A method for synergistically optimizing quasi-two-dimensional blue LED devices using two ligands

By leveraging the synergistic effect of two ligands, the phase distribution and defect passivation of the perovskite thin film are improved, solving the problems of low conductivity and low energy transfer efficiency in quasi-two-dimensional blue LED devices and achieving high-performance blue light emission.

CN117560981BActive Publication Date: 2026-11-10JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311775351.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2026-11-10
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

The low conductivity and uneven phase distribution of perovskite thin films in existing quasi-two-dimensional blue LED devices result in low energy transfer efficiency and numerous non-radiative recombination defects, which limit their industrial application.

Method used

High-performance blue LED devices were fabricated by leveraging the synergistic effect of two ligands, (2-carbazole-9-ylethyl)-phosphonic acid and methyl 2-aminopyridine-4-carboxylate, to improve the conductivity of perovskite thin films by enhancing phase distribution and defect passivation.

Benefits of technology

It significantly improves the luminous performance of quasi-two-dimensional blue LED devices, improves phase distribution and conductivity, enhances energy transfer efficiency and carrier mobility, and achieves high-brightness and high-efficiency blue light emission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117560981B_ABST
    Figure CN117560981B_ABST
Patent Text Reader

Abstract

This invention discloses a method for optimizing quasi-two-dimensional blue LED devices using the synergistic effect of two ligands, belonging to the field of light-emitting diode technology. By introducing (2-carbazole-9-ylethyl)phosphonic acid and methyl 2-aminopyridine-4-carboxylate as two ligands, the luminescence performance of perovskite thin films is improved through synergistic effects. (2-carbazole-9-ylethyl)phosphonic acid, as an organophosphonic acid, effectively improves the crystallization process, adjusts the phase distribution, and enhances carrier injection and transport. methyl 2-aminopyridine-4-carboxylate, as a passivating agent, effectively passivates film defects, achieving high-performance emission. Therefore, by using (2-carbazole-9-ylethyl)phosphonic acid and methyl 2-aminopyridine-4-carboxylate as two ligands to synergistically regulate the phase distribution of quasi-two-dimensional perovskite thin films, the energy transfer efficiency is accelerated, and the carrier mobility is improved, thereby enhancing device performance and achieving high-brightness, high-efficiency blue LED device performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of light-emitting diode technology, and more specifically to a method for optimizing quasi-two-dimensional blue LED devices by utilizing two ligands in synergy. Background Technology

[0002] Quasi-two-dimensional metal halide perovskite materials have broad prospects in light-emitting diode (LED) and display applications due to their high photoluminescence quantum yield, tunable optical bandgap, excellent color purity, and low-cost solution processability. However, the photoelectric properties of LEDs using perovskite materials as the emitting layer are still far inferior to those of state-of-the-art organic LEDs. This is mainly because the crystallization process of perovskite thin films is difficult to control, resulting in low conductivity, uneven phase distribution, and excessively low energy transfer efficiency. This leads to too many non-radiative recombination defects, severely restricting the industrial application of perovskite thin films and related devices. For quasi-two-dimensional blue LED devices, achieving blue light emission using quasi-two-dimensional perovskite requires a strong quantum confinement effect, which directly stems from the use of excessive organic cations. Under these conditions, the resulting quasi-two-dimensional thin films exhibit disordered phase distribution and poor conductivity, which is detrimental to light emission. To address these technical problems, a method for synergistically optimizing quasi-two-dimensional blue LED devices using two ligands is proposed. Summary of the Invention

[0003] To address the shortcomings of existing technologies, the purpose of this invention is to provide a method for synergistically optimizing quasi-two-dimensional blue LED devices using two ligands, thereby solving the problems mentioned in the background.

[0004] To achieve the above objectives, the present invention provides the following technical solution:

[0005] A method for optimizing a quasi-two-dimensional blue LED device by utilizing the synergistic effect of two ligands, the method comprising the following steps:

[0006] Step 1: Clean the ITO substrate repeatedly with deionized water, ethanol and acetone, and then clean it with a UV ozone generator for 20 minutes.

[0007] Step 2: Dissolve 36.7 mg lead bromide, 23.0 mg phenylbutylammonium bromide, and 21.3 mg cesium bromide in 1 mL of a polar organic solvent;

[0008] Step 3: Add 2.3 mg of methyl 2-aminopyridine-4-carboxylate and 2.8 mg of (2-carbazole-9-ylethyl)-phosphonic acid to the solution obtained in Step 2.

