMS6100") is used to measure the film under the conditions of tensile mode, frequency of 1 Hz, and heating rate of 5°C / min.

[0131] Furthermore, the average thickness Tt of the release film 10 is preferably 80 μm or more and 180 μm or less, and more preferably 90 μm or more and 160 μm or less. Furthermore, the relationship between the average thickness Tk of the buffer layer 3 and the average thickness T1 of the first release layer 1, i.e., T1 / Tk, is preferably 0.5 or less, and more preferably 0.3 or more and 0.4 or less. By satisfying these thickness relationships, a release film 10 that further balances both excellent embedding properties and excellent release properties can be obtained.

[0132] In addition, in the present embodiment, the release film 10 is composed of a laminated body formed by stacking a first release layer 1, a buffer layer 3 and a second release layer 2 in sequence, but is not limited to this structure. For example, it can be composed of a laminated body having an intermediate layer such as an adhesive layer arranged between the first release layer 1 and the buffer layer 3 and between the second release layer 2 and the buffer layer 3.

[0133] Furthermore, if the release film 10 can maintain excellent releasability between the glass cloths 300A and 300B and the release film 10 in the third step, the second release layer 2 in contact with the glass cloths 300A and 300B may be omitted.

[0134] As mentioned above, although the manufacturing method of the mold release film and the molded article of this invention was demonstrated, this invention is not limited to these.

[0135] For example, in the above-described embodiment, the mold release film of the present invention is used as a mold release film for roll-to-roll pressing suitable for manufacturing a flexible printed circuit substrate based on a roll-to-roll pressing machine, that is, the cover layer (functional layer) having a through recessed portion is bonded to the flexible circuit substrate (substrate) via an adhesive layer by pressing based on a roll-to-roll method, but the present invention is not limited thereto. Specifically, the mold release film of the present invention can be used even when a functional layer having a through recessed portion is bonded to a substrate via an adhesive layer using a press molding method different from the roll-to-roll method, a vacuum pressure molding method, or the like.

[0136] [Example]

[0137] Hereinafter, the present invention will be described in detail based on examples, but the present invention is not limited thereto.

[0138] 1. Preparation of raw materials

[0139] As raw materials for producing the release film, the following materials were prepared respectively.

[0140] (Thermoplastic resin material)

[0141] Poly 4-methyl-1-pentene resin I (4-methyl-1-pentene / hexadecene / octadecene copolymer, MFR=100g / 10min)

[0142] Poly 4-methyl-1-pentene resin II (4-methyl-1-pentene / decene-1 copolymer, MFR = 180 g / 10 min)

[0143] Poly 4-methyl-1-pentene resin III (4-methyl-1-pentene-decene-1 copolymer, MFR = 9 g / 10 min)

[0144] Poly 4-methyl-1-pentene resin IV (4-methyl-1-pentene / decene-1 copolymer, MFR = 21 g / 10 min)

[0145] Low-density polyethylene (LDPE, manufactured by Ube-Maruzen Polyethlene Co., Ltd., "R500")

[0146] Polypropylene (PP, manufactured by Sumitomo Chemical Co., Ltd., "FH1016")

[0147] Ethylene-methyl methacrylate copolymer (EMMA, manufactured by Sumitomo Chemical Co., Ltd., "WD106")

[0148] Ethylene-methyl acrylate copolymer (EMA, manufactured by DOW-MITSUI POLYCHEMICALS CO., LTD., "ELVALOY AC 1125")

[0149] (Particle material)

[0150] Amorphous silicon dioxide (Si, manufactured by NIPPON STEEL Chemical & Material Co., Ltd., φ12 μm, “SC10-32F”)

[0151] Acrylic beads (manufactured by Soken Chemical & Engineering Co., Ltd., φ10 μm, “MZ-10HN”)

[0152] (Nucleating agent)

[0153] GEL ALL DXR (manufactured by New Japan Chemical Co., Ltd.)

[0154] 2. Production of release film

[0155] <Example 1>

[0156] First, as the first thermoplastic resin composition and the second thermoplastic resin composition, poly-4-methyl-1-pentene resin I was prepared respectively. Furthermore, as the third thermoplastic resin composition, a composition composed of 50 parts by weight of low-density polyethylene (R500), 30 parts by weight of polypropylene (FH1016) and 20 parts by weight of poly-4-methyl-1-pentene resin I was prepared.

[0157] Next, the first thermoplastic resin composition, the third thermoplastic resin composition, and the second thermoplastic resin composition were stacked in a T-die to form a molten resin stack, which was then cooled and solidified to form a stack in which the buffer layer 3 and the second release layer 2 were sequentially stacked on the first release layer 1, thereby obtaining the release film 10 of Example 1. During cooling, the molten resin was sandwiched between a 100°C metal roll with an embossed shape and a 30°C rubber roll with an embossed shape, and the projections and depressions were transferred while cooling.

[0158] In the obtained release film 10 , the first release layer 1 had an average thickness T1 of 25 μm, the buffer layer 3 had an average thickness Tk of 70 μm, and the second release layer 2 had an average thickness T2 of 25 μm.

[0159] The storage modulus E't and storage modulus E'1 of the release film 10 and the first release layer 1 at 180° C. were measured using a dynamic viscoelasticity measuring apparatus (SII NanoTechnology Inc., “DMS6100”), and the results were 34 MPa and 72 MPa, respectively.

[0160] Furthermore, the ten-point average roughness (Rz) of the first release layer 1 and the second release layer 2 on the surface exposed on the side opposite to the buffer layer 3 was measured using a surface roughness measuring device (“SURFTEST SJ-210” manufactured by Mitutoyo Corporation) and the results were 15.8 μm and 10.3 μm, respectively.

[0161] <Example 2 to Example 10, Comparative Example 1 to Comparative Example 4>

[0162] The release films 10 of Examples 2 to 10 and Comparative Examples 1 to 4 were obtained in the same manner as in Example 1, except that the materials shown in Table 1 were used as the first thermoplastic resin composition, the second thermoplastic resin composition, and the third thermoplastic resin composition, and the first release layer 1, the buffer layer 3, and the second release layer 2 having the ten-point average surface roughness (Rz) and the average thickness shown in Table 1 were formed. In Examples 3, 4, and 9 in which particles were included in the first release layer and the second release layer, when the molten resin laminate was cooled, the molten resin was pressed against a metal roll with an embossed shape at 100°C by the wind pressure of an air knife, and the filler was exposed and cooled to form unevenness.

[0163] 3. Evaluation

[0164] The release films 10 of the respective Examples and Comparative Examples were evaluated as follows using a roll-to-roll press machine 100 .

[0165] 3-1. Release properties of release film

[0166] The release film 10 of each embodiment and each comparative example was formed to have a width of 270 mm. The release film 10 was pressed and attached to a flexible circuit substrate 210 having a concave-convex structure with a pitch of 50 μm, a width of 50 μm, and a height of 18 μm by a roll-to-roll press machine 100 under the conditions of 180° C., 11 MPa, and 120 sec. Immediately after the pressing, the flexible circuit substrate 210 and the release film 10 were peeled off by a release bar provided in a demolding mechanism 60 while being conveyed. The limiting peeling speed at which no wrinkles were observed in the release film 10 was measured.

[0167] 3-2. Filling properties of release film

[0168] The release film 10 of each embodiment and each comparative example was formed to have a width of 270 mm. The release film 10 was pressed into a laminate having a concave-convex structure with a pitch of 50 μm, a width of 50 μm, and a height of 18 μm formed by attaching a cover film 220 (manufactured by Arisawa Manufacturing Co., Ltd., Japan, "CMA0525") to a flexible circuit substrate 210 by a roll-to-roll press machine 100 under the conditions of 180°C, 11 MPa, and 120 s, and the adhesive layer 222 of the cover film 220 was on the flexible circuit substrate 210 side. Thereafter, the maximum amount of adhesive exuded from the concave portion of the laminate in a plan view was measured when one end of the release film 10 was peeled off while gripping it.

[0169] 3-3. Summary

[0170] Table 1 shows the evaluation results obtained in 3-1. Releasability of release film and 3-2. Embedding property of release film.

[0171]

[0172] As shown in Table 1, in each example, both the average thickness of the first release layer 1 was 12 μm or more and 38 μm or less and the storage modulus E't of the release film 10 at 180° C. was 30 MPa or more. As a result, the limiting peeling speed was 100 mm / sec or more and the maximum oozing amount of the adhesive was 100 μm or less, showing a balanced combination of excellent embedding property and excellent release property.