[0009] Step 4: Add appropriate amounts of the perovskite precursor solutions from Step 2 and 3 to the substrate surface from Step 1, and then spin-coat at 3000 rpm for 120 s to prepare a thin film. After 60 s, add 150 μL of ethyl acetate as an antisolvent to the surface of the perovskite film to rapidly crystallize the film and obtain the original and modified perovskite films. Then, place the above films on a heating stage for subsequent annealing and crystallization.

[0010] Step 5: Place the thin film obtained in step 7 into a vapor deposition apparatus and vapor deposit a 100nm aluminum electrode.

[0011] Step 6: Perform voltage-current curve tests on the devices obtained in Step 8;

[0012] Step 7: PEDOT:PSS(4083) solution was spin-coated onto the substrate surface from Step 6 at 3000 rpm for 30 s, and then annealed at 150 °C.

[0013] Step 8: A toluene solution of PMMA (0.1 mg / mL) was spin-coated onto the substrate surface from Step 11 at 4000 rpm for 60 s, and then annealed at 120 °C.

[0014] Step 9: Add appropriate amounts of the perovskite precursor solutions from Step 2 and 3 to the substrate surface from Step 6, and then spin-coat at 3000 rpm for 120 s to prepare a thin film. After 60 s, add 150 μL of ethyl acetate as an antisolvent to the surface of the perovskite film to rapidly crystallize the film and obtain the original and modified perovskite films. Then, place the above films on a heating stage for subsequent annealing and crystallization.

[0015] Step 10: Place the thin film obtained in step 9 into a vapor deposition apparatus to vapor deposit the electron transport layer and the aluminum electrode;

[0016] Step 11: Perform brightness, voltage, and current tests on the devices obtained in steps 9 and 10 respectively, and calculate the corresponding efficiency.

[0017] As a further embodiment of the present invention, the organic solvent in step 2 can be DMF, DMSO, or a mixture of the two in any proportion.

[0018] As a further embodiment of the present invention, the electron transport material in step 10 is one of TPBi / LiF, TPBi / Liq, Tmpypb / LiF, or Tmpypb / Liq.

[0019] As a further aspect of the present invention, the two ligand materials should be conducive to changing the quasi-two-dimensional blue light phase distribution, passivating defects, and improving electrical conductivity.

[0020] As a further embodiment of the present invention, the concentration ratio between methyl 2-aminopyridine-4-carboxylate and (2-carbazole-9-ylethyl)-phosphonic acid in step 3 is in the range of 5:1 to 1:5.

[0021] Compared with the prior art, the beneficial effects of the present invention are:

[0022] This invention employs (2-carbazole-9-ylethyl)phosphonic acid and methyl 2-aminopyridine-4-carboxylate as two ligand materials. Utilizing the synergistic effect of (2-carbazole-9-ylethyl)phosphonic acid and methyl 2-aminopyridine-4-carboxylate, specifically, after (2-carbazole-9-ylethyl)phosphonic acid and methyl 2-aminopyridine-4-carboxylate form hydrogen bonds, the change in electron cloud density effectively enhances the binding ability of (2-carbazole-9-ylethyl)phosphonic acid to organic cations. This improves the phase distribution and conductivity of the two-dimensional perovskite film, while also enhancing the defect passivation effect of methyl 2-aminopyridine-4-carboxylate on the two-dimensional perovskite film, thereby further improving the luminescent performance of blue light devices. Attached Figure Description

[0023] To more clearly illustrate the structural features and effects of the present invention, the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0024] Figure 1 The image shows a comparison of the photoluminescence spectra of the thin film before and after experimental optimization in an embodiment of the invention.

[0025] Figure 2 This is a comparison diagram of the thin film conductivity before and after experimental optimization in the embodiments of the invention.

[0026] Figure 3 The diagram shows a comparison of the device current density, brightness, and turn-on voltage before and after experimental optimization in the embodiments of the invention.

[0027] Figure 4 This is a comparison chart of the external quantum efficiency of the device before and after experimental optimization in the embodiments of the invention. Detailed Implementation

[0028] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0029] The specific implementation of the present invention will be described in detail below with reference to specific embodiments.