[0173] In contrast, in each comparative example, the average thickness of the first release layer 1 is not less than 12 μm and not more than 38 μm, and the storage modulus E't of the release film 10 at 180° C. is not satisfied. Therefore, it is shown that the limiting peeling speed is not less than 100 mm / sec and the maximum oozing amount of the adhesive is not less than 100 μm, and it cannot be said that both excellent embedding property and excellent release property are well-balanced.

[0174] Industrial Applicability

[0175] According to the present invention, a release film having both excellent embedding properties and excellent demoulding properties can be provided in a balanced manner. Therefore, when the release film is used, for example, to form a flexible printed circuit substrate using a flexible circuit substrate and a cover layer film, it is possible to reliably suppress or prevent the adhesive from seeping into the recess formed in the flexible printed circuit substrate. Furthermore, after the flexible printed circuit substrate is formed, when the release film is peeled off from the flexible printed circuit substrate, it is possible to reliably suppress or prevent the generation of creases and fractures in the flexible printed circuit substrate. Therefore, the present invention has industrial applicability.

Claims

1. A release film comprising a first release layer formed from a first thermoplastic resin composition and a buffer layer formed from a third thermoplastic resin composition, It is characterized in that The first thermoplastic resin composition comprises poly 4-methyl-1-pentene resin, The third thermoplastic resin composition comprises a poly 4-methylpentene-1 resin and a polyolefin resin different from the poly 4-methylpentene-1 resin. The average thickness of the first release layer is greater than or equal to 12 μm and less than or equal to 38 μm, and the average thickness of the buffer layer is greater than or equal to 60 μm and less than or equal to 110 μm. When the average thickness of the first release layer is set to T1 μm and the average thickness of the buffer layer is set to Tk μm, T1 / Tk satisfies the relationship of 0.21<T1 / Tk<0.50, The storage modulus E'1 of the first release layer at 180° C. is greater than 70 MPa and less than 95 MPa, and the storage modulus E't of the release film at 180° C. is greater than 30 MPa. Under the conditions of 180° C., 11 MPa, and 120 sec, the release film having a width of 270 mm is pressed and attached to a flexible circuit substrate having a concave-convex structure with a pitch of 50 μm, a width of 50 μm, and a height of 18 μm by a roll-to-roll press machine. When the flexible circuit substrate and the release film are peeled off while conveying immediately after the pressing, the limiting peeling speed at which no wrinkles are observed on the release film becomes 180 mm / sec or more, and Under the conditions of 180°C, 11 MPa, and 120 seconds, the release film with a width of 270 mm is pressed into a laminate formed by attaching a covering layer film of "CMA0525" manufactured by Arisawa Manufacturing Co., Ltd. of Japan to a flexible circuit substrate having projections and depressions with a pitch of 50 μm, a width of 50 μm, and a height of 18 μm, and the adhesive layer possessed by the covering layer film is on the side of the flexible circuit substrate. Then, when one end of the release film is grasped and peeled off, the maximum amount of adhesive seepage in the recessed portion of the laminate when viewed from above becomes less than 85 μm.

2. The release film according to claim 1, in, The average thickness of the release film is 80 μm or more and 180 μm or less.

3. The release film according to claim 1, in, In the first release layer, a ten-point average roughness Rz on a surface on the side opposite to the buffer layer is 3 μm or more and 20 μm or less.

4. The release film according to claim 1, in, When the average thickness of the first release layer is set to T1 μm and the storage modulus E′ of the first release layer at 180° C. is set to E′1 MPa, E′1 / T1 MPa / μm satisfies the relationship of 2.1<E′1 / T1<6.

0.

5. The release film according to claim 1, in, The release film includes a second release layer formed of a second thermoplastic resin composition and laminated on the side of the buffer layer opposite to the first release layer.

6. The release film according to claim 1, in, The release film is used by overlapping the surface of the object formed of a material containing a semi-cured thermosetting resin so that the surface on the first release layer side contacts the surface of the object.

7. A method for manufacturing a molded product, It is characterized in that The method for manufacturing the molded product includes a step of configuring the release film on the object in such a manner that the first release layer of the release film described in any one of claims 1 to 6 becomes the object side, and a step of heating and pressing the object on which the release film is configured, and in the step of configuring the release film, the surface of the side of the object on which the release film is configured is formed by a material containing a thermosetting resin in a semi-cured state.