[0030] In one embodiment, a method for synergistically optimizing a quasi-two-dimensional blue LED device using two ligands is described in [reference needed]. Figures 1-4(2-Carbazole-9-ylethyl)phosphonic acid and methyl 2-aminopyridine-4-carboxylate were added as ligands to the perovskite precursor solution and a light-emitting layer film was prepared by spin coating. This improved the phase distribution of the quasi-two-dimensional perovskite, improved the conductivity of the film, and enhanced the hole injection and transport performance, thereby improving the light-emitting performance of the device.

[0031] In one embodiment, see Figures 1-4 A method for optimizing a quasi-two-dimensional blue LED device by utilizing the synergistic effect of two ligands, the method comprising the following steps:

[0032] Step 1: Clean the transparent white glass substrate repeatedly with deionized water, ethanol and acetone, and then clean it with a UV ozone generator for 20 minutes.

[0033] Step 2: Dissolve 36.7 mg lead bromide, 23.0 mg phenylbutylammonium bromide, and 21.3 mg cesium bromide in 1 mL of DMSO solution;

[0034] Step 3: Add 2.3 mg of methyl 2-aminopyridine-4-carboxylate and 2.8 mg of (2-carbazole-9-ylethyl)-phosphonic acid to the solution obtained in Step 2;

[0035] Step 4: Add appropriate amounts of the perovskite precursor solutions from Step 2 and 3 to the substrate surface from Step 2, and then spin-coat at 3000 rpm for 120 s to prepare a thin film. After 60 s, add 150 μL of ethyl acetate as an antisolvent to the surface of the perovskite film to rapidly crystallize the film and obtain the original and modified perovskite films. Then, place the above films on a heating stage for subsequent annealing and crystallization.

[0036] Step 5: Compare the emission spectra of the perovskite films prepared in steps 1-4 with those prepared in steps 1, 3, and 4 to obtain... Figure 1 A comparison of emission spectra.

[0037] Step 6: Clean the ITO substrate repeatedly with deionized water, ethanol and acetone, and then clean it with a UV ozone generator for 20 minutes.

[0038] Step 7: Add appropriate amounts of the perovskite precursor solutions from Step 2 and 3 to the substrate surface from Step 6, and then spin-coat at 3000 rpm for 120 s to prepare a thin film. After 60 s, add 150 μL of ethyl acetate as an antisolvent to the surface of the perovskite film to rapidly crystallize the film and obtain the original and modified perovskite films. Then, place the above films on a heating stage for subsequent annealing and crystallization.

[0039] Step 8: Place the thin film obtained in step 7 into a vapor deposition apparatus and vapor deposit a 100nm aluminum electrode.

[0040] Step 9: Perform voltage-current curve tests on the devices obtained in Step 8 to obtain... Figure 2 The voltage-current curves are shown, and the conductivity is calculated.

[0041] Step 11: PEDOT:PSS(4083) solution was spin-coated onto the substrate surface from Step 6 at 3000 rpm for 30 s, and then annealed at 150 °C.

[0042] Step 12: A toluene solution of PMMA (0.1 mg / mL) was spin-coated onto the substrate surface from Step 11 at 4000 rpm for 60 s, and then annealed at 120 °C.

[0043] Step 13: Add appropriate amounts of the perovskite precursor solutions from Steps 2 and 3 to the substrate surface from Step 6, and then spin-coat at 3000 rpm for 120 s to prepare a thin film. After 60 s, add 150 μL of ethyl acetate as an antisolvent to the surface of the perovskite film to rapidly crystallize the film and obtain the original and modified perovskite films. Then, place the above films on a heating stage for subsequent annealing and crystallization.

[0044] Step 14: Place the thin film obtained in step 13 into a vapor deposition apparatus to vapor deposit the electron transport layer TPBi (45nm) / LiF (1nm) and the aluminum electrode (100nm);

[0045] Step 15: Perform brightness, voltage, and current tests on the devices obtained in steps 13 and 14 respectively, calculate the corresponding efficiencies, and compare them to obtain the results. Figure 3 ,4.

[0046] The total addition concentration of the two ligand materials can be 5%-30% of the corresponding lead bromide concentration, and the concentration ratio between methyl 2-aminopyridine-4-carboxylate and (2-carbazole-9-ylethyl)-phosphonic acid is in the range of 5:1-1:5.

[0047] In this embodiment, (2-carbazole-9-ylethyl)phosphonic acid and methyl 2-aminopyridine-4-carboxylate are introduced as two ligands to improve the luminescence performance of the perovskite thin film through synergistic effects. (2-carbazole-9-ylethyl)phosphonic acid, as an organophosphonic acid, can effectively improve the crystallization process, adjust the phase distribution, and enhance carrier injection and transport. methyl 2-aminopyridine-4-carboxylate, as a passivating agent, can effectively passivate film defects, achieving high-performance emission. Therefore, by using (2-carbazole-9-ylethyl)phosphonic acid and methyl 2-aminopyridine-4-carboxylate as two ligands to synergistically regulate the phase distribution of the quasi-two-dimensional perovskite thin film, the energy transfer efficiency is accelerated, and the carrier mobility is improved, thereby enhancing device performance and achieving high-brightness, high-efficiency blue LED device performance.

[0048] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for optimizing a quasi-two-dimensional blue LED device by utilizing the synergistic effect of two ligands, characterized in that, The method includes the following steps: Step 1: The ITO substrate is repeatedly washed with deionized water, ethanol, and acetone, followed by cleaning with a UV ozone generator for 20 minutes; Step 2: 36.7 mg lead bromide, 23.0 mg phenylbutylammonium bromide, and 21.3 mg cesium bromide are dissolved in 1 mL of an organic polar solvent, which may be DMF, DMSO, or a mixture of both in any proportion; Step 3: 2.3 mg methyl 2-aminopyridine-4-carboxylate and 2.8 mg (2-carbazole-9-ylethyl)-phosphonic acid are added to the solution obtained in Step 2. Step 4 in liquid chromatography: Appropriate amounts of the perovskite precursor solutions from steps 2 and 3 are dropped onto the substrate surface from step 1, and then a thin film is prepared by spin coating at 3000 rpm for 120 seconds. After 60 seconds, 150 μL of ethyl acetate is dropped onto the perovskite film surface as an antisolvent, thereby rapidly crystallizing the film to obtain the original and modified perovskite films. The films are then placed on a heating stage for subsequent annealing and crystallization. Step 5: The film obtained in step 7 is placed in a vapor deposition apparatus to deposit a 100 nm aluminum electrode. Step 6: The device obtained in step 8 is then subjected to... Voltage-current curve testing; Step 7: PEDOT:PSS-4083 solution was spin-coated onto the substrate surface from Step 6 at 3000 rpm for 30 s, and then annealed at 150°C; Step 8: PMMA toluene solution (0.1 mg / mL) was spin-coated onto the substrate surface from Step 11 at 4000 rpm for 60 s, and then annealed at 120°C. The concentration of PMMA toluene solution was 0.1 mg / mL; Step 9: Appropriate amounts of the perovskite precursor solutions from Steps 2 and 3 were added dropwise to... Step 6: The substrate surface is coated with a thin film by spin coating at 3000 rpm for 120 s. After 60 s, 150 μL of ethyl acetate is dropped onto the perovskite film surface as an antisolvent to rapidly crystallize the film and obtain the original and modified perovskite films. The films are then placed on a heating stage for subsequent annealing and crystallization. Step 10: The film obtained in Step 9 is placed in a vapor deposition apparatus to deposit the electron transport layer and aluminum electrode. Step 11: The brightness, voltage, and current of the devices obtained in Steps 9 and 10 are tested and the corresponding efficiencies are calculated.

2. The method for optimizing quasi-two-dimensional blue LED devices using the synergistic effect of two ligands according to claim 1, characterized in that, The organic solvent in step 2 is DMF, DMSO, or a mixture of the two in any proportion.

3. The method for synergistically optimizing a quasi-two-dimensional blue LED device using two ligands according to claim 1, characterized in that, The electron transport material in step 10 is one of TPBi / LiF, TPBi / Liq, Tmpypb / LiF, or Tmpypb / Liq.

4. The method for synergistically optimizing a quasi-two-dimensional blue LED device using two ligands according to claim 1, characterized in that, In step 3, the concentration ratio between methyl 2-aminopyridine-4-carboxylate and (2-carbazole-9-ylethyl)-phosphonic acid is in the range of 5:1 to 1:5.